Ti-Cr co-doped high-voltage spinel positive electrode material and preparation method thereof, lithium ion battery positive electrode and lithium ion battery
Through Ti-Cr co-doping and dispersant treatment, the problem of structural instability of high-voltage spinel cathode materials during the synthesis process was solved, and the cycle performance and material stability of lithium-ion batteries were improved.
Patent Information
- Application Number
- CN202210758193.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-06-29
AI Technical Summary
The high-voltage spinel LiNi0.5Mn1.5O4 cathode material suffers from the John-Teller effect during the synthesis process and the dissolution of the transition metal Mn under high-voltage operating conditions, resulting in structural instability and affecting the battery performance of lithium-ion batteries.
Ti-Cr co-doped high-voltage spinel cathode material is used, its chemical formula is LiNi0.5-xMn1.5-yTixCryO4. By mixing lithium source, nickel source, manganese source, titanium source, chromium source and solvent, ball milling is performed , drying, pre-sintering and secondary sintering preparation, adding dispersant to improve the uniformity and structural stability of the mixture.
Through the co-doping of Ti elements and Cr elements, the structural distortion of the material and the dissolution of transition metals are reduced, the structural strength and cycle stability of the material are enhanced, and the cycle performance of lithium-ion batteries is improved.
Smart Images

Figure CN114975985B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium-ion batteries, and in particular to a Ti-Cr co-doped high-voltage spinel positive electrode material and a preparation method thereof, a lithium-ion battery positive electrode and a lithium-ion battery. Background Art
[0002] With the rapid development of the new energy industry, lithium battery equipment has gradually entered people's daily life. The research on positive electrode materials has also gradually developed towards high working voltage and high energy density to meet the different usage needs of consumers. Compared with other positive electrode materials, high-voltage spinel LiNi 0.5 Mn 1.5 O4 cathode material has the advantages of high working voltage (~4.7V) and high energy density (650Wh / kg), and is considered to be an ideal next-generation cathode material. 0.5 Mn 1.5 The John-Teller effect that occurs during the synthesis of O4 positive electrode materials and the dissolution of transition metal Mn and structural instability under high voltage working conditions affect battery performance. Summary of the invention
[0003] The purpose of the present application is to provide a Ti-Cr co-doped high-voltage spinel positive electrode material and a preparation method thereof, a lithium ion battery positive electrode and a lithium ion battery, so as to solve the above problems.
[0004] To achieve the above objectives, this application adopts the following technical solutions:
[0005] A Ti-Cr co-doped high-voltage spinel cathode material, the chemical formula of which is LiNi 0.5-x Mn 1.5-y Ti x Cr y O4, where 0.001≤x≤0.06, 0.001≤y≤0.07.
[0006] The present application also provides a method for preparing the Ti-Cr co-doped high-voltage spinel positive electrode material, comprising:
[0007] Mixing raw materials including a lithium source, a nickel source, a manganese source, a titanium source, a chromium source, a solvent and a dispersant to obtain a slurry;
[0008] Drying the slurry to obtain a solid powder, and then pre-sintering the solid powder to obtain a precursor;
[0009] The precursor is subjected to secondary sintering to obtain the Ti-Cr co-doped high-voltage spinel positive electrode material.
[0010] Preferably, the lithium source includes one or more of lithium carbonate, lithium acetate, and lithium nitrate;
[0011] The nickel source includes nickel oxide and / or nickel acetate tetrahydrate;
[0012] The manganese source includes one or more of manganese oxide, manganese dioxide, and manganese tetraoxide;
[0013] The titanium source includes titanium monoxide and / or titanium dioxide;
[0014] The chromium source includes chromium dioxide and / or chromium trioxide;
[0015] The solvent includes anhydrous ethanol;
[0016] The dispersant includes isopropyl alcohol and / or polyvinyl pyrrolidone, and the amount of the dispersant is 1wt% of the slurry.
[0017] Preferably, the mixing further comprises ball milling;
[0018] The ball-to-material mass ratio of the ball mill is (60-90):1, the rotation speed is 500-650r / min, and the time is 4-5h.
[0019] Preferably, the drying temperature is 100-120° C. and the drying time is 4-5 h.
[0020] Preferably, the pre-sintering atmosphere is air;
[0021] The pre-sintering temperature program is as follows: the temperature rise rate before 100°C is 1-2°C / min, the temperature rise rate from 100°C to 500°C is 2-5°C / min, the temperature rise rate from 400°C to 500°C is 1-2°C / min, the terminal temperature of the temperature rise is 500-550°C, and the sintering time is 5-7h.
[0022] Preferably, the heating program of the secondary sintering is: the heating rate before 100°C is 1-2°C / min, the heating rate from 100°C to 850°C is 2-5°C / min, the heating rate from 850°C to 950°C is 1-2°C / min, the heating end temperature is 900-1000°C, and the sintering time is 10-12h.
[0023] Preferably, the secondary sintering further includes crushing and separation;
[0024] The sieve used for the separation is 200 mesh, and the material under the sieve is taken.
[0025] The present application also provides a lithium-ion battery positive electrode, the raw materials of which include the Ti-Cr co-doped high-voltage spinel positive electrode material.
[0026] The present application also provides a lithium-ion battery, comprising the lithium-ion battery positive electrode.
[0027] Compared with the prior art, the beneficial effects of this application include:
[0028] The Ti-Cr co-doped high-voltage spinel positive electrode material provided in the present application replaces and dopes Ni and Mn elements with Ti elements and Cr elements. The synergistic effect of Ti-Cr co-doping reduces the structural distortion of the material caused by the John-Telle effect during the preparation process, alleviates the dissolution of transition metals and the electrode / electrolyte interface side reactions during the cycle process, enhances the structural strength of the material, and effectively improves the stability of the material during long-term cycles.
[0029] The present application provides a method for preparing a Ti-Cr co-doped high-voltage spinel positive electrode material, in which a dispersant is added during the preparation process for dispersion treatment to improve the uniformity of the mixed material; the method has good process stability, a safe and controllable preparation process, a simple preparation process, and good industrialization prospects.
[0030] The lithium-ion battery positive electrode and lithium-ion battery provided in this application have good cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0032] Figure 1 The first cycle charge and discharge curves of Example 3, Comparative Example 1 and Comparative Example 2 at 30°C and 0.2C;
[0033] Figure 2 The performance curves of Example 3, Comparative Example 1 and Comparative Example 2 for 300 cycles at 30°C and 1C are shown;
[0034] Figure 3 The cycle performance curves of Example 3, Comparative Example 1 and Comparative Example 2 at different rates at 60°C are shown;
[0035] Figure 4 This is the SEM image of the Ti-Cr element co-doped high-voltage spinel positive electrode material obtained in Example 3. DETAILED DESCRIPTION
[0036] As used herein:
[0037] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0038] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0039] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0040] In these examples, parts and percentages are by mass unless otherwise indicated.
[0041] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0042] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0043] A Ti-Cr co-doped high-voltage spinel cathode material, the chemical formula of which is LiNi 0.5-x Mn 1.5-yTi x Cr y O4, where 0.001≤x≤0.06, 0.001≤y≤0.07.
[0044] Optionally, x may be 0.001, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06 or any value between 0.001 and 0.06; y may be 0.001, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07 or any value between 0.001 and 0.07.
[0045] The present application also provides a method for preparing the Ti-Cr co-doped high-voltage spinel positive electrode material, comprising:
[0046] Mixing raw materials including a lithium source, a nickel source, a manganese source, a titanium source, a chromium source, a solvent and a dispersant to obtain a slurry;
[0047] Drying the slurry to obtain a solid powder, and then pre-sintering the solid powder to obtain a precursor;
[0048] The precursor is subjected to secondary sintering to obtain the Ti-Cr co-doped high-voltage spinel positive electrode material.
[0049] In an optional embodiment, the lithium source includes one or more of lithium carbonate, lithium acetate, and lithium nitrate;
[0050] In an optional embodiment, the nickel source includes nickel oxide and / or nickel acetate tetrahydrate;
[0051] In an optional embodiment, the manganese source includes one or more of manganese oxide, manganese dioxide, and manganese tetraoxide;
[0052] In an optional embodiment, the titanium source includes titanium monoxide and / or titanium dioxide;
[0053] In an optional embodiment, the chromium source includes chromium dioxide and / or chromium trioxide;
[0054] In an optional embodiment, the solvent includes anhydrous ethanol;
[0055] In an optional embodiment, the dispersant includes isopropyl alcohol and / or polyvinyl pyrrolidone, and the amount of the dispersant is 1 wt % of the slurry.
[0056] In an optional embodiment, the mixing further comprises ball milling;
[0057] In an optional embodiment, the ball-to-material mass ratio of the ball mill is (60-90):1, the rotation speed is 500-650r / min, and the time is 4-5h.
[0058] Optionally, the ball-to-material mass ratio of the ball mill can be 60:1, 70:1, 80:1, 90:1 or any value between (60-90):1, the rotation speed can be 500r / min, 550r / min, 600r / min, 650r / min or any value between 500-650r / min, and the time can be 4h, 4.5h, 5h or any value between 4-5h.
[0059] In an optional embodiment, the drying temperature is 100-120° C. and the drying time is 4-5 hours.
[0060] Optionally, the drying temperature may be 100° C., 110° C., 120° C. or any value between 100-120° C., and the drying time may be 4 h, 4.5 h, 5 h or any value between 4-5 h.
[0061] In an optional embodiment, the pre-sintering atmosphere is air;
[0062] In an optional embodiment, the pre-sintering temperature program is: the heating rate before 100°C is 1-2°C / min, the heating rate from 100°C to 500°C is 2-5°C / min, the heating rate from 400°C to 500°C is 1-2°C / min, the terminal temperature of the heating is 500-550°C, and the sintering time is 5-7h.
[0063] Optionally, in the pre-sintering heating program: the heating rate before 100°C can be 1°C / min, 1.5°C / min, 2°C / min or any value between 1-2°C / min, the heating rate from 100°C to 500°C can be 2°C / min, 3°C / min, 4°C / min, 5°C / min or any value between 2-5°C / min, the heating rate from 400°C to 500°C can be 1°C / min, 1.5°C / min, 2°C / min or any value between 1-2°C / min, the heating end point temperature can be 500°C, 510°C, 520°C, 530°C, 540°C, 550°C or any value between 500-550°C, and the sintering time can be 5h, 6h, 7h or any value between 5-7h.
[0064] In an optional embodiment, the heating program of the secondary sintering is: the heating rate before 100°C is 1-2°C / min, the heating rate from 100°C to 850°C is 2-5°C / min, the heating rate from 850°C to 950°C is 1-2°C / min, the terminal temperature of the heating is 900-1000°C, and the sintering time is 10-12h.
[0065] Optionally, in the heating program of the secondary sintering: the heating rate before 100°C can be 1°C / min, 1.5°C / min, 2°C / min or any value between 1-2°C / min, the heating rate from 100°C to 850°C can be 2°C / min, 3°C / min, 4°C / min, 5°C / min or any value between 2-5°C / min, the heating rate from 850°C to 950°C can be 1°C / min, 1.5°C / min, 2°C / min or any value between 1-2°C / min, the heating end point temperature can be 900°C, 910°C, 920°C, 930°C, 940°C, 950°C, 960°C, 970°C, 980°C, 990°C, 1000°C or any value between 900-1000°C, and the sintering time can be 10h, 11h, 12h or any value between 10-12h.
[0066] In an optional embodiment, the secondary sintering further includes crushing and separation;
[0067] In an optional embodiment, the sieve used for separation is 200 mesh, and the material under the sieve is taken.
[0068] The present application also provides a lithium-ion battery positive electrode, the raw materials of which include the Ti-Cr co-doped high-voltage spinel positive electrode material.
[0069] The present application also provides a lithium-ion battery, comprising the lithium-ion battery positive electrode.
[0070] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0071] The nickel source used in the embodiments of the present application is nickel oxide (AR), the titanium source is titanium dioxide (TiO2≥99%), and the chromium source is chromium trioxide (AR), all of which are purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; the manganese source is manganese monoxide (MnO=99%), purchased from Shanghai McLean Biochemical Technology Co., Ltd.; the lithium source is Li2CO3 (AR), purchased from Xilong Science Co., Ltd.
[0072] Example 1
[0073] This embodiment provides a Ti-Cr co-doped high-voltage spinel positive electrode material, and the preparation method thereof includes:
[0074] (1) a lithium source, a nickel source, a manganese source, a titanium source, and a chromium source are first ground in an agate grinding mortar according to a molar ratio of 1:0.45:1.47:0.05:0.03, and then added to an agate grinding tank filled with anhydrous ethanol to dissolve to obtain a mixed suspension, and then 1 wt % of isopropanol is added to the suspension; the amount of anhydrous ethanol added is preferably such that the material is completely immersed;
[0075] (2) ball milling the mixed suspension obtained in step (1) to obtain a slurry; the equipment used for ball milling is a planetary ball mill, the medium is agate beads, the ball-to-material ratio is 90:1, the ball milling speed is 500 r / min, and the ball milling time is 4 hours;
[0076] (3) placing the slurry obtained in step (2) in a blast drying oven and drying to obtain a solid powder; the blast drying oven has an operating temperature of 100-120° C. and a drying time of 4-5 hours;
[0077] (4) The solid powder obtained in step (3) is loaded into a porcelain boat, transferred to a muffle furnace, and pre-sintered in an air atmosphere to obtain a precursor powder of a Ti-Cr element co-doped high-pressure spinel positive electrode material; the pre-sintering temperature is 500°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 500°C is 5°C / min, the heating rate from 400°C to 500°C is 2°C / min, the heating end temperature is 550°C, and the sintering time is 5h;
[0078] (5) The precursor powder of the high-pressure spinel positive electrode material obtained in step (4) is ground in an agate grinding mortar and then loaded into a porcelain boat, which is transferred to a muffle furnace for secondary sintering. The sintering atmosphere is air, the secondary sintering temperature is 950°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 850°C is 5°C / min, the heating rate from 850°C to 950°C is 2°C / min, the heating end temperature is 950°C, and the sintering time is 10h; the material obtained after the secondary sintering is ground and passed through a 200-mesh sieve to obtain a Ti-Cr element co-doped high-pressure spinel positive electrode material with a chemical formula of LiNi 0.45 Ti 0.05 Mn 1.47 Cr 0.03 O4.
[0079] The Ti-Cr element co-doped high-voltage spinel positive electrode material obtained above was assembled into a button battery (CR2035) using a button half-cell manufacturing method, and the charge and discharge voltage range was 3.2-4.95V.
[0080] The button half-cell production and performance test methods are as follows:
[0081] 1. Material drying (vacuum oven 110 degrees for 12 hours)
[0082] 2. Ingredient weighing (material: conductive agent: binder):
[0083] Materials: Conductive agent: binder (LNMO: conductive carbon: binder) = 90:5:5, solid content in the binder is 0.1g (with a binder of PVDF:NMP = 1:9, of which the PVDF content accounts for 10%).
[0084] 3. Mixing (material: conductive agent: binder) + NMP:
[0085] Step (1): Pour the weighed powder material and conductive agent into a centrifuge tank and mix them once;
[0086] Step (2): add a binder and an appropriate amount of NMP and mix twice; mixing centrifuge parameters (Step 1: revolution 960 time 150s, Step 2: revolution 1280 time 120s, Step 3: revolution 1460 time 90s).
[0087] 4. Coating production:
[0088] Step (1): moving the slurry transferred from the mixer into the coating machine for coating operation;
[0089] Step (2): placing the coated aluminum foil in a vacuum oven (110° C.) for 2 hours;
[0090] Step (3): compacting the dried aluminum foil using a roller press;
[0091] Step (4): Place the rolled aluminum foil in a vacuum oven (110° C.) for 12 hours.
[0092] 5. Make batteries;
[0093] Step (1): Cut the electrode sheet after rolling and drying into Φ14 mm round sheets using a cutting machine;
[0094] Step (2): Weigh the cut electrode with a balance and make corresponding records;
[0095] Step (3): Place the electrode in a vacuum oven and dry it at 110°C for 3 hours;
[0096] Step (4): Place the electrode in the glove box for assembly and assemble the battery. (The amount of electrolyte is slightly adjusted according to the active mass of the electrode);
[0097] Step (5): The assembled battery is sealed with a sealing machine.
[0098] 6.Battery performance test:
[0099] The battery capacity, cycle and rate performance were tested using Shenzhen Xinwei Electronics Co., Ltd. (CT-4000).
[0100] At 0.2C and a test temperature of 30°C, the first cycle discharge capacity was measured to be 112.31mAh / g; at 1C and a test temperature of 60°C, the capacity retention rate after 300 cycles was 31.02%. At different rates of 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C, and 0.1C and a test temperature of 60°C, the discharge specific capacities were measured to be 105.42mAh / g, 105.78mAh / g, 111.24mAh / g, 106.13mAh / g, 99.76Ah / g, 81.28mAh / g, 52.34mAh / g, and 104.92mAh / g, respectively.
[0101] Example 2
[0102] This embodiment provides a Ti-Cr co-doped high-voltage spinel positive electrode material, and the preparation method thereof includes:
[0103] (1) grinding a lithium source, a nickel source, a manganese source, a titanium source, and a chromium source in a molar ratio of 1:0.45:1.47:0.05:0.03 with an agate grinding mortar, and then adding them to an agate grinding tank filled with anhydrous ethanol to dissolve to obtain a mixed suspension, and then adding 1 wt % of polyvinyl pyrrolidone to the suspension; the amount of anhydrous ethanol added is preferably such that the material is completely immersed;
[0104] (2) ball milling the mixed suspension obtained in step (1) to obtain a slurry; the equipment used for ball milling is a planetary ball mill, the medium is agate beads, the ball-to-material ratio is 90:1, the ball milling speed is 500 r / min, and the ball milling time is 4 hours;
[0105] (3) placing the slurry obtained in step (2) in a blast drying oven and drying to obtain a solid powder; the blast drying oven has an operating temperature of 120° C. and a drying time of 4 hours;
[0106] (4) The solid powder obtained in step (3) is loaded into a porcelain boat, transferred to a muffle furnace, and pre-sintered in an air atmosphere to obtain a precursor powder of a Ti-Cr element co-doped high-pressure spinel positive electrode material; the pre-sintering temperature is 500°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 500°C is 5°C / min, the heating rate from 400°C to 500°C is 2°C / min, the heating end temperature is 550°C, and the sintering time is 7h;
[0107] (5) The precursor powder of the high-pressure spinel positive electrode material obtained in step (4) is ground in an agate grinding mortar and then loaded into a porcelain boat, which is transferred to a muffle furnace for secondary sintering. The sintering atmosphere is air, the secondary sintering temperature is 950°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 850°C is 5°C / min, the heating rate from 850°C to 950°C is 2°C / min, the heating end temperature is 950°C, and the sintering time is 10h; the material obtained after the secondary sintering is ground and passed through a 200-mesh sieve to obtain a Ti-Cr element co-doped high-pressure spinel positive electrode material with a chemical formula of LiNi 0.45 Ti 0.05 Mn 1.47 Cr 0.03 O4;
[0108] The Ti-Cr element co-doped high-voltage spinel positive electrode material obtained above was assembled into a button battery (CR2035) using the method of making a button half-cell, with a charge and discharge voltage range of 3.2-4.95V. At 0.2C and a test temperature of 30°C, the first cycle discharge capacity was measured to be 113.46mAh / g; at 1C and a test temperature of 60°C, the capacity retention rate was 34.28% after 300 cycles. At different rates of 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C, and 0.1C, and a test temperature of 60°C, the discharge specific capacities were measured to be 106.08mAh / g, 106.66mAh / g, 108.24mAh / g, 106.99mAh / g, 101.24Ah / g, 83.72mAh / g, 54.51mAh / g, and 105.39mAh / g, respectively.
[0109] Example 3
[0110] This embodiment provides a Ti-Cr co-doped high-voltage spinel positive electrode material, and the preparation method thereof includes:
[0111] (1) grinding a lithium source, a nickel source, a manganese source, a titanium source, and a chromium source in a molar ratio of 1:0.45:1.45:0.05:0.05 with an agate grinding mortar, and then adding them to an agate grinding tank filled with anhydrous ethanol to dissolve to obtain a mixed suspension, and then adding 1 wt % of isopropanol to the suspension; the amount of anhydrous ethanol added is preferably such that the material is completely immersed;
[0112] (2) ball milling the mixed suspension obtained in step (1) to obtain a slurry; the equipment used for ball milling is a planetary ball mill, the medium is agate beads, the ball-to-material ratio is 90:1, the ball milling speed is 500 r / min, and the ball milling time is 4 hours;
[0113] (3) placing the slurry obtained in step (2) in a blast drying oven and drying to obtain a solid powder; the blast drying oven has an operating temperature of 120° C. and a drying time of 4 hours;
[0114] (4) The solid powder obtained in step (3) is loaded into a porcelain boat, transferred to a muffle furnace, and pre-sintered in an air atmosphere to obtain a precursor powder of a Ti-Cr element co-doped high-pressure spinel positive electrode material; the pre-sintering temperature is 500°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 500°C is 5°C / min, the heating rate from 400°C to 500°C is 2°C / min, the heating end temperature is 500°C, and the sintering time is 5h;
[0115] (5) The precursor powder of the high-pressure spinel positive electrode material obtained in step (4) is ground in an agate grinding mortar and then loaded into a porcelain boat, which is transferred to a muffle furnace for secondary sintering. The sintering atmosphere is air, the secondary sintering temperature is 950°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 850°C is 5°C / min, the heating rate from 850°C to 950°C is 2°C / min, the heating end temperature is 950°C, and the sintering time is 10h; the material obtained after the secondary sintering is ground and passed through a 200-mesh sieve to obtain a Ti-Cr element co-doped high-pressure spinel positive electrode material with a chemical formula of LiNi 0.45 Ti 0.05 Mn 1.45 Cr 0.05 O4;
[0116] The Ti-Cr element co-doped high-voltage spinel cathode material obtained above was assembled into a button cell (CR2035) using the method of making a button half-cell, with a charge and discharge voltage range of 3.2-4.95V. At 0.2C and a test temperature of 30°C, the first cycle discharge capacity was measured to be 116.45mAh / g; at 1C and a test temperature of 60°C, the capacity retention rate was 78.92% after 300 cycles. At different rates of 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C, and 0.1C, and a test temperature of 60°C, the discharge specific capacities were measured to be 114.31mAh / g, 114.24mAh / g, 115.62mAh / g, 114.81mAh / g, 111.27Ah / g, 105.08mAh / g, 94.16mAh / g, and 105.57mAh / g, respectively.
[0117] Example 4
[0118] This embodiment provides a Ti-Cr co-doped high-voltage spinel positive electrode material, and the preparation method thereof includes:
[0119] (1) grinding a lithium source, a nickel source, a manganese source, a titanium source, and a chromium source in a molar ratio of 1:0.45:1.45:0.05:0.05 with an agate grinding mortar, and then adding them to an agate grinding tank filled with anhydrous ethanol to dissolve to obtain a mixed suspension, and then adding 1 wt % of polyvinyl pyrrolidone to the suspension; the amount of anhydrous ethanol added is preferably such that the material is completely immersed;
[0120] (2) ball milling the mixed suspension obtained in step (1) to obtain a slurry; the equipment used for ball milling is a planetary ball mill, the medium is agate beads, the ball-to-material ratio is 90:1, the ball milling speed is 500 r / min, and the ball milling time is 4 hours;
[0121] (3) placing the slurry obtained in step (2) in a blast drying oven and drying to obtain a solid powder; the blast drying oven has an operating temperature of 120° C. and a drying time of 4 hours;
[0122] (4) The solid powder obtained in step (3) is loaded into a porcelain boat, transferred to a muffle furnace, and pre-sintered in an air atmosphere to obtain a precursor powder of a Ti-Cr element co-doped high-pressure spinel positive electrode material; the pre-sintering temperature is 500°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 500°C is 5°C / min, the heating rate from 400°C to 500°C is 2°C / min, the heating end temperature is 550°C, and the sintering time is 5h;
[0123] (5) The precursor powder of the high-pressure spinel positive electrode material obtained in step (4) is ground in an agate grinding mortar and then loaded into a porcelain boat, which is transferred to a muffle furnace for secondary sintering. The sintering atmosphere is air, the secondary sintering temperature is 950°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 850°C is 5°C / min, the heating rate from 850°C to 950°C is 2°C / min, the heating end temperature is 950°C, and the sintering time is 10h; the material obtained after the secondary sintering is ground and passed through a 200-mesh sieve to obtain a Ti-Cr element co-doped high-pressure spinel positive electrode material with a chemical formula of LiNi 0.45 Ti 0.05 Mn 1.45 Cr 0.05 O4;
[0124] The Ti-Cr element co-doped high-voltage spinel cathode material obtained above was assembled into a button cell (CR2035) using the method of making a button half-cell, with a charge and discharge voltage range of 3.2-4.95V. At 0.2C and a test temperature of 30°C, the first cycle discharge capacity was measured to be 118.46mAh / g; at 1C and a test temperature of 60°C, the capacity retention rate was 92.06% after 300 cycles. At different rates of 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C, and 0.1C, and a test temperature of 60°C, the discharge specific capacities were measured to be 116.23mAh / g, 118.24mAh / g, 119.35mAh / g, 117.92mAh / g, 114.72Ah / g, 107.15mAh / g, 97.83mAh / g, and 118.90mAh / g, respectively.
[0125] Example 5
[0126] This embodiment provides a Ti-Cr co-doped high-voltage spinel positive electrode material, and the preparation method thereof includes:
[0127] (1) grinding a lithium source, a nickel source, a manganese source, a titanium source, and a chromium source in a molar ratio of 1:0.45:1.43:0.05:0.07 with an agate grinding mortar, and then adding them to an agate grinding tank filled with anhydrous ethanol to dissolve to obtain a mixed suspension, and then adding 1 wt % of isopropanol to the suspension; the amount of anhydrous ethanol added is preferably such that the material is completely immersed;
[0128] (2) ball milling the mixed suspension obtained in step (1) to obtain a slurry; the equipment used for ball milling is a planetary ball mill, the medium is agate beads, the ball-to-material ratio is 90:1, the ball milling speed is 500 r / min, and the ball milling time is 4 hours;
[0129] (3) placing the slurry obtained in step (2) in a blast drying oven and drying to obtain a solid powder; the blast drying oven has an operating temperature of 120° C. and a drying time of 4 hours;
[0130] (4) The solid powder obtained in step (3) is loaded into a porcelain boat, transferred to a muffle furnace, and pre-sintered in an air atmosphere to obtain a precursor powder of a Ti-Cr element co-doped high-pressure spinel positive electrode material; the pre-sintering temperature is 500°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 500°C is 5°C / min, the heating rate from 400°C to 500°C is 2°C / min, the heating end temperature is 550°C, and the sintering time is 5h;
[0131] (5) The precursor powder of the high-pressure spinel positive electrode material obtained in step (4) is ground in an agate grinding mortar and then loaded into a porcelain boat, which is transferred to a muffle furnace for secondary sintering. The sintering atmosphere is air, the secondary sintering temperature is 950°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 850°C is 5°C / min, the heating rate from 850°C to 950°C is 2°C / min, the heating end temperature is 950°C, and the sintering time is 12h; the material obtained after the secondary sintering is ground and passed through a 200-mesh sieve to obtain a Ti-Cr element co-doped high-pressure spinel positive electrode material with a chemical formula of LiNi 0.45 Ti 0.05 Mn 1.43 Cr 0.07 O4;
[0132] The Ti-Cr element co-doped high-voltage spinel cathode material obtained above was assembled into a button cell (CR2035) using the method of making a button half-cell, with a charge and discharge voltage range of 3.2-4.95V. At 0.2C and a test temperature of 30°C, the first cycle discharge capacity was measured to be 115.91mAh / g; at 1C and a test temperature of 60°C, the capacity retention rate was 70.88% after 300 cycles. At different rates of 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C, and 0.1C, and a test temperature of 60°C, the discharge specific capacities were measured to be 113.74mAh / g, 113.21mAh / g, 112.02mAh / g, 111.57mAh / g, 110.66Ah / g, 102.73mAh / g, 91.24mAh / g, and 104.30mAh / g, respectively.
[0133] Example 6
[0134] This embodiment provides a Ti-Cr co-doped high-voltage spinel positive electrode material, and the preparation method thereof includes:
[0135] (1) a lithium source, a nickel source, a manganese source, a titanium source, and a chromium source are first ground in an agate grinding mortar according to a molar ratio of 1:0.45:1.43:0.05:0.07, and then added to an agate grinding tank filled with anhydrous ethanol to dissolve to obtain a mixed suspension, and then 1 wt % of polyvinyl pyrrolidone is added to the suspension; the amount of anhydrous ethanol added is preferably such that the material is completely immersed;
[0136] (2) ball milling the mixed suspension obtained in step (1) to obtain a slurry; the equipment used for ball milling is a planetary ball mill, the medium is agate beads, the ball-to-material ratio is 90:1, the ball milling speed is 500 r / min, and the ball milling time is 4 hours;
[0137] (3) placing the slurry obtained in step (2) in a blast drying oven and drying to obtain a solid powder; the blast drying oven has an operating temperature of 120° C. and a drying time of 4 hours;
[0138] (4) The solid powder obtained in step (3) is loaded into a porcelain boat, transferred to a muffle furnace, and pre-sintered in an air atmosphere to obtain a precursor powder of a Ti-Cr element co-doped high-pressure spinel positive electrode material; the pre-sintering temperature is 500°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 500°C is 5°C / min, the heating rate from 400°C to 500°C is 2°C / min, the heating end temperature is 550°C, and the sintering time is 5h;
[0139] (5) The precursor powder of the high-pressure spinel positive electrode material obtained in step (4) is ground in an agate grinding mortar and then loaded into a porcelain boat, which is transferred to a muffle furnace for secondary sintering. The sintering atmosphere is air, the secondary sintering temperature is 950°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 850°C is 5°C / min, the heating rate from 850°C to 950°C is 2°C / min, the heating end temperature is 950°C, and the sintering time is 112h; the material obtained after the secondary sintering is ground and passed through a 200-mesh sieve to obtain a Ti-Cr element co-doped high-pressure spinel positive electrode material with a chemical formula of LiNi 0.45 Ti 0.05 Mn 1.43 Cr 0.07 O4;
[0140] The Ti-Cr element co-doped high-voltage spinel cathode material obtained above was assembled into a button cell (CR2035) using the method of making a button half-cell, with a charge and discharge voltage range of 3.2-4.95V. At 0.2C and a test temperature of 30°C, the first cycle discharge capacity was measured to be 114.71mAh / g; at 1C and a test temperature of 60°C, the capacity retention rate was 68.76% after 300 cycles. At different rates of 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C, and 0.1C, and a test temperature of 60°C, the discharge specific capacities were measured to be 113.23mAh / g, 114.02mAh / g, 115.72mAh / g, 113.08mAh / g, 109.42Ah / g, 101.56mAh / g, 88.46mAh / g, and 101.60mAh / g, respectively.
[0141] Comparative Example 1
[0142] According to the method described in Example 1, only LiNi 0.5 Mn 1.5 O4 (undoped) was prepared and the electrochemical performance was tested. At 0.2C and a test temperature of 30°C, the first cycle discharge capacity was measured to be 111.23mAh / g; at 1C and a test temperature of 30°C, the capacity retention rate was 29.87% after 300 cycles. At different rates of 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C, and 0.1C, and a test temperature of 60°C, the discharge specific capacities were measured to be 108.02mAh / g, 112.48mAh / g, 110.63mAh / g, 105.28mAh / g, 98.87mAh / g, 79.56mAh / g, 47.36mAh / g, and 113.72mAh / g, respectively.
[0143] Comparative Example 2
[0144] (1) grinding a lithium source, a nickel source, a manganese source, a titanium source, and a chromium source in a molar ratio of 1:0.45:1.43:0.05:0.07 with an agate grinding mortar and then adding the grinding mortar to an agate grinding tank filled with anhydrous ethanol to dissolve and obtain a mixed suspension;
[0145] (2) ball milling the mixed suspension obtained in step (1) to obtain a slurry; the equipment used for ball milling is a planetary ball mill, the medium is agate beads, the ball-to-material ratio is 90:1, the ball milling speed is 500 r / min, and the ball milling time is 4 hours;
[0146] (3) placing the slurry obtained in step (2) in a blast drying oven and drying to obtain a solid powder; the blast drying oven has an operating temperature of 120° C. and a drying time of 4 hours;
[0147] (4) The solid powder obtained in step (3) is loaded into a porcelain boat, transferred to a muffle furnace, and pre-sintered in an air atmosphere to obtain a precursor powder of a Ti-Cr element co-doped high-pressure spinel positive electrode material; the pre-sintering temperature is 500°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 500°C is 5°C / min, the heating rate from 400°C to 500°C is 2°C / min, the heating end temperature is 550°C, and the sintering time is 5h;
[0148] (5) The precursor powder of the high-pressure spinel positive electrode material obtained in step (4) is ground in an agate grinding mortar and then loaded into a porcelain boat, which is transferred to a muffle furnace for secondary sintering. The sintering atmosphere is air, the secondary sintering temperature is 950°C, the heating rate before 100°C is 2°C / min, the heating rate from 100°C to 850°C is 5°C / min, the heating rate from 850°C to 950°C is 2°C / min, the heating end temperature is 950°C, and the sintering time is 12h; the material obtained after the secondary sintering is ground and passed through a 200-mesh sieve to obtain a Ti-Cr element co-doped high-pressure spinel positive electrode material with a chemical formula of LiNi 0.45 Ti 0.05 Mn 1.47 Cr 0.03 O4;
[0149] The Ti-Cr element co-doped high-voltage spinel cathode material obtained above was assembled into a button cell (CR2035) using the method of making a button half-cell, with a charge and discharge voltage range of 3.2-4.95V. At 0.2C and a test temperature of 30°C, the first cycle discharge capacity was measured to be 114.53mAh / g; at 1C and a test temperature of 60°C, the capacity retention rate was 42.67% after 300 cycles. At different rates of 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C, and 0.1C, and a test temperature of 60°C, the discharge specific capacities were measured to be 112.99mAh / g, 117.77mAh / g, 115.71mAh / g, 113.20mAh / g, 109.58Ah / g, 100.54mAh / g, 86.51mAh / g, and 104.84mAh / g, respectively.
[0150] The first cycle charge and discharge curves of Example 3, Comparative Example 1 and Comparative Example 2 at 30°C and 0.2C are as follows: Figure 1 As shown; Example 3 and Comparative Example 1, Comparative Example 2 at 30 ° C, 1C 300 cycle performance curves as shown Figure 2 The cycle performance curves of Example 3, Comparative Example 1 and Comparative Example 2 at different rates at 60°C are shown as follows: Figure 3 The SEM image of the Ti-Cr element co-doped high-voltage spinel positive electrode material obtained in Example 3 is shown as follows: Figure 4 shown.
[0151] It can be seen from the first cycle charge and discharge curve that the material modified by Ti-Cr element doping and 1wt% isopropanol dispersion treatment has a higher discharge specific capacity. The increase in capacity can be attributed to the widening of the lithium ion diffusion channel after Ti-Cr co-doping and the 1wt% isopropanol reducing the agglomeration of the material during the synthesis process; after 300 cycles of testing, the material modified by Ti-Cr element doping and 1wt% isopropanol dispersion treatment has the highest capacity retention rate. This is because the strong bond energy of Ti-O bonds and Cr-O bonds improves the structural stability of the material. At the same time, the dispersing effect of 1wt% isopropanol also avoids the appearance of large particle agglomeration, thereby improving the material cycle performance; the room temperature rate performance test results also show that the material modified by Ti-Cr element doping and 1wt% isopropanol dispersion treatment has better high-rate discharge performance. After 10C high-rate discharge and then returning to 0.1C discharge, it can still return to the 0.1C starting test discharge capacity, which also shows the excellent reversible performance of the material; the SEM image shows that the synthesized material is a typical spinel polyhedron structure.
[0152] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0153] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for preparing a Ti-Cr co-doped high-voltage spinel positive electrode material, characterized in that: The chemical formula of the Ti-Cr co-doped high-voltage spinel cathode material is LiNi 0.5-x Mn 1.5-y Ti x Cr y O4, where 0.001≤x≤0.06, 0.001≤y≤0.07; The preparation method of the Ti-Cr co-doped high-voltage spinel positive electrode material comprises: Mixing raw materials including a lithium source, a nickel source, a manganese source, a titanium source, a chromium source, a solvent and a dispersant to obtain a slurry; Drying the slurry to obtain a solid powder, and then pre-sintering the solid powder to obtain a precursor; The precursor is subjected to secondary sintering to obtain the Ti-Cr co-doped high-voltage spinel positive electrode material; The lithium source includes one or more of lithium carbonate, lithium acetate, and lithium nitrate; The nickel source includes nickel oxide and / or nickel acetate tetrahydrate; The manganese source includes one or more of manganese oxide, manganese dioxide, and manganese tetraoxide; The titanium source includes titanium monoxide and / or titanium dioxide; The chromium source includes chromium dioxide and / or chromium trioxide; The solvent includes anhydrous ethanol; The dispersant includes isopropanol; the amount of the dispersant is 1wt% of the slurry; The drying temperature is 100-120°C, and the time is 4-5h; the pre-sintering atmosphere is air; the pre-sintering temperature rising program is: the heating rate before 100°C is 1-2°C / min, the heating rate from 100°C to 500°C is 2°C / min, the heating end temperature is 500-550°C, and the sintering time is 5-7h; the secondary sintering temperature rising program is: the heating rate before 100°C is 1-2°C / min, the heating rate from 100°C to 850°C is 2-5°C / min, the heating rate from 850°C to 950°C is 1-2°C / min, the heating end temperature is 900-1000°C, and the sintering time is 10-12h.
2. The method for preparing the Ti-Cr co-doped high-voltage spinel positive electrode material according to claim 1, characterized in that: The mixing further comprises ball milling; The ball-to-material mass ratio of the ball mill is (60-90):1, the rotation speed is 500-650r / min, and the time is 4-5h.
3. The method for preparing the Ti-Cr co-doped high-voltage spinel positive electrode material according to claim 1 or 2, characterized in that: The secondary sintering further includes crushing and separation; The sieve used for the separation is 200 mesh, and the material under the sieve is taken.
Citation Information
Patent Citations
Al-Ti-Mg element co-doped and LATP-coated high-voltage spinel LNMO positive electrode material and preparation method thereof
CN113555544A
Positive electrode active material for nonaqueous electrolyte secondary battery
JP2016181500A