Vacuum electron beam welding method for wide gap blanks
By performing electron beam scanning pre-welding on the upper and lower edges of the wide gap blank, the welding defect problem is solved, and the vacuum packaging and welding efficiency of the blank are improved.
Patent Information
- Application Number
- CN202210782722.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-29
- Publication Date
- 2025-02-25
- Estimated Expiration
- 2042-06-29
AI Technical Summary
The prior art is difficult to effectively weld wide gap blanks, resulting in welding defects such as missing welding, pits and cracks, which in turn damages the vacuum state between the blanks.
By scanning electron beams of the upper and lower edges of the gaps of the blank to be welded, the gap width is reduced to the weldable level, and then formal welding is performed.
The gap width is effectively reduced, welding defects are avoided, the vacuum state between the blanks is maintained, and vacuum electron beam welding of wide gap blanks is realized.
Smart Images

Figure CN114951942B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electron beam welding, in particular to a vacuum electron beam welding method for wide gap blanks, which is suitable for the vacuum electron beam packaging process of blanks to be welded with a gap of 0.5 to 3 mm. Background Art
[0002] Metal construction forming technology is a new large forging manufacturing technology proposed in the past 10 years. This technology uses multiple homogenized small-sized slabs as the basic elements, and through surface cleaning, vacuum packaging, high-temperature heating, deformation connection, forging and forming, etc., eliminates the interface, achieves "traceless" connection, and finally obtains an integrated large-sized homogeneous component. This technology cleverly combines traditional forging methods with emerging additive manufacturing, greatly shortening the performance gap between laboratory materials and engineering components, and is particularly suitable for solving the homogenization preparation problem of key large components in the nuclear power field.
[0003] Traditionally, when using metal construction forming technology, vacuum electron beam welding or manual welding is used for vacuum packaging to maintain a vacuum state between the construction elements and achieve complete connection during the subsequent thermal deformation process. However, for some metals to be welded, due to uneven surface processing or deformation caused by previous welding, the surface is uneven, which leads to a large gap between the two adjacent billets after stacking and assembly. It is impossible to use vacuum electron beam to directly seal the gap, or welding leaks, deep pits and cracks will occur after welding, resulting in the breaking of vacuum between the construction elements, the interface being polluted by the atmosphere, oxidation, and directly leading to construction failure. Therefore, if the welding problem of wide-gap billets using vacuum electron beam welding can be solved through new technology, the sealing efficiency of wide-gap billets will be greatly improved, thereby improving productivity. Summary of the invention
[0004] The object of the present invention is to provide a vacuum electron beam welding method for wide gap blanks, so as to solve the welding problem that vacuum electron beam welding of wide gap blanks is not possible.
[0005] The technical solution of the present invention is:
[0006] A vacuum electron beam welding method for wide gap blanks, wherein the gap between the blanks to be welded is 0.5 to 3 mm. During vacuum electron beam welding, the blanks are first pre-welded before welding, that is, the upper and lower edges of the gap of the blanks to be welded are pre-welded by electron beam scanning respectively to reduce the gap width, and then the weld is formally welded as a component.
[0007] The vacuum electron beam welding method for wide gap blanks comprises the following steps:
[0008] 1) Mechanically grind the blank to be welded and clean the surface to be welded;
[0009] 2) Stack the blanks to be welded so that the upper and lower surfaces of two adjacent blanks to be welded are in contact and aligned;
[0010] 3) Put the stacked blanks to be welded into a vacuum chamber and evacuate the chamber to make the space between two adjacent blanks to be welded a vacuum state;
[0011] 4) First, a smaller beam is used to scan and pre-weld along the upper edge of the gap between the blanks to be welded, and then the lower edge of the gap is scanned and pre-welded, thereby reducing the width of the gap between the blanks to be welded, so that the gap reaches a level that can be directly welded by electron beam welding;
[0012] 5) The welding beam is used to perform assembly welding on the blanks to be welded, and the weld surrounds the blanks to be welded to achieve vacuum packaging of two adjacent blanks to be welded, so that the vacuum state between the blanks to be welded is still maintained after leaving the vacuum chamber.
[0013] In the vacuum electron beam welding method for wide gap blanks, in step 2), after the blanks to be welded are aligned, the misalignment between adjacent blanks to be welded is no more than 2 mm.
[0014] The vacuum electron beam welding method for wide gap blanks, in step 3), the vacuum degree of the vacuum chamber is ≤8×10 -2 Pa.
[0015] The vacuum electron beam welding method for wide gap blanks adopts an electron beam to scan the upper edge of the gap of the blank to be welded for pre-welding, the electron beam scanning center position is 0.3 to 2 mm away from the upper edge of the gap of the blank to be welded, and the scanning radius is 0.5 to 3 mm; the acceleration voltage is 80 to 100 kV, the welding beam current is 50 to 100 mA, and the scanning speed is 150 to 400 mm / min.
[0016] The vacuum electron beam welding method for wide gap blanks adopts an electron beam to scan the lower edge of the gap of the blank to be welded for pre-welding, the electron beam scanning center position is 0.3 to 2 mm away from the lower edge of the gap of the blank to be welded, and the scanning radius is 0.5 to 3 mm; the acceleration voltage is 80 to 100 kV, the welding beam current is 50 to 100 mA, and the scanning speed is 150 to 400 mm / min.
[0017] In the vacuum electron beam welding method for wide gap blanks, in step 5), the welding sequence is: first weld one edge, then rotate the blank to be welded 180°, weld the second edge, then rotate 90° to weld the third edge, and finally rotate 180° to weld the fourth edge; when multiple layers of welds are welded simultaneously, the welding sequence is layer by layer from top to bottom.
[0018] In the vacuum electron beam welding method for wide gap blanks, when performing formal assembly welding, the welding acceleration voltage is 80-100 kV, the welding beam current is 80-150 mA, and the welding speed is 150-300 mm / min.
[0019] The design concept of the present invention is:
[0020] The present invention performs scanning pre-welding on the local blank near the weld of the blank to be welded, melts the metal at the edge of the gap by electron beam scanning welding, thereby reducing the gap width to a weldable level, and finally uses electron beam to complete the formal welding of the assembly.
[0021] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0022] 1. The present invention can be used to achieve electron beam welding of wide gap blanks, and then realize vacuum packaging of blanks. The existing electron beam welding technology has high requirements for the gap of the metal to be welded, and generally requires the gap to be less than 0.5mm. For blanks with larger gaps, machining is usually used to improve the flatness of the blanks, and the gap of the blanks after reducing the size of the blanks is complicated and has low production efficiency. It is difficult to improve the flatness of some large-sized blanks by machining, or the blanks are deformed during the previous welding process, resulting in unevenness. If electron beam welding is directly used, welding defects such as leaking welding, pits, and cracks are easily formed during the welding process, resulting in failure of vacuum packaging of the blanks. The vacuum electron beam packaging method proposed by the present invention can effectively reduce the gap of the blanks to be welded by scanning and pre-welding the local blanks along the upper and lower edges of the gap, and has sufficient penetration depth to avoid weld cracking, thereby being able to maintain the vacuum state of the interface between the blanks, and realizing vacuum electron beam welding of wide gap blanks.
[0023] 2. The present invention performs electron beam scanning welding on the upper and lower blanks of the gap, so that the local blanks along the upper and lower edges of the gap melt themselves, thereby reducing the gap width, avoiding the problem of being unable to weld by vacuum electron beam method due to the gap between the blanks to be welded being too large, eliminating the blank machining process and improving work efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the following briefly introduces the drawings required in the embodiment of the present invention:
[0025] Figure 1 Schematic diagram of electron beam scanning the upper edge of the pre-welding gap.
[0026] Figure 2 Schematic diagram of electron beam scanning the lower edge of the pre-welding gap.
[0027] Explanation of numbers in the figure: 1 electron beam emitting gun, 2 electron beam, 3 blank to be welded, 4 gap, 5 upper edge of gap, 6 lower edge of gap, 7 scanning center. DETAILED DESCRIPTION
[0028] In the specific implementation process, the present invention provides a vacuum electron beam welding method for wide gap billets. First, forged billets, cast billets, rolled billets, etc. are used as welding billets. After surface machining and cleaning, two or more billets to be welded are stacked together so that adjacent billets to be welded are aligned. Subsequently, the stacked two or more billets to be welded are placed in a vacuum chamber for evacuation, and an electron beam is used to scan and pre-weld the upper and lower edges of the gap between the billets, thereby reducing the gap width and achieving a state that can be directly welded; after pre-welding, the gap is formally welded, and finally the vacuum sealing of the billet is achieved. The specific steps of the method are as follows:
[0029] The first step is to clean the upper and lower surfaces of the processed blank to be welded, which can be done by machining, grinding, cleaning with cleaning fluid, laser cleaning, electrolytic polishing and other methods.
[0030] In the second step, the cleaned multiple building blocks are stacked so that the upper and lower planes of the blanks to be welded are opposite, and the upper and lower surfaces of two adjacent blocks are in contact and aligned, and the misalignment after alignment is no more than 2mm.
[0031] The third step is to put the stacked blanks into the vacuum chamber and evacuate the space between the two adjacent blanks. The vacuum degree of the vacuum chamber should be ≤8×10 -2 Pa.
[0032] The fourth step is to use a scanning welding process with an acceleration voltage of 80-100 kV, a beam current of 50-100 mA, and a scanning speed of 150-400 mm / min. First, scanning welding is performed on the edge of the upper edge of the blank at a distance of 0.3-2 mm from the gap ( Figure 1 ), and then the same process is used to scan and weld the lower edge of the gap ( Figure 2 ), the scanning radius is 0.5 to 3 mm, thereby reducing the width of the gap between the billets and making the gap reach a level that can be directly welded by electron beam.
[0033] like Figure 1-Figure 2 As shown, the electron beam outlet of the electron beam emitting gun 1 corresponds to the gap 4 between two adjacent layers of the blanks 3 to be welded in the horizontal direction, and the electron beam emitting gun 1 is used to generate an electron beam 2 for scanning welding. When scanning welding is performed on the edge of the blank at the upper edge 5 of the gap, the distance between the scanning center 7 and the upper edge 5 of the gap is 0.3 to 2 mm; when scanning welding is performed on the edge of the blank at the lower edge 6 of the gap, the distance between the scanning center 7 and the lower edge 6 of the gap is 0.3 to 2 mm.
[0034] The fifth step is to weld along the center of the gap between the billets, with the weld surrounding the billets, so as to achieve vacuum packaging of two adjacent building blocks, so that the vacuum state between the units can still be maintained after leaving the vacuum chamber. The welding sequence is: first weld one edge, then rotate the billet 180°, weld the second edge, then rotate 90° to weld the third edge, and finally rotate 180° to weld the fourth edge. When welding multiple layers of welds at the same time, the welding sequence is from top to bottom. The welding acceleration voltage is 80-100kV, the welding beam current is 80-150mA, and the welding speed is 150-300mm / min.
[0035] The following is a further detailed description of the embodiments of the present invention in conjunction with the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to illustrate the principles of the present invention, but cannot be used to limit the scope of the present invention, that is, the present invention is not limited to the embodiments, and any modifications, substitutions and improvements of equivalent modes are covered without departing from the spirit of the present invention.
[0036] Example 1
[0037] In this embodiment, the material of the blank to be welded is 316H stainless steel. Through surface machining and degreasing cleaning, the corner gap of the square blank to be welded after the blanks are stacked is 2.5mm, and the gap in the middle is 1-2mm. Then, the stacked multiple pieces (5 pieces in this embodiment) of the blanks to be welded are placed in a vacuum chamber for evacuation, and the upper and lower edges of the gaps between the blanks are scanned and pre-welded by an electron beam, thereby reducing the gap width and making it reach a state that can be directly welded; after pre-welding, the gap is formally welded, and finally the vacuum sealing of the blank is achieved. The specific steps of this method are as follows:
[0038] In the first step, the upper and lower surfaces of the processed blank to be welded are mechanically polished and then cleaned with alcohol.
[0039] In the second step, the cleaned blanks to be welded are stacked, and the upper and lower surfaces of the blanks to be welded are contacted and aligned, and the misalignment after alignment is 0.5mm.
[0040] The third step is to put the stacked blanks into the vacuum chamber and evacuate the space between the two adjacent blanks to be welded. The vacuum degree of the vacuum chamber is 6.6×10 -2 Pa.
[0041] The fourth step is to use a scanning welding process with an acceleration voltage of 90 kV, a beam current of 70 mA, and a scanning speed of 400 mm / min. First, scanning welding is performed on the edge of the upper edge of the blank to be welded at a distance of 1 mm from the gap. The scanning welding radius is 2 mm ( Figure 1 ), and then use the same process to scan the edge of the blank to be welded at a distance of 1mm from the gap, and the scanning welding radius is 2mm ( Figure 2), thereby reducing the width of the gap between the blanks to be welded, so that the gap reaches a level that can be directly welded by electron beam.
[0042] The fifth step is to weld along the center of the gap between the blanks to be welded, and the weld surrounds the blanks to be welded, thereby realizing the vacuum packaging of two adjacent building blocks, so that the vacuum state between the blocks can still be maintained after leaving the vacuum chamber. The welding sequence is: first weld one edge, then rotate the blank to be welded 180°, weld the second edge, then rotate 90° to weld the third edge, and finally rotate 180° to weld the fourth edge. The welding acceleration voltage is 90kV, the welding beam is 100mA, and the welding speed is 200mm / min, and finally the sealing welding is completed.
[0043] Example 2
[0044] In this embodiment, the material of the blank to be welded is Q345 steel. Through surface machining and degreasing cleaning, the corner gap of the square blank to be welded after the blanks are stacked is 1.5mm, and the gap in the middle is 1mm. Then, the stacked multiple pieces (10 pieces in this embodiment) of the blanks to be welded are placed in a vacuum chamber for evacuation, and the upper and lower edges of the gaps between the blanks to be welded are scanned and pre-welded by an electron beam, thereby reducing the gap width and making it reach a state that can be directly welded; after pre-welding, the gap is formally welded, and finally the vacuum sealing of the blank to be welded is achieved. The specific steps of this method are as follows:
[0045] In the first step, the upper and lower surfaces of the processed blank to be welded are mechanically polished and then cleaned with alcohol.
[0046] In the second step, the cleaned blanks to be welded are stacked, and the upper and lower surfaces of the blanks to be welded are contacted and aligned, and the misalignment after alignment is 1.0 mm.
[0047] The third step is to put the stacked blanks into the vacuum chamber and evacuate the space between the two adjacent blanks to be welded. The vacuum degree of the vacuum chamber is 5×10 -2 Pa.
[0048] The fourth step is to use a scanning welding process with an acceleration voltage of 100 kV, a beam current of 50 mA, and a scanning speed of 200 mm / min. First, scanning welding is performed on the edge of the upper edge of the blank to be welded at a distance of 0.5 mm from the gap. The scanning welding radius is 1 mm ( Figure 1 ), and then use the same process to perform scanning welding on the edge of the blank to be welded at a distance of 0.5mm from the gap, and the scanning welding radius is 1mm ( Figure 2 ), thereby reducing the width of the gap between the blanks to be welded, so that the gap reaches a level that can be directly welded by electron beam.
[0049] The fifth step is to weld along the center of the gap between the blanks to be welded, and the weld surrounds the blanks to be welded, thereby realizing the vacuum packaging of two adjacent building blocks, so that the vacuum state between the blocks can still be maintained after leaving the vacuum chamber. The welding sequence is: first weld one edge, then rotate the blank to be welded 180°, weld the second edge, then rotate 90° to weld the third edge, and finally rotate 180° to weld the fourth edge. The welding acceleration voltage is 100kV, the welding beam is 130mA, and the welding speed is 200mm / min, and finally the sealing welding is completed.
[0050] Example 3
[0051] In this embodiment, the material of the blank to be welded is SA508-3 steel. Through surface machining and degreasing cleaning, the corner gap of the square blank to be welded after the blanks are stacked is 3.0mm, and the gap in the middle is 1-2mm. Then, the stacked multiple pieces (7 pieces in this embodiment) of the blanks to be welded are placed in a vacuum chamber for evacuation, and an electron beam is used to scan and pre-weld the upper and lower edges of the gaps between the blanks to be welded, thereby reducing the gap width and making it reach a state that can be directly welded; after pre-welding, the gap is formally welded, and finally the vacuum sealing of the blank to be welded is achieved. The specific steps of this method are as follows:
[0052] In the first step, the upper and lower surfaces of the processed blank to be welded are mechanically polished and then cleaned with alcohol.
[0053] In the second step, the cleaned blanks to be welded are stacked, and the upper and lower surfaces of the blanks to be welded are contacted and aligned, and the misalignment after alignment is 2.0 mm.
[0054] The third step is to put the stacked blanks into the vacuum chamber and evacuate the space between the two adjacent blanks to be welded. The vacuum degree of the vacuum chamber is 7×10 -2 Pa.
[0055] The fourth step is to use a scanning welding process with an acceleration voltage of 100 kV, a beam current of 80 mA, and a scanning speed of 150 mm / min. First, scanning welding is performed on the edge of the upper edge of the blank to be welded 2 mm away from the gap, and the scanning welding radius is 3 mm ( Figure 1 ), and then use the same process to scan the edge of the blank to be welded at a distance of 2mm from the gap, and the scanning welding radius is 3mm ( Figure 2 ), thereby reducing the width of the gap between the blanks to be welded, so that the gap reaches a level that can be directly welded by electron beam.
[0056] The fifth step is to weld along the center of the gap between the blanks to be welded, and the weld surrounds the blanks to be welded, thereby realizing the vacuum packaging of two adjacent building blocks, so that the vacuum state between the blocks can still be maintained after leaving the vacuum chamber. The welding sequence is: first weld one edge, then rotate the blank to be welded 180°, weld the second edge, then rotate 90° to weld the third edge, and finally rotate 180° to weld the fourth edge. The welding acceleration voltage is 100kV, the welding beam is 150mA, and the welding speed is 250mm / min, and finally the sealing welding is completed.
[0057] Example 4
[0058] In this embodiment, the material of the blank to be welded is 304 stainless steel. Through surface machining and degreasing cleaning, the corner gap of the square blank to be welded after the blanks are stacked is 1mm, and the gap in the middle is 0.5mm. Then, the stacked multiple pieces (3 pieces in this embodiment) of the blanks to be welded are placed in a vacuum chamber for evacuation, and the upper and lower edges of the gaps between the blanks to be welded are scanned and pre-welded by an electron beam, thereby reducing the gap width and making it reach a state that can be directly welded; after pre-welding, the gap is formally welded, and finally the vacuum sealing of the blanks to be welded is achieved. The specific steps of this method are as follows:
[0059] In the first step, the upper and lower surfaces of the processed blank to be welded are mechanically polished and then cleaned with alcohol.
[0060] In the second step, the cleaned blanks to be welded are stacked, and the upper and lower surfaces of the blanks to be welded are contacted and aligned, and the misalignment after alignment is 1.5 mm.
[0061] The third step is to put the stacked blanks into the vacuum chamber and evacuate the space between the two adjacent blanks to be welded. The vacuum degree of the vacuum chamber is 6×10 -2 Pa.
[0062] The fourth step is to use a scanning welding process with an acceleration voltage of 80 kV, a beam current of 100 mA, and a scanning speed of 300 mm / min. First, scanning welding is performed on the edge of the upper edge of the blank to be welded at a distance of 0.3 mm from the gap, and the scanning welding radius is 0.5 mm ( Figure 1 ), and then the same process is used to perform scanning welding on the edge of the blank to be welded at a distance of 0.3mm from the gap, and the scanning welding radius is 0.5mm ( Figure 2 ), thereby reducing the width of the gap between the blanks to be welded, so that the gap reaches a level that can be directly welded by electron beam.
[0063] The fifth step is to weld along the center of the gap between the blanks to be welded, and the weld surrounds the blanks to be welded, thereby realizing the vacuum packaging of two adjacent building blocks, so that the vacuum state between the blocks can still be maintained after leaving the vacuum chamber. The welding sequence is: first weld one edge, then rotate the blank to be welded 180°, weld the second edge, then rotate 90° to weld the third edge, and finally rotate 180° to weld the fourth edge. The welding acceleration voltage is 80kV, the welding beam current is 120mA, and the welding speed is 250mm / min, and finally the sealing welding is completed.
[0064] The results of the embodiment show that the method of the present invention solves the problem of weld leakage, pits and cracks caused by too large a gap in the electron beam cross-welding process of wide gap blanks. The welding method of the present invention can effectively realize electron beam sealing welding of wide gap blanks and improve production efficiency.
[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A vacuum electron beam welding method for wide gap blanks, wherein the gap between the blanks to be welded is 0.5-3 mm, characterized in that: During vacuum electron beam welding, the blank is first pre-welded before welding, that is, the upper and lower edges of the gap of the blank to be welded are pre-welded by electron beam scanning, and the blank itself is melted locally at the upper and lower edges of the gap by electron beam scanning welding to reduce the gap width, and then the weld is formally welded; When the electron beam is used to scan the upper edge of the gap of the blank to be welded for pre-welding, the electron beam scanning center position is 0.3~2mm away from the upper edge of the gap of the blank to be welded, and the scanning radius is 0.5~3mm; the acceleration voltage is 80~100kV, the welding beam current is 50~100mA, and the scanning speed is 150~400mm / min; When the electron beam is used to scan the lower edge of the gap of the blank to be welded for pre-welding, the electron beam scanning center position is 0.3~2mm away from the lower edge of the gap of the blank to be welded, and the scanning radius is 0.5~3mm; the acceleration voltage is 80~100kV, the welding beam current is 50~100mA, and the scanning speed is 150~400mm / min; When the components are formally welded, the welding acceleration voltage is 80~100kV, the welding beam current is 80~150mA, and the welding speed is 150~300mm / min; The vacuum electron beam welding method for wide gap blanks comprises the following steps: 1) Mechanically grind the blank to be welded and clean the surface to be welded; 2) Stack the blanks to be welded so that the upper and lower surfaces of two adjacent blanks to be welded are in contact and aligned; 3) Put the stacked blanks to be welded into a vacuum chamber and evacuate the vacuum chamber to make the space between two adjacent blanks to be welded a vacuum state; 4) First, a smaller beam is used to scan and pre-weld along the upper edge of the gap between the blanks to be welded, and then the lower edge of the gap is scanned and pre-welded, thereby reducing the width of the gap between the blanks to be welded, so that the gap reaches a level that can be directly welded by electron beam welding; 5) The welding beam is used to perform assembly welding on the blanks to be welded. The weld surrounds the blanks to be welded, thereby realizing vacuum packaging of two adjacent blanks to be welded, so that the vacuum state between the blanks to be welded is still maintained after leaving the vacuum chamber.
2. The vacuum electron beam welding method for wide gap blanks according to claim 1, characterized in that: In step 2), after the blanks to be welded are aligned, the misalignment between adjacent blanks to be welded is no more than 2 mm.
3. The vacuum electron beam welding method for wide gap blanks according to claim 1, characterized in that: In step 3), the vacuum degree of the vacuum chamber is ≤ 8×10 -2 Pa.
4. The vacuum electron beam welding method for wide gap blanks according to claim 1, characterized in that: In step 5), the welding sequence is: first weld one edge, then rotate the blank to be welded 180°, weld the second edge, then rotate 90° to weld the third edge, and finally rotate 180° to weld the fourth edge; when multiple layers of welds are welded simultaneously, the welding sequence is layer by layer from top to bottom.
Citation Information
Patent Citations
Method of vacuum electron beam butt welding in condition of superstandard assembling clearance
CN102649192A
Vacuum electron beam welding method for special-shaped thin-walled metal plate welding structure cabin
CN106392294A
Method of improving seal welding efficiency of vacuum electron beam of multilayered slab
CN112475583A