Testing method for interlayer proximity of polymer composites

Using FRET technology to measure the distance between the fluorescent donor and the acceptor between the interface layers of polymer composite materials solves the problem of microscopic characterization of the interface layer in the existing technology, enables efficient evaluation of the interaction force of the interface layer, and improves the interface bonding strength.

CN114935563BActive Publication Date: 2024-10-29SHENZHEN POLYTECHNIC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210398310.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-16
Publication Date
2024-10-29
Estimated Expiration
2042-04-16

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively characterize the relative distance between the polymer chain and the metal or inorganic substrate between the interface layers of polymer composite materials from a microscopic perspective, resulting in thermal stress accumulation leading to interface layer damage and reduced bonding strength.

Method used

Using fluorescence resonance energy transfer (FRET) technology, the fluorescence donor group is grafted onto the polymer chain and the fluorescence acceptor group is grafted onto the surface of the metal or inorganic substrate, and fluorescence spectroscopy is used to measure the relationship between the interface between the polymer chain and the polymer chain. The relative distance between bases.

Benefits of technology

It achieves high spatial sensitivity detection of small distance changes between the polymer chain and the substrate between the interface layers, non-destructive detection, is suitable for the evaluation of the interface bonding strength under different heat treatment processes, and improves the interaction force of the interface layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114935563B_ABST
    Figure CN114935563B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for testing the inter-layer proximity of a polymer composite material, specifically a method for characterizing the relative distance between a polymer chain and a metal or inorganic substrate in an inter-layer of a polymer composite material based on fluorescence resonance energy transfer technology. The present invention grafts a fluorescent donor and a fluorescent acceptor molecule onto a polymer chain and a substrate surface of the polymer composite material, respectively, collects the fluorescence spectrum of the composite material after different process treatments by surface reflection, and obtains the inter-layer proximity between the polymer chain and the substrate by comparing the intensity ratio of the characteristic peaks of the fluorescent acceptor and the donor in the fluorescence spectrum. The strength of the interface bonding force of the composite material treated by different processes can be judged according to the change of the proximity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the application field of fluorescence resonance energy transfer (FRET) analysis technology, and specifically to a method for characterizing the relative distance between polymer chains and metal and inorganic substrates in the interface layer of polymer composite materials based on the fluorescence resonance energy transfer analysis technology. Background Art

[0002] With the continuous progress of science and technology, a single material can no longer meet the development needs of cutting-edge technology. Compounding different types of materials to give full play to their respective advantages and avoid their weaknesses is one of the important strategies for new material research. Polymer composites are multiphase solid materials formed by bonding polymer materials with other materials of different compositions, shapes and properties. Interfaces account for a large proportion of polymer composites, and the proximity and interaction strength between the polymer and other phases in the interface layer have an important influence on the performance and application of the composite material.

[0003] In the past decade, researchers have developed a nano-injection molding technology (NMT) that can achieve high-strength composites between polymers and metals. This technology directly injects polymer melts onto metal surfaces that have been pre-nano-treated. The polymer nanorods filled in the nanopores on the metal surface form a structure similar to an "anchor bolt", thereby achieving the connection between the polymer and the metal, and the bonding strength even exceeds the strength of the polymer material itself. The bonding strength of polymer / metal composite materials is greatly affected by the NMT heat treatment process. Chinese patent CN106273216B reports a heat treatment method for preparing metal-resin composites based on NMT. ​​By controlling the cooling rate of the composite, the bonding strength between the resin and the metal can be effectively improved. For amorphous resins such as polymethyl methacrylate (PMMA), after heat treatment by this method, the bonding strength of PMMA resin and metal is increased by about 500%. However, the patent does not give the reason for the large difference in the bonding strength between amorphous resins and metals under different heat treatment processes from a microscopic mechanism.

[0004] As we all know, there is a large difference in thermal expansion coefficients between polymers and metals and inorganic materials. Generally, the thermal expansion coefficient of polymers is one to two orders of magnitude higher than that of metals. Therefore, during the cooling and curing process of the polymer / metal composite system, the mismatch in the thermal expansion coefficients of the two will cause the interface layer to be subjected to thermal stress. If the thermal stress during the cooling process cannot be dissipated in time, the final accumulated residual stress may be as high as GPa. Such a large residual stress will damage the interface layer, causing changes in the proximity between the polymer chain and the metal in the interface layer, reducing the interaction force between the two, and seriously affecting the anchoring effect between the polymer / metal. Since the interface layer of the polymer composite material is a nanoscale micro-region and is located inside the material, the method of studying the interface failure of the composite material through morphological observation such as scanning electron microscopy (SEM) is no longer applicable. Therefore, it is urgent to develop a new method suitable for the characterization of the microstructure of the interface layer of polymer composite materials. Summary of the invention

[0005] The purpose of the present invention is to make up for the deficiencies of the prior art and provide a method for characterizing the proximity between polymer chains and metal and inorganic substrates at the interface of polymer composite materials based on fluorescence resonance energy transfer (FRET) technology. The method can be used to study the difference in the proximity between the interface layers of polymer composite materials caused by different heat treatment processes of NMT, resulting in changes in the interface bonding strength.

[0006] The present invention grafts a fluorescent donor group onto a polymer chain of a polymer composite material, and grafts a fluorescent acceptor group onto a metal or inorganic substrate surface, and measures the distance between the fluorescent donor and the fluorescent acceptor through a FRET experiment, thereby obtaining the relative distance between the interfacial polymer chain and the metal or inorganic substrate.

[0007] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions:

[0008] The present invention provides a method for testing the proximity between interface layers of a polymer composite material, the testing method comprising the following steps:

[0009] (1) grafting the fluorescent donor molecule onto the polymer chain by copolymerization or side group reaction to obtain a polymer matrix containing the fluorescent donor;

[0010] (2) preparing nanopores on the surface of the substrate by anodization or chemical etching, and grafting fluorescent receptor molecules onto the surface of the nanopores by chemical modification to obtain a substrate containing fluorescent receptors on the surface;

[0011] (3) compounding the polymer matrix containing the fluorescent donor with the substrate surface containing the fluorescent receptor by melt infiltration, and obtaining a polymer / substrate composite material by heat treatment;

[0012] (4) Collecting the fluorescence spectrum of the polymer / substrate composite material by surface reflection method, and obtaining the proximity between the polymer chain and the substrate in the interface layer by comparing the intensity ratio of the characteristic peaks of the fluorescence acceptor and the fluorescence donor in the fluorescence spectrum.

[0013] Furthermore, in the step (1), the molar concentration of the fluorescent donor in the polymer matrix is ​​0.05-1%.

[0014] Furthermore, the nanopores in step (2) have an average diameter of 10 to 500 nm and an average length of 1 to 100 μm.

[0015] Furthermore, in the step (2), the grafting density of the fluorescent receptor on the surface of the substrate is 0.01 to 0.5 nm. -2 .

[0016] Furthermore, the polymer matrix is ​​a thermoplastic resin, and the thermoplastic resin is selected from one or more of polystyrene (PS), polymethyl methacrylate (PMMA), and polybutyl methacrylate (PBMA).

[0017] Furthermore, the substrate is selected from metal or inorganic materials; the metal material is selected from aluminum, titanium, copper and stainless steel.

[0018] Furthermore, the heat treatment method in step (3) includes changing the cooling rate of the composite system or isothermal annealing treatment.

[0019] Furthermore, the cooling rate is 0.2 to 10 4 ℃ / min; the temperature range of the isothermal annealing is the thermoplastic resin T g Above 20~100℃.

[0020] Furthermore, the fluorescence donor in step (1) and the fluorescence acceptor in step (2) are a FRET molecule pair, and the fluorescence donor can undergo fluorescence resonance energy transfer to the fluorescence acceptor.

[0021] Further, the FRET molecular pair is carbazole (Cz) and anthracene (An) or nitrobenzoxadiazole (NBD) and spiropyranyl (SP).

[0022] Furthermore, the FRET molecule pair has a FRET efficiency higher than 85%.

[0023] By applying the technical solution of the present invention, compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The proximity between the polymer chain and the substrate in the interface layer of the polymer composite material is obtained by measuring the distance between the FRET fluorescence pairs. The tiny distance changes in the range of 1 to 10 nm in the interface layer can be tested, with very high spatial sensitivity;

[0025] (2) The sample preparation and instrument operation of the present application are relatively simple, and can realize in-situ non-destructive testing of polymer composite samples;

[0026] (3) This method can also be used to measure the proximity between interfacial layers in composites of polymers and nanofillers, as well as in multilayer composite membrane systems, and has a certain degree of universality. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0028] Figure 1 A schematic diagram showing fluorescence resonance energy transfer between a polymer chain and a substrate surface by a FRET fluorescence pair between an interface layer of a polymer composite material provided by an embodiment of the present invention is shown;

[0029] Figure 2 The fluorescence spectra of the polymer composite material containing FRET fluorescent pairs after being treated at different cooling rates according to Example 1 of the present invention and Comparative Example 5 are shown.

[0030] The above figures include the following figure marks: 11 is a substrate; 12 is an interface layer of a polymer composite material; 121 is a polymer chain; 122 is a fluorescence donor; 111 is a fluorescence donor; and r is a distance between the fluorescence donor and the fluorescence acceptor. DETAILED DESCRIPTION

[0031] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0032] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0033] Unless otherwise defined, technical or scientific terms used in the present disclosure shall have the common meanings understood by one of ordinary skill in the art to which the present invention belongs.

[0034] As analyzed in the background technology of this application, since the interface layer of the polymer composite material is a nanoscale micro-region and is located inside the material, the method of studying the interface failure of the composite material by morphological observation such as scanning electron microscopy (SEM) is no longer applicable. In order to solve this problem, this application provides a method for testing the proximity between the interface layers of a polymer composite material, specifically a method for characterizing the relative distance between the polymer chain and the metal and inorganic substrate between the interface layers of the polymer composite material based on fluorescence resonance energy transfer analysis technology.

[0035] Fluorescence resonance energy transfer (FRET) refers to a mechanism of energy transfer between two chromophores (donor and acceptor) through long-range dipole interactions. When the fluorescent donor and fluorescent acceptor molecules are within a specific distance range, the excited donor transfers energy to the acceptor in the form of resonance. The energy transfer efficiency (E) between the donor and the acceptor is inversely related to the sixth power of the distance (r), and the distance between the chromophores can be calculated by measuring the efficiency of energy transfer. Therefore, the FRET method can be used as a "spectral ruler" to measure distances in the range of 1 to 10 nm.

[0036] In a typical embodiment of the present application, a method for testing the proximity between interlayers of a polymer composite material interface is provided. The testing method comprises the following steps:

[0037] (1) grafting the fluorescent donor molecule onto the polymer chain by copolymerization or side group reaction to obtain a polymer matrix containing the fluorescent donor;

[0038] (2) preparing nanopores on the surface of the substrate by anodization or chemical etching, and grafting fluorescent receptor molecules onto the surface of the nanopores by chemical modification to obtain a substrate containing fluorescent receptors on the surface;

[0039] (3) compounding the polymer matrix containing the fluorescent donor with the substrate surface containing the fluorescent receptor by melt infiltration, and obtaining a polymer / substrate composite material by heat treatment;

[0040] (4) collecting the fluorescence spectrum of the polymer / substrate composite material by a surface reflection method, and comparing the fluorescence acceptor (I A ) and fluorescent donor (I D ) The intensity ratio of the characteristic peak I A / I D , to obtain the proximity between the interfacial polymer chains and the substrate.

[0041] The energy transfer from the fluorescent donor to the fluorescent acceptor may therefore depend on the distance between the fluorescent donor and the fluorescent acceptor. In this regard, energy transfer, especially the intensity and / or efficiency of energy transfer, may increase as the spatial spacing between the fluorescent donor and the fluorescent acceptor decreases. In other words, the increase in the spacing between the fluorescent donor and the fluorescent acceptor leads to a weakening of the energy transfer, accompanied by a change in the emission spectrum. The specific results can be seen from the changes in the emission spectrum, as the distance increases, the donor signal increases and / or the acceptor signal decreases. If the distance decreases, the donor signal is correspondingly weakened and the acceptor signal is enhanced as a result of the acceptor quenching effect. The larger the intensity ratio of the characteristic peaks of the fluorescent acceptor and the donor, the higher the efficiency of the fluorescent energy transfer, indicating that the relative distance between the interlayer polymer chain and the substrate is closer, and the degree of proximity between the two is high; conversely, it means that the relative distance between the interlayer polymer chain and the substrate is farther, and the degree of proximity between the two is low.

[0042] Furthermore, the molar concentration of the fluorescent donor in the polymer matrix in step (1) is 0.05-1%. Too low a concentration of the fluorescent donor will affect the sensitivity of FRET detection, while too high a concentration of the fluorescent donor will easily cause self-absorption of the fluorescent group.

[0043] Furthermore, the average diameter of the nanopores in step (2) is 10 to 500 nm, and the average length is 1 to 100 μm. The average diameter of the nanopores is lower than 10 nm, and the distance between the interface layers generated by different heat treatment processes varies little, which is lower than the lower limit of detection by the FRET method. The average diameter of the nanopores is higher than 500 nm. On the one hand, such large-sized nanopores are difficult to prepare. On the other hand, the distance between the interface layers generated by different heat treatment processes in large-sized pores varies greatly, which may exceed the upper limit of detection by the FRET method. The average length of the nanopores is lower than 1 μm. In the test method, the polymer content that penetrates into the nanopores is relatively small, and the signal-to-noise ratio of the measured fluorescence spectrum is poor. The average length of the nanopores is higher than 100 μm. On the one hand, it is difficult for polymer melts to fill the nanopores, and it is easy to produce polymer nanotube structures. On the other hand, it is difficult for incident light to penetrate such a deep thickness.

[0044] Furthermore, in the step (2), the grafting density of the fluorescent receptor on the surface of the substrate is 0.01 to 0.5 nm. -2 The grafting density of the fluorescent receptor on the surface of the substrate is less than 0.01 nm -2 Too low a density of receptor groups will result in reduced detection sensitivity of the FRET method. The grafting density of the fluorescent receptor on the surface of the substrate is higher than 0.5 nm. -2 Too high a density of acceptor groups can easily lead to self-absorption of acceptor fluorescent groups.

[0045] Furthermore, the polymer matrix is ​​a thermoplastic resin, and the thermoplastic resin is selected from one or more of polystyrene (PS), polymethyl methacrylate (PMMA), and polybutyl methacrylate (PBMA). Thermoplastic resin has excellent mechanical properties, relatively high tensile strength and modulus, excellent toughness, impact resistance, and damage tolerance.

[0046] Furthermore, the substrate is selected from metal or inorganic materials; the metal material is selected from aluminum, titanium, copper and stainless steel.

[0047] Furthermore, the heat treatment method in step (3) includes changing the cooling rate of the composite system or isothermal annealing. By adopting different heat treatment methods, polymer / substrate composite materials with different proximity between interface layers can be obtained.

[0048] Furthermore, the cooling rate is 0.2 to 10 4 ℃ / min; the temperature range of the isothermal annealing is 20 to 100℃ above the Tg of the thermoplastic resin. I A / I C The value is much lower than that of the sample with slow cooling. After rapid cooling, the distance between the polymer chain and the substrate in the interface layer is large, and the proximity is low. This is related to the fact that the thermal stress caused by the mismatch of thermal expansion coefficients cannot be dissipated in time during the rapid cooling process, and the accumulated residual stress is too large, resulting in the desorption of the polymer chain from the pore wall surface.

[0049] Furthermore, the fluorescence donor in step (1) and the fluorescence acceptor in step (2) are a FRET molecule pair, and the fluorescence donor can undergo fluorescence resonance energy transfer to the fluorescence acceptor.

[0050] Furthermore, the FRET molecular pair is carbazole (Cz) and anthracene (An) or nitrobenzoxadiazole (NBD) and spiropyran (SP). FRET experiments are all performed on a commercial fluorescence spectrometer.

[0051] Furthermore, the FRET molecule pair has a FRET efficiency higher than 85%.

[0052] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0053] Example 1

[0054] A polybutyl methacrylate (PBMA) sample containing a fluorescent donor carbazole (Cz) was prepared by copolymerization of carbazole methacrylate lactone and butyl methacrylate, with a molecular weight of 10,200 g / mol and a molar concentration of the fluorescent donor Cz of 0.4%. The surface of the aluminum sheet was anodized to prepare regular alumina channels with a pore size of 200 nm and a length of 50 μm. The surface of the alumina was modified with a silane coupling agent and subjected to a hydrosilylation reaction to graft the fluorescent acceptor anthracene (An) onto the alumina nanopore wall, where the grafting density of the fluorescent acceptor An was 0.2 nm. -2 .

[0055] A 100 μm thick PBMA film containing the fluorescent donor Cz was prepared by the solution casting method. The film was pressed with an anodized aluminum sheet with a fluorescent receptor An grafted on the surface, placed in a vacuum oven at 150°C for 12 hours, and then cooled to room temperature. Finally, the excess polymer film on the surface of the aluminum sheet was removed to obtain a PBMA / Al composite material sample containing a FRET fluorescent pair.

[0056] The PBMA / Al composite material sample containing the FRET fluorescent pair was placed in a vacuum oven at 150°C, and the composite material sample was slowly cooled to room temperature at a cooling rate of 0.5°C / min through program temperature control to obtain a composite material sample with slow cooling.

[0057] The fluorescence spectrum of the PBMA / Al composite material sample containing the FRET fluorescence pair was tested by surface reflection, and the excitation light wavelength was 294nm. In the fluorescence spectrum, the characteristic peak of the fluorescence donor Cz is located at 357nm, and the characteristic peak of the fluorescence acceptor An is located at 414nm. The characteristic peak intensity (I A ) and the characteristic peak intensity of the fluorescence donor Cz (I D ) can represent the efficiency of FRET energy transfer and reflect the distance between the donor and the acceptor, that is, the proximity between the polymer chain and the substrate in the interfacial layer.

[0058] Example 2

[0059] The difference from Example 1 is that the fluorescent donor is nitrobenzoxadiazole (NBD) and the fluorescent acceptor is spiropyranyl (SP). In the fluorescence test, the excitation light wavelength is 365nm, the characteristic peak of the fluorescent donor NBD is at 532nm, and the characteristic peak of the fluorescent acceptor SP is at 655nm.

[0060] Example 3

[0061] The difference from Example 1 is that the molar concentration of the fluorescence donor Cz is 0.05%, and the other aspects are the same as Example 1.

[0062] Example 4

[0063] The difference from Example 1 is that the molar concentration of the fluorescence donor Cz is 1%, and the other aspects are the same as Example 1.

[0064] Example 5

[0065] The difference from Example 1 is that the grafting density of the fluorescent acceptor An is 0.01nm -2 , the rest is the same as Example 1.

[0066] Example 6

[0067] The difference from Example 1 is that the grafting density of the fluorescent receptor An is 0.5 nm -2 , the rest is the same as Example 1.

[0068] Example 7

[0069] The difference from Example 1 is that the pore size of the alumina channel is 500 nm and the length is regular at 100 μm. The rest is the same as Example 1.

[0070] Example 8

[0071] The difference from Example 1 is that the pore size of the alumina channel is 10 nm and the length is 1 μm. The rest is the same as Example 1.

[0072] Example 9

[0073] The difference from Example 1 is that the thermoplastic resin is polymethyl methacrylate, and the rest is the same as Example 1.

[0074] Example 10

[0075] The difference from Example 1 is that the composite material sample is slowly cooled to room temperature at a cooling rate of 2° C. / min. The rest is the same as Example 1.

[0076] Embodiment 11

[0077] The difference from Example 1 is that the composite material sample is slowly cooled to room temperature at a cooling rate of 10° C. / min. The rest is the same as Example 1.

[0078] Comparative Example 1

[0079] The difference from Example 1 is that the molar concentration of the fluorescence donor Cz is 0.01%, and the other aspects are the same as Example 1.

[0080] Comparative Example 2

[0081] The difference from Example 1 is that the molar concentration of the fluorescence donor Cz is 1.1%, and the other aspects are the same as Example 1.

[0082] Comparative Example 3

[0083] The difference from Example 1 is that the grafting density of the fluorescent acceptor An is 0.005nm -2 , the rest is the same as Example 1.

[0084] Comparative Example 4

[0085] The difference from Example 1 is that the grafting density of the fluorescent acceptor An is 0.6 nm -2 , the rest is the same as Example 1.

[0086] Comparative Example 5

[0087] The difference from Example 1 is that the high-temperature sample is quickly transferred to liquid nitrogen, during which the cooling rate of the composite sample is about 6000° C. / min, and a composite sample with rapid cooling is obtained; the rest is the same as Example 1.

[0088] Performance Testing

[0089] The composite material specimens obtained by the above Examples 1-11 and Comparative Examples 1-5 were evaluated by the following test methods.

[0090] The polymer / substrate composite material specimens were prepared by NMT injection molding process. After heat treatment, the bonding strength between the polymer matrix and the substrate after treatment at different cooling rates was tested by a tensile testing machine.

[0091] Table 1. FRET fluorescence spectra and mechanical test results of polymer / substrate composite samples

[0092]

[0093]

[0094] According to Examples 1 and 2, carbazole (Cz) and anthracene (An) or nitrobenzoxadiazole (NBD) and spiropyran (SP) can be used as FRET molecular pairs to characterize the relative distance between the polymer chain and the substrate in the interface layer of the polymer composite material. It can be seen from Examples 1, 3-6 and Comparative Examples 1-4 that when the molar concentration of the fluorescent donor in the polymer matrix is ​​in the range of 0.05-1%, and the grafting density of the fluorescent receptor on the substrate surface is in the range of 0.01-0.5 nm -2range, the PBMA / Al composite material system can obtain a high-resolution FRET fluorescence spectrum, and the interfacial layer proximity and the interface bonding strength evaluated based on the ratio of the characteristic peak intensity of the acceptor and the donor in the fluorescence spectrum show a good corresponding relationship; on the contrary, on the one hand, the signal-to-noise ratio of the obtained fluorescence spectrum is poor, and on the other hand, there is an obvious inconsistency between the interfacial layer proximity and the interface bonding strength evaluated based on the ratio of the characteristic peak intensity of the acceptor and the donor. It can be seen from Examples 7 and 8 that if the diameter and length of the nanopores treated by anodization are changed, the signal and interface bonding strength of the FRET fluorescence spectrum will be affected to a certain extent. Therefore, the FRET fluorescence method of the present invention is more suitable for the lateral comparison of nanopores and polymer composite systems of the same morphology. It can be seen from Example 9 that the FRET fluorescence method of the present invention is also applicable to other thermoplastic resin systems such as PMMA. It can be seen from Examples 1, 10, 11 and Comparative Example 5 that the I A / I D The value is much lower than that of the sample with slow cooling, indicating that the distance between the polymer chains in the interface layer and the substrate is large and the proximity is low after the rapid cooling treatment. This is related to the fact that the thermal stress caused by the mismatch of thermal expansion coefficients cannot be dissipated in time during the rapid cooling process, and the accumulated residual stress is too large, resulting in the desorption of the polymer chains from the pore wall surface. The reduction in the proximity between the polymer chains in the interface layer and the pore wall in the PBMA / Al composite sample weakens the anchoring effect of NMT, causing the bonding strength of PBMA and Al in the NMT spline to decrease rapidly.

[0095] The above embodiments are only used to help understand the method of the present invention and its core concept. It should be noted that, for those skilled in the art, without departing from the principles of the present invention, several improvements and modifications may be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for testing the proximity of interlayers of polymer composite materials. It is characterized in that The test method comprises the following steps: (1) Grafting the fluorescent donor molecule onto the polymer chain by copolymerization or side group reaction to obtain a polymer matrix containing the fluorescent donor; (2) preparing nanopores on the surface of a metal or inorganic material substrate by anodization or chemical etching, and grafting fluorescent receptor molecules onto the surface of the nanopores by chemical modification to obtain a substrate having a fluorescent receptor on the surface; (3) compounding the polymer matrix containing the fluorescent donor with the substrate surface containing the fluorescent receptor by melt infiltration, and obtaining a polymer / substrate composite material by heat treatment; (4) Collecting the fluorescence spectrum of the polymer / substrate composite material by surface reflection method, and obtaining the proximity between the polymer chain and the substrate in the interface layer by comparing the intensity ratio of the characteristic peaks of the fluorescence acceptor and the fluorescence donor in the fluorescence spectrum.

2. The method for testing the proximity between interlayers of a polymer composite material according to claim 1, It is characterized in that The molar concentration of the fluorescent donor in the polymer matrix in step (1) is 0.05-1%.

3. The method for testing the proximity between interlayers of a polymer composite material according to claim 1, It is characterized in that The nanopores in step (2) have an average diameter of 10 to 500 nm and an average length of 1 to 100 μm.

4. The method for testing the proximity between interlayers of a polymer composite material according to claim 1, It is characterized in that The grafting density of the fluorescent receptor on the surface of the substrate in step (2) is 0.01 to 0.5 nm. -2 .

5. The method for testing the proximity between interlayers of a polymer composite material according to claim 1, It is characterized in that The polymer matrix is ​​a thermoplastic resin, and the thermoplastic resin is selected from one or more of polystyrene, polymethyl methacrylate, and polybutyl methacrylate.

6. The method for testing the proximity between interlayers of a polymer composite material according to claim 1, It is characterized in that The metal material is selected from aluminum, titanium, copper and stainless steel.

7. The method for testing the proximity between interlayers of a polymer composite material according to claim 1, It is characterized in that The heat treatment method in step (3) includes changing the cooling rate of the composite system or isothermal annealing treatment.

8. The method for testing the proximity between interlayers of a polymer composite material according to claim 7, It is characterized in that The cooling rate is 0.2-104°C / min; the temperature range of the isothermal annealing is 20-100°C above the Tg of the thermoplastic resin.

9. The method for testing the proximity between interlayers of a polymer composite material according to claim 1, It is characterized in that The fluorescence donor in step (1) and the fluorescence acceptor in step (2) form a FRET molecule pair, and the fluorescence donor can undergo fluorescence resonance energy transfer to the fluorescence acceptor.

10. The method for testing the proximity between interlayers of a polymer composite material according to claim 9, It is characterized in that The FRET molecular pair is a carbazole group and anthracene group or a nitrobenzoxadiazole group and a spiropyran group.

11. The method for testing the proximity between interlayers of a polymer composite material according to claim 9, It is characterized in that The FRET molecule pair has a FRET efficiency higher than 85%.

Citation Information

Patent Citations

  • Metal-resin composite and heat-treating method thereof

    CN106273216B

  • Preparation method of superhydrophobic microporous polymer film material

    CN103665415A

  • Method for detecting a spatial proximity of a first and a second epitope

    CN106715724A