Method for preparing color conversion crystal grains
By filling the color conversion blocks with bonding connectors with a height greater than that of the color conversion blocks, and bonding under vacuum conditions, the problem of quantum dots being susceptible to the influence of air and poor adhesion is solved, and the quantum dots are bonded. Effective protection and improvement of bonding effect, avoiding optical crosstalk.
Patent Information
- Application Number
- CN202210618234.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-01
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-06-01
AI Technical Summary
During the preparation process of color conversion grains, quantum dots are easily affected by air and have poor adhesion, resulting in optical crosstalk and difficulty in protection.
Fill the spaces between the color conversion blocks with bonding connectors that are larger than the color conversion blocks, and permanently bond the luminescent crystal grains to the bonding connectors in a vacuum environment to form a color conversion grain structure that covers the color conversion blocks. Isolates air and enhances bonding force.
It effectively protects the quantum dot structure, removes bubbles, enhances the bonding adhesion, improves the bonding effect, and avoids optical crosstalk.
Smart Images

Figure CN114975697B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of LED display, and in particular to a method for preparing a color conversion crystal grain. Background Art
[0002] Color conversion through quantum dots (QD) is currently the main method to achieve high-quality full color. Before making color conversion grains, QD ink needs to be injected into a sapphire substrate with pores, which is generally a substrate formed by electrochemical corrosion, referred to as an ECE substrate. Then the ECE substrate needs to be permanently bonded to the blue light grains, and the light color is converted to green or red by exciting green or red light quantum dots, and finally full colorization is achieved. During the whole process, there are problems that quantum dots need to be isolated from air for protection, as well as the problem of optical crosstalk. Summary of the invention
[0003] The object of the present invention is to provide a method for preparing color conversion crystal particles to avoid the problem that quantum dots are affected by air and have poor bonding strength.
[0004] In order to achieve the above-mentioned purpose, the present invention provides a method for preparing a color conversion grain, and the preparation method includes the following steps: providing a substrate, on which color conversion blocks arranged in an array are provided; filling bonding connectors between adjacent quantum dots, wherein the height of the bonding connectors is greater than the height of the color conversion blocks to form a cavity arranged around the color conversion blocks; providing luminescent grains corresponding to the color conversion blocks, wherein the luminescent grains have relative bonding surfaces and non-bonding surfaces, and the area of the bonding surfaces is greater than the area of the cavity opening; and permanently bonding the luminescent grains to the bonding connectors in a vacuum environment to cover the cavity, wherein the luminescent grains and the bonding connectors completely cover the color conversion blocks to form color conversion grains.
[0005] Preferably, a substrate is provided, on which color conversion blocks arranged in an array are provided, and the steps include: providing a substrate, corroding the surface of the substrate to form a plurality of pores; injecting quantum dot ink into the pores to form a quantum dot layer; and etching the quantum dot layer to form color conversion blocks arranged in an array.
[0006] Preferably, before the step of filling bonding connectors between adjacent color conversion blocks, wherein the height of the bonding connectors is greater than the height of the color conversion blocks to form a cavity arranged around the color conversion blocks, the method further includes: depositing a protective layer on the substrate, wherein the protective layer covers the color conversion blocks.
[0007] Preferably, a light-emitting crystal particle is provided corresponding to the color conversion block, the light-emitting crystal particle has relative bonding surfaces and non-bonding surfaces, and the area of the bonding surfaces is larger than the area of the cavity opening. The steps include: providing a substrate with the light-emitting crystal particle, the light-emitting crystal particle is arranged corresponding to the color conversion block, the light-emitting crystal particle has relative bonding surfaces and non-bonding surfaces, the area of the bonding surfaces is larger than the area of the cavity opening, and the bonding surfaces are connected to the substrate; installing the non-bonding surface of the light-emitting crystal particle on a temporary supporting plate through a temporary bonding film; and peeling off the substrate to form a temporary bonding structure of the light-emitting crystal particle.
[0008] Preferably, the light-emitting crystal grain is permanently bonded to the bonding connector in a vacuum environment to cover the cavity, and the light-emitting crystal grain and the bonding connector completely cover the color conversion block to form a color conversion crystal grain. The step includes: using a vacuum bonding machine to bond the light-emitting crystal grain to the bonding connector to cover the color conversion block.
[0009] Preferably, the light-emitting crystal grain is permanently bonded to the bonding connector in a vacuum environment to cover the cavity, and after the light-emitting crystal grain and the bonding connector completely cover the color conversion block to form a color conversion crystal grain, the step further includes: peeling off the temporary bonding film to separate the light-emitting crystal grain from the temporary bonding film and the temporary support plate.
[0010] Preferably, after the step of peeling off the temporary bonding film to separate the light-emitting crystal grain from the temporary bonding film and the temporary supporting plate, it also includes: thinning the substrate; cutting from the gap between adjacent light-emitting crystal grains toward the substrate to form a single color conversion crystal grain integrating the light-emitting crystal grain, the bonding connector and the color conversion block.
[0011] Preferably, the bonding connector is a metal or alloy having a melting point of 60-80° C., and the temperature at which the light-emitting crystal grain is bonded to the bonding connector is set corresponding to the melting point.
[0012] Preferably, the distance between the color conversion blocks is 30-35 micrometers, and the distance between the light-emitting crystal grains is 20-25 micrometers.
[0013] Preferably, the substrate is a sapphire substrate.
[0014] Compared with the prior art, the present invention fills bonding connectors with a height greater than the height of the color conversion blocks between the color conversion blocks, and permanently bonds the light-emitting crystal grains to the bonding connectors under vacuum conditions to form a color conversion crystal grain structure covering the color conversion blocks. This preparation method can effectively isolate the air, protect the quantum dot structure, remove bubbles, enhance the bonding force, and have a good bonding effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 Schematic diagram of the structure of the ECE substrate in the method for preparing the color conversion crystal grains according to an embodiment of the present invention.
[0016] Figure 2 It is a schematic diagram of the structure after quantum dot ink is injected onto the ECE substrate in the method for preparing the color conversion crystal grain according to an embodiment of the present invention.
[0017] Figure 3 It is a schematic structural diagram of a color conversion block array formed in the method for preparing a color conversion crystal grain according to an embodiment of the present invention.
[0018] Figure 4 Schematic diagram of the wafer structure after the color conversion block array is formed in the method for preparing the color conversion crystal grain according to the embodiment of the present invention.
[0019] Figure 5 It is a schematic structural diagram of forming a color conversion block protection layer in the method for preparing a color conversion crystal grain according to an embodiment of the present invention.
[0020] Figure 6 It is a schematic structural diagram of forming a bonding connector in a method for preparing a color conversion crystal grain according to an embodiment of the present invention.
[0021] Figure 7 It is a schematic structural diagram of a light-emitting crystal grain disposed on a substrate in a method for preparing a color conversion crystal grain according to an embodiment of the present invention.
[0022] Figure 8 It is a structural schematic diagram of a method for preparing a color conversion crystal grain according to an embodiment of the present invention, in which a light-emitting crystal grain disposed on a substrate is mounted on a temporary support plate through a temporary bonding film.
[0023] Fig. 9 Shown Figure 8 Schematic diagram of the structure of the light-emitting grains after removing the substrate.
[0024] Fig.10 Shown Fig. 9 After removing the substrate, the luminescent grains Figure 5 Schematic diagram of the structure after bonding of the bonding connector.
[0025] Fig.11 Shown Fig.10 Schematic diagram of the structure after removing the temporary bonding film and temporary bonding glue from the structure.
[0026] Fig.12 Shows the Fig.11 Schematic diagram of the structure of a single color conversion grain formed by cutting the prepared wafer structure. DETAILED DESCRIPTION
[0027] In order to explain the technical content, structural features and achieved effects of the present invention in detail, the following is a detailed description in conjunction with the implementation methods and the accompanying drawings.
[0028] like Figures 1 to 10 As shown, an embodiment of the present invention provides a method for preparing a color conversion crystal grain, and the preparation method comprises the following steps:
[0029] S1. Provide a substrate 1, on which color conversion blocks 2 arranged in an array are provided; the substrate 1 is a wafer structure, which can be a wafer of a size of 2 inches, 4 inches, 6 inches, etc., and the color conversion blocks 2 of the array structure are arranged on the upper part of the wafer. The thickness of the substrate is 600-850nm, and the thickness of the color conversion blocks is 10-15nm. Figure 3 to Figure 4 shown.
[0030] S2, filling the bonding connector 4 between the adjacent color conversion blocks 2, wherein the height of the bonding connector 4 is greater than the height of the color conversion block 2 to form a cavity 101 arranged around the color conversion block 2; specifically, refer to Figure 6 As shown, a layer of bonding connector 4 can be covered by deposition, screen printing, IJP (inkjet printing) dot printing, etc. The width of the bonding connector 4 is the etching width, and the height is 5 to 10 um higher than the color conversion block 2.
[0031] S3, corresponding to the color conversion block 2, a light-emitting crystal particle 6 is provided, wherein the light-emitting crystal particle 6 has a relative bonding surface 61 and a non-bonding surface 62, and the area of the bonding surface 61 is larger than the area of the opening of the cavity 101, which can be referred to Figure 7 As shown, each color conversion block 2 is covered with the light-emitting crystal grain 6 , and the distance between adjacent light-emitting crystal grains 6 is smaller than the distance between adjacent color conversion blocks 2 .
[0032] S4, under vacuum conditions, the light-emitting crystal grain 6 is permanently bonded to the bonding connector 4 to cover the cavity 101, and the light-emitting crystal grain 6 and the bonding connector 4 completely cover the color conversion block 2 to form a color conversion crystal grain, refer to Figure 10 to Figure 11 Shown
[0033] In the embodiment of the present invention, a bonding connector 4 having a height greater than that of the color conversion block 2 is filled between the color conversion blocks 2, and the light-emitting crystal grain 6 is permanently bonded to the bonding connector 4 under vacuum conditions to form a color conversion crystal grain structure covering the color conversion block 2. This preparation method can isolate the air, effectively protect the quantum dot structure, remove bubbles, enhance the bonding adhesion, and have a good bonding effect.
[0034] In the embodiment of the present invention, step S1 includes:
[0035] S11, providing a substrate 1, and corroding the surface of the substrate 1 to form a plurality of pores 11; specifically, Figure 1As shown, the substrate 1 is a sapphire substrate, and pores 11 are formed on the surface of the substrate 1 by electrochemical corrosion to form an ECE substrate (electrochemically etched substrate), and the ECE substrate is pre-treated by injection, and baked in a vacuum oven at 80-100° C. for 13-17 minutes to dry the water vapor in the ECE substrate; and then it is cleaned by plasma, wherein the ratio of argon to oxygen in the plasma is: Ar:O 2 =50:10~10:10, wash for 10~15 minutes to clean the dirt on the surface of the ECE substrate and the pores 11, so that the quantum dot ink 21 can penetrate better.
[0036] S12, injecting quantum dot ink 21 into the pores 11 to form a quantum dot layer 22. The quantum dot ink 21 may be injected by centrifugal injection, spin coating injection, vacuum injection, etc. The structure after the quantum dot ink 21 is injected is as follows: Figure 2 After the injection is completed, the ECE substrate will change from white to a substrate 1 with uniform color (ink color), which is placed in a vacuum oven and baked at 80-100° C. for 10-15 minutes to solidify the quantum dot ink 21 .
[0037] S13, etching the quantum dot layer 22 to form an array-arranged color conversion block 2. Specifically, the quantum dot layer 22 is etched by ICP (inductively coupled plasma) etching, and the etching width is about 30 to 35 um. The side view and top view of the structure after etching are as follows: Figure 3 and Figure 4 shown.
[0038] It should be noted that the substrate 1 is a sapphire substrate, which has a better light transmittance. Of course, a substrate 1 made of other materials can also be selected as long as a certain light transmittance can be guaranteed. In addition, the method of forming the array-arranged color conversion blocks 2 is not limited, as long as the above-mentioned color conversion block 2 array can be formed on the substrate 1.
[0039] In the embodiment of the present invention, before the step S2 of filling the bonding connector 4 between the adjacent color conversion blocks 2, wherein the height of the bonding connector 4 is greater than the height of the color conversion block 2 to form a cavity 101 arranged around the color conversion block 2, the step further includes:
[0040] S14, depositing a protective layer on the substrate 1, the protective layer covering the color conversion block 2. The color conversion block 2 after etching can be deposited with a protective layer using an ALD device (atomic layer deposition device), such as an aluminum oxide layer, with a thickness of 100 to 300 nm, to protect the quantum dots in the wafer after etching. For details, please refer to Figure 5 As shown, the quantum dot structure can be protected from damage in subsequent processes.
[0041] In the embodiment of the present invention, in step S3, a light-emitting crystal grain 6 is provided corresponding to the color conversion block 2, wherein the light-emitting crystal grain 6 has a relative bonding surface 61 and a non-bonding surface 62, and the area of the bonding surface 61 is larger than the area of the opening of the cavity 101. The steps include:
[0042] S31, providing a substrate 5 with the luminescent crystal grain 6, wherein the luminescent crystal grain 6 is arranged corresponding to the quantum dot 2, and the luminescent crystal grain 6 has a relative bonding surface 61 and a non-bonding surface 62, wherein the area of the bonding surface 61 is larger than the area of the opening of the cavity 101, and the bonding surface 61 is connected to the substrate 5; specifically, reference may be made to Figure 7 As shown, the substrate 5 is a sapphire substrate.
[0043] S32, mounting the non-bonding surface 62 of the light-emitting crystal grain 6 on the temporary support plate 8 through the temporary bonding film 7; specifically, as Figure 8 As shown, in order to prevent the light-emitting chip from scattering after laser lift-off (LLO), a temporary bonding film 7 and a temporary support plate 8 are used for bonding before LLO. The thickness of the temporary bonding film 7 is 50 to 60 um, and the thickness of the temporary support plate 8 is 650 to 800 um.
[0044] S33, peeling off the substrate 5 to form a temporary bonding structure of the light-emitting crystal grains 6. Specifically, using a 240-360 nm laser to irradiate the interface between the GaN layer and the sapphire substrate, the light-emitting crystal grains 6 are peeled off from the substrate 5. The spacing between the light-emitting crystal grains 6 is 20-25 um, and the spacing between the light-emitting crystal grains 6 is smaller than the spacing between the color conversion blocks. Fig. 9 Shown
[0045] In the embodiment of the present invention, in step S4, the light-emitting crystal grain 6 is bonded to the bonding connector 4 in a vacuum environment, and the step of the light-emitting crystal grain 6 covering the color conversion block 2 includes:
[0046] S41, using a vacuum bonding machine to bond the light-emitting crystal grain 6 to the bonding connector 4 to cover the color conversion block 2, specifically, as follows: Fig.10 As shown, the bonding surface 61 of the light-emitting crystal particle 6 and the bonding connector 4 are connected and placed in a vacuum bonding machine, and then the vacuum bonding machine is evacuated to 0-50 torr, and then a pressure of 50-100 kgf is applied and the pressure is maintained for 20-30 minutes. During the pressure maintenance process, the temperature of the bonding machine is maintained at 70-80°C to perform bonding at low temperature, thereby avoiding damage to the quantum dots and effectively protecting the quantum dots.
[0047] In the embodiment of the present invention, after step S4, the following steps are further performed: S5, peeling off the temporary bonding film 7 to separate the light-emitting crystal grain 6 from the temporary bonding film 7 and the temporary supporting plate 8. For details, please refer to Figure 10 to Figure 11As shown, laser is used to irradiate the junction of the temporary bonding film 7 and the temporary support plate 8 to separate the light-emitting crystal grain 6 from the temporary bonding film 7 and the temporary support plate 8. Specifically, a conventional temporary bonding process can be used, which will not be described in detail here.
[0048] In the embodiment of the present invention, after the step S5 of peeling off the temporary bonding film 7 to separate the light-emitting crystal grain 6 from the temporary bonding film 7 and the temporary supporting plate 8, the following steps are further included:
[0049] S61, thinning the substrate 1, the thickness of the substrate 5 after thinning is 80-100 um, reference Fig.12 As shown;
[0050] S62, cutting the substrate 1 from the gaps between adjacent light-emitting crystal grains 6 to form a single color conversion crystal grain that integrates the light-emitting crystal grain 6, the bonding connector 4 and the color conversion block 2. Specifically, Fig.12 As shown, cutting is performed along cutting line a, and a single color conversion grain is formed after cutting.
[0051] In the embodiment of the present invention, the bonding connector 4 is a metal or alloy with a melting point of 60-80°C, such as bismuth, lead, gallium, tin, cadmium, indium metal or its alloy, and the temperature when the light-emitting crystal grain 6 is bonded to the bonding connector 4 corresponds to the melting point setting. Because the bonding connector 4 is a metal structure and is not light-transmissive, when the color conversion crystal grains are used in a display screen, the problem of light crosstalk between each other can be avoided. In addition, the bonding temperature is lower than 80°C, which can effectively protect the quantum dots and avoid damage to the quantum dots by high temperature.
[0052] It should be noted that, in some other embodiments, the bonding connector 4 may also be made of other materials, as long as it can ensure that the bonding connector 4 can be effectively bonded to the light-emitting crystal grain 6 .
[0053] In the embodiment of the present invention, the ECE substrate injected with quantum dot ink 21 is etched before low-temperature bonding. The etching width will be wider than the width between the light-emitting crystal grains 6. The light-emitting crystal grains 6 can be, for example, blue light chips. Then, the bonding connectors are filled in the cutting paths etched on the ECE substrate. The bonding connectors can be, for example, low-temperature metals or alloys. Finally, the low-temperature metals will play three roles: low-temperature bonding, quantum dot protection, and blocking optical crosstalk. This ensures that the color conversion crystal grains after cutting can both strengthen the isolation protection of quantum dots and prevent optical crosstalk. Secondly, in the whole process, the problem of quantum dots not being resistant to high temperatures and the problem of weak bonding adhesion will be faced. In the embodiment of the present invention, a vacuum bonding machine will be used for degassing, and then a low-temperature metal will be used for low-temperature pressurized permanent bonding. This can avoid the damage of high temperature to quantum dots during permanent bonding, and can also improve the bonding strength of quantum dots.
[0054] The above disclosure is only a preferred embodiment of the present invention, and certainly cannot be used to limit the scope of rights of the present invention. Therefore, equivalent changes made according to the scope of the patent application of the present invention still fall within the scope covered by the present invention.
Claims
1. A method for preparing a color conversion crystal grain, characterized in that: The preparation method comprises the following steps: Providing a substrate, on which color conversion blocks arranged in an array are provided; Filling bonding connectors between adjacent color conversion blocks, wherein the height of the bonding connectors is greater than the height of the color conversion blocks to form a cavity arranged around the color conversion blocks; Providing a light-emitting crystal grain corresponding to the color conversion block, wherein the light-emitting crystal grain has a bonding surface and a non-bonding surface opposite to each other, and the area of the bonding surface is larger than the area of the cavity opening; The light-emitting crystal grain and the bonding connector are permanently bonded to cover the cavity in a vacuum environment. The light-emitting crystal grain and the bonding connector completely cover the color conversion block to form a color conversion crystal grain.
2. The method for preparing the color conversion crystal grain according to claim 1, characterized in that: Providing a substrate, on which color conversion blocks arranged in an array include: Providing a substrate, and etching the surface of the substrate to form a plurality of pores; injecting quantum dot ink into the pores to form a quantum dot layer; The quantum dot layer is etched to form color conversion blocks arranged in an array.
3. The method for preparing the color conversion crystal grain according to claim 1, characterized in that: Before the step of filling bonding connectors between adjacent color conversion blocks, wherein the height of the bonding connectors is greater than the height of the color conversion blocks to form a cavity arranged around the color conversion blocks, the method further includes: A protection layer is deposited on the substrate, wherein the protection layer covers the color conversion block.
4. The method for preparing the color conversion grain according to claim 1, characterized in that: Providing a light-emitting crystal grain corresponding to the color conversion block, wherein the light-emitting crystal grain has a relative bonding surface and a non-bonding surface, and the area of the bonding surface is larger than the area of the cavity opening, the steps include: Providing a substrate with the light-emitting crystal grain, wherein the light-emitting crystal grain is arranged corresponding to the color conversion block, the light-emitting crystal grain has a bonding surface and a non-bonding surface relative to each other, the area of the bonding surface is larger than the area of the cavity opening, and the bonding surface is connected to the substrate; Mounting the non-bonding surface of the light-emitting crystal grain on a temporary support plate through a temporary bonding film; The substrate is peeled off to form a temporary bonding structure of the light-emitting crystal grain.
5. The method for preparing the color conversion crystal grain according to claim 4, characterized in that: The steps of permanently bonding the light-emitting crystal grain and the bonding connector under a vacuum environment to cover the cavity, wherein the light-emitting crystal grain and the bonding connector completely cover the color conversion block to form a color conversion crystal grain include: The light-emitting crystal grain is bonded to the bonding connector by using a vacuum bonding machine to cover the color conversion block.
6. The method for preparing the color conversion crystal grain according to claim 5, characterized in that: The method further comprises: permanently bonding the light-emitting crystal grain to the bonding connector under a vacuum environment to cover the cavity, wherein the light-emitting crystal grain and the bonding connector completely cover the color conversion block to form a color conversion crystal grain; The temporary bonding film is peeled off to separate the light-emitting crystal grain from the temporary bonding film and the temporary supporting plate.
7. The method for preparing the color conversion crystal grain according to claim 6, characterized in that: After the step of peeling off the temporary bonding film to separate the light-emitting crystal grain from the temporary bonding film and the temporary supporting plate, the method further includes: Thinning the substrate; Cutting is performed from the gaps between adjacent light-emitting crystal grains toward the substrate to form a single color conversion crystal grain integrating the light-emitting crystal grains, bonding connectors and color conversion blocks.
8. The method for preparing the color conversion crystal grain according to claim 1, characterized in that: The bonding connector is a metal or alloy with a melting point of 60-80° C., and the temperature when the light-emitting crystal grain is bonded to the bonding connector is set corresponding to the melting point.
9. The method for preparing a color conversion crystal grain according to claim 1, characterized in that: The distance between the color conversion blocks is 30 to 35 micrometers, and the distance between the light-emitting crystal grains is 20 to 25 micrometers.
10. The method for preparing the color conversion crystal grain according to claim 1, characterized in that: The substrate is a sapphire substrate.
Citation Information
Patent Citations
Display panel, display device and preparation method of display panel
CN112133811A
Manufacturing method of RGB-LED device emitting three-primary-color polarized light
CN113540324A