A method for preparing a lithium-sulfur battery electrode material and a niobium selenide@selenium composite lithium-sulfur battery positive electrode material
Through the dry preparation process of using niobium selenide-containing composite materials in lithium sulfur batteries, the problems of slow reaction kinetics and poor conductivity of lithium sulfur batteries are solved, the discharge specific capacity and sulfur loading of the battery are improved, and the discharge specific capacity and sulfur loading of the battery are achieved. More efficient energy storage and conversion.
Patent Information
- Application Number
- CN202210619397.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-05
- Filing Date
- 2022-06-01
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Due to the slow reaction kinetics, poor conductivity, polysulfide shuttle and sulfur volume changes, lithium-sulfur batteries have low capacity, slow charging and short life, making it difficult to meet the needs of modern energy storage equipment with high capacity, fast charging and long life. Require.
The composite material containing niobium selenide is prepared by an oil bath method, and sulfur is poured into sulfur to obtain the composite active material of niobium selenide and sulfur, and mixed with conductive agent and binder, and a lithium sulfur battery is made by dry preparation process. The positive electrode increases the discharge specific capacity and sulfur load capacity of the battery.
The high discharge specific capacity and Coulomb efficiency performance of lithium sulfur batteries are achieved, and the problems of solvent use and low coating thickness in wet preparation are avoided, and higher sulfur loading capacity and capacity are obtained, while improving the cycling performance of the battery.
Smart Images

Figure CN114937767B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemical energy, and in particular relates to a method for preparing a dry-process positive electrode of a lithium-sulfur battery containing a niobium selenide@selenium composite material. Background Art
[0002] With the change of national energy layout, various new energy sources have gradually come on stage. Among them, electrochemical energy storage, as a leader in the field of energy storage, has attracted much attention. However, with the development of science and technology and the demand for more convenient life, the requirements for energy storage equipment have become increasingly stringent, not only requiring high capacity, fast charging, and long life, but also expecting it to be small in size and light in weight. Various emerging energy storage devices, such as lithium-ion batteries, zinc-ion batteries, sodium-ion batteries and various metal-air batteries have received widespread attention. Among them, lithium-sulfur batteries have attracted much attention due to their ultra-high theoretical specific capacity. However, lithium-sulfur batteries have various problems such as slow reaction kinetics, poor conductivity, polysulfide shuttle, sulfur volume change, and low sulfur loading. At present, there have been a lot of related studies on the above problems, such as adding catalysts to accelerate the reaction, adding conductive agents to increase conductivity, and adding porous polymers to control polysulfide shuttle and sulfur volume change to solve the problems of lithium-sulfur batteries, which is of great significance to the development of lithium-sulfur batteries.
[0003] As a homologous element of sulfur, selenium is regarded as a new type of positive electrode material for lithium-ion batteries due to its higher conductivity and high volumetric capacity. In addition, although the specific capacity of selenium is lower than that of sulfur, its high mass density determines its higher volumetric energy density. Therefore, it is of great practical significance to develop a new electrode material that combines the advantages of sulfur and selenium. Summary of the invention
[0004] In order to solve the above problems existing in lithium-sulfur batteries, the present invention provides a method for preparing a dry-process positive electrode for a lithium-sulfur battery containing a niobium selenide@selenium composite material. When the positive electrode obtained by the method is applied to a lithium-sulfur battery, it exhibits higher discharge specific capacity and sulfur loading, and higher coulombic efficiency performance.
[0005] The present invention provides a lithium-sulfur battery electrode material, comprising a niobium selenide@selenium composite material, characterized in that the electrode material comprises a composite active material of niobium selenide@selenium and sulfur obtained by impregnating the niobium selenide@selenium composite material with sulfur.
[0006] The present invention also provides a process for preparing a lithium-sulfur battery electrode material, comprising the following steps:
[0007] Step 1: preparing niobium selenide@selenium composite material by oil bath method;
[0008] Step 2: Fill the niobium selenide@selenium composite material obtained in step 1 with sulfur to obtain a composite active material of niobium selenide@selenium and sulfur.
[0009] Preferably, in step 1, niobium pentachloride and selenium powder are used as raw materials, oleylamine and 1-octadecene are used as morphology regulators, the ratio of oleylamine and 1-octadecene is adjusted to control the width of the niobium selenide sheet, tri-n-octylphosphine is used as solvent, and a high temperature oil bath is used at 300°C.
[0010] Preferably, in any of the above items, the raw material ratio is: niobium pentachloride: selenium powder = 1:2-3.
[0011] Any of the above items is preferably that in step 2, the ratio of sulfur injection is: niobium selenide@selenium:sulfur=1:4-2:3.
[0012] In a preferred embodiment of the present invention, a method for preparing a niobium selenide@selenium composite phase material is provided, wherein the niobium source is preferably niobium pentachloride, and the method comprises the following steps:
[0013] S1. Pour oleylamine (OA) and 1-octadecene (ODE) into a three-necked flask in sequence to obtain solution A;
[0014] S2, placing the three-necked flask containing solution A in step S1 in an oil bath, introducing argon gas, and keeping the temperature at 130° C. for 30 min to remove the dissolved water and oxygen in the solution;
[0015] S3. After step S2, niobium pentachloride (NbCl5), selenium powder (Se) and tri-n-octylphosphine (TOP) were added to solution A, nitrogen was continuously introduced, the temperature was raised to 300°C and kept at this temperature for 1.5h;
[0016] S4. When the solution of step S3 is cooled to room temperature, the solution and the precipitate are centrifuged, and then the solvent is removed by centrifugation with n-hexane and ethanol for multiple times, and the product after centrifugation is placed in a vacuum oven and dried at 60° C. to obtain a niobium selenide@selenium (NbSe2@Se) composite phase material.
[0017] In a specific embodiment, preferably, in step S1, the volume ratio of OA to ODE is 1:1.
[0018] In a specific embodiment, preferably, in step S3, 1 mMol NbCl5, 2 mMolSe powder, and 1 ml TOP are added to every 15 ml of solution A.
[0019] In a specific embodiment, preferably, in step S4, before each centrifugation, ultrasonic dispersion is performed after adding new solvent so that the solvent can be thoroughly washed away.
[0020] In another preferred embodiment of the present invention, a composite active material is formed by combining the NbSe2@Se composite phase material prepared by the above method with S. The specific implementation steps are:
[0021] 60% to 80% of S is mixed evenly with NbSe2@Se, and then melt-compounded in an argon environment to obtain a composite active material of NbSe2@Se and S.
[0022] In a specific embodiment, the preferred mixing method is to ball-mill the NbSe2@Se composite material and S powder.
[0023] In a specific embodiment, the melt reaction temperature is 155° C. and the time is 12 hours.
[0024] The present invention also provides a dry-process positive electrode preparation process containing niobium selenide@selenium for lithium-sulfur batteries, wherein the composite active material of niobium selenide@selenium and sulfur described in any of the above items is mixed with a binder and a conductive agent to obtain a positive electrode material, and an electrode sheet is obtained by a dry-process preparation process.
[0025] Preferably, the composite active material of niobium selenide@selenium and sulfur:conductive agent:binder=6-8:1-3:1.
[0026] In a preferred embodiment of the present invention, a positive electrode material for a lithium-sulfur battery is provided, comprising the composite active material of NbSe2@Se and S.
[0027] In a specific embodiment, preferably, the lithium-sulfur battery positive electrode material further comprises a conductive agent and a binder.
[0028] In a specific embodiment, preferably, the conductive agent includes but is not limited to Super P, carbon fiber (VGCF), carbon nanotube (CNT), graphene and the like.
[0029] In a specific embodiment, preferably, the binder includes but is not limited to polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMA) and styrene-butadiene rubber (SBR) and the like.
[0030] The present invention also provides application of the above-mentioned lithium-sulfur battery electrode material in the preparation of lithium-sulfur batteries.
[0031] The present invention also provides application of the above-mentioned preparation process of lithium-sulfur battery electrode material in preparation of lithium-sulfur battery.
[0032] The present invention also provides the application of the above-mentioned dry-process positive electrode preparation process containing niobium selenide@selenium for lithium-sulfur batteries in the preparation of lithium-sulfur batteries, including a lithium-sulfur positive electrode prepared by the dry process of the above-mentioned material.
[0033] In a preferred embodiment of the present invention, a lithium-sulfur battery is provided, which comprises a positive electrode made of the above-mentioned lithium-sulfur battery positive electrode material.
[0034] In a specific embodiment, preferably, the negative electrode material of the lithium-sulfur battery comprises 60-80 parts by weight of the composite active material of niobium selenide@selenium and sulfur, 10-30 parts by weight of a conductive agent, and 10 parts by weight of a binder.
[0035] Beneficial effects:
[0036] In the present invention, the NbSe2@Se composite material is firstly synthesized by an oil bath method, and then sulfur (S) powder and NbSe2@Se are uniformly mixed and melted in an argon environment to obtain a composite active material.
[0037] The active material of the present invention is used to prepare lithium-sulfur batteries, showing excellent cycle performance. At the same time, compared with the wet electrode preparation process, the dry electrode preparation process adopted by the present invention does not require the use of solvents, reduces the use of toxic organic solvents, and is beneficial to the health of experimental operators. At the same time, the low capacity caused by the low coating thickness of the wet electrode preparation process can also be avoided. The NbSe2@Se and sulfur composite active material provided by the present invention can be used through a dry electrode preparation process to obtain a higher sulfur loading and thus a higher capacity battery electrode. Therefore, the present invention has important value in the development of practical lithium-sulfur batteries and related materials in the field of energy storage and conversion.
[0038] The NbSe2@Se composite material of the present invention has the above-mentioned excellent properties. The essence is that NbSe2 has good catalytic performance, which effectively accelerates the conversion of solid sulfur into polysulfide, solves the slow reaction kinetics problem of lithium-sulfur batteries, and realizes the rapid reaction of lithium-sulfur batteries. At the same time, NbSe2 is considered to be a promising and promising anode alternative material for secondary batteries. The reaction that occurs is Theoretical capacity is 427 mAh g -1 As a lithium-ion main material, it is very promising. In addition, as a homologous element of sulfur, selenium has higher conductivity and high volumetric capacity. Doping some selenium as the main material in lithium-sulfur batteries is beneficial to ensure the capacity of the electrode while ensuring a certain conductivity, reducing the use of conductive agents that do not generate capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is the XRD diagram of the NbSe2@Se composite phase material prepared in the preferred embodiment 1 of the present invention.
[0040] Figure 2 This is the XPS graph of Se of the NbSe2@Se composite phase material prepared in the preferred embodiment 1 of the present invention.
[0041] Figure 3This is the XPS graph of Nb in the NbSe2@Se composite phase material prepared in the preferred embodiment 1 of the present invention.
[0042] Figure 4 This is a diagram of the long cycle performance of the composite material N of the NbSe2@Se composite phase material and sulfur powder prepared in the preferred embodiment 1 of the present invention as a positive electrode material for a lithium-sulfur battery. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be described in detail below in conjunction with specific embodiments and comparative examples. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.
[0044] Unless otherwise specified, the equipment used in the present embodiment, comparative example and experimental example are all conventional experimental equipment, and the materials and reagents used are all commercially available.
[0045] The conductive carbon used was purchased high-conductive carbon black Super P, and the XRD powder diffractometer was Bruker D8 (Cu Kα, ), the state of the material elements can be obtained from the X-ray photoelectron spectrometer (XPS, PHI5300), and the constant current charge and discharge test uses the Xinwei battery test system (LAND CT2001A) with a voltage test range from 1.7-2.8V.
[0046] Example 1
[0047] (1) Add 15 ml of OA and 15 ml of ODE into a three-necked flask, place it in an oil bath, add a stirrer for stirring, introduce argon, and degas for 30 min at 130°C.
[0048] (2) After degassing, add 2 mMol of NbCl5 and 4 mMol of Se powder to the three-necked flask in step (1), and at the same time, add 2 ml of TOP, continue stirring, continue to introduce argon, raise the temperature to 300°C, and react for 1.5 hours.
[0049] (3) After the reaction in step (2) is completed, the mixture is naturally cooled to room temperature, and the solution and the precipitate are centrifuged. After centrifugation, the supernatant is discarded, n-hexane is added, and ultrasonic treatment is performed for 2 to 3 minutes until the precipitate is completely dispersed. The mixture is centrifuged again, and the process is repeated three to four times. The same centrifugation step is then performed with ethanol to wash away the n-hexane.
[0050] (4) The precipitate obtained by centrifugation in step (3) is placed in a vacuum oven and dried at 60° C. to obtain a NbSe2@Se composite material.
[0051] (5) The NbSe2@Se composite material obtained in step (4) and S powder were ball-milled at a ratio of 1:4 for 3 h and mixed evenly. The mixture was then placed in a reactor, and the gas therein was replaced with argon. The mixture was placed in an oven and melt-reacted at 155°C for 12 h. After natural cooling, a composite active material of NbSe2@Se and S was obtained.
[0052] Lithium-sulfur battery cathode material and preparation of lithium-sulfur battery
[0053] The NbSe2@Se composite active material obtained in the embodiment was mixed evenly with the conductive agent Super P and the binder PVDF in a mass ratio of 8:1:1 by ball milling at room temperature for 3 hours, then placed in a twin-screw extruder and heated to 175°C to melt the binder dry powder, and then extruded into a continuous self-supporting dry coating electrode film with a film thickness of 300 μm. The electrode film was then pressed together with a carbon-containing aluminum foil at 175°C to form a positive electrode sheet.
[0054] The positive electrode was made into a lithium-sulfur battery for subsequent electrochemical performance testing. The battery was assembled in an argon-filled glove box (water and oxygen values were less than 0.01ppm), a 2032 button battery case was used, Celgard2500 was used as a diaphragm, a metal lithium sheet was used as a negative electrode, and the electrolyte was a mixed solvent of 1,3 dioxolane: ethylene glycol dimethyl ether = 1:1 (DOL:DME) with 1M lithium bistrifluoromethanesulfonyl imide (LiTFSI) and 1% lithium nitrate added.
[0055] The performance test results of the NbSe2@Se composite material and the lithium-sulfur battery positive electrode obtained in Example 1 are as follows: Figures 1 to 4 shown.
Claims
1. A lithium-sulfur battery electrode material, comprising a niobium selenide@selenium composite material, characterized in that The niobium selenide@selenium is NbSe2@Se, and its electrode material comprises the niobium selenide@selenium composite material being poured with sulfur in a mass ratio of niobium selenide@selenium:sulfur=1:4-2:3 to obtain a composite active material of niobium selenide@selenium and sulfur.
2. A process for preparing the lithium-sulfur battery electrode material according to claim 1, comprising the following steps: Step 1: preparing niobium selenide@selenium composite material by oil bath method; Step 2: Fill the niobium selenide@selenium composite material obtained in step 1 with sulfur to obtain a composite active material of niobium selenide@selenium and sulfur.
3. The preparation process according to claim 2, characterized in that: In step 1, niobium pentachloride and selenium powder are placed in a container as raw materials, and then three chemicals, oleylamine, 1-octadecene and tri-n-octylphosphine, are added to the container. The container filled with chemicals is placed in an oil bath pot and heated from room temperature to 300°C in the oil bath pot.
4. The preparation process according to claim 3, characterized in that: The molar ratio of the raw materials is: niobium pentachloride: selenium powder = 1:2-3.
5. A dry process for preparing a positive electrode containing niobium selenide@selenium for a lithium-sulfur battery, wherein the positive electrode comprises the lithium-sulfur battery electrode material according to claim 1, characterized in that: The composite active material of niobium selenide@selenium and sulfur is mixed with a binder and a conductive agent to obtain a positive electrode material, and an electrode sheet is obtained by adopting a dry preparation process.
6. The dry cathode preparation process according to claim 5, characterized in that: The mass ratio of the mixed materials is: niobium selenide@selenium and sulfur composite active material: conductive agent: binder = 6-8:1-3:
1.
7. Use of the lithium-sulfur battery electrode material according to claim 1 in the preparation of lithium-sulfur batteries.
8. Application of the preparation process of the lithium-sulfur battery electrode material according to any one of claims 2 to 4 in the preparation of lithium-sulfur batteries.
9. Application of the dry process for preparing positive electrode containing niobium selenide@selenium for lithium-sulfur battery according to claim 5 or 6 in the preparation of lithium-sulfur battery.
Citation Information
Patent Citations
Preparation and application of lithium ion battery electrode material
CN111422837A
Electrode material comprising metal sulfide
US20130017418A1
Electrode structures for lithium batteries
US20220109142A1