Positive electrode material and preparation method thereof and lithium ion battery
Through the porous material cladding layer modified by hydrophobic groups, the problem of residual alkali on the surface of the ternary positive electrode material is solved, efficient electrochemical performance improvement and cost reduction are achieved, and the shortcomings of water washing and surface coating methods in the prior art are solved.
Patent Information
- Application Number
- CN202210764411.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-06-29
AI Technical Summary
During the long cycle of the ternary positive electrode material, the gas bloating phenomenon caused by the residual alkali problem on the surface, and the existing water washing and surface coating methods cannot be effectively solved, and it will affect the material capacity and production cost.
The porous material modified with hydrophobic groups is used as the cladding layer, and the ternary positive electrode material is coated by initiating chemical vapor deposition to form a dense and uniform cladding layer, reducing the surface residual alkali content and improving the electrochemical performance of the material.
It realizes that the surface residual alkali is stable for a long time without affecting the capacity of the positive electrode material, improves the coating effect and battery circulation performance, simplifies the process flow and reduces production costs.
Smart Images

Figure CN114975968B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery materials, and in particular to a positive electrode material and a preparation method thereof, and a lithium-ion battery. Background Art
[0002] Lithium-ion batteries are a type of commercial battery that appeared in the 1990s. They have the advantages of high specific energy, high operating voltage, long cycle life, no memory effect, light weight, and small size. They are widely used in laptops, mobile phones, cameras, and other portable electronic devices, as well as electric vehicles, and have attracted much attention in energy and material research. As batteries develop towards sustainability, environmental friendliness, and high energy density, higher requirements are also placed on the cathode materials in lithium-ion batteries. Among them, the conductivity of Co and the high capacity of Ni in the ternary cathode material system, combined with the advantages of other transition metals, make it a research hotspot.
[0003] In the research of ternary positive electrode materials, it was found that the problem of residual alkali on the surface of the materials was serious and there were many defects, which led to obvious gas expansion of the battery during long cycles, inevitably affecting the stable output of energy. At present, the commonly used solution is to improve the surface structure of the material through water washing and surface coating, slow down the direct contact between the residual alkali in the material and the air, and reduce the stress rate. However, the product after water washing will reduce the capacity of the ternary material in the long-term battery cycle, affecting its capacity advantage, and cannot fundamentally solve the problem; and traditional surface coating cannot form a uniform and stable coating layer on the surface of the material, and the coating effect is not obvious. Sintering after coating increases the production cost, and a certain inert layer will be produced to affect the surface properties of the material, thereby affecting the processing performance of the material and the electrochemical performance of the battery.
[0004] Therefore, it is necessary to find a non-water washing post-treatment process to solve the problem of residual alkali on the surface of the material. At the same time, this method is also required to stably and long-term protect the surface of the positive electrode material from corrosion. Summary of the invention
[0005] In view of this, the present application provides a positive electrode material using a porous material modified with a hydrophobic group as a coating layer, which neither affects the capacity of the positive electrode material nor reduces the residual alkali content on the surface of the positive electrode material.
[0006] To achieve the above objectives, the technical solution of this application is as follows:
[0007] A positive electrode material comprises a lithium-nickel transition metal composite oxide and a coating layer at least partially located on the surface of the lithium-nickel transition metal oxide, wherein the coating layer comprises a porous material modified with a hydrophobic group.
[0008] In some embodiments, the hydrophobic group is bonded to the porous material via a covalent bond or a non-covalent bond.
[0009] In some embodiments, the hydrophobic group includes at least one of a hydrocarbon group, a hydroxyl group, an ester group, an ether group, an amine group, and an amide group.
[0010] In some embodiments, the hydrocarbon group includes at least one of an alkyl group, an alkenyl group, an aryl group, and an alkynyl group.
[0011] In some embodiments, the contact angle between the hydrophobic group-modified porous material and water is greater than or equal to 150°.
[0012] In some embodiments, the porous material comprises an organic porous material.
[0013] In some embodiments, the porous material comprises an organic porous material, and the organic porous material comprises at least one of a metal organic framework material, a zeolite imidazolate framework material, a covalent organic framework material, an intrinsic microporous polymer, and a polyvinyl pyridine porous material.
[0014] In some embodiments, the porous material includes at least one of COF-1, COF-102, ZIF-67, ZIF-8, and PIM-1.
[0015] In some embodiments, the porous material modified with hydrophobic groups has pores, and the diameter of the pores is 0.8 nm to 5 nm.
[0016] In some embodiments, the depth of the pores of the hydrophobic group-modified porous material is 1 nm to 50 nm.
[0017] In some embodiments, the thickness of the hydrophobic group-modified porous material is 0.5 nm to 5 nm.
[0018] In some embodiments, the general chemical formula of the lithium-nickel transition metal composite oxide is LiaNixCoyMzO2, wherein 0.95≤a≤1.05, 0.80≤x<1, 0<y+z≤0.20, and M includes any one of Mn, Al, Cu, Zn, and Cr.
[0019] In some embodiments, the average particle size of the lithium-nickel transition metal composite oxide is 7 μm to 20 μm.
[0020] In some embodiments, the coating layer has a thickness of 0.5 nm to 5 nm.
[0021] In some embodiments, the positive electrode material has a lithium hydroxide content of 0.012 wt% to 0.10 wt%, and a lithium carbonate content of 0.012 wt% to 0.10 wt%.
[0022] In some embodiments, 1 g of the positive electrode material is selected, heated to 300° C., and after 10 minutes, the moisture content is tested by a Karl Fischer titrator to be less than or equal to 300 ppm.
[0023] A method for preparing a positive electrode material, comprising:
[0024] Performing a first induced chemical vapor deposition process on a mixture containing a lithium-nickel transition metal composite oxide and a porous material to obtain a lithium-nickel transition metal composite oxide coated with a porous material;
[0025] A hydrophobic material and a lithium-nickel transition metal composite oxide coated with a porous material are subjected to a second induced chemical vapor deposition treatment to obtain a positive electrode material, wherein the positive electrode material includes a lithium-nickel transition metal composite oxide and a coating layer at least partially located on the surface of the lithium-nickel transition metal oxide, and the coating layer includes a porous material modified with a hydrophobic group.
[0026] In some embodiments, the chemical formula of the lithium-nickel transition metal composite oxide is Li a Ni x Co y M z O2, wherein 0.95≤a≤1.05, 0.80≤x<1, 0<y+z≤0.20, and M includes at least one of Mn, Al, Cu, Zn and Cr.
[0027] In some embodiments, the average particle size of the lithium-nickel transition metal composite oxide is 7 μm to 20 μm.
[0028] In some embodiments, the mass ratio of the porous material to the lithium-nickel transition metal composite oxide is (0.08-0.15):100.
[0029] In some embodiments, the mass ratio of the hydrophobic material to the lithium-nickel transition metal composite oxide is (0.01-0.05):100.
[0030] In some embodiments, the porous material comprises an organic porous material.
[0031] In some embodiments, the porous material comprises an organic porous material, and the organic porous material comprises at least one of a metal organic framework material, a zeolite imidazolate framework material, a covalent organic framework material, an intrinsic microporous polymer, and a polyvinyl pyridine porous material.
[0032] In some embodiments, the porous material includes at least one of COF-1, COF-102, ZIF-67, ZIF-8, and PIM-1.
[0033] In some embodiments, the hydrophobic material includes an organic hydrophobic group, and the organic hydrophobic group includes at least one of a hydrocarbon group, an ester group, an ether group, an amine group, and an amide group.
[0034] In some embodiments, the hydrocarbon group includes at least one of an alkyl group, an alkenyl group, an aryl group, and an alkynyl group.
[0035] In some embodiments, the hydrophobic material includes at least one of methane, ethylene, propyne, toluene, phenol, ethyl acetate, phenyl acetate, ethylene diethyl ester, methyl ether, ethyl ether, n-butyl ether, di-sec-butylamine, tert-butylamine, tert-octylamine, acetamide, cyclopropaneamide and acrylamide.
[0036] In some embodiments, the first induced chemical vapor deposition treatment of the mixture containing lithium nickel transition metal composite oxide and porous material also includes a preheating treatment; the preheating treatment includes evacuating the system of the induced chemical vapor deposition treatment and then heating it, and the temperature after heating is maintained at 60°C to 150°C for 3h to 5h.
[0037] In some embodiments, the first induced chemical vapor deposition process and the second induced chemical vapor deposition process are both performed in an oxygen-containing atmosphere.
[0038] In some embodiments, the pressure of the first induced chemical vapor deposition process and the second induced chemical vapor deposition process is 20Pa-100Pa.
[0039] In some embodiments, the temperature of the first induced chemical vapor deposition process is 60° C. to 150° C., and the time is 1 hour to 3 hours.
[0040] In some embodiments, the second induced chemical vapor deposition treatment comprises first reacting under the conditions of the first induced chemical vapor deposition treatment for 0.5 h to 1.5 h; then raising the temperature by 20° C. to 30° C. and keeping the temperature for 2 h to 5 h.
[0041] In some embodiments, the method for preparing the lithium-nickel transition metal composite oxide comprises: mixing a ternary precursor with a lithium source, and sintering to obtain the lithium-nickel transition metal composite oxide.
[0042] In some embodiments, the lithium nickel precursor comprises an oxide or hydroxide of NixCoyMz, wherein M comprises at least one of Mn, Al, Cu, Zn, and Cr, 0.8≤x<1,0 <y+z≤0.2,x+y+z=1。
[0043] In some embodiments, the lithium source includes lithium hydroxide or lithium carbonate.
[0044] In some embodiments, the molar ratio of the lithium element in the lithium source to the total metal elements in the lithium-containing nickel precursor is 1:(0.95-1.3).
[0045] In some embodiments, before sintering, the process further includes: grinding and crushing the material obtained by mixing the lithium-nickel precursor and the lithium source.
[0046] In some embodiments, after the sintering, the method further comprises: crushing the lithium-nickel transition metal composite oxide to a particle size of 7 μm to 20 μm.
[0047] In some embodiments, the sintering includes primary sintering and secondary sintering.
[0048] In some embodiments, the sintering atmosphere of the primary sintering is air, the temperature of the primary sintering is 400° C. to 500° C., and the time is 4 h to 6 h.
[0049] In some embodiments, the sintering atmosphere of the secondary sintering is oxygen, the temperature of the secondary sintering is 500° C. to 800° C., and the time is 10 h to 15 h.
[0050] In addition, the present application also provides a lithium-ion battery, comprising the above-mentioned positive electrode material.
[0051] Beneficial effects of this application:
[0052] This application uses porous materials to coat ternary positive electrode materials, making full use of the properties of porous materials to resist harmful substances. On the basis of not affecting the capacity of the positive electrode material, it reduces the residual alkali on the surface of the material, so that the coating film can optimize the ternary positive electrode material in a long term and effectively. In particular, this application uses hydrophobic groups to modify the porous materials of the coating film. These groups use porous materials as carriers to broaden the internal pore structure of the porous materials. At the same time, they can also adsorb harmful gases such as CO2, thereby enhancing the positive electrode material's resistance to the electrolyte, resisting the generation of residual alkali on the surface of the material, and not destroying the material structure, thereby maximizing the coating effect on the surface of the positive electrode material.
[0053] The preparation method of the present application is different from the traditional water washing and coating treatment method. It adopts a non-water washing process with a simple process. It reduces the residual alkali on the surface of the material without affecting the material capacity to form a dense and uniform coating layer.
[0054] This application adopts the induced chemical vapor deposition coating method. Compared with the traditional coating method, it can be evenly dispersed on the surface of the high-nickel ternary positive electrode material, with uniform thickness and excellent coating effect, which improves the processing performance of the material and the electrochemical performance of the battery. The use of porous organic polymers and hydrophobic materials combined with the induced chemical vapor deposition method can make the coating material more quickly, evenly and gently coated on the surface of the material, and can make the modified material more evenly modify the coating material, reduce the contact area with the ternary material, and avoid the influence of multi-phase coating on the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope of the present invention.
[0056] Figure 1 The cycle capacity retention rate curve of the battery prepared by the positive electrode materials in Examples 1 to 6 and Comparative Examples 1 to 4;
[0057] Figure 2 EIS impedance graphs of batteries prepared with the positive electrode materials in Examples 1 to 6 and Comparative Examples 1 to 4;
[0058] Figure 3 This is a scanning electron microscope image of the surface of the positive electrode material prepared in Example 1;
[0059] Figure 4 These are transmission electron micrographs of the materials prepared in different steps of Example 1. DETAILED DESCRIPTION
[0060] As used herein:
[0061] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0062] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0063] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0064] In these examples, parts and percentages are by mass unless otherwise indicated.
[0065] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0066] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0067] A positive electrode material in one embodiment includes a lithium-nickel transition metal composite oxide and a coating layer at least partially located on the surface of the lithium-nickel transition metal oxide, wherein the coating layer includes a porous material modified with a hydrophobic group.
[0068] This embodiment uses porous materials to coat the ternary positive electrode materials, making full use of the properties of porous materials to resist harmful substances. On the basis of not affecting the capacity of the positive electrode materials, it reduces the residual alkali on the surface of the materials, so that the coating film can optimize the ternary positive electrode materials in a long term and effectively. In particular, this application uses hydrophobic groups to modify the porous materials of the coating film. These groups use porous materials as carriers to broaden the internal pore structure of the porous materials. At the same time, they can also adsorb harmful gases such as CO2, resist the generation of residual alkali on the surface of the materials, do not destroy the material structure, and maximize the coating effect on the surface of the positive electrode materials.
[0069] In some embodiments, the lithium-nickel transition metal composite oxide has the general chemical formula Li a Ni x Co y M z O2, wherein 0.95≤a≤1.05, 0.80≤x<1, 0<y+z≤0.20, and M includes at least one of Mn, Al, Cu, Zn, and Cr.
[0070] In some embodiments, the particle size of the lithium nickel transition metal composite oxide is 7 μm to 20 μm, for example, 7 μm, 7.5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 17 μm, 20 μm or any value between 7 μm and 20 μm.
[0071] In the present embodiment, the term "hydrophobic" is defined as "the hydrophobic property of the surface of a material". As used herein, the term "hydrophobic materials" are distinguished from each other based on the wettability of the surface of the material by water. The wettability of the surface of the material by water can be quantitatively analyzed using the contact angle with water.
[0072] In some embodiments, the hydrophobic group is bonded to the porous material via covalent bonds or non-covalent bonds.
[0073] It should be noted that non-covalent bonds refer to a weak bond formed between the surface of the porous material and the hydrophobic group. Non-covalent bonds may be, for example, hydrogen bonds, van der Waals bonds, charge transfer, dipole-dipole interactions, π-π stacking interactions, etc. Non-covalent bonds may be formed by bonding the hydrophobic group to the porous material without causing defects on the surface of the porous material.
[0074] The covalent bond is a bond formed by a reaction between a reactive functional group directly attached to the surface of the porous material and a functional group of the hydrophobic group. For example, the reactive functional group directly attached to the surface of the porous material may be (a carbon-carbon double bond, a carbon-carbon triple bond, a hydroxyl group, a carboxyl group, an ether bond, an aldehyde group, a carbonyl group, etc.). For example, the covalent bond may be formed by (oxidation, halogenation, cycloaddition, free radical addition) and the like.
[0075] In some embodiments, the hydrophobic group includes at least one of a hydrocarbon group, a hydroxyl group, an ester group, an ether group, an amine group, and an amide group; for example, it can be formed by a combination of a hydrocarbon group and a hydroxyl group, or a hydrocarbon group and an ester group. These hydrophobic groups use porous materials as carriers to modify and widen the pore structure inside the porous materials. They can not only encapsulate and adsorb harmful gases such as CO2, but also use the characteristics of their own groups to exert their hydrophobic properties, resist the formation of residual alkali on the surface of the positive electrode material, and do not destroy the structure of the positive electrode material, thereby improving the resistance to the electrolyte and greatly improving the coating effect on the surface of the positive electrode material.
[0076] Furthermore, the hydrocarbon group includes at least one of an alkyl group, an alkenyl group, an aryl group, and an alkynyl group;
[0077] In some embodiments, the porous material comprises an organic porous material.
[0078] In some embodiments, the organic porous material includes at least one of metal organic frameworks (MOFs), zeolitic imidazolate frameworks (ZIFs), covalent organic frameworks (COFs), intrinsic microporous polymers (PIMs), and polyvinylpyridine porous materials.
[0079] It should be noted that COFs and PIMs belong to porous organic polymers (POPs), which are a type of porous network materials composed of organic building units connected by covalent bonds. They have the advantages of high surface area, high porosity, light weight, high stability and easy modification. They are generally composed of light elements connected by strong covalent bonds, which makes them have low density and high chemical stability. MOFs and ZIFs are porous structures formed by metals and organic matter. MOFs have a three-dimensional pore structure, generally with metal ions as the connection points, and organic ligands support the 3D extension of space. ZIFs are organic imidazole esters cross-linked to transition metals to form a tetrahedral framework structure.
[0080] Further, the porous material includes at least one of COF-1, COF-102, ZIF-67, ZIF-8 and PIM-1;
[0081] In some embodiments, the contact angle between the porous material modified with the hydrophobic group and water is greater than or equal to 150°.
[0082] In some embodiments, the porous material modified with the hydrophobic group has pores, and the diameter of the pores measured by SEM is 0.8 nm to 5 nm. Specifically, the diameter of the pores can be 0.8 nm, 1 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm or 5 nm.
[0083] In some embodiments, the depth of the pores of the porous material modified with hydrophobic groups is 1 nm to 50 nm as measured by SEM. Specifically, the depth of the pores may be 1 nm, 10 nm, 15 nm, 20 nm, 26 nm, 30 nm, 35 nm, 42 nm or 50 nm, etc. It should be noted that the pore depth refers to the pore length.
[0084] In some embodiments, the thickness of the porous material modified with hydrophobic groups is 0.5 nm to 5 nm as measured by SEM, and specifically, can be 0.5 nm, 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 4 nm, 5 nm, or any value between 0.5 nm and 5 nm.
[0085] In some embodiments, the thickness of the coating layer is 0.5 nm to 5 nm, for example, 0.5 nm, 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 4 nm, 5 nm or any value between 0.5 nm and 5 nm.
[0086] In some embodiments, the lithium hydroxide content of the positive electrode material is 0.012 wt% to 0.10 wt%, and the lithium carbonate content is 0.012 wt% to 0.10 wt%. The residual alkali mainly exists in the form of lithium hydroxide and lithium carbonate, and this embodiment can effectively reduce the residual alkali content.
[0087] In some embodiments, 1g of the positive electrode material is selected, heated to 300°C, and after 10 minutes, the moisture content is less than or equal to 300ppm using a Karl Fischer titrator. It should be noted that ppm refers to mass concentration. The moisture content of this embodiment is within this range, which can be more conducive to reducing residual alkali and improving the stability of the coating layer.
[0088] The ternary positive electrode material of the present application is a high-nickel ternary positive electrode material, which has a higher specific capacity than ordinary ternary positive electrode materials. Therefore, it is currently a hot research topic in lithium battery positive electrode materials and is also the choice with the most application prospects. However, the high-nickel ternary positive electrode material prepared by traditional technology has a lot of residual lithium and residual alkali on the surface, which makes the battery cycle performance poor. Therefore, in the technical solution of the present application, the high-nickel ternary positive electrode material is modified by surface coating to improve the performance of the high-nickel ternary positive electrode material, thereby improving the cycle performance of the lithium battery.
[0089] These porous materials of the present application have relatively good chemical stability. By utilizing their stability, they are coated on the surface of the ternary positive electrode material to effectively resist harmful substances. On the basis of not affecting the capacity of the positive electrode material, they can also adsorb the gas near the positive electrode material, thereby reducing the generation of residual alkali on the surface, so that the coating film can effectively optimize the ternary positive electrode material in the long term.
[0090] A preparation method of a cathode material according to another embodiment includes the following steps:
[0091] S100: Mix a lithium-containing nickel precursor with a lithium source and sinter to obtain a lithium-containing nickel transition metal composite oxide;
[0092] S200: Perform a first initiated chemical vapor deposition treatment on a mixture containing the lithium-containing nickel transition metal composite oxide and a porous material to obtain a lithium-containing nickel transition metal composite oxide coated with the porous material;
[0093] S300: Perform a second initiated chemical vapor deposition treatment on a hydrophobic material and the lithium-containing nickel transition metal composite oxide coated with the porous material to obtain the cathode material.
[0094] The following details this solution in combination with specific embodiments:
[0095] S100: Mix a lithium-containing nickel precursor with a lithium source and sinter to obtain a lithium-containing nickel transition metal composite oxide;
[0096] In some embodiments, the lithium-containing nickel precursor is a ternary precursor.
[0097] More specifically, the lithium-containing nickel precursor includes oxides or hydroxides of Ni x Co y M z where M includes at least one of Mn, Al, Cu, Zn, and Cr, 0.8 ≤ x < 1, 0 < y + z ≤ 0.2, and x + y + z = 1. Moreover, the range of the x value is between 0.8 and 1.0, which indicates that the ternary cathode material finally prepared in this application is a high-nickel ternary cathode material.
[0098] In some embodiments, the lithium source includes lithium hydroxide or lithium carbonate.
[0099] In some embodiments, the molar ratio of the lithium element in the lithium source to the total metal elements in the lithium-containing nickel precursor is 1:(0.95 - 1.3), for example, it can be 1:0.95, 1:1, 1:1.02, 1:1.05, 1:1.1, 1:1.2, 1:1.3, or any value in 1:(0.95 - 1.3). Preferably, the molar ratio of the lithium element in the lithium source to the total metal elements in the lithium-containing nickel precursor is 1:1.05.
[0100] In some embodiments, before sintering in step S100, it further includes: grinding and pulverizing the mixed lithium-containing nickel precursor and lithium source, and sintering the pulverized mixture. The small particle size of the pulverized mixture can increase the contact area of the reactants, ensuring sufficient reaction during subsequent sintering.
[0101] In some embodiments, after sintering in step S100, the process further includes crushing the sintered lithium-nickel transition metal composite oxide to a particle size of 7 μm to 20 μm, for example, 7 μm, 7.5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 17 μm, 20 μm or any value between 7 μm and 20 μm. Crushing the sintered lithium-nickel transition metal composite oxide can ensure that each positive electrode material particle surface has a coating layer when subsequently coated with a porous material, thereby better protecting the ternary positive electrode material from being destroyed by the electrolyte when used in the battery.
[0102] In some embodiments, the sintering in step S100 includes primary sintering and secondary sintering.
[0103] In some embodiments, the sintering temperature of the first sintering is 400°C to 500°C, for example, 400°C, 420°C, 450°C, 470°C, 500°C or any value between 400°C and 500°C, and the sintering time is 4h to 6h, for example, 4h, 5h, 6h or any value between 4h and 6h. When performing the first sintering, it can be selected to be carried out in an air atmosphere, which is conducive to expanding the structure in the mixture during the first mixing. After the first sintering is completed, in order to ensure that the second sintering reaction is more sufficient, the product of the first sintering generally needs to be ground again.
[0104] In some embodiments, the sintering temperature of the secondary sintering is 500°C to 800°C, for example, it can be 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C or any value between 500°C and 800°C, and the sintering time is 10h to 15h, for example, it can be 10h, 11h, 12h, 13h, 14h, 15h or any value between 10h and 15h. When performing the second sintering, the ground product after the first sintering needs to be transferred to an oxygen atmosphere for sintering, so that oxygen is easily embedded in the expanded structure of the mixture after the first sintering, which fully ensures the progress of the reaction, and finally a high-nickel ternary positive electrode material can be obtained.
[0105] In some embodiments, the lithium-nickel transition metal composite oxide has the general chemical formula Li a Ni x Co y M z O2, wherein 0.95≤a≤1.05, 0.80≤x<1, 0<y+z≤0.20, and M includes at least one of Mn, Al, Cu, Zn and Cr.
[0106] It should be noted that step S100 may also be omitted, and existing ternary positive electrode materials or ternary positive electrode materials prepared by other methods may be used, and this embodiment has no particular limitation.
[0107] S200: performing a first induced chemical vapor deposition process on a mixture containing a lithium-nickel transition metal composite oxide and a porous material to obtain a lithium-nickel transition metal composite oxide coated with a porous material;
[0108] In some embodiments, the mass ratio of the porous material to the lithium-nickel transition metal composite oxide is (0.08-0.15):100; for example, it can be 0.08:100, 0.09:100, 0.1:100, 0.12:100, 0.15:100 or any value between (0.08-0.15):100. Preferably, the mass ratio of the porous material to the lithium-nickel transition metal composite oxide is 0.1:100.
[0109] In some embodiments, the porous material comprises an organic porous material.
[0110] In some embodiments, the organic porous material includes at least one of a metal organic framework material, a zeolite imidazolate framework material, a covalent organic framework material, an intrinsic microporous polymer, and a polyvinylpyridine porous material.
[0111] It should be noted that the porous material of this embodiment can be directly purchased from finished materials on the market to be coated with lithium-nickel transition metal composite oxides. At the same time, this application can also use relevant raw materials to prepare porous materials, and then coat them with lithium-nickel transition metal composite oxides. For example, COFs materials can be synthesized from boric acid, triazine, imine, phenylhydrazone, ketone / enamine, polyimide, phthalocyanine and porphyrin raw materials to synthesize different types of COFs materials; MOFs materials can be divided into transition metal complexes or rare earth metal complexes.
[0112] In addition, in this embodiment, a precursor substance for generating a porous material can be prepared first, and after the precursor substance is mixed with a lithium nickel transition metal composite oxide, the porous material is reacted to form a coating layer on the surface of the ternary positive electrode material. For example, when a metal organic framework material (MOFs) is used as a coating film material in this embodiment, a metal salt substance (such as zinc acetate, zirconium acetate) can be mixed with 2-methylimidazole to form a precursor solution; then the precursor solution is mixed and dried with a lithium nickel transition metal composite oxide, and the drying temperature is selected to be -30°C to -10°C. In this way, drying at a low temperature can not destroy the structural characteristics of the precursor material itself, and at the same time, the activity of the precursor can be maintained, which is conducive to the subsequent growth into a porous metal organic framework material; the mixture after low temperature drying needs to be protected under an inert gas, and then the mixture is heated. At a certain temperature, the precursor on the surface of the lithium nickel transition metal composite oxide gradually reacts to generate a metal organic framework material, and finally forms a dense coating layer on the surface of the lithium nickel transition metal composite oxide.
[0113] Furthermore, the porous material includes at least one of COF-1, COF-102, ZIF-67, ZIF-8 and PIM-1.
[0114] In some embodiments, the mass ratio of the hydrophobic material to the lithium-nickel transition metal composite oxide is (0.01-0.05):100. For example, it can be 0.01:100, 0.02:100, 0.03:100, 0.04:1, 0.05:1 or any value between (0.01-00.05):100. When the mass ratio is greater than 0.05:100, the modified substance will block the pores of the material and affect the normal reaction of the whole material; when the mass ratio is greater than 0.01:100, effective modification cannot be formed, and the effect will deteriorate after the coating material reacts for a long time.
[0115] In some embodiments, the hydrophobic material includes an organic hydrophobic group, and the organic hydrophobic group includes at least one of a hydrocarbon group, an ester group, an ether group, an amine group, and an amide group.
[0116] In some embodiments, the hydrocarbon group includes a C10-C20 hydrocarbon group.
[0117] In some embodiments, the hydrocarbon group includes at least one of an alkyl group, an alkenyl group, an aryl group, and an alkynyl group;
[0118] In a specific example, the hydrophobic material includes at least one of methane, ethylene, propyne, toluene, phenol, ethyl acetate, phenyl acetate, ethylene diethyl ester, methyl ether, ethyl ether, n-butyl ether, di-sec-butylamine, tert-butylamine, tert-octylamine, acetamide, cyclopropaneamide and acrylamide.
[0119] In some embodiments, the mixture containing the lithium nickel transition metal composite oxide and the porous material further includes a preheating treatment before the first induced chemical vapor deposition treatment is performed.
[0120] Specifically, the preheating treatment includes: evacuating the system and then heating it, and the temperature after heating is maintained at 60℃~150℃ for 3h~5h; evacuating the induced chemical vapor deposition system and then heating it, and the heating temperature is maintained at 60℃~150℃, for example, it can be 60℃, 80℃, 100℃, 120℃, 140℃, 150℃ or any value between 60℃ and 150℃, and the holding time is 3h~5h, for example, it can be 3h, 3.5h, 4h, 4.5h, 5h or any value between 3h and 5h.
[0121] In some embodiments, the first induced chemical vapor deposition process and the second induced chemical vapor deposition process are both performed in an oxygen-containing atmosphere, and the oxygen-containing atmosphere contains 99.99% oxygen.
[0122] In some embodiments, the pressure of the first induced chemical vapor deposition process and the second induced chemical vapor deposition process is 20Pa to 100Pa; oxygen is introduced into the system after the pretreatment, so that the pressure of the system is 20Pa to 100Pa, for example, it can be 20Pa, 30Pa, 40Pa, 50Pa, 60Pa, 70Pa, 80Pa, 90Pa, 100Pa or any value between 20Pa and 100Pa. If the pressure is too high, the reaction rate of the material will be reduced, and if the pressure is too low, the coating effect of the material will be poor.
[0123] In some embodiments, the temperature of the first induced chemical vapor deposition treatment is 60°C to 150°C, and the time is 1h to 3h; for example, it can be 60°C, 80°C, 100°C, 120°C, 140°C, 150°C or any value between 60°C and 150°C, and the reaction is carried out for 3h to 5h, for example, it can be 3h, 3.5h, 4h, 4.5h, 5h or any value between 3h and 5h, so that the porous material can be coated on the surface of the lithium nickel transition metal composite oxide to obtain a ternary positive electrode material coated with the porous material.
[0124] The second induced chemical vapor deposition treatment includes first reacting for 0.5h to 1.5h under the conditions of the first induced chemical vapor deposition treatment; then raising the temperature by 20°C to 30°C and keeping it warm for 2h to 5h. It can be understood that when depositing in step S200, it is necessary to maintain the temperature of the system unchanged after adding the hydrophobic material, and continue to introduce oxygen for 0.5h to 1.5h, for example, oxygen can be introduced for 0.5h, 1h, 1.5h or any value between 0.5h and 1.5h; then the temperature of the system is raised by 20°C to 30°C, for example, by 20°C, 25°C, 30°C or any value between 20°C and 30°C, and after keeping it warm for 2h to 5h at this temperature, for example, it can be 2h, 3h, 4h, 5h or any value between 2h and 5h, to obtain a ternary positive electrode material coated with a porous material modified by a hydrophobic material. It should be noted that the above-mentioned increase in the temperature of the system by 20°C to 30°C specifically means that if the original system temperature is maintained at 100°C, after oxygen is passed for 0.5h to 1.5h, the system temperature needs to be increased to 120°C to 130°C to ensure that the modifying groups are modified to the surface of the porous material.
[0125] By using the above-mentioned preparation method of positive electrode materials, positive electrode materials with hydroxyl and / or hydrocarbon group modified coating layers can be prepared. These positive electrode materials do not use traditional methods, but can still form a dense and uniform coating layer, effectively coating the ternary positive electrode materials of the substrate, resisting the formation of residual alkali on the surface of the positive electrode materials, and improving the coating effect.
[0126] A lithium ion battery according to another embodiment includes the above-mentioned positive electrode material.
[0127] The embodiments of the present invention will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0128] Example 1
[0129] The positive electrode material of this embodiment is a high-nickel ternary positive electrode material coated with ZIF-67 modified by hydrocarbon groups, and the specific preparation method thereof is:
[0130] (1) Ni 0.8 Co 0.1 Mn 0.1The molar ratio of (OH)2 to LiOH is 1.05:1. After mixing, wet grinding is performed. The ground mixture is calcined at 450°C for 5 hours in a box furnace. After grinding into fine particles, it is transferred to a tube furnace in an oxygen atmosphere and sintered at high temperature for 15 hours. The sintering temperature is controlled at 750°C. The sintered high-nickel ternary positive electrode material is crushed to a particle size of 15 μm.
[0131] (2) Weighing the LiNi in step (1) 0.8 Co 0.1 Mn 0.1 The mass of O2 was measured, and then 0.001 times the mass of ZIF-67 was weighed. The two substances were mixed and placed in an initiated chemical vapor deposition (iCVD) system. After heating to 100°C in a vacuum environment for 3 hours, oxygen was introduced to make the system pressure reach 50 Pa. The reaction was continued at 100°C for 1 hour to obtain a high-nickel ternary positive electrode material coated with ZIF-67.
[0132] (3) Add 0.0001 times the mass of the high-nickel ternary positive electrode material of benzyl to the system, maintain the system temperature at 100°C, continue to pass oxygen for 1 hour, then raise the temperature to 120°C and keep warm for 3 hours to obtain the high-nickel ternary positive electrode material coated with toluene-modified ZIF-67.
[0133] The positive electrode material prepared in this embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the benzyl-modified ZIF-67 coating layer are located therein, the coating layer thickness is 3nm, the positive electrode material has a pore structure, the diameter of the pore structure is 0.1nm~5nm, and the thickness is 0.5~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0134] Example 2
[0135] The positive electrode material of this embodiment is a high-nickel ternary positive electrode material coated with phenol-modified ZIF-67, and its specific preparation method is:
[0136] The same as Example 1, except that in step (3), 0.0001 times the mass of the high-nickel ternary positive electrode material of phenol is added to the system.
[0137] The positive electrode material prepared in this embodiment includes LiNi 0.8 Co 0.1 Mn 0.1O2 and at least part of the phenolic hydroxyl-modified ZIF-67 coating layer are located therein, the coating layer thickness is 3nm, and it has a pore structure with a diameter of 0.1nm to 5nm and a thickness of 0.5nm to 5nm; the depth of the pore structure is 1nm to 50nm, and the average particle size of the positive electrode material is 12μm.
[0138] Example 3
[0139] The positive electrode material of this embodiment is a high-nickel ternary positive electrode material coated with toluene-modified COF-1, and the specific preparation method thereof is:
[0140] The same as Example 1, except that in step (2), 0.001 times the amount of COF-1 porous material as the high-nickel ternary positive electrode material is added.
[0141] The positive electrode material prepared in this embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the benzyl-modified COF-1 coating layer are located therein, the coating layer thickness is 3nm, the positive electrode material has a pore structure, the diameter of the pore structure is 0.1nm~5nm, and the thickness is 0.5nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0142] Example 4
[0143] The positive electrode material of this embodiment is a high-nickel ternary positive electrode material coated with hydroxyl-modified COF-1, and its specific preparation method is:
[0144] The same as Example 2, except that in step (2), 0.001 times the amount of COF-1 porous material as the high-nickel ternary positive electrode material is added.
[0145] The positive electrode material prepared in this embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the phenolic hydroxyl modified COF-1 coating layer, the coating layer thickness is 3nm, including a pore structure, the diameter of the pore structure is 0.1nm ~ 5nm, the thickness is 0.5 ~ 5nm; the depth of the pore structure is 1nm ~ 50nm, and the average particle size of the positive electrode material is 12μm.
[0146] Example 5
[0147] The positive electrode material of this embodiment is a high-nickel ternary positive electrode material coated with polyvinyl pyridine modified by hydrocarbon groups, and the specific preparation method thereof is:
[0148] The same as Example 1, except that in step (2), 0.001 times the amount of polyvinyl pyridine porous material as the high nickel ternary positive electrode material is added.
[0149] The positive electrode material prepared in this embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the benzyl-modified polyvinylpyridine coating layer are located therein, the coating layer thickness is 3nm, the positive electrode material has a pore structure, the diameter of the pore structure is 0.1nm~5nm, and the thickness is 0.5nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0150] Example 6
[0151] The positive electrode material of this embodiment is a high-nickel ternary positive electrode material coated with polyvinyl pyridine modified with hydroxyl groups, and the specific preparation method thereof is:
[0152] The same as Example 2, except that in step (2), 0.001 times the amount of polyvinyl pyridine porous material as the high nickel ternary positive electrode material is added.
[0153] The positive electrode material prepared in this embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and a hydrocarbon-modified polyvinylpyridine coating layer at least partially located therein, the coating layer thickness is 3nm, the positive electrode material includes a pore structure, the diameter of the pore structure is 0.1nm to 5nm, and the thickness is 0.5nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0154] Example 7
[0155] The difference between this embodiment and embodiment 1 is that the mass ratio of the porous material to the lithium-nickel transition metal composite oxide is 0.08:100, and the mass ratio of toluene to the lithium-nickel transition metal composite oxide is 0.05:100.
[0156] The positive electrode material prepared in this embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the benzyl-modified ZIF-67 coating layer, the coating layer thickness is 5nm, the contact angle with water is 160, including a pore structure, the diameter of the pore structure is 0.5nm~5nm, the thickness is 1nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0157] Example 8
[0158] The difference between this embodiment and embodiment 1 is that the mass ratio of the porous material to the lithium-nickel transition metal composite oxide is 0.15:100, and the mass ratio of toluene to the lithium-nickel transition metal composite oxide is 0.01:100.
[0159] The positive electrode material prepared in this embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the hydrocarbon-modified ZIF-67 coating layer are located therein, the coating layer thickness is 2nm, including a pore structure, the diameter of the pore structure is 0.05nm~5nm, the thickness is 0.2nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0160] Example 9
[0161] The difference between this embodiment and embodiment 1 is that the mass ratio of the porous material to the lithium-nickel transition metal composite oxide is 0.065:100, and the mass ratio of toluene to the lithium-nickel transition metal composite oxide is 0.075:100.
[0162] The positive electrode material prepared in this embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the hydrocarbon-modified ZIF-67 coating layer are located therein, the coating layer thickness is 10nm, the positive electrode material has a pore structure, the diameter of the pore structure is 0.1nm~5nm, and the thickness is 1nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0163] Example 10
[0164] The difference between this embodiment and embodiment 1 is that the mass ratio of the porous material to the lithium-nickel transition metal composite oxide is 0.2:100, and the mass ratio of toluene to the lithium-nickel transition metal composite oxide is 0.005:100.
[0165] The positive electrode material prepared in this embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the hydrocarbon-modified ZIF-67 coating layer are located therein, the coating layer thickness is 1nm, including a pore structure, the diameter of the pore structure is 0.1nm~5nm, the thickness is 1nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0166] Embodiment 11
[0167] The difference between this embodiment and embodiment 1 is that the pressure in step 2) is 20Pa.
[0168] The positive electrode material prepared in the embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least partially located in a hydrocarbon-modified ZIF-67 coating layer, the coating layer thickness is 2nm, the positive electrode material includes a pore structure, the diameter of the pore structure is 0.1nm~5nm, and the thickness is 1nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0169] Example 12
[0170] The difference between this embodiment and embodiment 1 is that the pressure in step 2) is 100 Pa.
[0171] The positive electrode material prepared in the embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the benzyl-modified ZIF-67 coating layer are located therein, the coating layer thickness is 3nm, the positive electrode material has a pore structure, the diameter of the pore structure is 0.1nm~5nm, and the thickness is 1nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0172] Example 13
[0173] The difference between this embodiment and embodiment 1 is that the pressure in step 2) is 15 Pa.
[0174] The positive electrode material prepared in the embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the hydrocarbon-modified ZIF-67 coating layer are located therein, the coating layer thickness is 2nm, the positive electrode material has a pore structure, the diameter of the pore structure is 0.1nm~5nm, and the thickness is 1~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0175] Embodiment 14
[0176] The difference between this embodiment and embodiment 1 is that the pressure in step 2) is 120Pa.
[0177] The positive electrode material prepared in the embodiment includes LiNi 0.8 Co 0.1 Mn 0.1O2 and at least part of the hydrocarbon-modified ZIF-67 coating layer are located therein, the coating layer thickness is 5nm, the positive electrode material has a pore structure, the diameter of the pore structure is 1nm~5nm, and the thickness is 1nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0178] Embodiment 15
[0179] The difference between this embodiment and embodiment 1 is that, in step 2), the gas pressure of the system reaches 50 Pa, and the reaction is continued at 60° C. for 3 hours to obtain a high-nickel ternary positive electrode material coated with ZIF-67;
[0180] (3) Add 0.0001 times the mass of high-nickel ternary positive electrode material of toluene into the system, maintain the system temperature at 60°C, continue to flow oxygen for 1 hour, then raise the temperature to 90°C and keep warm for 3 hours.
[0181] The positive electrode material prepared in the embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the hydrocarbon-modified ZIF-67 coating layer are located therein, the coating layer thickness is 3nm, the positive electrode material has a pore structure, the diameter of the pore structure is 1nm~5nm, the thickness is 1nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0182] Example 16
[0183] The difference between this embodiment and embodiment 1 is that, in step 2), the gas pressure of the system reaches 50 Pa, and the reaction is continued at 150° C. for 1 hour to obtain a high-nickel ternary positive electrode material coated with ZIF-67;
[0184] (3) Add 0.0001 times the mass of high-nickel ternary positive electrode material of toluene into the system, maintain the system temperature at 150°C, continue to flow oxygen for 1 hour, then raise the temperature to 180°C and keep warm for 3 hours.
[0185] The positive electrode material prepared in the embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the hydrocarbon-modified ZIF-67 coating layer are located therein, the coating layer thickness is 2nm, the positive electrode material has a pore structure, the diameter of the pore structure is 0.5nm~5nm, and the thickness is 1nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0186] Embodiment 17
[0187] The difference between this embodiment and embodiment 1 is that, in step 2), the gas pressure of the system reaches 50 Pa, and the reaction is continued at 50° C. for 1 hour to obtain a high-nickel ternary positive electrode material coated with ZIF-67;
[0188] (3) Add 0.0001 times the mass of high-nickel ternary positive electrode material of toluene into the system, maintain the system temperature at 50°C, continue to flow oxygen for 1 hour, then raise the temperature to 90°C and keep warm for 3 hours.
[0189] The positive electrode material prepared in the embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the hydrocarbon-modified ZIF-67 coating layer are located therein, the coating layer thickness is 4nm, the positive electrode material has a pore structure, the diameter of the pore structure is 0.1nm~5nm, and the thickness is 1nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0190] Embodiment 18
[0191] The difference between this embodiment and embodiment 1 is that, in step 2), the gas pressure of the system reaches 50 Pa, and the reaction is continued at 170° C. for 1 hour to obtain a high-nickel ternary positive electrode material coated with ZIF-67;
[0192] (3) Add 0.0001 times the mass of high-nickel ternary positive electrode material of toluene into the system, maintain the system temperature at 170°C, continue to flow oxygen for 1 hour, then raise the temperature to 180°C and keep warm for 3 hours.
[0193] The positive electrode material prepared in the embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the hydrocarbon-modified ZIF-67 coating layer are located therein, the coating layer thickness is 2nm, the positive electrode material has a pore structure, the diameter of the pore structure is 0.1nm~5nm, and the thickness is 1nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0194] Embodiment 19
[0195] (1) Ni 0.9 Co 0.1 Al 0.1 The molar ratio of (OH)2 to LiOH is 1.05:1. After mixing, wet grinding is performed. The ground mixture is calcined at 450°C for 5 hours in a box furnace. After grinding into fine particles, it is transferred to a tube furnace in an oxygen atmosphere and sintered at high temperature for 15 hours. The sintering temperature is controlled at 750°C. The sintered high-nickel ternary positive electrode material is crushed to a particle size of 15 μm.
[0196] (2) Weigh the Li in step (1) 0.98 Ni 0.9 Co 0.1 Al 0.1 The mass of O2 was measured, and then 0.001 times the mass of ZIF-67 was weighed. The two substances were mixed and placed in an initiated chemical vapor deposition (iCVD) system. After heating to 100°C in a vacuum environment for 3 hours, oxygen was introduced to make the system pressure reach 50 Pa. The reaction was continued at 100°C for 1 hour to obtain a high-nickel ternary positive electrode material coated with ZIF-67.
[0197] (3) Ethyl acetate in an amount of 0.0001 times the mass of the high-nickel ternary positive electrode material is added to the system, the system temperature is maintained at 100°C, oxygen is continuously passed for 1 hour, and then the temperature is raised to 120°C and kept warm for 3 hours to obtain a high-nickel ternary positive electrode material coated with ZIF-67 modified with ethyl acetate.
[0198] The positive electrode material prepared in this embodiment includes LiNi 0.8 Co 0.1 Al 0.1 O2 and at least part of it are located in the ethyl acetate-modified ZIF-67 coating layer, the coating layer thickness is 3nm, the positive electrode material has a pore structure, the diameter of the pore structure is 0.1nm~5nm, and the thickness is 0.5~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0199] Embodiment 20
[0200] The positive electrode material of this embodiment is a high-nickel ternary positive electrode material coated with COF-1 modified with acetamide, and the specific preparation method thereof is:
[0201] The same as Example 19, except that in step (3), 0.0001 times the mass of the high-nickel ternary positive electrode material of acetamide is added to the system.
[0202] The positive electrode material prepared in this embodiment includes Li0.98Ni 0.9 Co 0.1 Al 0.1 O2 and at least part of the phenolic hydroxyl modified COF-1 coating layer, the coating layer thickness is 3nm, with a pore structure, the diameter of the pore structure is 0.1nm ~ 5nm, the thickness is 0.5nm ~ 5nm; the depth of the pore structure is 1nm ~ 50nm, and the average particle size of the positive electrode material is 12μm.
[0203] Comparative Example 1
[0204] The positive electrode material of this comparative example is a high-nickel ternary positive electrode material without a coating layer, and its specific preparation method is:
[0205] (1) is the same as step (1) of Example 1;
[0206] (2) Add 200 ml of deionized water to a high-nickel ternary positive electrode material with a particle size of 15 μm, stir for 1.5 hours, and then filter the mixed solution for 15 minutes to collect the solid portion; dry the collected solid at 100° C. for 10 hours, sieve, demagnetize and package to obtain a high-nickel ternary positive electrode material without a coating layer.
[0207] Comparative Example 2
[0208] The positive electrode material of this comparative example is a high-nickel ternary positive electrode material coated with unmodified ZIF-67, and its specific preparation method is:
[0209] The method is the same as Example 1, except that after obtaining the high-nickel ternary positive electrode material coated with ZIF-67 in step (2), the temperature can be cooled to obtain the positive electrode material.
[0210] Comparative Example 3
[0211] The positive electrode material of this comparative example is a high-nickel ternary positive electrode material coated with unmodified COF-1, and its specific preparation method is:
[0212] The method is the same as Example 3, except that after obtaining the COF-1 coated high nickel ternary positive electrode material in step (2), the temperature can be cooled to obtain the positive electrode material.
[0213] Comparative Example 4
[0214] The positive electrode material of this comparative example is a high-nickel ternary positive electrode material coated with unmodified polyvinyl pyridine, and its specific preparation method is:
[0215] The method is the same as Example 5, except that after obtaining the high-nickel ternary positive electrode material coated with polyvinylpyridine in step (2), the temperature can be cooled to obtain the positive electrode material.
[0216] Comparative Example 5
[0217] The positive electrode material of this embodiment is a high-nickel ternary positive electrode material coated with ZIF-67 modified by hydrocarbon groups. The difference is that it is prepared by ordinary chemical deposition method. The specific preparation method is:
[0218] (1) Ni 0.8 Co 0.1 Mn 0.1The molar ratio of (OH)2 to LiOH is 1.05:1. After mixing, wet grinding is performed. The ground mixture is calcined at 450°C for 5 hours in a box furnace. After grinding into fine particles, it is transferred to a tube furnace in an oxygen atmosphere and sintered at high temperature for 15 hours. The sintering temperature is controlled at 750°C. The sintered high-nickel ternary positive electrode material is crushed to a particle size of 15 μm.
[0219] (2) Weigh the mass of NCM811 in step (1), then weigh 0.001 times the mass of ZIF-67 and 0.0001 times the mass of the high-nickel ternary positive electrode material of toluene, mix the two substances, mix them evenly in pure water, heat to 70 degrees, keep warm for 12 hours, and obtain a mixture. Further place it in an oven for drying for 12 hours to obtain a high-nickel ternary positive electrode material coated with hydrocarbon-modified ZIF-67.
[0220] Comparative Example 6
[0221] The positive electrode material of this embodiment is a high-nickel ternary positive electrode material coated with a hydrophobic porous polymer, and the specific preparation method thereof is:
[0222] (1) Ni0.8Co0.1Mn0.1(OH)2 and LiOH were mixed in a molar ratio of 1.05:1, and then wet-ground; the ground mixture was calcined at 450°C for 5 h in a box furnace, ground into fine particles, and then transferred to a tube furnace for high-temperature sintering in an oxygen atmosphere for 15 h, with the sintering temperature controlled at 750°C; the sintered high-nickel ternary positive electrode material was crushed to a particle size of 15 μm;
[0223] (2) A mixture of azobisisobutyronitrile, potassium bromide and tri(2,4-di-tert-butylphenyl)phosphite is stirred and heated to obtain a porous organic polymer, and the porous organic polymer and a high-nickel ternary positive electrode material are heated to react in a mass ratio of 1:15, washed and dried to obtain a high-nickel ternary positive electrode material coated with a porous organic polymer.
[0224] The positive electrode material prepared in this embodiment includes LiNi 0.8 Co 0.1 Mn 0.1 O2 and at least part of the hydrocarbon-modified ZIF-67 coating layer are located therein, the coating layer thickness is 3nm, the positive electrode material has a pore structure, the diameter of the pore structure is 0.1nm~5nm, the thickness is 0.5nm~5nm; the depth of the pore structure is 1nm~50nm, and the average particle size of the positive electrode material is 12μm.
[0225] The present application also mixes the positive electrode materials obtained in Examples 1 to 20 and Comparative Examples 1 to 6 with the conductive agent acetylene carbon black and the binder PVDF at a mass ratio of 96:2:2, adds an appropriate amount of 1-methyl-2-pyrrolidone and places it in a high-speed disperser, disperses it for 20 minutes, prepares it into a slurry, evenly applies it on an aluminum sheet, and then dries and presses it into a positive electrode sheet. Then, a metal lithium sheet is used as a negative electrode sheet and assembled into a 2032 button battery.
[0226] The test results of the residual alkali content, storage volume increment (wherein the storage volume increment is measured at 2.0V using a soft-pack battery) and moisture on the surface of the battery positive electrode materials prepared in Examples 1 to 6 and Comparative Examples 1 to 4 are shown in Table 1.
[0227] Residual alkali test method: Use Mettler G20S for testing, and use potentiometric titration to test the residual alkali content of the material. Among them, since high-nickel positive electrode materials are particularly easy to react in the air to generate lithium hydroxide, and lithium hydroxide and CO2, H2O are easy to react to generate lithium carbonate, so hydroxide and carbonate are used to represent the residual alkali content.
[0228] Storage volume increment: Use soft-pack batteries to perform charge and discharge cycle tests at 2V. After cycling 500 times at 45 degrees and 60 degrees respectively, stop charging and discharging. Test the voltage and current of the battery at this time, and convert them into capacity based on the actual active substances. Test the degree of battery expansion through the battery morphology and convert them into mL for calculation.
[0229] Moisture test method: Select 1g sample, heat to 300℃, and use Karl Fischer titrator to test the moisture content (mass concentration ppm) after 10 minutes.
[0230] Contact angle: Drop water directly on the surface of the positive electrode material, and then use a protractor to determine the contact angle directly or take a photo first.
[0231] The batteries prepared in Examples 1 to 20 and Comparative Examples 1 to 6 were tested for electrical performance using a blue-electric test system (charge and discharge voltage was 2.8 to 4.3 V, temperature was 25° C.). The cycle capacity retention rate curve of the obtained battery after discharge is shown in Table 2.
[0232] Table 1
[0233]
[0234]
[0235]
[0236] As shown in Table 1, the residual alkali content, storage volume increment and moisture content of Examples 1 to 20 and Comparative Examples 1 to 4 are compared. It can be clearly found that the residual alkali content on the surface of the positive electrode material coated with the porous material modified by the hydrophobic group is lower than that on the surface of the positive electrode material coated with the unmodified porous material, indicating that the performance of the positive electrode material can be improved after the porous material modified by the group is coated on the positive electrode material. Further, the residual alkali, storage volume increment and moisture reduction of Examples 1, 3 and 5 are more obvious than those of Examples 2, 4 and 6, indicating that the ternary positive electrode material with the hydrocarbon-modified coating layer has the best effect, because the hydrocarbon-modified coating layer is conducive to improving the material's resistance to moisture and gases such as CO2. In addition, according to the test results of moisture in Table 1, it is also obvious that the hydrophobic effect of the material with the hydrocarbon-modified coating layer is very significant, while the material with the hydroxyl-modified coating layer has no substantial hydrophobic effect. Under the 45° test condition, the degree of bulging of the batteries in different embodiments is not much different. When the high-temperature cycle is 60°, the degree of bulging of different embodiments is quite different. This is because different coating materials have different barriers to side reactions.
[0237] Table 2
[0238]
[0239]
[0240]
[0241] Figure 1 The data of button-type battery cycle performance after Examples 1 to 6 and Comparative Examples 1-4 are assembled. Compared with Comparative Example 1, it can be found that the positive electrode materials prepared by the non-water washing method in Examples 1-6 and Comparative Examples 2-4 of the present application have more obvious advantages. This is because although the water washing scheme washes out the residual alkali on the surface of the material, it sacrifices the capacity of the material to a certain extent and is not conducive to the long-term cycle performance of the material.
[0242] Figure 2 1-4 are EIS impedance diagrams after Examples 1-6 and Comparative Examples 1-4 are assembled into button cells. It can be seen from the diagram that the impedance of the positive electrode material of Comparative Example 1 after water washing is the largest when used in the battery, while in Examples 1-6, since the residual alkali content on the surface of the positive electrode material modified with hydrocarbon groups or hydroxy groups is significantly reduced, the side reactions of the battery are also reduced after being assembled into the battery, and the electrochemical performance is further improved.
[0243] Figure 3This is a scanning electron microscope image of the positive electrode material prepared in Example 1. From the figure, it can be seen that the surface of the porous material and the inside of the pores are not smooth. Instead, some small clusters of substances are distributed. These are the products modified by hydrocarbon groups attached to the surface of the porous material, which can resist the erosion of the internal positive electrode material by the electrolyte to a certain extent and resist the formation of residual alkali on the surface of the positive electrode material.
[0244] Figure 4 The transmission electron microscope images of the materials prepared in different steps in Example 1, wherein (a) is the uncoated high-nickel ternary positive electrode material prepared in step (1), (b) is a partial enlarged image of the uncoated high-nickel ternary positive electrode material, (c) is the positive electrode material modified by hydrocarbon group and coated with ZIF-67 in step (3), and (d) is a partial enlarged image of the positive electrode material modified by hydrocarbon group and coated with ZIF-67. It can be clearly seen from the figure that a dense and uniform coating layer is formed on the surface of the positive electrode material prepared in the present application, indicating that the preparation method of the positive electrode material in the present application is beneficial for uniform coating of the product.
[0245] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
[0246] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present invention and to form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present invention and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A positive electrode material, characterized in that: It comprises a lithium-nickel transition metal composite oxide and a coating layer at least partially located on the surface of the lithium-nickel transition metal composite oxide, wherein the coating layer comprises a porous material modified with a hydrophobic group; The hydrophobic group includes at least one of a hydrocarbon group, a hydroxyl group, an ester group, an ether group, an amine group and an amide group; The porous material comprises an organic porous material, and the organic porous material comprises at least one of a metal organic framework material, a zeolite imidazolate framework structure material, a covalent organic framework material, an intrinsic microporous polymer, and a polyvinyl pyridine porous material; The general chemical formula of the lithium-nickel transition metal composite oxide is Li a Ni x Co y M z O2, wherein 0.95≤a≤1.05, 0.80≤x<1, 0<y+z≤0.20, and M includes any one of Mn, Al, Cu, Zn, and Cr.
2. The positive electrode material according to claim 1, characterized in that It satisfies at least one of the following characteristics a~d: a. The hydrophobic group is bonded to the porous material via a covalent bond or a non-covalent bond; c. the hydrocarbon group comprises at least one of an alkyl group, an alkenyl group, an aryl group and an alkynyl group; d. The contact angle between the porous material modified with the hydrophobic group and water is greater than or equal to 150°.
3. The positive electrode material according to claim 1 or 2, characterized in that It satisfies at least one of the following characteristics a~f: c. The porous material includes at least one of COF-1, COF-102, ZIF-67, ZIF-8 and PIM-1; d. The hydrophobic group-modified porous material has pores, and the diameter of the pores is 0.8 nm to 5 nm; e. The depth of the pores of the hydrophobic group-modified porous material is 1 nm to 50 nm; f. The thickness of the porous material modified with the hydrophobic group is 0.5 nm to 5 nm.
4. The positive electrode material according to any one of claims 1 to 3, characterized in that It satisfies at least one of the following characteristics a~e: b. The average particle size of the lithium-nickel transition metal composite oxide is 7 μm to 20 μm; c. The thickness of the coating layer is 0.5nm~5nm; d. The lithium hydroxide content of the positive electrode material is 0.012 wt%~0.10 wt%, and the lithium carbonate content is 0.012 wt%~0.10 wt%; e. Select 1g of the positive electrode material, heat it to 300°C, and after 10 minutes, use a Karl Fischer titrator to test the moisture content to be less than or equal to 300ppm.
5. A method for preparing the positive electrode material according to any one of claims 1 to 4, characterized in that: include: Performing a first induced chemical vapor deposition process on a mixture containing a lithium-nickel transition metal composite oxide and a porous material to obtain a lithium-nickel transition metal composite oxide coated with a porous material; The hydrophobic material and the lithium-nickel transition metal composite oxide coated with a porous material are subjected to a second initiated chemical vapor deposition process to obtain a positive electrode material, wherein the positive electrode material comprises a lithium-nickel transition metal composite oxide and a coating layer at least partially located on the surface of the lithium-nickel transition metal composite oxide, wherein the coating layer comprises a porous material modified with a hydrophobic group; The hydrophobic material includes an organic hydrophobic group, and the organic hydrophobic group includes at least one of a hydrocarbon group, an ester group, an ether group, an amine group, and an amide group.
6. The preparation method according to claim 5, characterized in that: It satisfies at least one of the following characteristics a~j: a. The general chemical formula of the lithium-nickel transition metal composite oxide is Li a Ni x Co y M z O2, wherein 0.95≤a≤1.05, 0.80≤x<1, 0<y+z≤0.20, and M includes at least one of Mn, Al, Cu, Zn and Cr; b. The average particle size of the lithium-nickel transition metal composite oxide is 7 μm to 20 μm; c. The mass ratio of the porous material to the lithium-nickel transition metal composite oxide is (0.08-0.15): 100; d. The mass ratio of the hydrophobic material to the lithium-nickel transition metal composite oxide is (0.01-0.05): 100; e. The porous material comprises an organic porous material; f. The porous material comprises an organic porous material, wherein the organic porous material comprises at least one of a metal organic framework material, a zeolite imidazolate framework material, a covalent organic framework material, an inherent microporous polymer, and a polyvinyl pyridine porous material; g. The porous material includes at least one of COF-1, COF-102, ZIF-67, ZIF-8 and PIM-1; i. The hydrocarbon group includes at least one of an alkyl group, an alkenyl group, an aryl group and an alkynyl group; j. The hydrophobic material includes at least one of methane, ethylene, propyne, toluene, phenol, ethyl acetate, phenyl acetate, ethylene diethyl ester, methyl ether, ethyl ether, n-butyl ether, di-sec-butylamine, tert-butylamine, tert-octylamine, acetamide, cyclopropaneamide and acrylamide.
7. The preparation method according to claim 5 or 6, characterized in that: It satisfies at least one of the following characteristics a~e: a. The method further comprises a preheating treatment before the first induced chemical vapor deposition treatment of the mixture containing lithium nickel transition metal composite oxide and porous material; the preheating treatment comprises evacuating the system of the induced chemical vapor deposition treatment and then heating it, and the temperature after heating is maintained at 60°C to 150°C for 3h to 5h; b. The first induced chemical vapor deposition process and the second induced chemical vapor deposition process are both carried out in an oxygen-containing atmosphere; c. The pressure of the first induced chemical vapor deposition process and the second induced chemical vapor deposition process is 20Pa~100Pa; d. The temperature of the first induced chemical vapor deposition treatment is 60°C~150°C, and the time is 1h~3h; e. The second induced chemical vapor deposition treatment comprises first reacting under the conditions of the first induced chemical vapor deposition treatment for 0.5h~1.5h; then raising the temperature by 20℃~30℃ and keeping it warm for 2h~5h.
8. The preparation method according to claim 5, characterized in that: The preparation method of the lithium-nickel-containing transition metal composite oxide comprises: mixing a lithium-nickel-containing precursor with a lithium source, and sintering to obtain the lithium-nickel-containing transition metal composite oxide.
9. The preparation method according to claim 8, characterized in that: It satisfies at least one of the following characteristics a~h: a. The lithium-nickel precursor comprises Ni x Co y M z Oxides or hydroxides, wherein M comprises at least one of Mn, Al, Cu, Zn, and Cr, 0.8≤x<1, 0 <y+z≤0.2,x+y+z=1; b. The lithium source comprises lithium hydroxide or lithium carbonate; c. The molar ratio of the lithium element in the lithium source to the total metal elements in the lithium-containing nickel precursor is 1: (0.95-1.3); d. Before the sintering, the step further comprises: grinding and crushing the material mixed with the lithium nickel precursor and the lithium source; e. After the sintering, the step further comprises: crushing the lithium-nickel transition metal composite oxide to a particle size of 7 μm to 20 μm; f. The sintering comprises a primary sintering and a secondary sintering; g. The primary sintering atmosphere is air, the primary sintering temperature is 400 ℃ ~ 500 ℃, and the time is 4h ~ 6h; h. The sintering atmosphere of the secondary sintering is oxygen, the temperature of the secondary sintering is 500°C~800°C, and the time is 10h~15h.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode material according to any one of claims 1 to 3.