Method for manufacturing polarizing film
By controlling the degree of drying and the application of the adhesive composition during the polarization film manufacturing process, the problems of bubble generation and decreased adhesion were solved, enabling stable production and high-quality manufacturing of polarization films.
Patent Information
- Application Number
- CN202180008379.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-01-06
AI Technical Summary
In the manufacturing process of polarizing films, existing technologies have difficulty in effectively suppressing bubble generation and ensuring the stability and uniformity of the adhesive layer. In particular, when using active energy ray-cured adhesives, the presence of water can hinder cationic polymerization reactions, leading to a decrease in adhesion.
By applying an easy-to-bond composition containing water and hydrophilic monomers, and an adhesive composition containing free radicals and cationic polymeric compounds to the bonding surfaces of the polarizer and the transparent protective film, respectively, and controlling the degree of drying to meet a specific ratio through online measurement and adjustment of the temperature and airflow of the dryer, the water is fully removed, thus achieving stable bonding.
This enabled continuous and stable production of polarizing films, suppressed bubble formation, and improved the adhesion and water resistance between the polarizer and the transparent protective film, ensuring the appearance quality of the polarizing films.
Smart Images

Figure CN114930211B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a polarizing film having a transparent protective film disposed on at least one side of a polarizer via an adhesive layer. The polarizing film can be used alone to form an image display device such as a liquid crystal display (LCD), an organic EL display device, a CRT, a PDP, or the like, or in the form of an optical film laminated with the polarizing film to form an image display device such as a liquid crystal display (LCD), an organic EL display device, a CRT, a PDP, or the like. Background Art
[0002] Liquid crystal display devices are rapidly expanding in the market for watches, mobile phones, PDAs, notebook computers, computer monitors, DVD players, TVs, etc. Liquid crystal display devices are devices that visualize the polarization state of liquid crystal switches, and use polarizers based on their display principles. In particular, in applications such as TVs, high brightness, high contrast, and wide viewing angles are increasingly required, and polarizing films are increasingly required to have high transmittance, high polarization degree, and high color reproducibility.
[0003] As a polarizer, the most widely used one is an iodine-based polarizer having a structure in which iodine is adsorbed on polyvinyl alcohol (hereinafter also referred to as "PVA") and stretched, from the perspective of having high transmittance and high polarization degree. In general, a polarizing film uses a polarizing film in which a transparent protective film is bonded to both sides of the polarizer using a so-called aqueous adhesive made by dissolving a polyvinyl alcohol-based material in water (Patent Document 1 below). As the transparent protective film, triacetyl cellulose with high moisture permeability is used. When the above-mentioned aqueous adhesive is used (so-called wet lamination), a drying process is required after bonding the polarizer and the transparent protective film.
[0004] On the other hand, active energy ray-curable adhesives have been proposed as an alternative to the aqueous adhesives. When a polarizing film is produced using an active energy ray-curable adhesive, a drying step is not required, and thus the productivity of the polarizing film can be improved.
[0005] For example, Patent Document 2 proposes an active energy ray-curable adhesive composition that can bond a polyvinyl alcohol film to a plastic film simply and with sufficient strength, the composition comprising: (A) a (meth) acrylic free radical polymerizable compound, (B) a cationically polymerizable compound, (C) a photoradical polymerization initiator, and (D) a photocationic polymerization initiator.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2001-296427
[0009] Patent Document 2: Japanese Patent No. 5046721 Summary of the invention
[0010] Problems to be solved by the invention
[0011] In recent years, in the field of optical films such as polarizing films, displays have been thinned and refined, requiring more stringent appearance quality. In such a case, a countermeasure is needed to suppress the generation of bubbles when the polarizer and the protective film are bonded with an adhesive. As a countermeasure to suppress the generation of bubbles, increasing the coating thickness of the adhesive and reducing the viscosity of the adhesive are effective, but if the coating thickness of the adhesive is increased, there is a problem of discoloration after humidification. In addition, the low viscosity of the adhesive has the problem of increasing the restrictions on meeting optical properties and adhesion.
[0012] In addition, as a method of reducing the viscosity of the adhesive, it is effective to mix water, which is a non-hazardous substance, with the adhesive. However, in the case of a cationic polymerization type adhesive as described in Patent Document 2, water has the problem of inhibiting the cationic polymerization reaction.
[0013] The present invention solves the above-mentioned problems, and an object of the present invention is to provide a method for continuously and stably producing a polarizing film having excellent adhesion between a polarizer and a transparent protective film and an adhesive layer and in which the generation of bubbles is suppressed.
[0014] Solutions to the problem
[0015] The above-mentioned problems can be solved by the following configuration.
[0016] That is, the present invention relates to a method for manufacturing a polarizing film, wherein a transparent protective film is provided on at least one side of a polarizer via an adhesive layer, the method comprising:
[0017] A first coating step of coating a bonding surface of the polarizer with an easily adhesive composition containing water and a hydrophilic monomer to form a wet first coating film while the polarizer is being conveyed;
[0018] a second coating step of coating an adhesive composition containing a radical polymerizable compound and a cation polymerizable compound on the bonding surface of the transparent protective film while the transparent protective film is being conveyed to form a second coating film;
[0019] a first thickness measuring step of measuring the thickness of the wet first coating film online;
[0020] After the first thickness measuring step, a drying step of removing water from the wet first coating film using a dryer to form a dry first coating film;
[0021] After the drying step, a second thickness measuring step of measuring the thickness of the dried first coating film online;
[0022] A drying degree adjusting step of adjusting the degree of dryness of the newly formed dry first coating film by adjusting the temperature and / or air volume of the drying machine in such a manner that the ratio of the thickness of the wet first coating film obtained by the online measurement to the thickness of the dry first coating film satisfies the following formula (A);
[0023] a laminating step of laminating the dried first coating film formed on the laminating surface of the polarizer and the second coating film formed on the laminating surface of the transparent protective film to form an uncured adhesive layer; and
[0024] a bonding step of bonding the polarizer and the transparent protective film together via the adhesive layer obtained by curing the uncured adhesive layer,
[0025] (Thickness of dry first coating film / Thickness of wet first coating film)-(Content ratio of water in the easy-adhesion composition)≤0.05 (A).
[0026] In the method for producing a polarizing film, it is preferred that the easy-adhesion composition contains a compound represented by the following general formula (1) and / or an organic metal compound having an MO bond in the structural formula:
[0027] [Chemical formula 1]
[0028]
[0029] (In formula (1), X is a functional group containing a reactive group, R 1 and R 2 (a) and (b) are each independently a hydrogen atom, an aliphatic hydrocarbon group, an aryl group or a heterocyclic group, and the aliphatic hydrocarbon group, the aryl group and the heterocyclic group may have a substituent. It should be noted that in the present invention, the compound represented by the above general formula (1) is also referred to as a "boron-containing compound".
[0030] In the method for producing a polarizing film, the compound represented by the general formula (1) is preferably a compound represented by the following general formula (1'):
[0031] [Chemical formula 2]
[0032]
[0033] (In formula (1'), Y is an organic group, X, R 1 and R 2 Same meaning as above).
[0034] In the above-mentioned method for manufacturing the polarizing film, the reactive group possessed by the compound represented by the above-mentioned general formula (1) is preferably at least one reactive group selected from α,β-unsaturated carbonyl group, vinyl group, vinyl ether group, epoxy group, oxetane group, amino group, aldehyde group, mercapto group and halogen group.
[0035] In the method for producing a polarizing film, it is preferred that the polarizer has a moisture content of 15% by mass or less.
[0036] In the method for producing a polarizing film, it is preferable that the first coating step and the second coating step are coating steps using a post-measurement coating method.
[0037] In the method for producing a polarizing film, it is preferable that the post-measurement coating method is a gravure roll coating method using a gravure roll.
[0038] Effects of the Invention
[0039] The method for manufacturing a polarizing film of the present invention is characterized in that water for suppressing the generation of bubbles by lowering the viscosity is added to the easy-to-bond composition applied to the bonding surface of the polarizer, and on the other hand, a free radical polymerizing compound and a cationically polymerizing compound are contained in the adhesive composition applied to the bonding surface of the transparent protective film in order to improve the adhesion.
[0040] In the continuous production of polarizing films, when water remains in the first coating film obtained by applying the above-mentioned easy-bonding composition on the bonding surface of the polarizer, water remains in the uncured adhesive layer obtained by bonding the first coating film and the second coating film obtained by applying the above-mentioned adhesive composition. As a result, the undesirable situation that the cationic polymerization reaction of the uncured adhesive layer is hindered occurs, and the adhesion of the adhesive layer is reduced. Therefore, the water in the first coating film needs to be removed in the drying process. It can be imagined that in the drying process, the initial set temperature and set air volume of the dryer are determined based on the amount of water formulated in the easy-bonding composition, and the water in the first coating film is fully removed to a degree that does not hinder the cationic polymerization reaction according to the initially set drying conditions.
[0041] However, due to various main reasons such as deterioration and damage of the drying equipment piping, blockage of the exhaust port, and temperature changes in the surrounding environment, the drying degree of the first coating film may deviate during the continuous production of the polarizing film, and sometimes the water in the first coating film is not fully removed, and a large amount of water remains in the first coating film after the drying process. As a result, as described above, the cationic polymerization reaction of the uncured adhesive layer may be hindered by the remaining water, making it difficult to stably form an adhesive layer with uniform adhesive properties, and it is difficult to continuously and stably manufacture a polarizing film with excellent adhesiveness.
[0042] According to the method for manufacturing a polarizing film of the present invention, the temperature and / or air volume of the dryer are adjusted in such a way that the ratio of the thickness of the wet first coating film obtained by online measurement to the thickness of the dry first coating film satisfies the above formula (A), and the degree of dryness of the newly formed dry first coating film is adjusted, thereby being able to continuously and stably form a dry first coating film with a small deviation in the degree of dryness and with water fully removed. In this way, it is possible to prevent the undesirable situation that the cationic polymerization reaction of the uncured adhesive layer is hindered by the remaining water, and it is possible to continuously and stably form an adhesive layer with uniform adhesive properties.
[0043] As described above, according to the method for producing a polarizing film of the present invention, a polarizing film having excellent adhesion between the polarizer and the transparent protective film and the adhesive layer and having suppressed generation of bubbles and having a high appearance quality can be produced continuously and stably.
[0044] It is preferred that the above-mentioned easy-adhesion composition contains the above-mentioned boron-containing compound. The above-mentioned boron-containing compound can react with functional groups such as hydroxyl groups possessed by the polarizer, thereby improving the adhesion between the polarizer and the adhesive layer, and as a result, the effect of improving the water-resistant adhesion of the polarizing film can be exerted. Among them, when the moisture content of the polarizer is low, for example, when the moisture content of the polarizer is less than 15% by mass, there is a situation where the boron-containing compound and the functional groups possessed by the polarizer cannot fully react and the above-mentioned effect cannot be fully obtained. However, even in the case where the moisture content of the polarizer is low, since the easy-adhesion composition contains water, the reactivity of the boron-containing compound to the functional groups possessed by the polarizer can be improved, thereby improving the adhesion between the polarizer and the adhesive layer. As a result, even in the case where the moisture content of the polarizer is low, the improvement of the water-resistant adhesion of the polarizing film, the improvement of the coating properties of the easy-adhesion composition, and the suppression of bubble generation in the polarizing film can be achieved.
[0045] Preferably, the above-mentioned easy-adhesion composition contains the above-mentioned organometallic compound. The above-mentioned organometallic compound becomes an active metal species through the inclusion of water, and as a result, the organometallic compound can form a strong bond with the polarizer. However, the above-mentioned organometallic compound has multiple reaction points, and therefore, the organometallic compound that reacts with the polarizer also has unreacted points. Moreover, the above-mentioned organometallic compound can form a strong bond with the curable component in the second coating film formed on the bonding surface of the transparent protective film. As described above, since the above-mentioned organometallic compound can form a strong bond with both the polarizer and the adhesive layer, the water-resistant adhesion between the polarizer and the adhesive layer is greatly improved.
[0046] The first coating process and the second coating process are preferably coating processes using a post-measurement coating method. As a result, the adhesion of the polarizing film can be improved, and the coating properties when the easy-to-adhesive composition and the adhesive composition are applied can be improved, and the thickness uniformity of the first coating film and the second coating film can be improved. It should be noted that in the present invention, the "post-measurement coating method" refers to a method of applying an external force to the liquid film to remove excess liquid to obtain a given coating film thickness. Specific examples of the post-measurement coating method include a gravure roller coating method, a forward roller coating method, an air knife coating method, a rod / rod coating method, and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 This is a schematic diagram showing an example of the method for producing the polarizing film of the present invention.
[0048] Explanation of symbols
[0049] 1: Polarizing film
[0050] 2: Polarizer
[0051] 3: Transparent protective film
[0052] 4, 5: Coating machine
[0053] 6, 8: Film thickness tester
[0054] 7: Dryer
[0055] 9: Roller Laminator DETAILED DESCRIPTION
[0056] The present invention relates to a method for producing a polarizing film in which a transparent protective film is provided on at least one side of a polarizer via an adhesive layer, the method comprising:
[0057] A first coating step of coating a bonding surface of the polarizer with an easily adhesive composition containing water and a hydrophilic monomer to form a wet first coating film while the polarizer is being conveyed;
[0058] a second coating step of coating an adhesive composition containing a radical polymerizable compound and a cation polymerizable compound on the bonding surface of the transparent protective film while the transparent protective film is being conveyed to form a second coating film;
[0059] a first thickness measuring step of measuring the thickness of the wet first coating film online;
[0060] After the first thickness measuring step, a drying step of removing water from the wet first coating film using a dryer to form a dry first coating film;
[0061] After the drying step, a second thickness measuring step of measuring the thickness of the dried first coating film online;
[0062] A drying degree adjusting step of adjusting the degree of dryness of the newly formed dry first coating film by adjusting the temperature and / or air volume of the drying machine in such a manner that the ratio of the thickness of the wet first coating film obtained by the online measurement to the thickness of the dry first coating film satisfies the following formula (A);
[0063] a laminating step of laminating the dried first coating film formed on the laminating surface of the polarizer and the second coating film formed on the laminating surface of the transparent protective film to form an uncured adhesive layer; and
[0064] A bonding step of bonding the polarizer and the transparent protective film together via the adhesive layer obtained by curing the uncured adhesive layer.
[0065] (Thickness of dry first coating film / Thickness of wet first coating film) - (Content ratio of water in the adhesive composition) ≤ 0.05 (A)
[0066] Hereinafter, the method for producing the polarizing film of the present invention will be described in detail.
[0067] <Easy-adhesion composition>
[0068] The easy-adhesion composition contains at least water and a hydrophilic monomer.
[0069] The hydrophilic monomer is not particularly limited as long as it is a monomer soluble in water, and examples thereof include: carboxyl group-containing monomers such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, fumaric acid, maleic acid, citraconic acid, monobutyl hydroxyfumarate, and monobutyl hydroxyitaconate, and salts thereof; 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, diethylene glycol mono(meth)acrylate, triethylene glycol mono(meth)acrylate, and polyethylene glycol mono(meth)acrylate. Hydroxyl-containing monomers such as esters; acrylamide monomers such as (meth)acrylamide, diacetone acrylamide, and N-hydroxymethyl (meth)acrylamide; heterocyclic (meth)acrylamide derivatives such as N-acryloylmorpholine, N-acryloylpiperidine, N-methacryloylpiperidine, and N-acryloylpyrrolidine; both end ester compounds of ethylene glycol oligomers such as diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate; both end ester compounds of propylene glycol oligomers, etc. They can be used alone or in combination of two or more. Among these, hydroxyl-containing monomers are preferably used.
[0070] The content of the hydrophilic monomer in the adhesive composition is not particularly limited, but is preferably 20% by mass or more, more preferably 40% by mass or more, and preferably 80% by mass or less, more preferably 65% by mass or less, from the viewpoint of improving adhesion.
[0071] The easy-adhesion composition may contain an SP value of 21.0 (MJ / m 3 ) 1 / 2 Above and 26.0 (MJ / m 3 ) 1 / 2 The following polymerizable compound X serves as a curable component.
[0072] The polymerizable compound X has a radical polymerizable group such as a (meth)acrylate group and an SP value of 21.0 (MJ / m 3 ) 1 / 2 Above and 26.0 (MJ / m 3 ) 1 / 2 The following compounds can be used without limitation. Examples of polymerizable compound X include N-methoxymethyl acrylamide (SP value 22.9), N-ethoxymethyl acrylamide (SP value 22.3), etc. It should be noted that commercially available products can also be used as polymerizable compound X, such as Wasmer2MA (manufactured by Kasano Kosan Co., Ltd., SP value 22.9), Wasmer EMA (manufactured by Kasano Kosan Co., Ltd., SP value 22.3), Wasmer3MA (manufactured by Kasano Kosan Co., Ltd., SP value 22.4), etc. They can be used alone or in combination of two or more.
[0073] Here, the calculation method of the SP value (solubility parameter) in the present invention is described below.
[0074] (Calculation method of solubility parameter (SP value))
[0075] In the present invention, the solubility parameter (SP value) of the polymerizable compound X is calculated by the calculation method of Fedors [see "Polymer Eng. & Sci.", Vol. 14, No. 2 (1974), pp. 148-154].
[0076] [Mathematical formula 1]
[0077]
[0078] (where Δei is the evaporation energy attributable to an atom or group at 25°C, and Δvi is the molar volume at 25°C).
[0079] In the above mathematical formula, Δei and Δvi represent certain numerical values assigned to i atoms and groups in the main molecule. In addition, representative examples of numerical values of Δe and Δv assigned to atoms or groups are shown in Table 1 below.
[0080] [Table 1]
[0081] Atom or group Δe(J / mol) <![CDATA[Δv(cm 3 / mol)]]> <![CDATA[CH 3 ]]> 4086 33.5 C 1465 -19.2 Phenyl 31940 71.4 Phenylene 31940 52.4 COOH 27628 28.5 <![CDATA[CONH 2 ]]> 41861 17.5 <![CDATA[NH 2 ]]> 12558 19.2 -N= 11721 5.0 CN 25535 24.0 <![CDATA[NO 2 (Fatty Acids)]]> 29302 24.0 <![CDATA[NO 3 (Aromatic)]]> 15363 32.0 O 3349 3.8 OH 29805 10.0 S 14149 12.0 F 4186 18.0 C1 11553 24.0 Br 15488 30.0
[0082] The content of the polymerizable compound X in the easy-adhesion composition is not particularly limited, but is preferably 0.5% by mass or less.
[0083] Furthermore, the easy-adhesion composition preferably contains a compound represented by the following general formula (1).
[0084] [Chemical formula 3]
[0085]
[0086] (In formula (1), X is a functional group containing a reactive group, R 1 and R 2 Each independently represents a hydrogen atom, an aliphatic hydrocarbon group which may have a substituent, an aryl group or a heterocyclic group). Examples of the aliphatic hydrocarbon group include a linear or branched alkyl group having 1 to 20 carbon atoms which may have a substituent, a cyclic alkyl group having 3 to 20 carbon atoms which may have a substituent, and an alkenyl group having 2 to 20 carbon atoms. Examples of the aryl group include a phenyl group having 6 to 20 carbon atoms which may have a substituent, a naphthyl group having 10 to 20 carbon atoms which may have a substituent, and the like. Examples of the heterocyclic group include a 5-membered ring or a 6-membered ring group which contains at least one heteroatom and may have a substituent. They may be linked to each other to form a ring. In the general formula (1), R 1 and R 2 , preferably a hydrogen atom, a linear or branched alkyl group having 1 to 3 carbon atoms, and most preferably a hydrogen atom. It should be noted that the compound represented by general formula (1) may be present in the final adhesive layer in an unreacted state or in a state where each functional group has reacted.
[0087] X in the compound represented by the general formula (1) is a functional group containing a reactive group, which is a functional group capable of reacting with the curable component constituting the adhesive layer. Examples of the reactive group contained in X include a hydroxyl group, an amino group, an aldehyde group, a carboxyl group, a vinyl group, a (meth)acryloyl group, a styryl group, a (meth)acrylamide group, a vinyl ether group, an epoxy group, an oxetanyl group, an α,β-unsaturated carbonyl group, a mercapto group, and a halogen group. In the case where the adhesive composition constituting the adhesive layer is active energy ray curable, the reactive group contained in X is preferably at least one reactive group selected from vinyl, (meth) acryloyl, styryl, (meth) acrylamide, vinyl ether, epoxy, oxetane and mercapto. In particular, since the adhesive composition of the present invention constituting the adhesive layer is free radical polymerizable, the reactive group contained in X is preferably at least one reactive group selected from (meth) acryloyl, styryl and (meth) acrylamide. In the case where the compound represented by the general formula (1) has a (meth) acrylamide group, the reactivity is high and the copolymerization rate with the active energy ray adhesive composition is improved, which is more preferred. In addition, the (meth) acrylamide group has high polarity and excellent adhesion, and therefore, it is also preferred from the perspective of efficiently obtaining the effect of the present invention. In addition, since the adhesive composition of the present invention constituting the adhesive layer is cationically polymerizable, the reactive group contained in X preferably has at least one functional group selected from the group consisting of a hydroxyl group, an amino group, an aldehyde group, a carboxyl group, a vinyl ether group, an epoxy group, an oxetanyl group, and a mercapto group. In particular, when an epoxy group is included, the adhesive layer obtained has excellent adhesion to the adherend, which is preferred. When a vinyl ether group is included, the adhesive composition has excellent curing properties, which is preferred.
[0088] Preferred specific examples of the compound represented by the general formula (1) include compounds represented by the following general formula (1'):
[0089] [Chemical formula 4]
[0090]
[0091] (In formula (1'), Y is an organic group, X, R 1 and R 2 The same meaning as above). Further preferred examples include the following compounds (1a) to (1d).
[0092] [Chemical formula 5]
[0093]
[0094] In the present invention, the compound represented by the general formula (1) may be a compound in which a reactive group is directly bonded to a boron atom, but as shown in the above specific examples, the compound represented by the general formula (1) is preferably a compound in which a reactive group is bonded to a boron atom via an organic group, that is, preferably a compound represented by the general formula (1'). In the case where the compound represented by the general formula (1) is a compound bonded to a reactive group, for example, via an oxygen atom bonded to a boron atom, there is a tendency for the water-resistant adhesion of the polarizing film to deteriorate. On the other hand, when the compound represented by the general formula (1) does not have a boron-oxygen bond, but is bonded to an organic group via a boron atom, has a boron-carbon bond, and contains a reactive group (when it is the general formula (1')), the water-resistant adhesion of the polarizing film is improved, and thus it is preferred. The organic group specifically refers to an organic group having 1 to 20 carbon atoms which may have a substituent, and more specifically, for example, a linear or branched alkylene group having 1 to 20 carbon atoms which may have a substituent, a cyclic alkylene group having 3 to 20 carbon atoms which may have a substituent, a phenylene group having 6 to 20 carbon atoms which may have a substituent, and a naphthylene group having 10 to 20 carbon atoms which may have a substituent.
[0095] Examples of the compound represented by the general formula (1) include, in addition to the compounds exemplified above, esters of (meth)acrylic acid esters with boric acid, such as esters of hydroxyethylacrylamide with boric acid, esters of hydroxymethylacrylamide with boric acid, esters of hydroxyethyl acrylate with boric acid, and esters of hydroxybutyl acrylate with boric acid.
[0096] In the easy-adhesion composition, when the content of the compound represented by the general formula (1) is too small, the proportion of the compound represented by the general formula (1) present at the interface between the polarizer and the adhesive layer is sometimes reduced, and the easy-adhesion effect becomes low. Therefore, in the easy-adhesion composition, the content of the compound represented by the general formula (1) is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, further preferably 0.1% by mass or more, and particularly 0.5% by mass or more. In addition, in the easy-adhesion composition, the content of the compound represented by the general formula (1) is usually 5% by mass or less, preferably 3% by mass or less, and more preferably 2% by mass or less.
[0097] In addition, the easy-adhesion composition preferably contains an organic metal compound having a MO bond (M is silicon, titanium, aluminum or zirconium, and O is an oxygen atom) in the structural formula. It should be noted that the above-mentioned organic metal compound may exist in an unreacted state in the adhesive layer finally formed, or may exist in a state in which each functional group has reacted.
[0098] The organometallic compound has a MO bond in the structural formula (M is silicon, titanium, aluminum or zirconium, and O is an oxygen atom). The organometallic compound is preferably at least one selected from the group consisting of an organosilicon compound, a metal alkoxide, and a metal chelate.
[0099] As the above-mentioned organosilicon compound, an organosilicon compound having a Si-O bond can be used without particular limitation, and as a specific example, an organosilicon compound that is curable by active energy rays or an organosilicon compound that is not curable by active energy rays can be cited. It is particularly preferred that the number of carbon atoms of the organic group possessed by the organosilicon compound is 3 or more. As specific examples of active energy ray-curable compounds, vinyl trichlorosilane, vinyl trimethoxysilane, vinyl triethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, 3-glycidoxypropyl trimethoxysilane, 3-glycidoxypropyl methyl diethoxysilane, 3-glycidoxypropyl triethoxysilane, p-phenylene trimethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl methyl diethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-acryloxypropyl trimethoxysilane, etc. can be cited.
[0100] 3-Methacryloxypropyltrimethoxysilane and 3-acryloxypropyltrimethoxysilane are preferred.
[0101] As the inactive energy ray-curable compound, a compound having an amino group is preferred. Specific examples of the compound having an amino group include γ-aminopropyl trimethoxysilane, γ-aminopropyl triethoxysilane, γ-aminopropyl triisopropoxysilane, γ-aminopropyl methyl dimethoxysilane, γ-aminopropyl methyl diethoxysilane, γ-(2-aminoethyl) aminopropyl trimethoxysilane, γ-(2-aminoethyl) aminopropyl methyl dimethoxysilane, γ-(2-aminoethyl) aminopropyl triethoxysilane, γ-(2-aminoethyl) aminopropyl methyl diethoxysilane, γ-(2-aminoethyl) aminopropyl triisopropoxysilane, γ-(2-(2-aminoethyl) aminoethyl) aminopropyl trimethoxysilane, γ-(6-aminohexyl) aminopropyl trimethoxysilane, Amino group-containing silanes such as 3-(N-ethylamino)-2-methylpropyltrimethoxysilane, γ-ureidopropyltrimethoxysilane, γ-ureidopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-benzyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, N-cyclohexylaminomethyltriethoxysilane, N-cyclohexylaminomethyldiethoxymethylsilane, N-phenylaminomethyltrimethoxysilane, (2-aminoethyl)aminomethyltrimethoxysilane, and N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine; ketimine-type silanes such as N-(1,3-dimethylbutylene)-3-(triethoxysilyl)-1-propylamine.
[0102] The compound having an amino group may be used alone or in combination. Among these, in order to ensure good adhesion, preferred are γ-aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropylmethyldiethoxysilane, and N-(1,3-dimethylbutylene)-3-(triethoxysilyl)-1-propylamine.
[0103] Specific examples of inactive energy ray-curable compounds other than the above include 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatepropyltriethoxysilane, and imidazole silane.
[0104] The metal alkoxide is a compound in which at least one alkoxy group as an organic group is bonded to a metal, and the metal chelate is a compound in which an organic group is bonded or coordinated to a metal via an oxygen atom. As the metal, titanium, aluminum, and zirconium are preferred. Among them, aluminum and zirconium are more reactive than titanium, and there is a case where the pot life of the adhesive composition is shortened and the effect of improving the water-resistant adhesion is reduced. Therefore, from the viewpoint of improving the water-resistant adhesion of the adhesive layer, titanium is more preferred as the metal of the organic metal compound.
[0105] When the easy-adhesion composition contains a metal alkoxide as an organic metal compound, the metal alkoxide used is preferably a metal alkoxide having an organic group with carbon atoms of 3 or more, more preferably 6 or more. When the carbon number is 2 or less, the pot life of the easy-adhesion composition may be shortened and the effect of improving water-resistant adhesion may be reduced. As an organic group with carbon atoms of 6 or more, for example, octyloxy can be mentioned, which can be suitably used. Suitable metal alkoxides include, for example, tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, tetraoctyl titanate, tert-amyl titanate, tetra-tert-butyl titanate, tetrastearyl titanate, zirconium tetraisopropoxide, zirconium tetra-n-butoxide, zirconium tetraoctoxide, zirconium tetra-tert-butoxide, zirconium tetrapropoxide, aluminum sec-butoxide, aluminum ethoxide, aluminum isopropylate, aluminum butyrate, aluminum diisopropylate monosecondarybutyrate, monosec-butoxyaluminum diisopropylate, etc. Among them, tetraoctyl titanate is preferred.
[0106] When the easy-adhesion composition contains a metal chelate as an organic metal compound, it is preferred that the metal chelate contains an organic group having carbon atoms of 3 or more. When the carbon number is 2 or less, the pot life of the easy-adhesion composition is shortened and the effect of improving the water-resistant adhesion of the polarizing film is reduced. Examples of the organic group having carbon atoms of 3 or more include acetylacetonate, ethyl acetoacetate, isostearate, and octanediol ester. Among these, from the viewpoint of improving the water-resistant adhesion of the adhesive layer, acetylacetonate or ethyl acetoacetate is preferred as the organic group. Examples of suitable metal chelates include titanium acetylacetonate, titanium octanediol, titanium tetraacetylacetonate, titanium ethyl acetoacetate, titanium polyhydroxystearate, dipropoxy titanium bisacetylacetonate, dibutoxy bis(octanediol ester) titanium, dipropoxy bis(ethyl acetoacetate) titanium, titanium lactate, titanium diethanolamine, titanium triethanolamine, dipropoxy bis(lactate) titanium, dipropoxy bis(triethanolamine) titanium, di-n-butoxy bis(triethanolamine) titanium, tri-n-butoxy titanium monostearate, diisopropoxy bis(ethyl acetoacetate) titanium, diisopropoxy bis(acetoacetate) titanium, diisopropoxy bis(acetylacetone) titanium, titanium phosphate compounds, titanium ammonium lactate, 1,3-propanedioxy titanium bis(ethyl acetoacetate), titanium dodecylbenzenesulfonate Compounds, aminoethylaminoethanol titanium, tetraacetylacetonate zirconium, monoacetylacetonate zirconium, diacetylacetonate zirconium, diacetylacetonate zirconium ethyl acetoacetate, zirconium acetate, tri-n-butoxyethyl acetoacetate zirconium, di-n-butoxybis(ethyl acetoacetate) zirconium, n-butoxytris(ethyl acetoacetate) zirconium, tetra(n-propyl acetoacetate) zirconium, tetra(acetylacetoacetate) zirconium, tetra(ethyl acetoacetate) zirconium, ethyl acetoacetate aluminum, acetylacetonate aluminum, diacetylacetonate aluminum, diisopropoxyethyl acetoacetate aluminum, diisopropoxy acetylacetonate aluminum, isopropoxybis(ethyl acetoacetate) aluminum, isopropoxybis(acetylacetonate) aluminum, tris(ethyl acetoacetate) aluminum, tris(acetylacetonate) aluminum, monoacetylacetonate bis(ethyl acetoacetate) aluminum. Among them, titanium acetylacetonate and titanium acetylacetate are preferred.
[0107] Examples of the organic metal compound that can be used in the present invention include, in addition to the above, organic carboxylic acid metal salts such as zinc octylate, zinc laurate, zinc stearate, and tin octylate; and zinc chelate compounds such as zinc acetylacetonate chelate, zinc benzoylacetonate chelate, zinc dibenzoylmethane chelate, and ethyl acetoacetate zinc chelate.
[0108] In the easy-adhesion composition, when the content of the organic metal compound is too small, the proportion of the organic metal compound present at the interface between the polarizer and the adhesive layer decreases, and there is a case where the easy-adhesion effect becomes lower. Therefore, in the easy-adhesion composition, the content of the organic metal compound is preferably 0.01 mass % or more, more preferably 0.05 mass % or more, and further preferably 0.1 mass % or more. In addition, in the easy-adhesion composition, the content of the organic metal compound is usually 10 mass % or less.
[0109] The easy-adhesion composition contains water as a solvent. An organic solvent may be blended into the easy-adhesion composition within a range not impairing the effects of the present invention, but it is preferred that no organic solvent be blended.
[0110] The easy-adhesion composition may contain additives.
[0111] Examples of the additives include binder resins, surfactants, plasticizers, tackifiers, low molecular weight polymers, polymerizable monomers, surface lubricants, leveling agents, antioxidants, preservatives, light stabilizers, ultraviolet absorbers, polymerization inhibitors, silane coupling agents, titanium coupling agents, inorganic or organic fillers, metal powders, particles, foils, and the like.
[0112] <Adhesive composition>
[0113] The adhesive composition of the present invention may be thermosetting or active energy ray-curable. As resins constituting thermosetting adhesive compositions, polyvinyl alcohol resins, epoxy resins, unsaturated polyesters, urethane resins, acrylic resins, urea resins, melamine resins, phenolic resins, etc. may be cited, and curing agents may be combined as needed. As resins constituting thermosetting adhesive compositions, polyvinyl alcohol resins and epoxy resins are more preferably used. As active energy ray-curable adhesive compositions, the classification based on active energy rays can be roughly divided into electron beam curing, ultraviolet curing, and visible light curing. In addition, as a classification based on curing reactions, free radical polymerizable adhesive compositions and cationic polymerizable adhesive compositions can be divided. In the present invention, free radical polymerizable and cationic polymerizable adhesive compositions are used. It should be noted that in the present invention, active energy rays in the wavelength range of 10nm to less than 380nm are recorded as ultraviolet rays, and active energy rays in the wavelength range of 380nm to 800nm are recorded as visible light.
[0114] In the method for producing a polarizing film of the present invention, the adhesive composition is preferably active energy ray-curable, and particularly preferably visible light-curable by visible light of 380 nm to 450 nm.
[0115] The adhesive composition of the present invention contains at least a radical polymerizable compound and a cation polymerizable compound.
[0116] The free radical polymerizable compound can be exemplified by compounds having free radical polymerizable functional groups of carbon-carbon double bonds such as (meth)acryloyl and vinyl. Any of monofunctional free radical polymerizable compounds or polyfunctional free radical polymerizable compounds having difunctionality or higher can be used. In addition, these free radical polymerizable compounds can be used alone or in combination of two or more. As these free radical polymerizable compounds, compounds having, for example, a (meth)acryloyl group are preferred. It should be noted that in the present invention, (meth)acryloyl refers to acryloyl and / or methacryloyl, and "(meth)" has the same meaning below.
[0117] Examples of the monofunctional radical polymerizable compound include compounds represented by the following general formula (2).
[0118] [Chemical formula 6]
[0119]
[0120] (Where R 3 is a hydrogen atom or a methyl group, R 4 and R 5 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group or a cyclic ether group, R 4 and R 5 The number of carbon atoms in the alkyl group, hydroxyalkyl group, and / or alkoxyalkyl group is not particularly limited, and examples thereof include 1 to 4. 4 and R 5 The cyclic heterocycle which may be formed may be exemplified by N-acryloylmorpholine.
[0121] Specific examples of the compound represented by the general formula (2) include N-methyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-butyl (meth)acrylamide, N-hexyl (meth)acrylamide and the like N-alkyl (meth)acrylamide derivatives; N-hydroxymethyl (meth)acrylamide, N-hydroxyethyl (meth)acrylamide, N-hydroxymethyl-N-propyl (meth)acrylamide and the like N-hydroxyalkyl (meth)acrylamide derivatives; N-methoxymethyl acrylamide, N-ethoxymethyl acrylamide and the like N-alkoxy (meth)acrylamide derivatives. In addition, examples of the cyclic ether group-containing (meth)acrylamide derivatives include heterocyclic (meth)acrylamide derivatives in which the nitrogen atom of the (meth)acrylamide group forms a heterocyclic ring, such as N-acryloylmorpholine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylpyrrolidine and the like.
[0122] The adhesive composition may contain a monofunctional radical polymerizable compound other than the above as a curable component. Examples of the monofunctional radical polymerizable compound include various (meth)acrylic acid derivatives having a (meth)acryloyloxy group. Examples of the (meth)acrylic acid derivatives include (meth)acrylic acid (having 1 to 20 carbon atoms) alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, tert-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, hexadecyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and n-octadecyl (meth)acrylate.
[0123] Examples of the (meth)acrylic acid derivatives include cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate and cyclopentyl (meth)acrylate; aralkyl (meth)acrylates such as benzyl (meth)acrylate; 2-isobornyl (meth)acrylate, 2-norbornyl methyl (meth)acrylate, 2-norbornyl methyl (meth)acrylate, 5-norbornene-2-yl methyl (meth)acrylate, 3-methyl-2-norbornyl methyl (meth)acrylate, Polycyclic (meth)acrylates such as dicyclopentenyl acrylate, dicyclopentenyloxyethyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; (meth)acrylates containing alkoxy groups or phenoxy groups such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, and alkylphenoxypolyethylene glycol (meth)acrylate; etc. Among these, dicyclopentenyloxyethyl acrylate and phenoxyethyl acrylate are preferred because of their excellent adhesion to various protective films.
[0124] Examples of the (meth)acrylic acid derivatives include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate; hydroxyl-containing (meth)acrylates such as [4-(hydroxymethyl)cyclohexyl]methyl acrylate, cyclohexanedimethanol mono(meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate; epoxy-containing (meth)acrylates such as glycidyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate glycidyl ether; and 2,2,2-trifluoroethyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, and 2, Halogen-containing (meth)acrylates such as 2,2-trifluoroethyl ethyl ester, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate; alkylaminoalkyl (meth)acrylates such as dimethylaminoethyl (meth)acrylate; oxetanyl (meth)acrylate-containing (meth)acrylates such as 3-oxetanyl methyl (meth)acrylate, 3-methyloxetanyl methyl (meth)acrylate, 3-ethyloxetanyl methyl (meth)acrylate, 3-butyloxetanyl methyl (meth)acrylate, and 3-hexyloxetanyl methyl (meth)acrylate; (meth)acrylates having heterocyclic rings such as tetrahydrofurfuryl (meth)acrylate and butyrolactone (meth)acrylate, hydroxypivalic acid neopentyl glycol (meth)acrylate adduct, and p-phenylphenol (meth)acrylate. Among them, 2-hydroxy-3-phenoxypropyl acrylate is preferred because of its excellent adhesion to various protective films.
[0125] Examples of the monofunctional radical polymerizable compound include carboxyl group-containing monomers such as (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, and ω-carboxypolycaprolactone mono(meth)acrylate.
[0126] Examples of monofunctional free radical polymerizable compounds include lactam vinyl monomers such as N-vinylpyrrolidone, N-vinyl-ε-caprolactam, and methylvinylpyrrolidone; vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, and vinyl Vinyl monomers having a nitrogen-containing heterocyclic ring such as oxazole and vinyl morpholine, etc.
[0127] In the adhesive composition of the present invention, when containing hydroxyl-containing (meth) acrylate, carboxyl-containing (meth) acrylate, phosphoric acid-containing (meth) acrylate, etc. with high polarity in a monofunctional free radical polymerizable compound, the adhesion to various substrates is improved. Relative to the adhesive composition, the content of hydroxyl-containing (meth) acrylate is preferably 1% by mass to 30% by mass. In the case where the content of hydroxyl-containing (meth) acrylate is too much, the water absorption rate of the cured product becomes high, and there is a situation where water resistance deteriorates. Relative to the adhesive composition, the content of carboxyl-containing (meth) acrylate is preferably 1% by mass to 20% by mass. In the case where the content of carboxyl-containing (meth) acrylate is too much, the optical durability of the polarizing film is reduced, and it is not preferred. As phosphoric acid-containing (meth) acrylate, 2-(meth) acryloyloxyethyl acid phosphate can be cited, and its content is preferably 0.1% by mass to 10% by mass relative to the adhesive composition. In the case where the content of phosphoric acid-containing (meth) acrylate is too much, the optical durability of the polarizing film is reduced, and it is not preferred.
[0128] In addition, as a monofunctional free radical polymerizable compound, a free radical polymerizable compound having an active methylene group can be used. The free radical polymerizable compound having an active methylene group is a compound having an active double bond group such as a (meth) acrylic group at the end or in the molecule and having an active methylene group. Examples of the active methylene group include acetoacetyl, alkoxymalonyl, or cyanoacetyl. The above-mentioned active methylene group is preferably acetoacetyl. Examples of the radical polymerizable compound having an active methylene group include acetoacetoxyethyl alkyl (meth)acrylates such as 2-acetoacetoxyethyl (meth)acrylate, 2-acetoacetoxyethyl propyl (meth)acrylate, and 2-acetoacetoxyethyl-1-methylethyl (meth)acrylate; 2-ethoxymalonyloxyethyl (meth)acrylate, 2-cyanoacetoxyethyl (meth)acrylate, N-(2-cyanoacetoxyethyl)acrylamide, N-(2-propionylacetoxybutyl)acrylamide, N-(4-acetoacetoxyethylmethylbenzyl)acrylamide, and N-(2-acetoacetylaminoethyl)acrylamide. The radical polymerizable compound having an active methylene group is preferably acetoacetoxyethyl alkyl (meth)acrylate.
[0129] Examples of the polyfunctional radical polymerizable compound having two or more functional groups include N,N'-methylenebis(meth)acrylamide as a polyfunctional (meth)acrylamide derivative, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol diacrylate, 2-ethyl-2-butylpropylene glycol di(meth)acrylate, bisphenol A di(meth)acrylate, bisphenol A ethylene oxide adduct di(meth)acrylate, bisphenol A propylene oxide adduct di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, neopentyl glycol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, dimethacrylate, and the like. Esterification products of (meth)acrylic acid and polyols such as alkanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and EO-modified diglycerol tetra(meth)acrylate, and 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene. Specific examples thereof include ARONIX M-220 (manufactured by Toagosei Co., Ltd.), LIGHT ACRYLATE 1,9ND-A (manufactured by Kyoeisha Chemical Co., Ltd.), LIGHT ACRYLATE DGE-4A (manufactured by Kyoeisha Chemical Co., Ltd.), LIGHT ACRYLATE DCP-A (manufactured by Kyoeisha Chemical Co., Ltd.), SR-531 (manufactured by Sartomer Co., Ltd.), and CD-536 (manufactured by Sartomer Co., Ltd.). In addition, as required, various epoxy (meth)acrylates, urethane (meth)acrylates, polyester (meth)acrylates, various (meth)acrylate monomers, etc. It should be noted that the multifunctional (meth)acrylamide derivative is preferably included in the adhesive composition because it has not only a fast polymerization speed and excellent productivity, but also excellent crosslinking properties when the adhesive composition is made into a cured product.
[0130] From the viewpoint of combining adhesion with polarizers and various transparent protective films and optical durability under harsh environments, the radical polymerizable compound preferably uses a monofunctional radical polymerizable compound and a polyfunctional radical polymerizable compound in combination. It should be noted that the liquid viscosity of the monofunctional radical polymerizable compound is low, so by including a monofunctional radical polymerizable compound in the adhesive composition, the liquid viscosity of the adhesive composition can be reduced. In addition, the monofunctional radical polymerizable compound often has a functional group that exhibits various functions. By including a monofunctional radical polymerizable compound in the adhesive composition, various functions can be exhibited in the adhesive composition and / or the cured product of the adhesive composition. The polyfunctional radical polymerizable compound is preferably contained in the adhesive composition because it can make the cured product of the adhesive composition three-dimensionally cross-linked. Relative to 100 parts by mass of the monofunctional radical polymerizable compound, the polyfunctional radical polymerizable compound is preferably used in an amount of 10 to 1000 parts by mass.
[0131] From the viewpoint of improving the adhesiveness of the adhesive layer, the content of the radically polymerizable compound in the adhesive composition is preferably 55 to 80% by mass, more preferably 65 to 80% by mass, and even more preferably 67 to 75% by mass.
[0132] When electron beams or the like are used as the active energy rays, the adhesive composition does not need to contain a photoradical polymerization initiator. However, when ultraviolet rays or visible light are used as the active energy rays, the adhesive composition preferably contains a photoradical polymerization initiator.
[0133] The photoradical polymerization initiator can be appropriately selected according to the active energy ray. In the case of curing by ultraviolet light or visible light, a photoradical polymerization initiator that is cleaved by ultraviolet light or visible light is used. As the photoradical polymerization initiator, for example, benzophenone compounds such as benzil, benzophenone, benzoylbenzoic acid, 3,3′-dimethyl-4-methoxybenzophenone, aromatic ketone compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α′-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, α-hydroxycyclohexylphenylketone, acetophenone compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, etc. can be listed; benzoin methyl ether, Benzoin alkyl ether compounds such as benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, and anisole methyl ether; aromatic ketal compounds such as benzil dimethyl ketal; aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone; camphorquinone; halogenated ketones; acylphosphine oxides; acylphosphonates, etc.
[0134] The content of the photoradical polymerization initiator in the adhesive composition is preferably 20% by mass or less, more preferably 0.01 to 20% by mass, further preferably 0.05 to 10% by mass, particularly preferably 0.1 to 5% by mass.
[0135] When the adhesive composition of the present invention is used as a visible light curable adhesive containing a radical polymerizable compound as a curable component, it is particularly preferred to use a photoradical polymerization initiator that is highly sensitive to light of 380 nm or longer. The photoradical polymerization initiator that is highly sensitive to light of 380 nm or longer will be described later.
[0136] As the photoradical polymerization initiator, it is preferred to use a compound represented by the following general formula (3) alone, or to use a compound represented by the general formula (3) in combination with a photoradical polymerization initiator having high sensitivity to light of 380 nm or longer described later.
[0137] [Chemical formula 7]
[0138]
[0139] (Where R 6 and R 7 Indicates -H, -CH 2CH 3 , -iPr or Cl, R 6 and R 7 When the compound represented by the general formula (3) is used, the adhesion is excellent compared with the case where a photo-radical polymerization initiator having high sensitivity to light of 380 nm or more is used alone. Among the compounds represented by the general formula (3), R 6 and R 7 -CH 2 CH 3 The composition ratio of the compound represented by the general formula (3) in the adhesive composition is preferably 0.1 to 5 mass %, more preferably 0.5 to 4 mass %, and even more preferably 0.9 to 3 mass %, relative to the total amount of the adhesive composition.
[0140] In addition, it is preferred to add a polymerization initiation aid as needed. Examples of the polymerization initiation aid include triethylamine, diethylamine, N-methyldiethanolamine, ethanolamine, 4-dimethylaminobenzoic acid, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, isopentyl 4-dimethylaminobenzoate, and the like, with ethyl 4-dimethylaminobenzoate being particularly preferred. When a polymerization initiation aid is used, the amount thereof added is generally 0 to 5% by mass, preferably 0 to 4% by mass, and most preferably 0 to 3% by mass relative to the total amount of the adhesive composition.
[0141] In addition, as required, known photo-radical polymerization initiators can be used. The transparent protective film with UV absorption ability does not penetrate the light below 380nm, therefore, as a photo-radical polymerization initiator, it is preferred to use a photo-radical polymerization initiator that is highly sensitive to light above 380nm. Specifically, it can be listed: 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(η5-2,4-cyclopentadiene-1-yl)bis(2,6-difluoro-3-(1H-pyrrole-1-yl)phenyl)titanium, etc.
[0142] In particular, as the photoradical polymerization initiator, in addition to the photoradical polymerization initiator of the general formula (3), it is preferred to further use a compound represented by the following general formula (4);
[0143] [Chemical formula 8]
[0144]
[0145] (Where R 8 , R 9 and R 10 Indicates -H, -CH 3 、-CH 2 CH 3 , -iPr or Cl, R 8 , R 9 and R 10 The compounds represented by the general formula (4) may be the same or different. As the compound represented by the general formula (4), 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one (trade name: IRGACURE907, manufacturer: BASF), which is a commercially available product, may be suitably used. In addition, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone (trade name: IRGACURE369, manufacturer: BASF) and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholino)phenyl]-1-butanone (trade name: IRGACURE379, manufacturer: BASF) are preferred because of their high sensitivity.
[0146] In the above-mentioned adhesive composition, when a radical polymerizable compound having an active methylene group is used as the radical polymerizable compound, it is preferably used in combination with a radical polymerization initiator having a hydrogen abstraction effect. According to this composition, the adhesion of the adhesive layer possessed by the polarizing film is significantly improved, especially even just after being taken out of a high humidity environment or water (non-dry state). The reason is not yet clear, but it is believed to be the following. That is, the radical polymerizable compound having an active methylene group is polymerized together with other radical polymerizable compounds constituting the adhesive layer, and enters the main chain and / or side chain of the base polymer in the adhesive layer to form the adhesive layer. In this polymerization process, if there is a radical polymerization initiator having a hydrogen abstraction effect, the base polymer constituting the adhesive layer is formed, and hydrogen is abstracted from the radical polymerizable compound having an active methylene group to generate free radicals in the methylene group. Moreover, the methylene group generated by the free radical reacts with the hydroxyl group of the polarizer such as PVA to form a covalent bond between the adhesive layer and the polarizer. As a result, it is estimated that the adhesiveness of the adhesive layer included in the polarizing film is significantly improved even in a non-dried state.
[0147] In the present invention, as a free radical polymerization initiator having a hydrogen abstraction effect, for example, thioxanthone free radical polymerization initiators, benzophenone free radical polymerization initiators, etc. are listed. The above-mentioned free radical polymerization initiator is preferably a thioxanthone free radical polymerization initiator. As a thioxanthone free radical polymerization initiator, for example, a compound represented by the above-mentioned general formula (3) can be listed. As specific examples of the compound represented by the general formula (3), for example, thioxanthone, dimethylthioxanthone, diethylthioxanthone, isopropylthioxanthone, chlorothioxanthone, etc. can be listed. Among the compounds represented by the general formula (3), R is particularly preferred. 6 and R 7 -CH 2 CH 3 of diethylthioxanthone.
[0148] Cationic polymerizable compounds can be classified into monofunctional cationic polymerizable compounds having one cationic polymerizable functional group in the molecule and polyfunctional cationic polymerizable compounds having two or more cationic polymerizable functional groups in the molecule.
[0149] Since the liquid viscosity of the monofunctional cationically polymerizable compound is relatively low, the liquid viscosity of the adhesive composition can be reduced by including the monofunctional cationically polymerizable compound in the adhesive composition. In addition, the monofunctional cationically polymerizable compound often has a functional group that exhibits various functions, and by including the monofunctional cationically polymerizable compound in the adhesive composition, various functions can be exhibited in the adhesive composition and / or the cured product of the adhesive composition.
[0150] The polyfunctional cationically polymerizable compound can three-dimensionally crosslink the cured product of the adhesive composition.
[0151] Examples of the cationically polymerizable functional group include an epoxy group, an oxetanyl group, and a vinyl ether group.
[0152] Examples of the compound having an epoxy group include aliphatic epoxy compounds, alicyclic epoxy compounds, and aromatic epoxy compounds. From the viewpoint of excellent curability and adhesiveness, alicyclic epoxy compounds are preferred.
[0153] Examples of the alicyclic epoxy compound include 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, caprolactone-modified products of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, trimethyl caprolactone-modified products, and valerolactone-modified products. Specific examples include CELLOXIDE 2021, CELLOXIDE 2021A, CELLOXIDE 2021P, CELLOXIDE 2081, CELLOXIDE 2083, and CELLOXIDE 2085 (all manufactured by Daicel Chemical Industries, Ltd.), Cyracure UVR-6105, Cyracure UVR-6107, Cyracure 30, and R-6110 (all manufactured by Dow Chemical Japan Ltd.).
[0154] Examples of the compound having an oxetane group include 3-ethyl-3-hydroxymethyloxetane, 1,4-bis[(3-ethyl-3-oxetane)methoxymethyl]benzene, 3-ethyl-3-(phenoxymethyl)oxetane, di[(3-ethyl-3-oxetane)methyl]ether, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, and novolac oxetane. Specific examples include ARON OXETANE OXT-101, ARON OXETANE OXT-121, ARON OXETANE OXT-211, ARON OXETANE OXT-221, and ARON OXETANE OXT-212 (all manufactured by Toagosei Co., Ltd.).
[0155] Examples of the compound having a vinyl ether group include 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, triethylene glycol divinyl ether, cyclohexanedimethanol divinyl ether, cyclohexanedimethanol monovinyl ether, tricyclodecane vinyl ether, cyclohexyl vinyl ether, methoxyethyl vinyl ether, ethoxyethyl vinyl ether, and pentaerythritol-type tetravinyl ether.
[0156] From the viewpoint of improving the adhesiveness of the adhesive layer, the content of the cationically polymerizable compound in the adhesive composition is preferably 5 to 40% by mass, more preferably 10 to 30% by mass, and even more preferably 15 to 25% by mass.
[0157] Since the adhesive composition of the present invention contains a cationic polymerizable compound as a curable component, it is preferably contained in a photocationic polymerization initiator. The photocationic polymerization initiator generates cationic species or Lewis acid by irradiation with active energy rays such as visible light, ultraviolet rays, X-rays, electron beams, etc., thereby initiating the polymerization reaction of epoxy groups and oxetane groups. As a photocationic polymerization initiator, a photoacid generator and a photobase generator can be suitably used, and the photoacid generator described later can be suitably used. In addition, when the adhesive composition used in the present invention is used as a visible light curable, it is particularly preferred to use a photocationic polymerization initiator with high sensitivity to light above 380nm, but the photocationic polymerization initiator is a compound that usually shows maximum absorption in a wavelength region near 300nm or shorter than 300nm. Therefore, by combining a photosensitizer that shows maximum absorption in a wavelength region longer than it, specifically, a light with a wavelength longer than 380nm, it can sense light of a wavelength near it, and promote the generation of cationic species or acids from the photocationic polymerization initiator. As photosensitizers, for example, anthracene compounds, pyrene compounds, carbonyl compounds, organic sulfur compounds, persulfides, redox compounds, azo and diazo compounds, halogen compounds, photoreduction pigments, etc., can be cited, and they can also be mixed with two or more. In particular, anthracene compounds have excellent photosensitizing effects, so they are preferred, and specifically Anthracure UVS-1331 and Anthracure UVS-1221 (Kawasaki Chemical Co., Ltd.) can be cited. The content of the photosensitizer is preferably 0.1% to 5% by mass, and more preferably 0.5% to 3% by mass.
[0158] Examples of the photoacid generator include compounds represented by the following general formula (5).
[0159] [Chemical formula 9]
[0160] L + X -
[0161] (In the formula, L+ represents any In addition, X- represents a cation selected from PF6 6 -、SbF 6 -、AsF 6 -, SbCl 6 -、BiCl 5 -、SnCl 6 -、ClO 4 -, dithiocarbamate anion, counter anion in SCN-. )
[0162] Next, the counter anion X- in the general formula (5) will be described.
[0163] In principle, there is no particular limitation on the counter anion X- in the general formula (5), and non-nucleophilic anions are preferred. When the counter anion X is a non-nucleophilic anion, it is not easy to cause nucleophilic reactions of coexisting cations in the molecule or various materials used in combination, and as a result, the stability of the photoacid generator represented by the general formula (5) itself and the composition using the photoacid generator can be improved over time. The non-nucleophilic anion mentioned here refers to an anion with a low ability to cause nucleophilic reactions. Examples of such anions include: PF 6 -、SbF 6 -、AsF 6 -, SbCl 6 -、BiCl 5 -、SnCl 6 -、ClO 4 -, dithiocarbamate anion, SCN-, etc.
[0164] Specifically, “CYRACURE UVI-6992”, “CYRACURE UVI-6974” (above, manufactured by Dow Chemical Japan Limited), “Adekaoptomer SP150”, “Adekaoptomer SP152”, “Adekaoptomer SP170”, “Adekaoptomer SP172” (above, manufactured by ADEKA Co., Ltd.), “IRGACURE 250” (manufactured by Ciba Specialty Chemicals Inc.), “CI-5102”, “CI-2855” (above, manufactured by Nippon Soda Co., Ltd.), “San-Aid SI-60L”, “San-Aid SI-80L”, “San-Aid SI-100L”, “San-Aid SI-110L”, “San-Aid SI-180L” (above, manufactured by Sanshin Chemical Co., Ltd.), “CPI-100P”, “CPI-110P”, “CPI-100A” (above, manufactured by San-Apro Ltd.), "WPI-069", "WPI-113", "WPI-116", "WPI-041", "WPI-044", "WPI-054", "WPI-055", "WPAG-281", "WPAG-567", "WPAG-596" (all manufactured by Wako Pure Chemical Industries, Ltd.) can be cited as preferred specific examples of the photoacid generator of the present invention.
[0165] The content of the photoacid generator is 10% by mass or less, preferably 0.01 to 10% by mass, more preferably 0.05 to 5% by mass, and particularly preferably 0.1 to 3% by mass, based on the total amount of the adhesive composition.
[0166] The photobase generator is a compound that changes the molecular structure or cleaves the molecules by irradiation with ultraviolet light, visible light, etc., to generate one or more basic substances that can function as catalysts for the polymerization reaction of free radical polymerizable compounds and epoxy resins. Examples of basic substances include secondary amines and tertiary amines. Examples of photobase generators include the above-mentioned α-aminoacetophenone compounds, the above-mentioned oxime ester compounds, compounds having substituents such as acyloxyimino groups, N-formylated aromatic amino groups, N-acylated aromatic amino groups, nitrobenzyl carbamate groups, and alkoxybenzyl carbamate groups. Among them, oxime ester compounds are preferred.
[0167] Examples of the compound having an acyloxyimino group include O,O'-succinic acid dibenzoacetophenone oxime, O,O'-succinic acid dinaphthobenzophenone oxime, and a benzophenone oxime acrylate-styrene copolymer.
[0168] Examples of the compound having an N-formylated aromatic amino group or an N-acylated aromatic amino group include di-N-(p-formylamino)diphenylmethane, di-N-(p-acetylamino)diphenylmethane, di-N-(p-benzamido)diphenylmethane, 4-formylaminostilbene, 4-acetylaminostilbene, 2,4-diformylaminostilbene, 1-formylaminonaphthalene, 1-acetylaminonaphthalene, 1,5-diformylaminonaphthalene, 1-formylaminoanthracene, 1,4-diformylaminoanthracene, 1-acetylaminoanthracene, 1,4-diformylaminoanthraquinone, 1,5-diformylaminoanthraquinone, 3,3′-dimethyl-4,4′-diformylaminobiphenyl, and 4,4′-diformylaminobenzophenone.
[0169] Examples of the compound having a nitrobenzyl carbamate group and an alkoxybenzyl carbamate group include bis{{(2-nitrobenzyl)oxy}carbonyl}diaminodiphenylmethane, 2,4-bis{(2-nitrobenzyl)oxy}stilbene, bis{(2-nitrobenzyloxy)carbonyl}hexane-1,6-diamine, and o-xylidine{{(2-nitro-4-chlorobenzyl)oxy}amide.
[0170] The photobase generator is preferably at least one selected from an oxime ester compound and an α-aminoacetophenone compound, and is more preferably an oxime ester compound. As the α-aminoacetophenone compound, an α-aminoacetophenone compound having two or more nitrogen atoms is particularly preferred.
[0171] As other photobase generators, WPBG-018 (trade name, 9-anthrylmethyl N,N'-diethylcarbamate), WPBG-027 (trade name, (E)-1-[3-(2-hydroxyphenyl)-2-propenoyl]piperidine), WPBG-082 (trade name, guanidinium2-(3-benzoylphenyl)propionate), WPBG-140 (trade name, 1-(anthraquinon-2-yl)ethylimidazolecarboxylate) and the like can be used.
[0172] In the above adhesive composition, a photoacid generator and a compound containing either an alkoxy group or an epoxy group may be used in combination in the adhesive composition.
[0173] When using a compound having one or more epoxy groups in the molecule or a polymer (epoxy resin) having two or more epoxy groups in the molecule, a compound having two or more functional groups reactive with epoxy groups in the molecule can be used in combination. Among them, the functional group reactive with epoxy groups can be listed, for example, as carboxyl, phenolic hydroxyl, mercapto, primary or secondary aromatic amino, etc. Considering the three-dimensional curing property, it is particularly preferred to have two or more of these functional groups in one molecule.
[0174] Examples of polymers having one or more epoxy groups in the molecule include epoxy resins, including bisphenol A type epoxy resins derived from bisphenol A and epichlorohydrin, bisphenol F type epoxy resins derived from bisphenol F and epichlorohydrin, bisphenol S type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, bisphenol F novolac type epoxy resins, alicyclic epoxy resins, diphenyl ether type epoxy resins, hydroquinone type epoxy resins, naphthalene type epoxy resins, biphenyl type epoxy resins, fluorene type epoxy resins, trifunctional epoxy resins, tetrafunctional epoxy resins and other multifunctional epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, hydantoin type epoxy resins, isocyanurate type epoxy resins, aliphatic chain epoxy resins, and the like. These epoxy resins may be halogenated or hydrogenated. Examples of commercially available epoxy resin products include JER code 828, 1001, 801N, 806, 807, 152, 604, 630, 871, YX8000, YX8034, and YX4000 manufactured by Japan Epoxy Resin, EPICLON830, EXA835LV, HP4032D, and HP820 manufactured by DIC Corporation, EP4100 series, EP4000 series, and EPU series manufactured by ADEKA Corporation, and Daicel Chemical Co., Ltd. Industries, Ltd. CELLOXIDE series (2021, 2021P, 2083, 2085, 3000, etc.), Epolead series, EHPE series, YD series, YDF series, YDCN series, YDB series, phenoxy resin (polyhydroxy polyether synthesized from bisphenols and epichlorohydrin, and having epoxy groups at both ends; YP series, etc.), Denacol series made by Nagase ChemteX Corporation, Epolight series made by Kyoeisha Chemical Co., Ltd., etc., but not limited to these. These epoxy resins can be used in combination of two or more.
[0175] The compound having an alkoxy group in the molecule is not particularly limited as long as it has one or more alkoxy groups in the molecule, and known compounds can be used. Representative examples of such compounds include melamine compounds, amino resins, and silane coupling agents.
[0176] The amount of the compound containing any one of an alkoxy group and an epoxy group is usually 30% by mass or less relative to the total amount of the adhesive composition. If the content of the compound in the composition is too much, the adhesion is reduced, and the impact resistance to the drop hammer test is sometimes deteriorated. The content of the compound in the composition is more preferably 20% by mass or less. On the other hand, from the perspective of water resistance, it is preferred that the compound be contained in the composition at 2% by mass or more, and more preferably at 5% by mass or more.
[0177] The adhesive composition used in the present invention preferably contains the polymerizable compound X as a curable component. The polymerizable compound X has an SP value close to the SP value of transparent protective films such as unsaponified triacetyl cellulose film and acrylic film, and therefore the polymerizable compound X contributes to improving the adhesion between the adhesive layer and the transparent protective film.
[0178] The content of the polymerizable compound X in the adhesive composition is not particularly limited, but is preferably 80% by mass or less, more preferably 60% by mass or less, and preferably 25% by mass or more, more preferably 35% by mass or more, from the viewpoint of improving the adhesion between the adhesive layer and the transparent protective film.
[0179] In the present invention, the compound described in the general formula (1) can be mixed with the adhesive composition, preferably the compound described in the general formula (1'), and more preferably the compound described in the general formula (1a) to (1d). In addition, in the present invention, the above-mentioned organic metal compound can be mixed with the adhesive composition. When these compounds are mixed with the adhesive composition, the adhesion with the polarizer and the transparent protective film is sometimes improved, so it is preferred. From the viewpoint of improving the adhesion and water resistance when the polarizer is bonded to the transparent protective film through the adhesive layer, the content of the compound described in the general formula (1) in the adhesive composition is preferably 0.001 to 50% by mass, more preferably 0.1 to 30% by mass, and more preferably 1 to 10% by mass. In addition, in the adhesive composition, the content of the above-mentioned organic metal compound is preferably 0.1 to 10% by mass, more preferably 0.5 to 7% by mass, and more preferably 1 to 5% by mass.
[0180] The bubble inhibitor is a compound that can reduce the surface tension by being added to the adhesive composition, thereby having the effect of reducing bubbles between the adhesive composition and the transparent protective film to be bonded. As the bubble inhibitor, for example, a silicone bubble inhibitor having a polysiloxane skeleton such as polydimethylsiloxane, a (meth)acrylic bubble inhibitor having a (meth)acryloyl skeleton formed by polymerizing (meth)acrylate, a polyether bubble inhibitor formed by polymerizing vinyl ether, cyclic ether, etc., a fluorine bubble inhibitor formed by a fluorine-containing compound having a perfluoroalkyl group, etc., which has the effect of reducing the surface tension of the adhesive composition when added to the adhesive composition, can be used.
[0181] The bubble inhibitor preferably has a reactive group in the compound. In this case, when the polarizer and the transparent protective film are laminated, the generation of lamination bubbles can be reduced. As the reactive group possessed by the bubble inhibitor, polymerizable functional groups can be listed, specifically, free radical polymerizable functional groups with olefinic double bonds such as (meth) acryloyl, vinyl, allyl, epoxy groups such as glycidyl, oxetane, vinyl ether, cyclic ether, cyclic thioether, lactone, etc. can be listed. From the viewpoint of reactivity in the adhesive composition, it is preferred to have a bubble inhibitor with a double bond as a reactive group, and more preferably a bubble inhibitor with a (meth) acryloyl group.
[0182] In consideration of the lamination bubble suppression effect and the adhesion improvement effect, among the above bubble suppressors, silicone bubble suppressors are preferred. In addition, among the bubble suppressors, in consideration of the adhesion of the adhesive layer, bubble suppressors containing a urethane bond or an isocyanurate ring structure in the main chain skeleton or the side chain are preferred. As silicone bubble suppressors, commercially available products can also be suitably used, for example, "BYK-UV3505" (manufactured by BYK-Chemie Japan Co., Ltd.) which is an acryl-modified polydimethylsiloxane can be cited.
[0183] In order to achieve both the adhesive strength of the obtained adhesive layer and the effect of reducing lamination bubbles, the content of the bubble inhibitor is preferably 0.01 to 0.6% by mass when the total amount of the adhesive composition is 100% by mass.
[0184] In the adhesive composition used in the present invention, in addition to the curable component of the above-mentioned free radical polymerizable compound, an acrylic oligomer formed by polymerizing a (meth) acrylic acid monomer may also be contained. By containing the acrylic oligomer in the adhesive composition, the curing shrinkage when the composition is irradiated with active energy rays and cured can be reduced, and the interfacial stress between the adhesive and the adherends such as polarizers and transparent protective films can be reduced. As a result, the adhesion between the adhesive layer and the adherend can be suppressed. In order to fully suppress the curing shrinkage of the adhesive layer, the content of the acrylic oligomer is preferably 20% by mass or less, more preferably 15% by mass or less relative to the total amount of the adhesive composition. When the content of the acrylic oligomer in the adhesive composition is too much, the reaction speed when the composition is irradiated with active energy rays is sharply reduced, and there is a situation where the curing becomes poor. On the other hand, relative to the total amount of the adhesive composition, it is preferably contained 3% by mass or more of the acrylic oligomer, and more preferably 5% by mass or more.
[0185] In consideration of workability and uniformity during coating, the adhesive composition preferably has a low viscosity, and thus the acrylic oligomer obtained by polymerizing the (meth)acrylic acid monomer also preferably has a low viscosity. As a low-viscosity acrylic oligomer capable of preventing the curing shrinkage of the adhesive layer, its weight average molecular weight (Mw) is preferably 15,000 or less, more preferably 10,000 or less, and particularly preferably 5,000 or less. On the other hand, in order to fully suppress the curing shrinkage of the adhesive layer, the weight average molecular weight (Mw) of the acrylic oligomer is preferably 500 or more, more preferably 1,000 or more, and particularly preferably 1,500 or more.Specific examples of the (meth)acrylic monomer constituting the acrylic oligomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, tert-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, and tert-butyl (meth)acrylate. (meth)acrylate (carbon number 1-20) alkyl esters such as cetyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and n-octadecyl (meth)acrylate, and cycloalkyl (meth)acrylates (such as cyclohexyl (meth)acrylate and cyclopentyl (meth)acrylate), aralkyl (meth)acrylates (such as benzyl (meth)acrylate), polycyclic (meth)acrylates (such as 2-isobornyl (meth)acrylate, 2-isobornyl (meth)acrylate, and 2-isobornyl (meth)acrylate). methyl (meth)acrylate, 5-norbornene-2-ylmethyl (meth)acrylate, 3-methyl-2-norbornylmethyl (meth)acrylate, etc.), hydroxyl-containing (meth)acrylates (e.g. hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2,3-dihydroxypropylmethylbutyl (meth)acrylate, etc.), alkoxy- or phenoxy-containing (meth)acrylates (2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, (meth)acrylate ethyl carbitol ester, (meth)acrylate phenoxyethyl ester, etc.), epoxy-containing (meth)acrylates (such as (meth)acrylate glycidyl ester, etc.), halogen-containing (meth)acrylates (such as (meth)acrylate 2,2,2-trifluoroethyl ester, (meth)acrylate 2,2,2-trifluoroethyl ester, (meth)acrylate tetrafluoropropyl ester, (meth)acrylate hexafluoropropyl ester, (meth)acrylate octafluoropentyl ester, (meth)acrylate heptadecafluorodecyl ester, etc.), (meth)acrylate alkylaminoalkyl esters (such as (meth)acrylate dimethylaminoethyl ester, etc.). These (meth)acrylates can be used alone or in combination of two or more. Specific examples of acrylic oligomers include "ARUFON" manufactured by Toagosei Co., Ltd., "ACTFLOW" manufactured by Soken Chemical Co., Ltd., and "JONCRYL" manufactured by BASF Japan Ltd.
[0186] When the adhesive composition used in the present invention is active energy ray-curable, it is preferable to use an active energy ray-curable compound as the silane coupling agent. However, even if it is not active energy ray-curable, similar water resistance can be imparted.
[0187] Specific examples of the silane coupling agent include vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-phenylvinyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane, which are active energy ray-curable compounds.
[0188] 3-Methacryloxypropyltrimethoxysilane and 3-acryloxypropyltrimethoxysilane are preferred.
[0189] As a specific example of the inactive energy ray-curable silane coupling agent, a silane coupling agent having an amino group is preferred. As a specific example of the silane coupling agent having an amino group, γ-aminopropyl trimethoxysilane, γ-aminopropyl triethoxysilane, γ-aminopropyl triisopropoxysilane, γ-aminopropyl methyl dimethoxysilane, γ-aminopropyl methyl diethoxysilane, γ-(2-aminoethyl)aminopropyl trimethoxysilane, γ-(2-aminoethyl)aminopropyl methyl dimethoxysilane, γ-(2-aminoethyl)aminopropyl triethoxysilane, γ-(2-aminoethyl)aminopropyl methyl diethoxysilane, γ-(2-aminoethyl)aminopropyl triisopropoxysilane, γ-(2-(2-aminoethyl)aminoethyl)aminopropyl trimethoxysilane, γ-(6-aminohexyl)aminopropyl trimethoxysilane , 3-(N-ethylamino)-2-methylpropyltrimethoxysilane, γ-ureidopropyltrimethoxysilane, γ-ureidopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-benzyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, N-cyclohexylaminomethyltriethoxysilane, N-cyclohexylaminomethyldiethoxymethylsilane, N-phenylaminomethyltrimethoxysilane, (2-aminoethyl)aminomethyltrimethoxysilane, N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine and other amino-containing silanes; N-(1,3-dimethylbutylene)-3-(triethoxysilyl)-1-propylamine and other ketimine-type silanes.
[0190] The silane coupling agent having an amino group may be used alone or in combination. Among these, in order to ensure good adhesion, γ-aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropylmethyldiethoxysilane, and N-(1,3-dimethylbutylene)-3-(triethoxysilyl)-1-propylamine are preferred.
[0191] The amount of the silane coupling agent is preferably in the range of 0.01 to 20% by mass, more preferably 0.05 to 15% by mass, and still more preferably 0.1 to 10% by mass relative to the total amount of the adhesive composition. This is because when the amount is greater than 20% by mass, the storage stability of the adhesive composition deteriorates, and when the amount is less than 0.1% by mass, it is difficult to fully exert the effect of water-resistant adhesiveness.
[0192] Specific examples of the inactive energy ray-curable silane coupling agents other than those mentioned above include 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatepropyltriethoxysilane, and imidazole silane.
[0193] When the adhesive composition used in the present invention contains a compound having a vinyl ether group, the water-resistant adhesion between the polarizer and the adhesive layer is improved, so it is preferred. The reason for this effect is not clear, but one of the reasons is speculated to be that the adhesion between the polarizer and the adhesive layer is improved by the interaction between the vinyl ether group of the compound and the polarizer. In order to further improve the water-resistant adhesion between the polarizer and the adhesive layer, the compound is preferably a free radical polymerizable compound having a vinyl ether group. In addition, with respect to the content of the compound, it is preferred to contain 0.1 to 19 mass % relative to the total amount of the adhesive composition.
[0194] The adhesive composition used in the present invention may contain a compound that produces keto-enol tautomerism. For example, in an adhesive composition containing a crosslinking agent or an adhesive composition that can be used in combination with a crosslinking agent, it is preferred to use a method that contains the above-mentioned compound that produces keto-enol tautomerism. Thus, the excessive viscosity increase, gelation, and microgel formation of the adhesive composition after the organic metal compound is combined can be suppressed, and the effect of extending the pot life of the composition can be achieved.
[0195] As the above-mentioned compound that produces keto-enol tautomerism, various β-dicarbonyl compounds can be used. As specific examples, β-diketones such as acetylacetone, 2,4-hexanedione, 3,5-heptanedione, 2-methylhexane-3,5-dione, 6-methylheptane-2,4-dione, and 2,6-dimethylheptane-3,5-dione can be listed; acetoacetic acid esters such as methyl acetoacetate, ethyl acetoacetate, isopropyl acetoacetate, and tert-butyl acetoacetate; propionoacetic acid esters such as methyl propionoacetate, ethyl propionoacetate, isopropyl propionoacetate, and tert-butyl propionoacetate; isobutyrylacetates such as methyl isobutyrylacetate, ethyl isobutyrylacetate, isopropyl isobutyrylacetate, and tert-butyl isobutyrylacetate; malonic acid esters such as methyl malonate and ethyl malonate; etc. Among them, acetylacetone and acetoacetic acid esters can be listed as suitable compounds. The above-mentioned compounds that undergo keto-enol tautomerism may be used alone or in combination of two or more.
[0196] The amount of the compound that produces keto-enol tautomerism can be set to 0.05 to 10 parts by mass, preferably 0.2 to 3 parts by mass (e.g., 0.3 to 2 parts by mass) relative to 1 part by mass of the organometallic compound. If the amount of the above compound is less than 0.05 parts by mass relative to 1 part by mass of the organometallic compound, it is sometimes difficult to exert a sufficient effect of use. On the other hand, if the amount of the compound is greater than 10 parts by mass relative to 1 part by mass of the organometallic compound, it is sometimes difficult to exhibit the target water resistance due to excessive interaction with the organometallic compound.
[0197] The adhesive composition of the present invention may also contain a polyrotaxane. The polyrotaxane has a cyclic molecule, a linear molecule penetrating the opening of the cyclic molecule, and a capping group disposed at both ends of the linear molecule so that the cyclic molecule does not detach from the linear molecule. Preferably, the cyclic molecule has an active energy ray-curable functional group.
[0198] The cyclic molecule is not particularly limited as long as its opening includes a linear molecule in a string, can move on the linear molecule, and has an active energy ray polymerizable group. It should be noted that in this specification, the "cyclic" of "cyclic molecule" means substantially "cyclic". That is, as long as it can move on the linear molecule, the cyclic molecule may not be completely ring-closed.
[0199] As specific examples of cyclic molecules, cyclic polymers such as cyclic polyethers, cyclic polyesters, cyclic polyetheramines, and cyclodextrins such as α-cyclodextrin, β-cyclodextrin, and γ-cyclodextrin can be listed. Among them, α-cyclodextrin, β-cyclodextrin, γ-cyclodextrin, and other cyclodextrins that are relatively easy to obtain and can select a variety of chain-capping groups are preferred. Two or more cyclic molecules can be mixed in a polyrotaxane or an adhesive.
[0200] In the polyrotaxane used in the present invention, the cyclic molecule has an active energy ray polymerizable group. Thus, the polyrotaxane reacts with the active energy ray curable component to obtain an adhesive whose crosslinking points are movable even after curing. The active energy ray polymerizable group possessed by the cyclic molecule can be any group that can polymerize with the active energy ray curable compound, and examples thereof include free radical polymerizable groups such as (meth)acryloyl and (meth)acryloyloxy groups.
[0201] When cyclodextrin is used as the cyclic molecule, it is preferred to introduce an active energy ray polymerizable group into the hydroxyl group of cyclodextrin via any appropriate linker. The number of active energy ray polymerizable groups in one molecule of polyrotaxane is preferably 2 to 1280, more preferably 50 to 1000, and even more preferably 90 to 900.
[0202] It is preferred to introduce a hydrophobic modifying group into the cyclic molecule. By introducing a hydrophobic modifying group, the compatibility with the active energy ray-curable component can be improved. In addition, since the hydrophobicity is imparted, when used in a polarizing film, water can be prevented from penetrating into the interface between the adhesive layer and the polarizer, and the water resistance can be further improved. Examples of the hydrophobic modifying group include polyester chains, polyamide chains, alkyl chains, oxyalkylene chains, ether chains, and the like. As specific examples, the groups described in
[0027] to
[0042] of WO2009 / 145073 can be cited.
[0203] The polarizing film using a resin composition containing a polyrotaxane as an adhesive has excellent water resistance. The reason for the improved water resistance of the polarizing film has not yet been determined, but it is speculated as follows. That is, it is believed that due to the mobility of the cyclic molecules of the polyrotaxane, the cross-linking points can move (the so-called pulley effect), thereby imparting flexibility to the cured adhesive and increasing the adhesion to the surface unevenness of the polarizer, thereby preventing water from invading the interface between the polarizer and the adhesive layer. In addition, it is believed that by giving the polyrotaxane a hydrophobic modifying group, the adhesive can be given hydrophobicity, which also helps to prevent water from invading the interface between the polarizer and the adhesive layer. The content of the polyrotaxane is preferably 2% to 50% by mass relative to the resin composition.
[0204] <Polarizing filter>
[0205] In the present invention, from the viewpoint of improving optical durability in a harsh environment under high temperature and high humidity, a thin polarizer with a thickness of 3 μm or more and 15 μm or less is preferably used as the polarizer, more preferably 12 μm or less, further preferably 10 μm or less, and particularly preferably 8 μm or less. Such a thin polarizer has less uneven thickness, excellent visual recognition, and less dimensional change, and therefore has excellent durability against thermal shock.
[0206] It should be noted that thin polarizers generally have a low moisture content, specifically, in most cases, the moisture content is 15% by mass or less. Such a thin polarizer with a low moisture content has the above-mentioned effects, but on the other hand, the reactivity with the boron-containing compound or organic metal compound contained in the easy-adhesive composition used in the present invention is low, and sometimes the effect of improving the adhesion between the polarizer and the adhesive layer is insufficient. Therefore, in the method for manufacturing a polarizing film of the present invention, when a polarizer with a moisture content of 15% or less is used, when the total amount of the easy-adhesive composition is set to 100% by mass, the water content is preferably 5 to 90% by mass, more preferably 30 to 80% by mass, and even more preferably 40 to 70% by mass.
[0207] The polarizer uses a polyvinyl alcohol resin. Examples of the polarizer include films obtained by adsorbing dichroic substances such as iodine and dichroic dyes on hydrophilic polymer films such as polyvinyl alcohol films, partially formalized polyvinyl alcohol films, and partially saponified films of ethylene-vinyl acetate copolymers and then uniaxially stretching them, and polyene oriented films such as dehydrated products of polyvinyl alcohol and dehydrochlorinated products of polyvinyl chloride. Among these, a polarizer formed of a polyvinyl alcohol film and a dichroic substance such as iodine is preferred.
[0208] A polarizer formed by dyeing a polyvinyl alcohol film with iodine and uniaxially stretching can be made, for example, as follows: dyeing is performed by immersing polyvinyl alcohol in an aqueous solution of iodine, and stretching to 3 to 7 times the initial length. As required, it can also be immersed in an aqueous solution of boric acid, zinc sulfate, zinc chloride, or potassium iodide. In addition, as required, the polyvinyl alcohol film can also be immersed in water and washed before dyeing. By washing the polyvinyl alcohol film with water, not only can the stains and anti-blocking agents on the surface of the polyvinyl alcohol film be cleaned, but it also has the effect of preventing uneven dyeing, etc. by swelling the polyvinyl alcohol film. Stretching can be performed after dyeing with iodine, or it can be stretched while dyeing, and it can also be dyed with iodine after stretching. It can also be stretched in an aqueous solution of boric acid, potassium iodide, etc., or in a water bath.
[0209] From the perspective of tensile stability and humidification reliability, the polarizer preferably contains boric acid. In addition, from the perspective of suppressing the occurrence of through cracks, the boric acid content in the polarizer is preferably 22% by mass or less, and more preferably 20% by mass or less relative to the total amount of the polarizer. From the perspective of tensile stability and humidification reliability, the boric acid content is preferably 10% by mass or more, and more preferably 12% by mass or more relative to the total amount of the polarizer.
[0210] Representative thin polarizers include those described in Japanese Patent No. 4751486, Japanese Patent No. 4751481, Japanese Patent No. 4815544, Japanese Patent No. 5048120, International Publication No. 2014 / 077599, International Publication No. 2014 / 077636, etc., or those obtained by the production methods described in these documents.
[0211] As the above-mentioned thin polarizer, in the manufacturing method including the step of stretching in the state of a laminate and the step of dyeing, from the viewpoint of being able to stretch to a high ratio and improving the polarization performance, it is preferable to use a thin polarizer obtained by a manufacturing method including the step of stretching in an aqueous boric acid solution as described in Japanese Patent No. 4751486, Japanese Patent No. 4751481, and Japanese Patent No. 4815544, and it is particularly preferable to use a thin polarizer obtained by a manufacturing method including the step of auxiliary stretching in a gas atmosphere before stretching in an aqueous boric acid solution as described in Japanese Patent No. 4751481 and Japanese Patent No. 4815544. These thin polarizing films can be obtained by a manufacturing method including the step of stretching a polyvinyl alcohol resin (hereinafter, also referred to as a PVA resin) layer and a stretching resin substrate in the state of a laminate and the step of dyeing. According to this production method, even if the PVA-based resin layer is thin, it can be stretched by being supported by the stretchable resin substrate without causing problems such as breakage due to stretching.
[0212] <Transparent protective film>
[0213] As a transparent protective film, it is preferred that the transparency, mechanical strength, thermal stability, moisture barrier, isotropy, etc. are excellent. For example, polyester polymers such as polyethylene terephthalate and polyethylene naphthalate, cellulose polymers such as cellulose diacetate and cellulose triacetate, acrylic polymers such as polymethyl methacrylate, polystyrene, polyolefin polymers such as acrylonitrile-styrene copolymer (AS resin), polycarbonate polymers, etc. can be listed. In addition, polyethylene, polypropylene, polyolefins with ring or norbornene structures, polyolefin polymers such as ethylene-propylene copolymers, vinyl chloride polymers, nylon, amide polymers such as aromatic polyamides, imide polymers, sulfone polymers, polyethersulfone polymers, polyetheretherketone polymers, polyphenylene sulfide polymers, vinyl alcohol polymers, vinylidene chloride polymers, vinyl butyral polymers, polyarylate polymers, polyoxymethylene polymers, epoxy polymers, or mixtures of the above polymers can also be listed as examples of polymers forming the above transparent protective film. The transparent protective film may contain one or more arbitrary appropriate additives. Examples of additives include ultraviolet absorbers, antioxidants, lubricants, plasticizers, mold release agents, anti-coloring agents, flame retardants, nucleating agents, antistatic agents, pigments, colorants, etc. The content of the thermoplastic resin in the transparent protective film is preferably 50 to 100% by mass, more preferably 50 to 99% by mass, further preferably 60 to 98% by mass, and particularly preferably 70 to 97% by mass. When the content of the thermoplastic resin in the transparent protective film is less than 50% by mass, there is a concern that the high transparency originally possessed by the thermoplastic resin cannot be fully exhibited.
[0214] In addition, as a transparent protective film, a polymer film described in Japanese Patent Publication No. 2001-343529 (WO01 / 37007) can be cited, such as (A) a resin composition containing a thermoplastic resin having a substituted and / or unsubstituted imide group in the side chain and a thermoplastic resin having a substituted and / or unsubstituted phenyl and nitrile group in the side chain. As a specific example, a film of a resin composition containing an alternating copolymer formed by isobutylene and N-methylmaleimide and an acrylonitrile-styrene copolymer can be cited. The film can be formed by a mixed extrusion product of the resin composition. These films have a small phase difference and a small photoelastic coefficient, so they can eliminate the unevenness caused by the strain of the polarizing film. In addition, the moisture permeability is small, so the humidification durability is excellent.
[0215] In addition, in the present invention, the moisture permeability of the transparent protective film preferably used is 150 g / m 2 / 24h or less. According to this structure, moisture in the air is not easy to enter the polarizing film, and the change of the moisture content of the polarizing film itself can be suppressed. As a result, the curling and dimensional change of the polarizing film caused by the storage environment can be suppressed.
[0216] As the transparent protective film provided on one or both sides of the polarizer, a transparent protective film having excellent transparency, mechanical strength, thermal stability, moisture barrier property, isotropy, etc. is preferred, and a moisture permeability of 150 g / m 2 / 24h or less, particularly preferably 120g / m 2 / 24h or less, more preferably 5 to 70g / m 2 / 24h or less.
[0217] As the material for forming the transparent protective film satisfying the above-mentioned low moisture permeability, polyester resins such as polyethylene terephthalate and polyethylene naphthalate; polycarbonate resins; polyarylate resins; amide resins such as nylon and aromatic polyamide; polyolefin polymers such as polyethylene, polypropylene, and ethylene-propylene copolymers, cyclic olefin resins having a cyclic or norbornene structure, (meth) acrylic resins, or mixtures thereof can be used. Among the above-mentioned resins, polycarbonate resins, cyclic polyolefin resins, and (meth) acrylic resins are preferred, and cyclic polyolefin resins and (meth) acrylic resins are particularly preferred.
[0218] The thickness of the transparent protective film can be appropriately determined, and is generally preferably 5 to 100 μm, particularly preferably 10 to 60 μm, and more preferably 13 to 40 μm from the viewpoints of strength, workability such as handling properties, and thinness.
[0219] The above-mentioned transparent protective film usually uses a transparent protective film with a front phase difference of less than 40nm and a thickness direction phase difference of less than 80nm. The front phase difference Re is represented by Re=(nx-ny)×d. The thickness direction phase difference Rth is represented by Rth=(nx-nz)×d. In addition, the Nz coefficient is represented by Nz=(nx-nz) / (nx-ny). [Wherein, the refractive indices in the slow axis direction, fast axis direction and thickness direction of the film are set to nx, ny, nz respectively, and d (nm) is set to the thickness of the film. The slow axis direction is set to the direction in which the refractive index in the film surface reaches the maximum. ]. It should be noted that the transparent protective film is preferably as colorless as possible. It is preferred to use a protective film with a phase difference value in the thickness direction of -90nm to +75nm. By using a protective film with a phase difference value (Rth) in the thickness direction of -90nm to +75nm, the coloring (optical coloring) of the polarizing film caused by the transparent protective film can be basically eliminated. The thickness direction retardation value (Rth) is more preferably -80 nm to +60 nm, particularly preferably -70 nm to +45 nm.
[0220] On the other hand, as the above-mentioned transparent protective film, a phase difference plate having a front phase difference of 40 nm or more and / or a thickness direction phase difference of 80 nm or more can be used. The front phase difference is usually controlled to a range of 40 to 200 nm, and the thickness direction phase difference is usually controlled to a range of 80 to 300 nm. When a phase difference plate is used as a transparent protective film, the phase difference plate also acts as a transparent protective film, so that thinning can be achieved.
[0221] As a phase difference plate, there can be listed: a birefringent film formed by unidirectional or bidirectional stretching of a polymer raw material, an oriented film of a liquid crystal polymer, a phase difference plate formed by an oriented layer of a liquid crystal polymer supported by a film, etc. The thickness of the phase difference plate is not particularly limited, and is usually about 20 to 150 μm. As a polymer raw material, for example: polyvinyl alcohol, polyvinyl butyral, polymethyl vinyl ether, polyhydroxyethyl acrylate, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, polycarbonate, polyacrylate, polysulfone, polyethylene terephthalate, polyethylene naphthalate, polyether sulfone, polyphenylene sulfide, polyphenylene ether, polyallyl sulfonic acid, polyamide, polyimide, polyolefin, polyvinyl chloride, cellulose resin, cyclic polyolefin resin (norbornene resin), or various copolymers, graft copolymers, mixtures thereof, etc. These polymer raw materials become oriented objects (stretched films) by stretching, etc.
[0222] As liquid crystal polymers, for example, various liquid crystal polymers of main chain type and side chain type, etc., which introduce conjugated linear atomic groups (mesogens) that impart liquid crystal orientation into the main chain of the polymer and the side chain, can be listed. As a specific example of a main chain type liquid crystal polymer, a structure in which a mesogen group is bonded by a spacer that imparts bending, such as a polyester liquid crystal polymer of nematic orientation, a discotic polymer, a cholesteric polymer, etc. can be listed. As a specific example of a side chain type liquid crystal polymer, a liquid crystal polymer having a mesogen part composed of a para-substituted cyclic compound unit imparting nematic orientation as a side chain with polysiloxane, polyacrylate, polymethacrylate or polymalonate as the main chain skeleton, and a spacer composed of conjugated atomic groups can be listed. These liquid crystal polymers are, for example, liquid crystal polymers formed by grinding the surface of a film such as polyimide and polyvinyl alcohol formed on a glass plate, liquid crystal polymers formed by oblique evaporation of silicon oxide, etc., and a solution of a liquid crystal polymer is developed on its orientation treatment surface and heat-treated.
[0223] The phase difference plate can be, for example, various wave plates, a phase difference plate with an appropriate phase difference depending on the purpose of use, such as the purpose of utilizing the coloring of the birefringence of the liquid crystal layer, the purpose of compensating for the viewing angle, etc., or it can be a phase difference plate in which two or more phase difference plates are stacked to control optical properties such as phase difference.
[0224] The phase difference plate can be selected to use a phase difference plate that satisfies the relationship of nx=ny>nz, nx>ny>nz, nx>ny=nz, nx>nz>ny, nz=nx>ny, nz>nx>ny, nz>nx=ny according to various uses. It should be noted that ny=nz includes not only the case where ny and nz are completely the same, but also the case where ny and nz are substantially the same.
[0225] For example, among the phase difference plates satisfying nx>ny>nz, it is preferred to use a phase difference plate whose front phase difference satisfies 40 to 100nm, whose thickness direction phase difference satisfies 100 to 320nm, and whose Nz coefficient satisfies 1.8 to 4.5. For example, for the phase difference plate (positive A plate) satisfying nx>ny=nz, it is preferred to use a phase difference plate whose front phase difference satisfies 100 to 200nm. For example, for the phase difference plate (negative A plate) satisfying nz=nx>ny, it is preferred to use a phase difference plate whose front phase difference satisfies 100 to 200nm. For example, for the phase difference plate satisfying nx>nz>ny, it is preferred to use a phase difference plate whose front phase difference satisfies 150 to 300nm, and whose Nz coefficient satisfies greater than 0 and less than 0.7. In addition, as described above, for example, a phase difference plate satisfying nx=ny>nz, nz>nx>ny, or nz>nx=ny can be used.
[0226] The transparent protective film can be appropriately selected according to the liquid crystal display device to be applied. For example, in the case of VA (Vertical Alignment, including MVA, PVA), it is preferred that the transparent protective film on at least one side (unit side) of the polarizing film has a phase difference. As a specific phase difference, it is preferably in the range of Re=0~240nm, Rth=0~500nm. When recorded in three-dimensional refractive index, it is preferred that nx>ny=nz, nx>ny>nz, nx>nz>ny, nx=ny>nz (positive A plate, biaxial, negative C plate) is used. In the VA type, it is preferably used in the form of a combination of a positive A plate and a negative C plate, or a bidirectional film. When a polarizing film is used on the upper and lower sides of the liquid crystal unit, the upper and lower sides of the liquid crystal unit may both have a phase difference, or any of the upper and lower transparent protective films may have a phase difference.
[0227] For example, it can be used in the case of IPS (In-Plane Switching, including FFS), the case where the transparent protective film on one side of the polarizing film has a phase difference, or the case where there is no phase difference. For example, the case where there is no phase difference is preferably the case where the upper and lower sides (unit sides) of the liquid crystal unit also have no phase difference. The case where there is a phase difference is preferably the case where both the upper and lower sides of the liquid crystal unit have a phase difference, or the case where either the upper and lower sides have a phase difference (for example, the upper side has a bidirectional film satisfying the relationship nx>nz>ny, and the lower side has no phase difference, or the upper side has a positive A plate, and the lower side has a positive C plate). In the case where there is a phase difference, the range of Re=-500~500nm and Rth=-500~500nm is preferred. When recorded in three-dimensional refractive index, nx>ny=nz, nx>nz>ny, nz>nx=ny, nz>nx>ny (positive A plate, biaxial, positive C plate) are preferred.
[0228] The transparent protective film may be further laminated with a releasable substrate to improve its mechanical strength and handling properties. The releasable substrate may be peeled off from the laminate containing the transparent protective film and the polarizer before or after laminating the transparent protective film and the polarizer, during the process or in another process.
[0229] <Method for producing polarizing film>
[0230] Below, refer to Figure 1 Each step in the method for producing a polarizing film of the present invention will be described.
[0231] <First coating step>
[0232] The first coating step is a step of coating the bonding composition on the bonding surface of the polarizer 2 to form a wet first coating film while conveying the polarizer 2. The bonding composition may be coated on one surface of the polarizer 2 or on both surfaces.
[0233] <Second coating step>
[0234] The second coating step is a step of coating the adhesive composition on the bonding surface of the transparent protective film 3 while the transparent protective film 3 is being conveyed to form a second coating film.
[0235] The polarizer 2 and the transparent protective film 3 may be subjected to surface modification treatment before the coating process. It is particularly preferred to perform surface modification treatment on the surface of the polarizer 2. Examples of surface modification treatments include corona treatment, plasma treatment, excimer treatment, and flame treatment, with corona treatment being particularly preferred. By performing corona treatment, reactive functional groups such as carbonyl and amino groups are generated on the surface of the polarizer 2, thereby improving adhesion to the adhesive layer. In addition, impurities on the surface can be removed or surface irregularities can be reduced by an ashing effect, thereby producing a polarizing film having excellent appearance characteristics.
[0236] The coaters 4 and 5 are not particularly limited, and examples thereof include reverse coaters, gravure coaters (direct, reverse, and offset), rod-type reverse coaters, roll coaters, die coaters, wire rod coaters, and bar coaters.
[0237] The method of applying the easy-bonding composition on the laminating surface of the polarizer 2 and the method of applying the adhesive composition on the laminating surface of the transparent protective film 3 can be appropriately selected according to the viscosity and target thickness of the above-mentioned compositions. From the viewpoint of removing foreign matter on the surface of the polarizer 2 and the transparent protective film 3, coating property, and thickness control of the coating film, it is preferred to utilize the post-measurement coating method. As a specific example of the post-measurement coating method, a gravure roller coating method, a forward roller coating method, an air knife coating method, a rod / rod coating method, etc. can be cited. Among these, from the viewpoint of removing foreign matter on the surface of the polarizer 2 and the transparent protective film 3, coating property, and thickness control of the coating film, a gravure roller coating method is particularly preferred.
[0238] In the gravure roller coating method, various patterns can be formed on the surface of the gravure roller, for example, a honeycomb pattern, a trapezoidal pattern, a lattice pattern, a conical pattern or a diagonal line pattern. In order to effectively prevent the appearance defects of the polarizing film finally obtained, the pattern formed on the surface of the gravure roller is preferably a honeycomb pattern. In the case of the honeycomb pattern, in order to improve the surface accuracy of the coated surface after coating, the unit volume is preferably 1 to 5 cm 3 / m 2 , more preferably 2 to 3 cm 3 / m 2 Similarly, in order to improve the surface accuracy of the coated surface after coating, the number of unit lines per inch of the roller is preferably 200 to 3000 lines / inch. In addition, the rotation speed ratio of the gravure roller relative to the travel speed of the polarizer 2 and the transparent protective film 3 is preferably 100 to 300%.
[0239] <First thickness measurement step>
[0240] The first thickness measurement process is a process for measuring the thickness of the wet first coating film online. The film thickness tester 6 for online measurement preferably uses an optical (non-contact) film thickness tester. The optical (non-contact) film thickness tester is not particularly limited, and examples thereof include: a spectroscopic interference film thickness tester, a reflection spectroscopic film thickness tester, and a confocal film thickness tester. A spectroscopic interference film thickness tester that can measure the thickness of the coating film with a total width is particularly preferred.
[0241] <Drying process>
[0242] The easy-adhesive composition contains water, therefore, after the thickness of the wet first coating film is measured online, the water in the wet first coating film is removed using a dryer 7. When water remains in the dry first coating film, water will remain in the uncured adhesive layer obtained by laminating the dry first coating film and the second coating film. As a result, undesirable conditions such as segregation of polymerization initiator in the uncured adhesive layer and hindering the cationic curing of the uncured adhesive layer will occur, thereby reducing the adhesion of the adhesive layer. Therefore, a drying process is provided and the water in the wet first coating film is removed as much as possible. The drying process can be carried out by methods well known to those skilled in the art, such as air drying, heat drying or hot air drying.
[0243] The temperature of the dryer 7 is not particularly limited, but is preferably 15 to 40° C., more preferably 20 to 35° C. The air volume of the dryer 7 is not particularly limited, but is preferably 3.8 to 30.0 m per unit width (m). 3 / min, more preferably 6.0 to 15.5m 3 / min.
[0244] <Dryness adjustment process>
[0245] After the above-mentioned drying process, the thickness of the dried first coating film is measured online by a film thickness tester 8, and the temperature and / or air volume of the dryer 7 are adjusted so that the ratio of the thickness of the wet first coating film obtained by the above-mentioned online measurement to the thickness of the dried first coating film satisfies the following formula (A), thereby adjusting the degree of dryness of the newly formed dried first coating film.
[0246] (Thickness of dry first coating film / Thickness of wet first coating film)-(Content ratio of water in the adhesive composition)≤0.05(A)
[0247] (Thickness of dry first coating film / thickness of wet first coating film)-(content of water in the easily adhesive composition) is preferably 0.04 or less, more preferably 0.03 or less, and even more preferably 0.02 or less.
[0248] The film thickness tester 8 used for online measurement preferably uses an optical (non-contact) film thickness tester. The optical (non-contact) film thickness tester is not particularly limited, and examples thereof include the above-mentioned film thickness tester. A spectroscopic interference film thickness tester that can measure the thickness of the dried first coating film with the total width is particularly preferred.
[0249] <Lamination process>
[0250] The laminating step is a step of laminating the dried first coating film formed on the laminating surface of the polarizer 2 and the second coating film formed on the laminating surface of the transparent protective film 3 to form an uncured adhesive layer. The laminating can be performed by a roll laminator 9 or the like.
[0251] <Bonding process>
[0252] The bonding step is a step of bonding the polarizer 2 and the transparent protective film 3 together via an adhesive layer obtained by curing an uncured adhesive layer to produce the polarizing film 1 .
[0253] After the polarizer 2 and the transparent protective film 3 are attached, active energy rays (electron beam, ultraviolet rays, visible light, etc.) are irradiated or heated to cure the uncured adhesive layer, thereby forming an adhesive layer. The irradiation direction of the active energy rays (electron beam, ultraviolet rays, visible light, etc.) can be irradiated from any appropriate direction. It is preferred to irradiate from the side of the transparent protective film 3. If irradiated from the side of the polarizer 2, there is a concern that the polarizer 2 will deteriorate due to the active energy rays (electron beam, ultraviolet rays, visible light, etc.).
[0254] The irradiation conditions in the case of electron beam irradiation can be any appropriate conditions as long as they are conditions that can cure the above-mentioned uncured adhesive layer. For example, the acceleration voltage in electron beam irradiation is preferably 5kV to 300kV, and more preferably 10kV to 250kV. When the acceleration voltage is less than 5kV, there is a concern that the electron beam cannot reach the uncured adhesive layer and the curing becomes insufficient. If the acceleration voltage is greater than 300kV, there is a concern that the penetration force is too strong and the transparent protective film and polarizer are damaged. The irradiation dose is preferably 5 to 100kGy, and more preferably 10 to 75kGy. When the irradiation dose is less than 5kGy, the uncured adhesive layer is not sufficiently cured. If it is greater than 100kGy, the transparent protective film and polarizer are damaged, the mechanical strength is reduced, yellowing occurs, and there is a tendency that the given optical properties cannot be obtained.
[0255] Electron beam irradiation is usually performed in an inert gas, but can be performed in the atmosphere with a small amount of oxygen introduced as needed. Depending on the material of the transparent protective film, oxygen is appropriately introduced so that oxygen is brought into contact with the transparent protective film surface that is first contacted by the electron beam, thereby causing oxygen barrier, thereby preventing damage to the transparent protective film and allowing efficient electron beam irradiation of only the uncured adhesive layer.
[0256] In the method for manufacturing the polarizing film of the present invention, as the active energy ray, it is preferred to use an active energy ray containing visible light in the wavelength range of 380nm to 450nm, especially an active energy ray with the largest irradiation amount of visible light in the wavelength range of 380nm to 450nm. When ultraviolet rays, visible light, and a transparent protective film endowed with ultraviolet absorption ability (ultraviolet non-transmissive transparent protective film) are used, light with a wavelength shorter than about 380nm is absorbed, so light with a wavelength shorter than 380nm does not reach the adhesive composition and does not contribute to its polymerization reaction. In addition, the light with a wavelength shorter than 380nm absorbed by the transparent protective film is converted into heat, and the transparent protective film itself generates heat, which becomes the cause of defects such as curling / wrinkling of the polarizing film. Therefore, in the present invention, when ultraviolet rays and visible light are used, it is preferred to use a device that does not emit light with a wavelength shorter than 380 nm as an active energy ray generating device. More specifically, the ratio of the cumulative illuminance in the wavelength range of 380 to 440 nm to the cumulative illuminance in the wavelength range of 250 to 370 nm is preferably 100:0 to 100:50, and more preferably 100:0 to 100:40. In the method for manufacturing a polarizing film of the present invention, as active energy rays, a metal halide lamp enclosed in gallium or an LED light source that emits light in the wavelength range of 380 to 440 nm is preferred. Alternatively, a light source containing ultraviolet rays and visible light, such as a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, an incandescent lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a metal halide lamp, a fluorescent lamp, a tungsten lamp, a gallium lamp, an excimer laser or sunlight, can be used, and ultraviolet rays with a wavelength shorter than 380 nm can also be blocked by a bandpass filter before use. In order to improve the adhesion performance of the adhesive layer between the polarizer and the transparent protective film and prevent curling of the polarizing film, it is preferred to use a metal halide lamp encapsulated with gallium, and use active energy rays obtained by a bandpass filter that can block light with a wavelength shorter than 380nm, or active energy rays with a wavelength of 405nm obtained using an LED light source.
[0257] It is preferred to heat the uncured adhesive layer before irradiation with ultraviolet rays or visible light (pre-irradiation heating), in which case, it is preferably heated to 40° C. or higher, more preferably heated to 50° C. or higher. It is also preferred to heat the adhesive layer after irradiation with ultraviolet rays or visible light (post-irradiation heating), in which case, it is preferably heated to 40° C. or higher, more preferably heated to 50° C. or higher.
[0258] The adhesive composition used in the present invention can be particularly suitably used in the case of forming an adhesive layer formed by bonding a polarizer to a transparent protective film having a transmittance of less than 5% at a wavelength of 365 nm. Here, the adhesive composition used in the present invention contains the above-mentioned photoradical polymerization initiator of the general formula (3), and can be cured to form an adhesive layer by irradiating ultraviolet rays through a transparent protective film having UV absorption ability. Therefore, even for a polarizing film having a transparent protective film having UV absorption ability laminated on both sides of the polarizer, the adhesive layer can be cured. However, of course, for a polarizing film having a transparent protective film without UV absorption ability laminated, the adhesive layer can also be cured. It should be noted that the transparent protective film having UV absorption ability refers to a transparent protective film having a transmittance of less than 10% for light at 380 nm.
[0259] Examples of a method for imparting UV absorption capability to a transparent protective film include a method of incorporating an ultraviolet absorber into the transparent protective film and a method of laminating a surface treatment layer containing an ultraviolet absorber on the surface of the transparent protective film.
[0260] Specific examples of the ultraviolet absorber include conventionally known oxybenzophenone compounds, benzotriazole compounds, salicylate compounds, benzophenone compounds, cyanoacrylate compounds, nickel complex compounds, triazine compounds, and the like.
[0261] In the method for producing a polarizing film of the present invention, the linear speed varies depending on the curing time of the uncured adhesive layer, and is preferably 1 to 500 m / min, more preferably 5 to 300 m / min, and further preferably 10 to 100 m / min. If the linear speed is too low, productivity is insufficient, or damage to the transparent protective film is too great, and a polarizing film that can withstand durability tests, etc. cannot be produced. If the linear speed is too high, the curing of the uncured adhesive layer may become insufficient, and the target adhesion may not be obtained.
[0262] <Adhesive layer>
[0263] The adhesive layer is formed by curing an uncured adhesive layer. The thickness of the adhesive layer is preferably 0.01 to 3 μm. When the thickness of the adhesive layer is too thin, the cohesive force of the adhesive layer is insufficient and the peeling force is reduced, which is not preferred. When the thickness of the adhesive layer is too thick, it is easy to cause peeling when stress is applied to the cross section of the polarizing film, and poor peeling due to impact occurs, which is not preferred. The thickness of the adhesive layer is more preferably 0.1 to 2.5 μm, and further preferably 0.5 to 1.5 μm.
[0264] <Optical film>
[0265] The polarizing film of the present invention can be used as an optical film laminated with other optical layers in practical use. The optical layer is not particularly limited, and examples thereof include optical layers that are sometimes used in the formation of liquid crystal display devices, such as phase difference films (including wave plates such as 1 / 2 wave plates and 1 / 4 wave plates), visual compensation films, brightness enhancement films, reflective plates, and anti-transmission plates.
[0266] As the retardation film, a retardation film having a front retardation of 40 nm or more and / or a thickness direction retardation of 80 nm or more can be used. The front retardation is usually controlled to be in the range of 40 to 200 nm, and the thickness direction retardation is usually controlled to be in the range of 80 to 300 nm.
[0267] As the phase difference plate, there are: birefringent films obtained by uniaxial or biaxial stretching of polymer raw materials, oriented films of liquid crystal polymers, and phase difference plates obtained by supporting the oriented layer of liquid crystal polymers with films. The thickness of the phase difference film is not particularly limited, and is generally about 20 to 150 μm.
[0268] As the retardation film, a reverse wavelength dispersion type retardation film satisfying the following formulas (1) to (3) can be used:
[0269] 0.70<Re
[450] / Re
[550] <0.97···(1)
[0270] 1.5×10 -3 <Δn<6×10 -3 ···(2)
[0271] 1.13<NZ<1.50···(3)
[0272] (Wherein, Re
[450] and Re
[550] are the in-plane phase difference values of the phase difference film measured at 23°C using light of wavelengths of 450nm and 550nm, respectively; Δn is nx-ny, i.e., in-plane birefringence, when the refractive indices in the slow axis direction and fast axis direction of the phase difference film are set to nx and ny, respectively; NZ is the ratio of nx-nz to nx-ny when nz is set to the refractive index in the thickness direction of the phase difference film, wherein nx-nz is the birefringence in the thickness direction and nx-ny is the in-plane birefringence).
[0273] The polarizing film or the optical film laminated with at least one polarizing film may be provided with an adhesive layer for bonding with other components such as a liquid crystal cell. The adhesive forming the adhesive layer is not particularly limited, and an adhesive having a base polymer such as acrylic polymer, silicone polymer, polyester, polyurethane, polyamide, polyether, fluorine, rubber, etc. may be appropriately selected and used. It is particularly preferred to use an adhesive such as an acrylic adhesive that has excellent optical transparency and exhibits appropriate adhesive properties such as wettability, cohesion and adhesion, and has excellent weather resistance, heat resistance, etc.
[0274] The adhesive layer may be provided on one or both sides of the polarizing film or optical film in the form of a laminated layer of layers of different compositions or types. In addition, when provided on both sides, adhesive layers of different compositions, types, thicknesses, etc. may be formed on the surface and back of the polarizing film or optical film. The thickness of the adhesive layer may be appropriately determined according to the purpose of use, adhesive strength, etc., and is usually 1 to 500 μm, preferably 1 to 200 μm, and particularly preferably 1 to 100 μm.
[0275] The exposed surface of the adhesive layer is temporarily covered by a diaphragm for the purpose of preventing contamination during the period until it is actually used. Thus, it is possible to prevent contact with the adhesive layer under normal handling conditions. As a diaphragm, in addition to the above-mentioned thickness conditions, a diaphragm such as a diaphragm coated with a suitable thin layer such as a plastic film, a rubber sheet, paper, a cloth, a non-woven fabric, a net, a foam sheet, a metal foil, or a laminate thereof with a suitable release agent such as silicone, a long-chain alkyl, a fluorine, or molybdenum sulfide as required can be used.
[0276] <Image Display Device>
[0277] The polarizing film or optical film of the present invention can be preferably used for forming various devices such as liquid crystal display devices. The formation of the liquid crystal display device can be carried out in a conventional manner. That is, the liquid crystal display device is usually formed by appropriately assembling a liquid crystal cell with a polarizing film or optical film, and components such as a lighting system used as needed, and loading a driving circuit, etc. In the present invention, except for the use of the polarizing film or optical film of the present invention, there is no particular limitation, and it can be carried out in a conventional manner. Regarding the liquid crystal cell, any type of liquid crystal cell such as TN type, STN type, π type, etc. can be used.
[0278] Suitable liquid crystal display devices such as a liquid crystal display device with a polarizing film or an optical film disposed on one side or both sides of a liquid crystal cell, and a liquid crystal display device using a backlight or a reflector in the lighting system can be formed. In this case, the polarizing film or the optical film of the present invention can be disposed on one side or both sides of the liquid crystal cell. In the case where the polarizing film or the optical film is disposed on both sides, they can be the same or different. Furthermore, when forming the liquid crystal display device, one or more layers of suitable components such as a diffusion plate, an anti-glare layer, an anti-reflection film, a protective plate, a prism array, a lens array sheet, a light diffusion plate, a backlight, etc. can be disposed at a suitable position.
[0279] Example
[0280] Although examples of the present invention are described below, the embodiments of the present invention are not limited to these.
[0281] <Polarizing filter>
[0282] First, a laminate having a 9 μm thick PVA layer formed on an amorphous PET substrate was subjected to auxiliary stretching in a gas atmosphere at a stretching temperature of 130°C to produce a stretched laminate. Next, the stretched laminate was dyed to produce a colored laminate. The colored laminate was further stretched in a boric acid aqueous solution at a stretching temperature of 65 degrees so that the total stretching ratio became 5.94 times and the laminate was stretched together with the amorphous PET substrate to produce an optical film laminate containing a 5 μm thick PVA layer. By such two-step stretching, an optical film laminate containing a 5 μm thick PVA layer constituting a thin polarizer can be obtained. The PVA molecules of the PVA layer formed on the amorphous PET substrate of the thin polarizer are highly oriented, and the iodine adsorbed by dyeing is highly oriented in one direction in the form of a polyiodide ion complex. The moisture content of the thin polarizer (PVA layer) is 10% by mass.
[0283] <Transparent protective film>
[0284] As the transparent protective film, a cycloolefin polymer film having a thickness of 13 μm (ZF-14 manufactured by ZEON Corporation of Japan) was used.
[0285] <Active energy rays>
[0286] As active energy rays, a UV irradiation device (a high-pressure mercury lamp manufactured by Toshiba Corporation) was used to irradiate from the transparent protective film side with a maximum illuminance of 500 mW / cm 2 、Accumulated light intensity 800mJ / cm 2 Ultraviolet rays are used to make polarizing films.
[0287] <Preparation of easy-adhesion composition>
[0288] An easily adhesive composition was prepared by mixing 54 parts by mass of 4-hydroxybutyl acrylate, 1 part by mass of 3-acrylamidephenylboric acid (manufactured by Junsei Chemical Co., Ltd.), and 45 parts by mass of water, and stirring at 25° C. for 10 minutes. The water content in the easily adhesive composition was 0.45.
[0289] <Preparation of Adhesive Composition>
[0290] ω-carboxy polycaprolactone (n≈2) monoacrylate (M5300, manufactured by Toagosei Co., Ltd.) 5 parts by mass, isobornyl acrylate 10 parts by mass, acryloyl morpholine (ACMO, manufactured by Kojin Co., Ltd., SP value: 22.9) 20 parts by mass, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate (CELLOXIDE 2021P, manufactured by Daicel Chemical Co., Ltd.) 1 part by mass, 2,4,6-trimethylbenzoyldiphenylphosphine oxide (TPO, manufactured by Ciba Specialty Chemicals Co., Ltd.), and p-phenylthiophenyl diphenylsulfonium PF 60 were mixed. 6 2 parts by mass of sodium bicarbonate (CPI-110P manufactured by San-Apro Ltd.) was mixed and stirred at 50° C. for 1 hour to prepare an adhesive composition.
[0291] Example 1
[0292] The prepared easy-adhesion composition was applied to the PVA surface of the produced optical film laminate including a 5 μm thick PVA layer at an initial set thickness of 1190 nm using a gravure roll coating method with a gravure roll to continuously form a wet first coating film.
[0293] On the other hand, in another continuous production line, the prepared adhesive composition was applied to the bonding surface of the transparent protective film at an initial set thickness of 1500 nm using a gravure roll coating method equipped with a gravure roll to continuously form a second coating film.
[0294] Then, the thickness of the wet first coating film was measured online on a continuous production line using a spectroscopic interference film thickness tester (manufactured by Haiyang Optical Co., Ltd.: spectrometer "USB2000+", light source "HL-2000", optical fiber "OCF-103995").
[0295] Furthermore, on a continuous production line, a dryer was used at 25°C and an average air volume per unit width (m) of 12.5 m 3 / min is used to dry the first wet coating film to remove the water, and the thickness of the first dried coating film is measured online using a spectroscopic interference film thickness tester (manufactured by Haiyang Optics: spectrometer "USB2000+", light source "HL-2000", optical fiber "OCF-103995"), and the temperature and air volume of the dryer are adjusted based on the measurement results to adjust the degree of dryness of the newly formed first dried coating film. It should be noted that the degree of dryness of the first dried coating film is adjusted by appropriately adjusting the temperature of the dryer to 22 to 28°C and the air volume to 6.0 to 15.5 m / s in a manner that satisfies the following formula (A). 3 / min.
[0296] (Thickness of dry first coating film / Thickness of wet first coating film)-(Content ratio of water in the adhesive composition)≤0.05(A)
[0297] Next, a roller machine was used to laminate the dried first coating formed on the laminating surface of the optical film laminate and the second coating formed on the laminating surface of the transparent protective film to form an uncured adhesive layer. Then, the ultraviolet rays were irradiated from the laminated transparent protective film side by an active energy ray irradiation device to bond the polarizer and the transparent protective film via the adhesive layer, and then hot air drying was performed at 70°C for 3 minutes to peel off and remove the amorphous PET substrate, thereby obtaining a polarizing film having a transparent protective film on one side of the polarizer. The lamination was performed at a line speed of 25 m / min. Through the above series of steps, the polarizing film was continuously manufactured for 15 hours.
[0298] Comparative Example 1
[0299] The prepared easy-adhesion composition was applied to the PVA surface of the produced optical film laminate including a 5 μm thick PVA layer at an initial set thickness of 1195 nm using a gravure roll coating method with a gravure roll to continuously form a wet first coating film.
[0300] On the other hand, in another continuous production line, the prepared adhesive composition was applied to the bonding surface of the transparent protective film at an initial set thickness of 1500 nm using a gravure roll coating method equipped with a gravure roll to continuously form a second coating film.
[0301] Then, the thickness of the wet first coating film was measured online on a continuous production line using a spectroscopic interference film thickness tester (manufactured by Haiyang Optical Co., Ltd.: spectrometer "USB2000+", light source "HL-2000", optical fiber "OCF-103995").
[0302] Furthermore, on a continuous production line, a dryer was used at 25°C and an average air volume per unit width (m) of 12.5 m 3The drying was performed at an initial setting of 100 rpm to remove water in the wet first coating film, thereby forming a dry first coating film.
[0303] Next, a roller machine was used to laminate the dried first coating formed on the laminating surface of the optical film laminate and the second coating formed on the laminating surface of the transparent protective film to form an uncured adhesive layer. Then, the ultraviolet rays were irradiated from the laminated transparent protective film side by an active energy ray irradiation device to bond the polarizer and the transparent protective film via the adhesive layer, and then hot air drying was performed at 70°C for 3 minutes to peel off and remove the amorphous PET substrate, thereby obtaining a polarizing film having a transparent protective film on one side of the polarizer. The lamination was performed at a line speed of 25 m / min. Through the above series of steps, the polarizing film was continuously manufactured for 15 hours.
[0304] Comparative Example 2
[0305] The prepared easy-adhesion composition was applied to the PVA surface of the produced optical film laminate including a 5 μm thick PVA layer at an initial set thickness of 1200 nm using a gravure roll coating method with a gravure roll to continuously form a wet first coating film.
[0306] On the other hand, in another continuous production line, the prepared adhesive composition was applied to the bonding surface of the transparent protective film at an initial set thickness of 1500 nm using a gravure roll coating method equipped with a gravure roll to continuously form a second coating film.
[0307] Then, the thickness of the wet first coating film was measured online on a continuous production line using a spectroscopic interference film thickness tester (manufactured by Haiyang Optical Co., Ltd.: spectrometer "USB2000+", light source "HL-2000", optical fiber "OCF-103995").
[0308] Furthermore, on a continuous production line, a dryer was used at 25°C and an average air volume per unit width (m) of 12.5 m 3 By drying at an initial setting of 100 rpm / min, water in the wet first coating film was removed to form a dry first coating film.
[0309] Next, a roller machine was used to laminate the dried first coating formed on the laminating surface of the optical film laminate and the second coating formed on the laminating surface of the transparent protective film to form an uncured adhesive layer. Then, the ultraviolet rays were irradiated from the laminated transparent protective film side by an active energy ray irradiation device to bond the polarizer and the transparent protective film via the adhesive layer, and then hot air drying was performed at 70°C for 3 minutes to peel off and remove the amorphous PET substrate, thereby obtaining a polarizing film having a transparent protective film on one side of the polarizer. The lamination was performed at a line speed of 25 m / min. Through the above series of steps, the polarizing film was continuously manufactured for 15 hours.
[0310] (Evaluation of Adhesion Strength)
[0311] The polarizing film was cut into 200 mm in a direction parallel to the stretching direction of the polarizer and 15 mm in a direction perpendicular to the polarizer 5 minutes and 15 hours after the start of production, and the polarizing film was bonded to a glass plate. Then, a cutter was used to cut an incision between the transparent protective film and the polarizer, and the transparent protective film and the polarizer were peeled off at a peeling speed of 1000 mm / min in a tensile testing machine in a 90-degree direction, and the peeling strength (N / 15 mm) was measured, and the adhesive strength was evaluated according to the following criteria.
[0312] ○: When the peeling force is 1N or more
[0313] ×: When the peeling force is less than 1N
[0314] (Evaluation of bubbles)
[0315] The number of bubbles on both sides of the polarizing film was counted by optical microscope observation 5 minutes and 15 hours after the start of production. The number of bubbles was counted in an area of 5 cm x 5 cm, and the case where the total number of bubbles on both sides was less than 3 was evaluated as ○, and the case where 3 or more was evaluated as ×.
[0316]
[0317] According to Table 2, in Example 1, the drying degree adjustment step was performed, so that in the continuous production, the variation of the drying degree of the first coating film was suppressed, and a polarizing film with excellent adhesive strength could be stably obtained even 15 hours after the start of production. In addition, it can be seen that the generation of bubbles was suppressed in the obtained polarizing film. On the other hand, it can be seen that in Comparative Examples 1 and 2, the drying degree adjustment step was not performed, so that in the continuous production, the variation of the drying degree of the first coating film became large. For the polarizing film 15 hours after the start of production, the cationic polymerization reaction was hindered by the water remaining in the first coating film, and therefore, the adhesive strength of the adhesive layer was low.
[0318] Industrial Applicability
[0319] The polarizing film of the present invention can be used alone in image display devices such as liquid crystal display devices (LCD), organic EL display devices, CRT, PDP, etc., or in the form of an optical film laminated with the polarizing film.
Claims
1. A method for manufacturing a polarizing film, wherein a transparent protective film is provided on at least one side of a polarizer via an adhesive layer, the method comprising: a first coating step of coating a bonding surface of the polarizer with an easily adhesive composition containing water and a hydrophilic monomer to form a wet first coating film while the polarizer is being conveyed; a second coating step of coating an adhesive composition containing a radical polymerizable compound and a cation polymerizable compound on the bonding surface of the transparent protective film while the transparent protective film is being conveyed to form a second coating film; a first thickness measuring step of measuring the thickness of the wet first coating film online; After the first thickness measuring step, a drying step of removing water from the wet first coating film using a dryer to form a dry first coating film; After the drying step, a second thickness measuring step of measuring the thickness of the dried first coating film online; A drying degree adjusting step of adjusting the degree of dryness of the newly formed dry first coating film by adjusting the temperature and / or air volume of the drying machine so that the ratio of the thickness of the wet first coating film obtained by the online measurement to the thickness of the dry first coating film satisfies the following formula (A); a laminating step of laminating the dried first coating film formed on the laminating surface of the polarizer and the second coating film formed on the laminating surface of the transparent protective film to form an uncured adhesive layer; and a bonding step of bonding the polarizer and the transparent protective film together via the adhesive layer obtained by curing the uncured adhesive layer, (Thickness of the dry first coating film / Thickness of the wet first coating film)-(Content ratio of water in the easy-adhesion composition)≤0.05(A), The water content of the polarizer is 15% by mass or less, and the water content is 40 to 70% by mass when the total amount of the easy-adhesion composition is 100% by mass.
2. The method for producing a polarizing film according to claim 1, wherein: The easy-adhesion composition contains a compound represented by the following general formula (1) and / or an organic metal compound having a MO bond in the structural formula. In formula (1), X is a functional group containing a reactive group, R 1 and R 2 Each independently represents a hydrogen atom, an aliphatic hydrocarbon group which may have a substituent, an aryl group or a heterocyclic group, M is silicon, titanium, aluminum or zirconium, and O is an oxygen atom.
3. The method for manufacturing a polarizing film according to claim 2, wherein: The compound represented by the general formula (1) is a compound represented by the following general formula (1'): In formula (1'), Y is an organic group, X, R 1 and R 2 Same meaning as above.
4. The method for manufacturing a polarizing film according to claim 2, wherein: The reactive group possessed by the compound represented by the general formula (1) is at least one reactive group selected from the group consisting of an α,β-unsaturated carbonyl group, a vinyl group, a vinyl ether group, an epoxy group, an oxetanyl group, an amino group, an aldehyde group, a mercapto group and a halogen group.
5. The method for producing a polarizing film according to any one of claims 1 to 4, wherein: The first coating step and the second coating step are coating steps using a post-measurement coating method.
6. The method for manufacturing a polarizing film according to claim 5, wherein: The post-measurement coating method is a gravure roll coating method using a gravure roll.
Citation Information
Patent Citations
JP1973015544B1
JP1975046721A
JP1975048120A
Method for manufacturing polarizing plate and liquid crystal display device
JP2001296427A
Protective film for polarizer and its manufacturing method
JP2001343529A