A layered cathode material for batteries, its preparation method and application
By forming a pinned heterophase structure on the crystal structure surface of the layered positive electrode material of the lithium-ion battery, the problems of slip, collapse and microcrack of the transition group metal layer are solved, and the high voltage cycle stability and capacity of the battery are improved, so as to achieve More excellent electrochemical properties.
Patent Information
- Application Number
- CN202180007629.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-10-09
AI Technical Summary
The existing lithium-ion battery layered positive electrode material is formed during the high voltage charging and discharge process due to the slip, collapse, twisting and microcracks of the transition group metal layer, resulting in rapid attenuation of capacity. The existing coating treatment is difficult to effectively solve these problems.
The heterogeneous phase structure is used to pierce the surface of the crystal structure through pinning to form a uniform crystal surface layer, build a three-dimensional lithium ion diffusion network, isolate the electrolyte, inhibit interface side reactions, and improve the phase stability of the layered positive electrode material.
The electrochemical performance of the layered cathode material is significantly improved, especially under high voltage conditions, which shows excellent capacity, magnification and cycling stability, extending the service life of the battery.
Smart Images

Figure CN114930576B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery cathode materials, and particularly to a layered cathode material for batteries, a preparation method thereof, and an application thereof. Background Art
[0002] With the development of the times, the increasing demand for energy has led to energy shortages and environmental deterioration becoming global problems.
[0003] Currently, fossil fuels, as the main energy source for humans, produce a large amount of CO 2 and other greenhouse gases during use, causing the earth's temperature to rise and the ecological environment to deteriorate. Based on this, China has proposed the national strategies of "carbon peak" and "carbon neutrality" to achieve the transformation of the national energy utilization method from non-renewable fossil energy to renewable clean energy, such as wind energy, solar energy, etc. This transformation presents opportunities and challenges for the development and application of energy storage devices.
[0004] Since the advent of lithium-ion batteries, due to advantages such as high open-circuit voltage, long cycle life, high power density, low self-discharge, and no memory effect, they have shown broad application prospects not only in the 3C application fields, including mobile phones, digital cameras, laptop computers, etc., but also in application fields such as electric vehicles, drones, and electric boats.
[0005] The performance of lithium-ion batteries is closely related to the selection, preparation process, and performance of the battery electrode materials. Currently, lithium cobaltate LiCoO 2 and ternary cathode materials Li[Ni x Co y Mn 1-x-y O 2 (0 < x < 1, 0 < y < 1) have become the cathode materials for lithium batteries such as 3C digital products, drones, and electric vehicle power sources due to characteristics such as high capacity, high rate, and simple synthesis process. Both of these two types of cathode materials have a typical layered structure, that is, a crystal structure in which transition metal layers and lithium layers are alternately stacked. During the charge and discharge process of the layered structure of these two types of cathode materials, along with the repeated Li + insertion / extraction process, the transition metal layer will undergo slip, stacking fault, distortion, and even microcracks will be generated. This situation is particularly serious during the high-voltage charge and discharge process. During the repeated high-voltage charge and discharge process, the slip, stacking fault, distortion, and generation of microcracks in the transition metal layer lead to the collapse of the interface structure, pulverization of the active material, and the aggravation of interface side reactions caused by high-valence active Ni / Co ions, etc., ultimately resulting in an increase in battery internal resistance and rapid capacity decay.
[0006] To solve the above problems, the more effective strategy currently adopted is to coat the surface of the active material. The interface coating generally has high ionic conductivity and can effectively isolate the direct contact between the electrolyte and the active material. Although these strategies can help inhibit side reactions and delay the increase of internal resistance, they have no significant effect on solving the problems of transition metal layer slip, collapse, distortion and microcrack formation.
[0007] Therefore, how to effectively solve the slippage, collapse, distortion and microcrack formation of transition metal layers is the key to fundamentally solving the rapid capacity decay of battery layered positive electrode materials, and is also the research focus and difficulty in this field. Summary of the invention
[0008] The purpose of the present application is to provide an improved battery layered positive electrode material and a preparation method and application thereof.
[0009] This application adopts the following technical solutions:
[0010] One aspect of the present application discloses a battery layered positive electrode material, the crystal structure of which has a heterogeneous phase structure that is pinned into the surface interface layer and the bulk layer of the crystal structure; the heterogeneous phase structure is evenly distributed on the surface of the crystal structure, encapsulating the crystal structure and forming a uniform crystal surface layer.
[0011] It should be noted that the battery layered positive electrode material of the present application has a heterogeneous phase structure on the surface of the crystal structure, and the heterogeneous phase at the interface is pinned into each layer, which can play a role in ensuring the stability of each layered phase, and fundamentally solve the problems of slippage, collapse, distortion and microcracks of each layer of the battery layered positive electrode material; and the crystal surface layer of the coated crystal structure formed by the heterogeneous phase structure can isolate the electrolyte, inhibit the interface side reaction, and solve the problem of rapid capacity decay of the battery layered positive electrode material. Therefore, the battery layered positive electrode material of the present application greatly improves the electrochemical performance of the layered positive electrode material, especially at high voltage (>4.3Vv.Li / Li + ) shows excellent capacity, rate and cycle stability under charge and discharge conditions. In the present application, the so-called "heterogeneous phase structure" refers to a structure formed by element replacement or doping on the surface interface of the crystal structure of the battery layered positive electrode material, that is, the element composition is different from that of the battery layered positive electrode material; in one implementation of the present application, this "heterogeneous phase structure" is formed by the extension of the bulk layer lattice of the crystal structure of the battery layered positive electrode material, and is a spinel phase or rock salt phase structure with a eutectic lattice of the bulk layer of the crystal structure of the battery layered positive electrode material.
[0012] It should also be noted that the battery layered positive electrode material of the present application, whose heterogeneous phase structure is pinned into the bulk phase layers and surface interfaces of the crystal structure, can also construct a three-dimensional lithium ion diffusion network to improve cycle stability, capacity and rate performance. It can be understood that the crystal surface layer of the present application is the surface layer formed by the heterogeneous phase structure uniformly coating the crystal structure; the crystal surface layer of the present application is a layer coated on the surface of the crystal structure formed from the microscopic crystal structure level, which is essentially different from the existing macroscopic positive electrode material surface coating modification.
[0013] In one implementation of the present application, the heterogeneous phase structure is a spinel phase or a rock salt phase structure.
[0014] It should be noted that the spinel phase structure and the rock salt phase structure are only heterogeneous phase structures specifically formed in one implementation of the present application and pinned into each layer of the crystal structure, and other heterogeneous phase structures are not excluded.
[0015] In one implementation of the present application, the heterogeneous phase structure is formed by epitaxial growth of the bulk phase layer of the crystal structure of the battery layered positive electrode material to the surface interface layer of the crystal structure according to the same lattice, that is, the heterogeneous phase structure and the bulk phase layer of the crystal structure share a lattice.
[0016] It should be noted that the eutectic lattice heterogeneous phase structure is only one implementation method of the present application, which is formed by epitaxial growth of the lattice of the bulk phase layer. Theoretically, as long as a pinned heterogeneous phase structure can be formed, other non-eutectic lattice methods are not excluded.
[0017] In one implementation of the present application, the thickness of the crystal surface layer is greater than or equal to 10 nm.
[0018] It should be noted that the crystal surface layer of the present application is actually a microstructure layer located on the surface of the crystal structure formed by the heterogeneous phase structure covering the crystal structure; therefore, the thickness of the crystal surface layer is actually the depth of the pinned heterogeneous phase structure into each layer of the crystal structure. In order to ensure the stabilizing effect of the heterogeneous phase structure on each layered phase and the isolation effect of the crystal surface layer on the electrolyte, the present application preferably has a crystal surface layer thickness of not less than 10nm.
[0019] In one implementation of the present application, the battery layered positive electrode material is Li 1+x TMO 2+y , wherein 0≤x≤1, 0≤y≤1, and TM is at least one of Co, Mn, Ni and Al.
[0020] It should be noted that the lithium-ion battery layered positive electrode material is only a battery layered positive electrode material specifically tested in one implementation of the present application. According to the inventive concept of the present application, it is not excluded that it can also be other ion battery layered positive electrode materials. It can be understood that the transition metal is at least one of Co, Mn, Ni and Al, which are just more common lithium-ion battery layered positive electrode materials, and it is not excluded that it can also be other transition metals.
[0021] In one implementation of the present application, the battery layered positive electrode material is at least one of lithium cobalt oxide, high nickel binary material, high nickel multi-element material, and lithium manganese-rich positive electrode material; wherein high nickel means that the nickel content is greater than or equal to 50%.
[0022] It should be noted that the binary materials and multi-component materials in this application refer to positive electrode materials containing two or more of nickel, cobalt, manganese, aluminum, etc.; that is, binary materials are positive electrode materials containing two of them; multi-component materials are positive electrode materials containing more than two of them, for example, containing three of them, that is, ternary materials.
[0023] In one implementation of the present application, the layered positive electrode material of the battery is LiNi 0.8 Co 0.1 Mn 0.1 O 2 、LiNi 0.5 Co 0.3 Mn 0.2 O 2 and LiCoO 2 At least one of .
[0024] It can be understood that the above-mentioned several specific battery layered positive electrode materials are only several lithium-ion battery layered positive electrode materials specifically prepared in one implementation of the present application, and other battery layered positive electrode materials may also be used.
[0025] In one implementation of the present application, the constituent elements of the crystal surface layer include cations and anions, the cations include at least one of Li, Co, Mn, Ni, Al, B, Mg, Ca and Zn, and the anions include O and / or F.
[0026] In one implementation of the present application, the content of Al, B, Mg, Ca, Zn and / or fluorine gradually increases from the inside to the outside, and the content of Co, Mn, Ni and / or O gradually decreases from the inside to the outside.
[0027] It should be noted that in one implementation of the present application, the layer of the heterogeneous phase structure of the eutectic lattice is mainly composed of the elements in the raw materials used in the pretreatment and the elements in the battery layered positive electrode material, and the two are formed by the mutual diffusion of anions and cations during heat treatment. Therefore, the constituent elements of the heterogeneous phase structure layer are mainly composed of the pretreated raw materials and the battery layered positive electrode material. It can be understood that although the heterogeneous phase is formed by the lattice epitaxial growth of the bulk layer of the crystal structure; however, according to the source of its constituent elements, each element is distributed in a gradient from the inside to the outside, increasing or decreasing. For example, the constituent elements are mainly provided by the battery layered positive electrode material Co, Mn, Ni and O, and their content gradually decreases from the inside to the outside; the constituent elements are mainly provided by the pretreated raw materials Al, B, Mg, Ca, Zn and fluorine, and their content gradually increases from the inside to the outside. In the present application, from the inside to the outside refers to from the bulk layer of the crystal structure to the surface layer.
[0028] Another aspect of the present application discloses a method for preparing the battery layered positive electrode material of the present application, comprising subjecting a conventional battery layered positive electrode material to the following treatment to obtain a battery layered positive electrode material having a pinned heterogeneous phase structure in the crystal structure;
[0029] Step 1: pretreating conventional battery layered positive electrode materials by at least one of the following methods:
[0030] (a) Solution immersion method, which involves immersing conventional battery layered cathode materials in a solution containing Li + , borate, Al 3+ Mg 2+ , Ca 2+ 、Zn 2+ and F - The immersion condition is 0-160° C. and 1-24 h to obtain a pretreated battery layered positive electrode material;
[0031] (b) Sol-gel method, which involves mixing conventional battery layered cathode materials with Li-containing + , borate, Al 3+ Mg 2+ , Ca 2 + 、Zn 2+ and F - uniformly mixing at least one of the sol-gels, heating and drying, to obtain a pre-treated battery layered positive electrode material;
[0032] (c) Ball milling, which involves mixing conventional battery layered cathode materials with Li-containing + , borate, Al 3+ Mg 2+ , Ca 2+ 、Zn 2+ and F -ball-milling the at least one solid material to obtain a pre-treated battery layered positive electrode material;
[0033] Step 2: heat-treat the pretreated battery layered positive electrode material obtained in step 1 at 400-700°C for more than the threshold time in an inert atmosphere or a reducing atmosphere, and then control the cooling rate to be less than or equal to 1°C / min, and cool it to room temperature to obtain a battery layered positive electrode material having a pinned heterogeneous phase structure in the crystal structure and a crystal surface thickness greater than or equal to 10nm; wherein the inert atmosphere is a nitrogen or argon atmosphere; the reducing atmosphere is a nitrogen + hydrogen atmosphere, or an argon + hydrogen atmosphere. The threshold time satisfies the formula τ = 36-0.04T, wherein τ is the threshold time, in h; T is the heat treatment temperature, in °C. In other words, the higher the heat treatment temperature, the smaller the threshold time.
[0034] It should be noted that in the present application, by subjecting the pretreated layered cathode material in step 1 to a heat treatment at a high temperature of 400-700°C for a time exceeding the threshold value, and at the same time, controlling the cooling rate to be less than or equal to 1°C / min, it is a necessary condition for forming a surface heterogeneous phase structure with a eutectic lattice of the bulk layered structure. By controlling the heat treatment time at high temperature, the diffusion of the surface-added replacement metal and fluorine elements to the internal bulk layered structure can be achieved, and the heterogeneous phase structure with the eutectic lattice of the bulk layered structure is gradually formed during the diffusion process; at the same time, the slower cooling rate ensures that the heterogeneous phase structure with the eutectic lattice of the bulk layered structure can be completely retained from high temperature to room temperature, and eliminates the internal stress of the material caused by the two-phase eutectic lattice. In the present application, the selection of the heat treatment process in step 2 can also make the thickness of the heterogeneous phase structure in the surface area of the layered cathode material greater than or equal to 10nm, so as to ensure that the surface area heterogeneous phase has sufficient pinning effect on the layered structure, thereby inhibiting the slip, collapse and microcrack generation of the layered structure under high voltage.
[0035] It should also be noted that in step 1 of the present application, a thin and uniform covering is introduced on the surface of the original layered positive electrode material powder by solution immersion, sol-gel method, and ball milling method, but the biggest role of this covering is to replace / diffusion of elements in the surface area of the material in step 2 to form a surface interface heterogeneous phase structure layer with a thickness greater than 10nm, which is very different from the role of the traditional coating layer in conducting lithium and isolating the electrolyte. It should also be noted that the heat treatment time in step 2 needs to be long enough, and at the same time, the cooling rate after the heat treatment is slow enough to obtain a uniform heterogeneous phase structure area with sufficient thickness on the surface, so as to play a role in pinning and stabilizing the bulk layered material during the high voltage cycle, which is also very different from the traditional coating layer. If the heat treatment time is too short or the cooling rate is too fast, the thickness of the heterogeneous phase region on the surface of the material is less than 10nm, which is not enough to keep the layered structure of the layered positive electrode material with a particle size of more than 5μm stable under high voltage charge and discharge conditions. It is difficult to avoid layered structure slippage, collapse, and microcracks caused by large structural stress inside the material, which ultimately affects the cycle stability of the layered positive electrode material.
[0036] It should also be noted that the heterogeneous phase structure on the surface of the layered positive electrode material is closely related to the heat treatment temperature and time. Generally speaking, under the premise of "heat treatment at a high temperature of 400-700°C for a time exceeding the threshold, and at the same time, controlling the cooling rate to be less than 1°C / min", the higher the temperature, the longer the heat treatment time, and the slower the cooling rate, the easier it is to form a spinel phase structure, and vice versa, it is easy to form a rock salt phase structure. The rock salt phase structure can also pin the layers of the crystal structure, playing a role in ensuring the stability of each layer.
[0037] In this application, conventional battery layered positive electrode materials refer to battery layered positive electrode materials with a normal main metal layer on the surface of the crystal structure; for example, conventional LiCoO 2 , that is, the surface of the crystal structure is a normal lithium layer, and the lithium cobalt oxide has a normal lithium oxygen structure. The present application directly performs pretreatment and subsequent heat treatment on conventional battery layered positive electrode materials to obtain the battery layered positive electrode material of the present application, the surface of which has a heterogeneous phase structure with a eutectic lattice with the bulk layered structure.
[0038] Another aspect of the present application discloses the application of the battery layered positive electrode material of the present application in the preparation of power batteries, large-scale energy storage batteries, or lithium-ion batteries for 3C consumer electronic products, drones or electronic cigarettes.
[0039] It can be understood that the battery layered positive electrode material of the present application has the advantages of high voltage, high reversible charge and discharge capacity, high rate and good cycle stability, and can be better used in power batteries or large-scale energy storage batteries, such as power batteries for electric vehicles or other medium and large electric equipment. Similarly, the battery layered positive electrode material of the present application can also be used in lithium-ion batteries for 3C consumer electronic products, drones or electronic cigarettes.
[0040] Another aspect of the present application discloses a lithium-ion battery using the battery layered positive electrode material of the present application.
[0041] It can be understood that the lithium-ion battery of the present application, due to the use of the battery layered positive electrode material of the present application, enables the battery to operate at a higher charge and discharge voltage, and has a higher reversible charge and discharge capacity and rate, and better cycle stability.
[0042] The beneficial effects of this application are:
[0043] The battery layered positive electrode material of the present application has a heterogeneous phase structure pinned into each layer in its crystal structure. The pinning effect of the heterogeneous phase structure can, on the one hand, ensure the stability of each layered phase and solve the problems of slip, collapse, distortion and microcracks of each layer in the crystal structure; on the other hand, the crystal surface layer formed by the heterogeneous phase structure can conduct electricity and lithium, and play a role in isolating the electrolyte at the interface. The battery layered positive electrode material of the present application also has high capacity, rate and cycle stability at a high voltage greater than 4.3V, and exhibits excellent electrochemical performance under high voltage charge and discharge conditions. In addition, the preparation method of the battery layered positive electrode material of the present application is simple and easy to large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is LiCoO in the embodiment of this application. 2 XRD characterization results of @LCAF-S;
[0045] Figure 2 It is LiCoO in the embodiment of this application. 2 @LCAF-S surface morphology, element distribution and electron diffraction characteristics analysis results;
[0046] Figure 3 It is LiCoO in the embodiment of this application. 2 @LCAF-S vs. conventional LiCoO 2 Positive electrode at 3-4.6V vs.Li / Li + The left figure is a comparison of the rate performance of the two, and the right figure is a comparison of the cycle stability of the two. DETAILED DESCRIPTION
[0047] In recent years, the academic and industrial communities have been eager to achieve a greater reversible capacity storage for lithium-ion batteries by increasing the charge and discharge voltage. However, for layered cathode active materials represented by lithium cobaltate LiCoO 2 and ternary cathode materials Li[Ni x Co y Mn 1-x-y O 2 (0 < x < 1, 0 < y < 1), during the cycling process at high voltage (>4.35V vs. Li / Li + ), they not only face the problem of increased internal resistance of the battery due to the increase in interfacial side reactions, but more importantly, in the bulk of the material, problems such as the slip, collapse, distortion, and formation of microcracks of the transition metal layer due to the phase structure evolution will occur, ultimately leading to the pulverization of the active material. The pulverization of the active material further promotes the interfacial side reactions between the active material and the electrolyte, further increasing the internal resistance and accelerating the decay of the battery performance. That is to say, the main problem faced by layered cathode materials at high voltage is the problem of the accumulation of internal stress in the material caused by a large number of ion insertions / extractions, which induces the slip, collapse, and crack growth of the layered structure. Therefore, at high voltage, if we want to solve this problem, the most important thing is to propose a strategy to improve the stability of the layered structure.
[0048] Based on this, if we want to improve the cycling stability of lithium batteries at high voltage, it is far from enough to simply coat the layered cathode active material with a traditional electrochemically inert coating layer to reduce interfacial side reactions. Moreover, the traditional electrochemically inert coating layer sacrifices the reversible capacity of the material to obtain high cycling stability, which is not conducive to industrial applications. The inventors of this application creatively proposed that from the perspective of surface structure / element regulation and design of the cathode material, by constructing a surface heterophase structure, the structural stability of the transition metal layer of the layered cathode material during a large amount of lithium deintercalation under high-voltage working conditions can be increased to prevent the generation of a large number of irreversible microcrack structure defects and reduce the possibility of rapid decay of the layered cathode material at high voltage.
[0049] Previous studies have mainly focused on increasing interfacial ion / electron conductivity and suppressing side reactions, while there are few related studies on optimizing the crystal structure to improve the stability of the layered structure. The research of this application shows that a heterophase structure formed on the surface of the crystal structure, for example, in one implementation of this application, specifically, the spinel phase or rock salt phase formed by the epitaxial growth of the bulk layered material to the surface interface. For the battery layered cathode material with this crystal structure, since the spinel structure or rock salt phase structure can remain stable during the high-voltage charge and discharge process and can provide a three-dimensional lithium-ion transport network, it can effectively inhibit the problems of slip, collapse, distortion, and microcrack formation of the transition metal layer at high voltage while improving the capacity and rate performance of the layered cathode material.
[0050] Based on the above research and understanding, the present application creatively proposes a new battery layered positive electrode material, whose crystal structure has a heterogeneous phase structure that is pinned into the surface interface layer and the bulk layer of the crystal structure in a pinning manner; the heterogeneous phase structure is uniformly distributed on the surface of the crystal structure, encapsulating the crystal structure to form a uniform crystal surface layer.
[0051] In the present application, the heterogeneous phase structure epitaxially grown with the bulk layered structure is very stable. During the high voltage charge and discharge process, it can play a strong pinning role on the bulk layered structure, effectively inhibiting the slip, collapse, distortion and microcrack formation of the transition metal layer caused by the evolution of the phase structure. Therefore, the interface optimization strategy of the present application can effectively inhibit the aggravation of side reactions and the rapid increase of internal resistance during the high voltage cycle process, thereby making the layered positive electrode material at high voltage (>4.3Vvs.Li / Li + ) to achieve high capacity, rate and cycle stability.
[0052] The present application is further described in detail below through specific examples. The following examples are only used to further illustrate the present application and should not be construed as limiting the present application.
[0053] Embodiment 1
[0054] In this example, commercial lithium cobalt oxide is used as a raw material, and is pretreated by a solution immersion method, and then the pretreated lithium cobalt oxide is heat treated to obtain a lithium cobalt oxide layered positive electrode material having a eutectic spinel phase interface on the crystal structure surface of this example. The specific preparation method is as follows:
[0055] Step 1: pretreatment, 0.3 mmol of aluminum sulfate is placed in 40 mL of deionized water, stirred for 10 min to form a clear solution A; 1 g of commercial lithium cobalt oxide (D50 is 10-13 microns, tungsten) and 0.5 g of polyethylene glycol are placed in solution A, stirred for 10 min to form a black suspension B; 1.8 mmol of lithium fluoride is placed in 40 mL of deionized water, stirred for 2 min to form a solution C; solution C is added dropwise to the suspension solution B, and stirring is continued during the dropwise addition process to form a suspension D; the suspension D is transferred to a 60°C water bath for hydrothermal reaction for 6 hours, then filtered, washed with deionized water and anhydrous ethanol, and dried in a vacuum oven at 100°C to obtain a pretreated lithium cobalt oxide powder.
[0056] Step 2: subsequent heat treatment and sintering to convert the pre-treated LiCoO 2 The powder was heat treated at 600°C for 24 h in air atmosphere, and then cooled to room temperature at a cooling rate of 1°C / min. The obtained powder was sieved with 100 mesh to obtain LiCoO with spinel phase of Li, Al, Co, O and F components on the surface. 2 Powder, labeled as LiCoO2 @LCAF-Spinel-1#.
[0057] Electrochemical test: NMP was used as solvent to 2 @LCAF-Spinel, carbon black and PVDF were uniformly mixed in a mass ratio of 8:1:1 to prepare the positive electrode sheet, with an active material loading of about 2.1 mg cm -2 A half-cell with a lithium sheet as the negative electrode was prepared using a 2032 button cell, a Celgard 2035 separator and a high voltage electrolyte (mass ratio LiPF 6 :EMC:FEC=15:55:30), the half cell is at 3-4.6V (vs.Li / Li + ) cycles between.
[0058] Material characterization and electrochemical results: XRD analysis results show that the obtained LiCoO 2 @LCAF-Spinel-1# unit cell parameters belong to R-3m, which is a typical lithium cobalt oxide layered structure, such as Figure 1 TEM EDS-mapping element analysis results show that there is a gradient layer with a thickness of about 20nm containing Co, Mg, F and O elements, as shown in Figure 2. Figure 2 As shown. Further analysis of the electron diffraction characteristics of the interface layer shows that the interface layer with a thickness of about 20nm exhibits obvious spinel structural characteristics, indicating that there is a spinel structure layer containing Li, Co, Mg, O and F on the surface, that is, the surface of the crystal structure has a eutectic lattice spinel phase interface layer. The analysis results show that the eutectic lattice spinel phase interface is formed by the bulk layer of the crystal structure of the battery layered positive electrode material epitaxially growing to the surface interface of the crystal structure according to its same lattice; the eutectic spinel in the spinel phase interface is pinned into the surface area and bulk layer of the crystal structure; and the eutectic spinel in the spinel phase interface is uniformly distributed on the surface interface. Comprehensive analysis of various results shows that the synthesized material is a lithium cobalt oxide layered positive electrode material pinned with surface gradient spinel, that is, the content of metal elements Al and F gradually increases from the inside to the outside, and the content of Co and oxygen gradually decreases from the inside to the outside. The electrochemical test results show that the positive electrode material LiCoO 2 @LCMF-Spinel-1# Button cell with lithium metal negative electrode, 3-4.6V vs.Li / Li + During the interval charge and discharge cycle, compared with the purchased LiCoO without any treatment 2 , in this case, the pre-treated and heat-treated LiCoO 2It exhibits higher rate and cycle stability, with discharge capacities of ~218 mAh / g and ~109 mAh / g at 0.1C and 10C currents, respectively, and a capacity retention rate of ~79.4% after 200 cycles at 45°C at 2C current.
[0059] Embodiment 2
[0060] In this example, commercial lithium cobalt oxide is used as raw material, ball milling is used to pre-treat it, and then the pre-treated lithium cobalt oxide is heat-treated to obtain the lithium cobalt oxide layered positive electrode material with a eutectic spinel phase interface on the crystal structure surface of this example. The specific preparation method is as follows:
[0061] Step 1: Pretreatment: 0.3 mmol of zinc fluoride (nano powder, D 50 About 20nm), 0.3mmol lithium fluoride (nano powder, D 50 about 15nm) and 10mmol of commercial lithium cobalt oxide (D 50 The mixed powder is placed in a vacuum oven at 120°C and dried for more than 12 hours, sieved through 100 meshes, and set aside to obtain the pre-treated lithium cobalt oxide powder containing Li, Co, Zn, O and F on the surface.
[0062] Step 2: subsequent heat treatment and sintering to convert the pretreated LiCoO 2 The powder was heat treated at 650 °C in a rotary tube furnace for 24 h under an Ar inert atmosphere, and the cooling rate was controlled to be less than 1 °C / min. The obtained powder was sieved with 100 mesh and labeled as LiCoO 2 @LZF-Spinel-2#. For comparison, the material that has not been processed in step 2 is marked as LiCoO 2 @LF+AF.
[0063] Electrochemical test: NMP was used as solvent to 2 @LZF-Spinel-2#, carbon black and PVDF were uniformly mixed in a mass ratio of 8:1:1 to prepare the positive electrode sheet, with an active material loading of about 2.5 mg cm -2 A half-cell with a lithium sheet as the negative electrode was prepared using a 2032 button cell, a Celgard 2035 separator and a high voltage electrolyte (mass ratio LiPF 6 :EMC:FEC=15:55:30), the half cell is at 3-4.6V (vs.Li / Li + ) cycles between.
[0064] Material characterization and electrochemical results: XRD analysis results show that the obtained LiCoO2 @LZF-Spinel-2# has R-3m unit cell parameters, which is a typical layered structure of lithium cobalt oxide. TEM EDS-mapping and diffraction analysis results show that there is a spinel layer with a thickness of about 25nm on the surface. The elemental composition of the spinel layer includes Li, Co, Al, O and F, that is, the material surface has a spinel layer. Analysis of materials that have not been processed in step 2 shows that there are only several 5-20nm nanoscale lithium fluoride and aluminum fluoride nanoparticle attachment layers on the surface of the obtained material, and no spinel phase is formed.
[0065] The electrochemical test results show that the positive electrode material LiCoO 2 @LCZF-S and lithium metal anode button cell, 3-4.6V vs.Li / Li + During the interval charge and discharge cycle, compared with the purchased LiCoO without any treatment 2 and LiCoO without step 2 treatment 2 @LF+AF material shows higher rate and cycle stability, with discharge capacities of ~220 mAh / g and ~129 mAh / g at 0.1C and 10C respectively, and a capacity retention rate of 89.4% after 200 cycles at 2C. LiCoO without step 2 treatment 2 @LF+AF material, the discharge capacity at 0.1C and 10C currents are ~201mAh / g and ~65mAh / g respectively, and the capacity retention rate is 59.1% after 200 cycles at 2C current.
[0066] Embodiment 3
[0067] In this example, commercial lithium cobalt oxide is used as a raw material, and the sol-gel method is used to pre-treat the lithium cobalt oxide, and then the pre-treated lithium cobalt oxide is subjected to subsequent heat treatment, so as to obtain a lithium cobalt oxide layered positive electrode material having a eutectic spinel phase interface on the crystal structure surface of this example. The specific preparation method is as follows:
[0068] Step 1: Pretreatment: 10 mmol of commercial lithium cobalt oxide (D 50 10-13 microns, tungsten) and 1g of polyethylene glycol (molecular weight greater than 2000) were poured into 40mL of deionized water and stirred evenly to form a suspension solution A; 0.3mmol of magnesium sulfate and 0.3mmol of lithium sulfate were added to solution A, and the mixture was continuously stirred to dissolve to form a suspension solution B; 0.9mmol of potassium fluoride was added to 40mL of deionized water to form a solution C; solution C was added dropwise into solution B, and stirring was continued at 90°C until the water was evaporated; the obtained material was dried in a vacuum oven at 120°C for more than 12h, sieved through 100 mesh, and used for later use.
[0069] Step 2: subsequent heat treatment and sintering: the powder pretreated in step 1 is heat treated at 650°C in a rotary tube furnace under an Ar inert atmosphere for 24 hours, and the cooling rate is controlled to be less than 1°C / min. The obtained powder is sieved with 100 mesh and marked as LiCoO 2 @LMF-Spinel-3#.
[0070] Electrochemical test: NMP was used as solvent to 2 @LCMF-Spinel-3#, carbon black and PVDF were uniformly mixed in a mass ratio of 8:1:1 to prepare the positive electrode sheet, with an active material loading of about 2.5 mg cm -2 A half-cell with a lithium sheet as the negative electrode was prepared using a 2032 button cell, a Celgard 2035 separator and a high voltage electrolyte (mass ratio LiPF 6 :EMC:FEC=15:55:30), the half cell is at 3-4.6V (vs.Li / Li + ) cycles between.
[0071] Material characterization and electrochemical results: XRD analysis results show that the obtained LiCoO 2 @LCMF-Spinel-3# has R-3m unit cell parameters, which is a typical layered structure of lithium cobalt oxide. TEM EDS-mapping and diffraction analysis results show that there is a spinel layer with a thickness of about 28nm on the surface. The elemental composition of the spinel layer includes Li, Co, Al, O and F, that is, the material surface has a spinel layer.
[0072] The electrochemical test results show that the positive electrode material LiCoO 2 @LCMF-S and lithium metal anode button cell, 3-4.6V vs.Li / Li + During the interval charge and discharge cycle, compared with the purchased LiCoO without any treatment 2 , showing higher rate and cycle stability, with discharge capacities of ~225 mAh / g and ~134 mAh / g at 0.1C and 10C currents, respectively, and a capacity retention rate of 92.3% after 200 cycles at 2C current.
[0073] Embodiment 4
[0074] The same ball milling and heat treatment as in Example 2 were used to 0.8 Co 0.1 Mn 0.1 O 2 and LiNi 0.5 Co 0.3 Mn 0.2O 2 After the pretreatment and subsequent heat treatment of step 1 and step 2, the obtained materials are marked as NCM811@LZF-spinel and NCM532@LZF-spinel, respectively. 0.8 Co 0.1 Mn 0.1 O 2 and LiNi 0.5 Co 0.3 Mn 0.2 O 2 The lithium cobalt oxide in Example 2 is replaced by an equal amount, and the rest remains unchanged.
[0075] XRD analysis results show that the obtained NCM811@LZF-spinel and NCM532@LZF-spinel are typical layered structures. TEM EDS-mapping and diffraction analysis results show that there is a layer of spinel phase area with a thickness of about 35nm and 27nm, respectively, which is evenly distributed at the surface interface. The elemental composition of the spinel phase layer includes Li, Ni, Co, Mn, Zn, O and F. Both materials treated in step one and step two showed better rate and cycle stability.
[0076] The button cell with positive electrode material NCM811@LZF-spinel and lithium metal negative electrode has a voltage of 3-4.3V vs.Li / Li + During the interval charge and discharge cycle process, its discharge capacity at 0.1C and 10C currents was ~215mAh / g and ~125mAh / g respectively, and the capacity retention rate was 89.3% after 200 cycles at 2C current.
[0077] The button cell with positive electrode material NCM532@LZF-spinel and lithium metal negative electrode has a voltage of 3-4.3V vs.Li / Li + During the interval charge and discharge cycle, its discharge capacity at 0.1C and 10C currents was ~205mAh / g and ~113mAh / g respectively, and the capacity retention rate was 84.3% after 200 cycles at 2C current.
[0078] Embodiment 5
[0079] The same ball milling method and heat treatment as in Example 2 were used to treat some typical high-nickel binary materials, such as LiNi 0.8 Co 0.2 O 2 (NC82), LiNi 0.8 Mn 0.2 O 2 (NM82), LiNi 0.6 Co0.4 O 2 (NC64), LiNi 0.6 Mn 0.4 O 2 (NM64); high nickel ternary materials, such as LiNi 0.6 Co 0.2 Mn 0.2 O 2 (NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O 2 (NCM811), LiNi 0.8 Co 0.1 Al 0.1 O 2 (NCA811); high nickel multi-element materials, such as LiNi 0.7 Co 0.1 Mn 0.1 Al 0.1 O 2 (NCMA7111) was subjected to step 1 and step 2 pretreatment and subsequent heat treatment. After the synthesis, the obtained sample was subjected to electrochemical testing in the potential range of 3-4.3 V. The results are shown in Table 1.
[0080] Table 1 Electrochemical properties of typical high-nickel cathode materials treated by the method of Example 2
[0081]
[0082]
[0083] By analyzing the electrochemical data results of several typical high-nickel materials before and after ball milling and heat treatment in Table 1, it can be seen that surface heterogeneous phase pinning has beneficial effects on the rate, capacity and cycle stability of all typical high-nickel materials.
[0084] Embodiment 6
[0085] The same ball milling method as in Example 2 was used to mill commercial LiCoO 2 Materials (D 50 The surface spinel phase layer of different thickness is obtained by adjusting the heat treatment temperature / time and the cooling control time in the subsequent heat treatment process of step 2. Specifically, the heat treatment process conditions are shown in Table 2.
[0086] Table 2 Heat treatment process conditions and cathode material performance test results
[0087]
[0088]
[0089] The positive electrode material having a spinel phase interface with a eutectic lattice on the surface of the crystal structure prepared in this example was subjected to a 0.1C / 10C capacity test and a 2C cycle 200 cycle capacity retention rate test using the same method as in Example 2. The results are shown in Table 2.
[0090] By analyzing the results in Table 2, we can draw the following conclusions:
[0091] 1) Comparison of 6 samples heat treated at 350-750℃ for 24h with a cooling rate of less than 1℃ / min, it was found that no obvious spinel phase layer was found on the surface of the 350℃ sample. As the heat treatment temperature increases, the capacity retention rate of 2C cycles for 200 cycles gradually increases, but the corresponding capacity and rate performance decrease.
[0092] 2) By comparing five samples that were heat treated at 600℃ for 24h but had different cooling rates, it was found that with the increase of cooling rate, the material capacity and rate did not change much, but the cycle stability gradually decreased.
[0093] 3) By comparing the three samples that were heat treated at 400°C for 6h, 12h and 24h, with the cooling rates all lower than 1°C / min, it was found that the thickness of the spinel phase layer gradually increased with the extension of the heat treatment time, but the spinel phase thickness of the sample heat treated at 400°C for 12h was still less than 10nm, resulting in poor cycle stability; by comparing the three samples that were heat treated at 700°C for 6h, 12h and 24h, with the cooling rates all lower than 1°C / min, it was found that the thickness of the spinel phase layer gradually increased with the extension of the heat treatment time, and the spinel phase thickness on the surface of the sample heat treated at 700°C for more than 6h was greater than 10nm. At the same time, the capacity retention rates were greater than 80% after 200 cycles at 2C.
[0094] 4) For the electrochemical data of samples heat treated at 750℃ for 24h with a cooling rate of less than 1℃ / min, it was found that when the temperature exceeded 700℃, although the cycle stability was greatly improved, it was not conducive to the utilization of rate and capacity.
[0095] The results of this embodiment show that the time threshold for obtaining "spinel phase structure thickness greater than or equal to 10nm" is different at different heat treatment temperatures. The higher the heat treatment temperature, the lower the time threshold; in principle, as long as the heat treatment time exceeds the threshold time τ at a specific heat treatment temperature T, the two satisfy the formula τ = 36-0.04T, where τ is the threshold time, in units of h; T is the heat treatment temperature, in units of ° C. Under high temperature conditions of 700 ° C, a spinel phase interface layer with a thickness of more than 10nm can be obtained by heat treatment for more than 6 hours. In the actual production process, based on energy consumption considerations, we select appropriate temperatures and times for heat treatment of materials. Therefore, it is preferred to use 400-700 ° C heat treatment for more than the threshold time. At the same time, the results of this embodiment show that the cooling rate has little effect on the material capacity and rate, but has a great impact on the material cycle stability. Only when the cooling rate is less than or equal to 1 ° C / min, the cycle stability of the obtained layered positive electrode material can be guaranteed.
[0096] The above contents are further detailed descriptions of the present application in combination with specific implementation methods, and it cannot be determined that the specific implementation of the present application is limited to these descriptions. For ordinary technicians in the technical field to which the present application belongs, several simple deductions or substitutions can be made without departing from the concept of the present application.
Claims
1. A method for preparing a battery layered positive electrode material, Features: The crystal structure of the battery layered positive electrode material has a heterogeneous phase structure that is pinned into the surface interface layer and the bulk layer of the crystal structure; the heterogeneous phase structure is evenly distributed on the surface of the crystal structure, covering the crystal structure therein to form a uniform crystal surface layer; The heterogeneous phase structure is a spinel phase or a rock salt phase structure; The heterogeneous phase structure is formed by epitaxial growth of the bulk phase layer of the crystal structure of the battery layered positive electrode material to the surface interface layer of the crystal structure according to the same lattice, that is, the heterogeneous phase structure and the bulk phase layer of the crystal structure form a eutectic lattice; The preparation method comprises performing the following treatments on a conventional battery layered positive electrode material to obtain a battery layered positive electrode material having a pinned heterogeneous phase structure in a crystal structure; Step 1: pretreating conventional battery layered positive electrode materials by at least one of the following methods: (a) Solution immersion method, which involves immersing conventional battery layered cathode materials in a solution containing Li + , borate, Al 3+ Mg 2+ , Ca 2+ 、Zn 2+ and F - The immersion condition is 0-160° C. and 1-24 h to obtain a pretreated battery layered positive electrode material; (b) Sol-gel method, which involves mixing conventional battery layered cathode materials with Li-containing + , borate, Al 3+ Mg 2+ , Ca 2+ 、Zn 2+ and F - uniformly mixing at least one of the sol-gels, heating and drying, to obtain a pre-treated battery layered positive electrode material; (c) Ball milling, which involves mixing conventional battery layered cathode materials with Li-containing + , borate, Al 3+ Mg 2+ , Ca 2+ 、Zn 2+ and F - ball-milling the at least one solid material to obtain a pre-treated battery layered positive electrode material; Step 2: heat-treating the pretreated battery layered positive electrode material obtained in step 1 at 400-700° C. for a time exceeding a threshold value in an inert atmosphere or a reducing atmosphere, and then cooling the temperature to room temperature at a cooling rate of less than or equal to 1° C. / min, thereby obtaining a battery layered positive electrode material having a pinned heterogeneous phase structure in the crystal structure and a crystal surface layer thickness greater than or equal to 10 nm; The inert atmosphere is a nitrogen atmosphere or an argon atmosphere; the reducing atmosphere is an atmosphere of nitrogen plus hydrogen, or an atmosphere of argon plus hydrogen; The threshold time satisfies the formula τ=36-0.04T, wherein τ is the threshold time, in units of h; and T is the heat treatment temperature, in units of °C.
2. The preparation method according to claim 1, Features: The thickness of the crystal surface layer is greater than or equal to 10 nm.
3. The preparation method according to claim 1 or 2, Features: The battery layered positive electrode material is Li 1+ x TMO 2+y , wherein 0≤x≤1, 0≤y≤1, and TM is at least one of Co, Mn, Ni and Al.
4. The preparation method according to claim 3, Features: The battery layered positive electrode material is at least one of lithium cobalt oxide, high nickel binary material, high nickel multi-element material, and lithium manganese-rich positive electrode material; The high nickel content means that the nickel content is greater than or equal to 50%.
5. The preparation method according to claim 4, Features: The battery layered positive electrode material is LiNi 0.8 Co 0.1 Mn 0.1 O 2 、LiNi 0.5 Co 0.3 Mn 0.2 O 2 and LiCoO 2 At least one of .
6. The preparation method according to claim 4, Features: The constituent elements of the crystal surface layer include cations and anions, the cations include at least one of Li, Co, Mn, Ni, Al, B, Mg, Ca and Zn, and the anions include O and / or F.
7. The preparation method according to claim 6, Features: In the crystal surface layer, the content of Al, B, Mg, Ca, Zn and / or fluorine gradually increases from the inside to the outside, and the content of Co, Mn, Ni and / or O gradually decreases from the inside to the outside.