Positive electrode active material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
By adding Sr, Ca, Ba and other elements to the surface of the lithium transition metal composite oxide to form a surface modification layer, the problem of structural instability of the lithium transition metal composite oxide during charge and discharge cycles is solved, and the output power and cycle of the battery are improved. features, extending the battery life.
Patent Information
- Application Number
- CN202080093594.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-27
- Filing Date
- 2020-12-01
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-12-01
AI Technical Summary
The existing lithium transition metal composite oxide cathode active material has an unstable layered structure during charge and discharge cycles, resulting in reduced battery capacity, and the output power and discharge cycle characteristics need to be improved.
A lithium transition metal composite oxide formed by primary particle aggregation is used, and a surface modification layer containing Sr, Ca, and Ba is formed on the surface to stabilize the structure through electronic interaction, inhibit reaction with the electrolyte, and improve output power and cycle characteristics.
The charge-discharge cycle characteristics and output power of lithium-ion secondary batteries are significantly improved, the service life of the battery is extended, and the reduction of battery capacity is reduced.
Smart Images

Figure CN114982013B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a positive electrode active material for a nonaqueous electrolyte secondary battery and a nonaqueous electrolyte secondary battery. Background Art
[0002] In recent years, as a high-output, high-capacity secondary battery, a nonaqueous electrolyte secondary battery having a positive electrode, a negative electrode, and a nonaqueous electrolyte, which allows lithium ions to move between the positive electrode and the negative electrode for charge and discharge, has been widely used. From the perspectives of low resistance and high capacity of the battery, it is required to improve the characteristics of the positive electrode active material contained in the positive electrode of the battery.
[0003] For example, Patent Document 1 discloses, as a positive electrode active material for high-output applications, an NCA-based (nickel-cobalt-aluminum-based) positive electrode active material having a layered structure and containing a trace amount of alkaline earth metal in a solid solution.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 5245210 Summary of the invention
[0007] For the lithium transition metal composite oxide contained in the positive electrode active material, in order to obtain a high discharge capacity, a design of increasing the Ni content is considered. However, when the ratio of Ni to the total molar number of metal elements other than Li is 80 mol% or more, the layered structure of the lithium transition metal composite oxide becomes unstable, and the battery capacity may decrease with the charge and discharge cycle. The technology of Patent Document 1 does not take into account the reduction in battery capacity associated with the charge and discharge cycle, and there is still room for improvement.
[0008] A positive electrode active material for a non-aqueous electrolyte secondary battery as one embodiment of the present invention is characterized in that it comprises: a lithium transition metal composite oxide having secondary particles formed by aggregation of primary particles, and a surface modification layer formed on the surface of the primary particles of the lithium transition metal composite oxide, wherein the lithium transition metal composite oxide contains at least Al and 80 mol % or more of Ni relative to the total molar number of metal elements other than Li, and the surface modification layer contains at least any one of Sr and Ca, and Ba.
[0009] A nonaqueous electrolyte secondary battery as one embodiment of the present disclosure is characterized by comprising a positive electrode containing the positive electrode active material for a nonaqueous electrolyte secondary battery, a negative electrode, and a nonaqueous electrolyte.
[0010] According to the positive electrode active material for a nonaqueous electrolyte secondary battery as one embodiment of the present disclosure, a nonaqueous electrolyte secondary battery having high output and improved charge and discharge cycle characteristics can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of an embodiment. DETAILED DESCRIPTION
[0012] The layered structure of the lithium transition metal composite oxide contains transition metal layers such as Ni, Li layers, and oxygen layers, and the Li ions present in the Li layer reversibly enter and exit, thereby performing the charge and discharge reaction of the battery. Here, in the lithium transition metal composite oxide contained in the positive electrode active material, when the ratio of Ni is 80 mol% or more relative to the total molar number of metal elements other than Li, a lot of Li ions are taken away by the Li layer during the charging of the battery, so the layered structure is likely to become unstable. On the surface of the lithium transition metal composite oxide where the layered structure becomes unstable, a metamorphic layer is formed due to the reaction with the electrolyte. The structural changes of the lithium transition metal composite oxide are further carried out with the metamorphic layer as the starting point, so the battery capacity gradually decreases with charging and discharging. However, as a positive electrode active material for a non-aqueous electrolyte secondary battery in one mode of the present invention, by containing a specified amount of Sr and Ca in the surface modification layer formed on the surface of the lithium transition metal composite oxide, the reaction with the electrolyte in the surface is suppressed by utilizing the synergistic effect with Al, and the surface structure is stabilized, so that the battery capacity reduction accompanying the charge and discharge cycle can be suppressed. Since Al does not change its oxidation number even during charge and discharge, it is speculated that the structure of the transition metal layer is stabilized by being contained in the transition metal layer. It is speculated that Sr and Ca provide changes to the surface state of the lithium transition metal composite oxide through the interaction of electrons. In addition, by also containing Ba whose electronegativity is lower than that of Sr and Ca in the surface modification layer, in addition to the discharge cycle characteristics, the output power characteristics are also improved.
[0013] An example of an embodiment of the non-aqueous electrolyte secondary battery disclosed in the present invention is described in detail below. The following example shows a cylindrical battery in which a wound electrode body is contained in a cylindrical battery case, but the electrode body is not limited to a wound type, and may also be a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked by separators. In addition, the battery case is not limited to a cylindrical shape, and may be, for example, a square, a coin shape, etc., or may be a battery case composed of a laminated sheet including a metal layer and a resin layer.
[0014] Figure 1 FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery 10 as an example of an embodiment. Figure 1As shown in the example, the nonaqueous electrolyte secondary battery 10 includes an electrode body 14, a nonaqueous electrolyte (not shown), and a battery case 15 that accommodates the electrode body 14 and the nonaqueous electrolyte. The electrode body 14 has a winding structure in which a positive electrode 11 and a negative electrode 12 are wound via a separator 13. The battery case 15 is composed of an outer can 16 in a bottomed cylindrical shape and a sealing body 17 that blocks the opening of the outer can 16.
[0015] The electrode body 14 is composed of a long positive electrode 11, a long negative electrode 12, two long separators 13, a positive electrode tab 20 joined to the positive electrode 11, and a negative electrode tab 21 joined to the negative electrode 12. The negative electrode 12 is formed to be one size larger than the positive electrode 11 in order to prevent lithium precipitation. That is, the negative electrode 12 is formed longer in the length direction and the width direction (short side direction) than the positive electrode 11. The two separators 13 are formed to be at least one size larger than the positive electrode 11, and are arranged, for example, in a manner of sandwiching the positive electrode 11.
[0016] The nonaqueous electrolyte secondary battery 10 includes insulating plates 18 and 19 disposed above and below the electrode body 14 , respectively. Figure 1 In the example shown, the positive electrode tab 20 mounted on the positive electrode 11 extends to the sealing body 17 side through the through hole of the insulating plate 18, and the negative electrode tab 21 mounted on the negative electrode 12 extends to the bottom side of the outer can 16 through the outside of the insulating plate 19. The positive electrode tab 20 is connected to the lower surface of the bottom plate 23 of the sealing body 17 by welding or the like, and the lid 27 of the sealing body 17 electrically connected to the bottom plate 23 forms a positive terminal. The negative electrode tab 21 is connected to the bottom inner surface of the outer can 16 by welding or the like, and the outer can 16 forms a negative terminal.
[0017] The outer can 16 is, for example, a metal container in a bottomed cylindrical shape. A gasket 28 is provided between the outer can 16 and the sealing body 17 to seal the internal space of the battery case 15. The outer can 16 has, for example, a groove 22 formed by applying pressure to the side surface from the outside to support the sealing body 17. The groove 22 is preferably formed in an annular shape along the circumferential direction of the outer can 16, and supports the sealing body 17 on its upper surface.
[0018] The sealing body 17 has a structure in which a bottom plate 23, a lower valve core 24, an insulating member 25, an upper valve core 26, and a cover 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve core 24 and the upper valve core 26 are connected to each other at their respective central portions, and the insulating member 25 is sandwiched between their respective peripheral portions. If the internal pressure of the battery increases due to abnormal heat generation, the lower valve core 24 is deformed and broken in a manner that pushes the upper valve core 26 to the cover 27 side, and the current path between the lower valve core 24 and the upper valve core 26 is blocked. Furthermore, if the internal pressure increases, the upper valve core 26 breaks, and gas is discharged from the opening of the cover 27.
[0019] The positive electrode 11 , the negative electrode 12 , the separator 13 , and the nonaqueous electrolyte constituting the nonaqueous electrolyte secondary battery 10 , particularly the positive electrode active material contained in the positive electrode active material layer 31 constituting the positive electrode 11 , will be described in detail below.
[0020] [positive electrode]
[0021] The positive electrode 11 has a positive electrode collector 30 and a positive electrode active material layer 31 formed on both sides of the positive electrode collector 30. The positive electrode collector 30 can be made of a foil of a metal such as aluminum or aluminum alloy that is stable in the potential range of the positive electrode 11, a thin film of the metal disposed on the surface, etc. The positive electrode active material layer 31 contains a positive electrode active material, a conductive material, and a binding material. The thickness of the positive electrode active material layer 31 is, for example, 10 μm to 150 μm on one side of the positive electrode collector 30. The positive electrode 11 can be made as follows: a positive electrode slurry containing a positive electrode active material, a conductive material, and a binding material is applied to the surface of the positive electrode collector 30, and after the coating is dried, the positive electrode active material layer 31 is formed on both sides of the positive electrode collector 30 by compression, thereby making the positive electrode 11.
[0022] As the conductive material contained in the positive electrode active material layer 31, carbon materials such as carbon black, acetylene black, Ketjen black, and graphite can be exemplified. As the binding material contained in the positive electrode active material layer 31, fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, etc. can be exemplified. These resins can be used in combination with carboxymethylcellulose (CMC) or its salt, polyethylene oxide (PEO), etc.
[0023] The positive electrode active material contained in the positive electrode active material layer 31 includes: a lithium transition metal composite oxide having secondary particles formed by aggregation of primary particles, and a surface modification layer formed on the surface of the primary particles of the lithium transition metal composite oxide. This can inhibit the reaction with the electrolyte. Here, the surface modification layer is formed on the surface of the primary particle means that the surface modification layer exists on the surface of the secondary particle, or at the interface where the primary particles are in contact with each other.
[0024] The secondary particles of the lithium transition metal composite oxide are preferably 3 μm to 30 μm, more preferably 5 μm to 25 μm, and particularly preferably 7 μm to 15 μm particles based on volume. D50 refers to the particle size at which the cumulative frequency from the smaller particle size is 50% in the volume-based particle size distribution, also known as the median diameter. The particle size distribution of the secondary particles of the lithium transition metal composite oxide can be measured using a laser diffraction particle size distribution measuring device (e.g., MT3000II manufactured by MicrotracBEL Corp.) using water as a dispersion medium.
[0025] The particle size of the primary particles constituting the secondary particles is, for example, 0.05 μm to 1 μm. The particle size of the primary particles is measured as the diameter of the circumscribed circle in the particle image observed by a scanning electron microscope (SEM).
[0026] The lithium transition metal composite oxide may have, for example, a layered structure belonging to the space group R-3m, a layered structure belonging to the space group C2 / m, etc. Among them, from the viewpoints of high capacity and stability of the crystal structure, etc., a layered structure belonging to the space group R-3m is preferred. The layered structure of the lithium transition metal composite oxide includes a transition metal layer, a Li layer, and an oxygen layer.
[0027] The lithium transition metal composite oxide contains at least Al and 80 mol% or more of Ni relative to the total molar amount of metal elements other than Li. By having the ratio of Ni relative to the total molar amount of metal elements other than Li in the lithium transition metal composite oxide be 80 mol% or more, a battery with high capacity can be obtained.
[0028] The ratio of Ni relative to the total molar amount of metal elements other than Li in the lithium transition metal composite oxide is preferably 90 mol% or more. Thereby, a battery with higher capacity can be obtained.
[0029] The lithium transition metal composite oxide may form a composite oxide represented by the general formula Li a Ni x Al y Co z M w O 2-b (wherein, 0.95 < a < 1.05, 0.8 ≤ x ≤ 0.96, 0 < y ≤ 0.10, 0 ≤ z ≤ 0.15, 0 ≤ w ≤ 0.1, 0 ≤ b < 0.05, x + y + z + w = 1, and M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo, and Zn). It should be noted that in the positive electrode active material, a lithium transition metal composite oxide or other compound other than that represented by the above general formula may be contained within the range that does not impair the object of the present disclosure. The molar fraction of the metal elements contained in all the particles of the lithium transition metal composite oxide is measured by inductively coupled plasma (ICP) emission spectrometry.
[0030] a representing the ratio of Li in the lithium transition metal composite oxide preferably satisfies 0.95 ≤ a < 1.05, and more preferably satisfies 0.97 ≤ a ≤ 1.03. When a is less than 0.95, the battery capacity may decrease compared with the case where a satisfies the above range. When a is 1.05 or more, the charge-discharge cycle characteristics may deteriorate compared with the case where a satisfies the above range.
[0031] The y representing the ratio of Al to the total molar amount of metal elements other than Li in the lithium transition metal composite oxide preferably satisfies 0 < y ≤ 0.10, more preferably 0.03 ≤ y ≤ 0.07. Since Al does not cause a change in oxidation number even during charge and discharge, it is considered that the structure of the transition metal layer is stabilized by being contained in the transition metal layer. On the other hand, when y exceeds 0.10, Al impurities are generated and the battery capacity may decrease. In addition, when y is 0.07 or less, the layered structure of the lithium transition metal composite oxide tends to become unstable, and thus the effect of structure stabilization caused by containing any one of Sr and Ca is significant. Al can be uniformly dispersed in the layered structure of the lithium transition metal composite oxide, for example, or can be present in a part of the layered structure.
[0032] Co and M (M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo, and Zn) are optional components. The z and w representing the ratios of Co and M to the total molar amount of metal elements other than Li in the lithium transition metal composite oxide preferably satisfy 0 ≤ z ≤ 0.15 and 0 ≤ w ≤ 0.1, respectively. Since Co is expensive, it is preferable to suppress the Co content from the viewpoint of manufacturing cost.
[0033] The surface modification layer contains at least any one of Sr and Ca, and Ba. The surface modification layer can contain Sr or a compound containing Sr, or Ca or a compound containing Ca, for example. As the compound containing Sr, SrO can be exemplified. As the compound containing Ca, CaO can be exemplified. In addition, the surface modification layer can contain Ba or a compound containing Ba, for example. As the compound containing Ba, BaO can be exemplified.
[0034] The surface modification layer can further contain Al. The Al contained in the surface modification layer can be Al or a compound containing Al, for example. As the compound containing Al, Al2O3 can be exemplified. In addition, as the compound containing Al, it can be a compound containing Al and Sr, Ca, Ba, and SrAlO4, CaAlO4, BaAlO4 can be exemplified. The surface modification layer can further contain Li.
[0035] The ratios of Sr and Ca in the surface modification layer can be set to 0.05 mol% to 0.25 mol% relative to the total molar amount of metal elements other than Li in the lithium transition metal composite oxide. If it is within this range, the surface state of the lithium transition metal composite oxide can be changed by the interaction of electrons.
[0036] The ratio of Ba in the surface modification layer can be set to 0.000001 mol% to 0.00001 mol% in the lithium transition metal composite oxide, for example. If it is within this range, the reaction resistance of the battery can be reduced, and the output power characteristics can be improved. It should be noted that for this degree of Ba, although the presence can be confirmed by ICP, it may not be possible to quantitatively measure the content due to the trace amount.
[0037] The thickness of the surface modification layer is, for example, 0.1 nm to 2 nm. Within this range, the reaction between the surface of the lithium transition metal composite oxide and the electrolyte can be suppressed.
[0038] The content of the lithium transition metal composite oxide in the positive electrode active material is preferably 90 mass % or more, more preferably 99 mass % or more, relative to the total mass of the positive electrode active material, from the viewpoint of improving the capacity of the battery and effectively suppressing the reduction in charge and discharge cycle characteristics.
[0039] In addition, the positive electrode active material of this embodiment may contain other lithium transition metal composite oxides in addition to the lithium transition metal composite oxide of this embodiment. As other lithium transition metal composite oxides, for example, lithium transition metal composite oxides having a Ni content of 0 mol% or more and less than 85 mol% may be listed.
[0040] Next, an example of a method for producing a positive electrode active material including a lithium transition metal composite oxide and a surface modification layer will be described.
[0041] The method for producing a positive electrode active material comprises, for example, a first step of obtaining a composite oxide containing Ni, Al and an arbitrary metal element; a second step of mixing the composite oxide obtained in the first step with a Li compound and the like to obtain a mixture; and a third step of calcining the mixture. Parameters such as the composition of the surface modification layer in the finally obtained positive electrode active material are adjusted by, for example, controlling the mixing ratio of the raw materials in the second step, the calcination temperature and time in the third step, and the like.
[0042] In the first step, for example, a solution of a metal salt containing Ni, Al and any metal element (Co, Mn, Fe, etc.) is stirred while an alkaline solution such as sodium hydroxide is added dropwise to adjust the pH to the alkaline side (e.g., 8.5 to 12.5), thereby precipitating (coprecipitating) a composite hydroxide containing Ni, Al and any metal element, and calcining the composite hydroxide to obtain a composite oxide containing Ni, Al and any metal element. The calcination temperature is not particularly limited, and is, for example, in the range of 300° C. to 600° C.
[0043] In the second step, the composite oxide, Li compound, Sr compound or Ca compound obtained in the first step and the Ba compound are mixed to obtain a mixture. Examples of the Li compound include Li2CO3, LiOH, Li2O2, Li2O, LiNO3, LiNO2, Li2SO4, LiOH·H2O, LiH, LiF, etc. Examples of the Sr compound include Sr(OH)2, Sr(OH)2·8H2O, SrO, SrCo3, SrSO4, Sr(NO3)2, etc. Examples of the Ca compound include Ca(OH)2, CaO, CaCO3, CaSO4, Ca(NO3)2, etc. Examples of the Ba compound include Ba(OH)2·H2O, BaO, BaCO3, BaSO4, etc. For the mixing ratio of the composite oxide obtained in the first step and the Li compound, from the viewpoint of facilitating the adjustment of the above parameters within the above-specified range, for example, the molar ratio of the metal element other than Li: Li is preferably in the range of 1:0.98 to 1:1.1. In addition, for the mixing ratio of the composite oxide obtained in the first step and at least one of the Sr compound and the Ca compound, from the viewpoint of facilitating the adjustment of the above parameters within the above-specified range, for example, the molar ratio of the metal element other than Li: (Sr+Ca) is preferably in the range of 1:0.0005 to 1:0.0025. In addition, for the mixing ratio of the composite oxide obtained in the first step and the Ba compound, from the viewpoint of facilitating the adjustment of the above parameters within the above-specified range, for example, the molar ratio of the metal element other than Li: Ba is preferably in the range of 1:0.000001 to 1:0.00001. In the second step, when the composite oxide, Li compound, Sr compound or Ca compound, and Ba compound obtained in the first step are mixed, other metal raw materials may be added as needed. Other metal raw materials are oxides containing metal elements other than the metal elements constituting the composite oxide obtained in the first step.
[0044] In the third step, the mixture obtained in the second step is roasted at a specified temperature and time to obtain the positive electrode active material of the present embodiment. The roasting of the mixture in the third step, for example, has a multi-stage roasting step, which includes: a first roasting step of roasting at a first temperature rise rate in a roasting furnace under an oxygen flow until a first set temperature of 450°C or more and 680°C or less; and a second roasting step of roasting the roasted product obtained by the first roasting step in a roasting furnace under an oxygen flow until a second set temperature of more than 680°C and less than 800°C is roasted at a second temperature rise rate. Here, the first temperature rise rate is within the range of 1.5°C / min to 5.5°C / min, and the second temperature rise rate is slower than the first temperature rise rate and is within the range of 0.1°C / min to 3.5°C / min. Through this multi-stage roasting, in the positive electrode active material of the present embodiment finally obtained, the parameters such as the composition of the surface modification layer can be adjusted to the above-mentioned specified range. It should be noted that if the first heating rate and the second heating rate are within the above-specified range, multiple settings can be made in each temperature range. From the viewpoint of adjusting the above-mentioned parameters of the lithium transition metal composite oxide within the above-specified range, the holding time of the first set temperature in the first roasting process is preferably 0 hours or more and 5 hours or less, more preferably 0 hours or more and 3 hours or less. The holding time of the first set temperature refers to the time for maintaining the first set temperature after reaching the first set temperature. From the viewpoint of adjusting the above-mentioned parameters of the lithium transition metal composite oxide within the above-specified range, the holding time of the second set temperature in the second roasting process is preferably 1 hour or more and 10 hours or less, more preferably 1 hour or more and 5 hours or less. The holding time of the second set temperature refers to the time for maintaining the second set temperature after reaching the second set temperature. When roasting the mixture, from the viewpoint of adjusting the above-mentioned parameters within the above-specified range, for example, it is carried out in an oxygen flow with an oxygen concentration of 60% or more, and the flow rate of the oxygen flow is 10 cm 3 The calcination rate in the calcining furnace can be set in the range of 0.2 mL / min to 4 mL / min and at least 0.3 L / min per 1 kg of the mixture.
[0045] The method for manufacturing a positive electrode active material may include a washing step of washing the positive electrode active material with water after the third step. Thereby, unreacted components such as Li compounds and impurities in the positive electrode active material obtained in the third step can be removed. The washing step includes, for example, mixing the positive electrode active material with water so that the slurry concentration is in the range of 500 g / L to 2000 g / L, stirring for 3 minutes to 1 hour, and then filtering. In addition, a W compound or a solution containing W may be added to the positive electrode active material after the washing step. Thereby, the generation and erosion of the structural deterioration layer on the surface of the lithium transition metal composite oxide due to the reaction with the electrolyte solution, etc. can be further suppressed, and the charge-discharge cycle characteristics can be improved. Li compounds remain in the positive electrode active material after the washing step, and the remaining Li compounds dissolve in the water contained in the positive electrode active material to form an alkaline aqueous solution. When a W compound is added to the positive electrode active material, the W compound dissolves in the alkaline aqueous solution and spreads to the entire surface of the positive electrode active material. Examples of the W compound include tungsten oxide (WO3), lithium tungstate (Li2WO4, Li4WO5, Li6W2O9), etc. The amount of W added may be 0.5 mol% or less, preferably 0.3 mol% or less, relative to the total molar number of metal elements other than Li in the positive electrode active material. In addition, when a solution containing W is added to the positive electrode active material, the W concentration in the solution containing W is, for example, 0.05 mol / L or more, preferably 0.1 mol / L to 1 mol / L. The solution containing W is not particularly limited as long as it contains W, and a solution obtained by dissolving a W compound easily soluble in an alkaline solution such as tungsten oxide, lithium tungstate, or ammonium tungstate in an aqueous solution of lithium hydroxide is preferably used.
[0046] The molar fractions of the metal elements contained in the above-obtained positive electrode active material are measured by inductively coupled plasma (ICP) emission spectrometry, and can be represented by the general formula Li a Ni x Al y Co z M1 w M2 α Ba β O 2-b (where 0.95 < a < 1.05, 0.8 ≤ x ≤ 0.96, 0 < y ≤ 0.10, 0 ≤ z ≤ 0.15, 0 ≤ w ≤ 0.1, 0.05 ≤ α ≤ 0.25, 0.0001 ≤ β ≤ 0.001, 0 ≤ b < 0.05, x + y + z + w = 1, M1 is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo, and Zn, and M2 is at least one element selected from Sr and Ca). It should be noted that Sr is not dissolved in the lithium transition metal composite oxide but is contained in the surface modification layer existing on the surface of the lithium transition metal composite oxide. In addition, a part of Al may be contained in the surface modification layer.
[0047] [Negative electrode]
[0048] The negative electrode 12 has a negative electrode current collector 40 and negative electrode active material layers 41 formed on both surfaces of the negative electrode current collector 40. As the negative electrode current collector 40, foils of metals such as copper and copper alloys that are stable in the potential range of the negative electrode 12, thin films with such metals disposed on the surface layer, etc. can be used. The negative electrode active material layer 41 contains a negative electrode active material and a binder material. The thickness of the negative electrode active material layer 41 is, for example, 10 μm to 150 μm on one side of the negative electrode current collector 40. The negative electrode 12 can be manufactured as follows: a negative electrode paste containing a negative electrode active material, a binder material, etc. is coated on the surface of the negative electrode current collector 40, and after drying the coating film, it is rolled to form the negative electrode active material layer 41 on both surfaces of the negative electrode current collector 40, thereby manufacturing the negative electrode 12.
[0049] As the negative electrode active material contained in the negative electrode active material layer 41, there is no particular limitation as long as it can reversibly occlude and release lithium ions, and generally carbon materials such as graphite are used. The graphite can be any of natural graphite such as flake graphite, massive graphite, and earthy graphite, massive artificial graphite, graphitized mesophase carbon microbeads, etc. artificial graphite. In addition, as the negative electrode active material, metals alloyed with Li such as Si and Sn, metal compounds containing Si, Sn, etc., lithium titanium composite oxides, etc. can be used. In addition, a negative electrode active material provided with a carbon coating film thereon can also be used. For example, a compound containing Si represented by SiO x (0.5 ≤ x ≤ 1.6), or a compound containing Si in which fine particles of Si are dispersed in a lithium silicate phase represented by Li 2y SiO (2+y) (0 < y < 2) can be used in combination with graphite.
[0050] The binder material contained in the negative electrode active material layer 41 can be a fluororesin such as PTFE and PVdF, PAN, polyimide, acrylic resin, polyolefin, etc., in the same manner as in the case of the positive electrode 11, and styrene-butadiene rubber (SBR) is preferably used. In addition, CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc. can be contained in the negative electrode active material layer 41.
[0051] [Separator]
[0052] The separator 13 uses, for example, a porous sheet having ion permeability and insulation. As a specific example of the porous sheet, a microporous film, a woven fabric, a nonwoven fabric, etc. can be cited. As the material of the separator, polyolefins such as polyethylene and polypropylene, cellulose, etc. are preferred. The separator 13 can be a single-layer structure or have a laminated structure. In addition, a resin layer with high heat resistance such as an aromatic polyamide resin, a filler layer containing a filler of an inorganic compound, etc. can be provided on the surface of the separator 13.
[0053] [Non-aqueous electrolyte]
[0054] The non-aqueous electrolyte contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. As the non-aqueous solvent, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and a mixed solvent of two or more thereof can be used, for example. The non-aqueous solvent may contain a halogenated product obtained by substituting at least a part of the hydrogen of these solvents with a halogen atom such as fluorine. Examples of the halogenated product include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated linear carbonates, and fluorinated linear carboxylates such as methyl fluoropropionate (FMP).
[0055] Examples of the above esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate; linear carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate; cyclic carboxylates such as γ-butyrolactone (GBL), γ-valerolactone (GVL); and linear carboxylates such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), ethyl propionate (EP).
[0056] Examples of the above ethers include cyclic ethers such as 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-epoxybutane, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, crown ether; and linear ethers such as 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether.
[0057] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1 < x < 6, n is 1 or 2), LiB 10 Cl10 , LiCl, LiBr, LiI, lithium chloroborane, lithium lower aliphatic carboxylate, Li2B4O7, Li(B(C2O4)F2) and other borates, LiN(SO2CF3)2, LiN(C1F 2l+1 SO2)(C m F 2m+1 SO2) {l, m is an integer greater than 0} and other imide salts. The lithium salt can be used alone or in combination. Among them, LiPF6 is preferably used from the viewpoints of ion conductivity, electrochemical stability, etc. The concentration of the lithium salt is, for example, 0.8 mol to 1.8 mol relative to 1L of the non-aqueous solvent. In addition, vinylene carbonate and propane sultone additives can also be added.
[0058] <Example>
[0059] The present disclosure will be further described below by way of examples and comparative examples, but the present disclosure is not limited to the following examples.
[0060] [Preparation of positive electrode active material]
[0061] <Example 1>
[0062] The [Ni 0.82 Al 0.05 Co 0.13 The composite hydroxide represented by ](OH)2 was calcined at 500°C for 8 hours to obtain a composite oxide (Ni 0.82 Al 0.05 Co 0.13 Next, LiOH, the composite oxide, Sr(OH)2, and Ba(OH)2 were mixed in such a manner that the molar ratio of the total amount of Li, Ni, Al, and Co, and Sr, and Ba was 1.03:1:0.0005:0.000001 to obtain a mixture. The mixture was heated under an oxygen flow with an oxygen concentration of 95% (per 10 cm 3 The mixture was heated at a rate of 2.0°C / min from room temperature to 650°C, and then calcined at a rate of 0.5°C / min from 650°C to 780°C. Water was added to the calcined product so that the slurry concentration became 1500g / L, stirred for 15 minutes, and then filtered to obtain a positive electrode active material. Furthermore, an ICP emission spectrometer (manufactured by Thermo Fisher Scientific, trade name "iCAP6300") was used to determine the composition of the positive electrode active material obtained above, and the composition was LiNi 0.82 Al 0.05 Co 0.13 Sr0.0005 Ba β O2. This was used as the positive electrode active material of Example 1. Here, it can be confirmed that Ba is contained in the positive electrode active material, but the content β of Ba is too small to be quantified. It is estimated from the added amount that β is about 0.000001.
[0063] [Production of positive electrode]
[0064] The positive electrode active material of Example 1 is mixed at a ratio of 91 parts by mass, 7 parts by mass of acetylene black as a conductive material, and 2 parts by mass of polyvinylidene fluoride as a binder, and mixed with N-methyl-2-pyrrolidone (NMP) to produce a positive electrode slurry. The slurry is then applied to a positive electrode collector formed of an aluminum foil having a thickness of 15 μm, and after the coating is dried, the coating is rolled by a calendering roller and cut into a specified electrode size to obtain a positive electrode having a positive electrode active material layer formed on both sides of the positive electrode core. It should be noted that an exposed portion exposed on the surface of the positive electrode core is provided on a portion of the positive electrode.
[0065] [Production of negative electrode]
[0066] As the negative electrode active material, natural graphite is used. The negative electrode active material, sodium carboxymethyl cellulose (CMC-Na), and styrene-butadiene rubber (SBR) are mixed in an aqueous solution at a solid content mass ratio of 100:1:1 to produce a negative electrode slurry. The negative electrode slurry is applied to both sides of a negative electrode core formed of copper foil, and after the coating is dried, the coating is rolled by a calendering roller and cut into a specified electrode size to obtain a negative electrode having a negative electrode active material layer formed on both sides of the negative electrode core. It should be noted that an exposed portion exposed on the surface of the negative electrode core is provided on a portion of the negative electrode.
[0067] [Manufacturing of non-aqueous electrolyte]
[0068] Ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed at a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF6) was dissolved in the mixed solvent to a concentration of 1.2 mol / L, thereby producing a non-aqueous electrolyte.
[0069] [Production of test battery cells]
[0070] An aluminum lead was installed on the exposed portion of the positive electrode containing the positive electrode active material of Example 1, and a nickel lead was installed on the exposed portion of the negative electrode. The positive electrode and the negative electrode were spirally wound with a polyolefin separator, and then pressed in the radial direction to produce a flat wound electrode body. The electrode body was housed in an outer casing, and after the non-aqueous electrolyte was injected, the opening of the outer casing was sealed to obtain a test battery cell.
[0071] [Measurement of reaction resistance]
[0072] For the above test battery cell, a constant current charge of 0.7 mA was performed under a temperature condition of 25°C until the battery cell voltage became 4.3V, and then a constant voltage charge of 4.3V was performed until the current value became 0.07 mA. Then, a constant current discharge of 0.7 mA was performed until the battery cell voltage became 2.5V. Then, a constant current charge of 0.7 mA was performed again under a temperature condition of 25°C until the battery cell voltage became 4.3V, and then a constant voltage charge of 4.3V was performed until the current value became 0.07 mA. Then, the AC impedance of the test battery cell at 20kHz to 0.01Hz was measured using an AC impedance meter, and a Cole-Cole plot was drawn from the measured data, and the reaction resistance was calculated from the size of the arc between 10Hz and 0.1Hz. It should be noted that the reaction resistance shown in Table 1 is a value that relatively represents the reaction resistance of other test battery cells, with the reaction resistance of the test battery cell containing the positive electrode active material of Comparative Example 1 as 100.
[0073] [Evaluation of capacity maintenance rate]
[0074] The test cell was subjected to the following cycle test. The discharge capacity at the first cycle and the discharge capacity at the 100th cycle of the cycle test were obtained, and the capacity retention rate was calculated by the following formula.
[0075] Capacity retention rate (%) = (100th cycle discharge capacity ÷ 1st cycle discharge capacity) × 100
[0076] <Cycle test>
[0077] The test battery cell was charged at a constant current of 0.5 It until the battery voltage reached 4.2 V under a temperature environment of 45°C, and then charged at a constant voltage of 4.2 V until the current value reached 1 / 50 It. Then, the constant current was discharged at a constant current of 0.5 It until the battery voltage reached 2.5 V. This charge and discharge cycle was repeated 100 times.
[0078] <Comparative Example 1>
[0079] A positive electrode active material was obtained in the same manner as in Example 1 except that Sr(OH) 2 and Ba(OH) 2 were not added in the step of obtaining the mixture (second step).
[0080] <Comparative Example 2>
[0081] A positive electrode active material was obtained in the same manner as in Example 1 except that Sr(OH) 2 was not added in the step of obtaining the mixture (second step).
[0082] <Comparative Example 3>
[0083] A positive electrode active material was obtained in the same manner as in Example 1 except that Ba(OH) 2 was not added in the step of obtaining the mixture (second step).
[0084] <Example 2>
[0085] Use [Ni 0.88 Al 0.03 Co 0.09 ](OH)2 gives a composite hydroxide (Ni 0.88 Al 0.03 Co 0.09 O2), LiOH, the composite oxide, Sr(OH)2, and Ba(OH)2 were mixed in a manner such that the total amount of Li, Ni, Al, and Co, and the molar ratio of Sr and Ba were 1.03:1:0.001:0.000002 to obtain a mixture, and the positive electrode active material was obtained in the same manner as in Example 1. The composition of the obtained positive electrode active material is LiNi 0.88 Al 0.03 Co 0.09 Sr 0.001 Ba β O2. This was used as the positive electrode active material of Example 2. As in Example 1, it was confirmed that Ba was contained in the positive electrode active material, but the content β of Ba was too small to be quantified. Based on the added amount, β was estimated to be about 0.000002.
[0086] <Example 3>
[0087] A positive electrode active material was obtained in the same manner as in Example 2 except that Ca(OH) 2 was added in place of Sr(OH) 2 in the step of obtaining the mixture (second step).
[0088] <Comparative Example 4>
[0089] A positive electrode active material was obtained in the same manner as in Example 2 except that Sr(OH) 2 and Ba(OH) 2 were not added in the step of obtaining the mixture (second step).
[0090] <Comparative Example 5>
[0091] A positive electrode active material was obtained in the same manner as in Example 2 except that Sr(OH) 2 was not added in the step of obtaining the mixture (second step).
[0092] <Comparative Example 6>
[0093] A positive electrode active material was obtained in the same manner as in Example 2 except that Ba(OH) 2 was not added in the step of obtaining the mixture (second step).
[0094] <Comparative Example 7>
[0095] A positive electrode active material was obtained in the same manner as in Example 2 except that Ca(OH) 2 was added instead of Sr(OH) 2 in the step of obtaining the mixture (second step) and Ba(OH) 2 was not added.
[0096] <Example 4>
[0097] Use [Ni 0.91 Al 0.04 Co 0.05 ](OH)2 gives a composite hydroxide (Ni 0.91 Al 0.04 Co 0.05 O2), LiOH, the composite oxide, Sr(OH)2, and Ba(OH)2 were mixed in a manner such that the total amount of Li, Ni, Al, and Co, and the molar ratio of Sr and Ba were 1.03:1:0.0007:0.000004 to obtain a mixture, and the positive electrode active material was obtained in the same manner as in Example 1. The composition of the obtained positive electrode active material is LiNi 0.91 Al 0.04 Co 0.05 Sr 0.0007 Ba β O2. This was used as the positive electrode active material of Example 4. As in Example 1, it was confirmed that Ba was contained in the positive electrode active material, but the content β of Ba was too small to be quantified. Based on the added amount, β was estimated to be about 0.000004.
[0098] <Example 5>
[0099] In the step of obtaining a mixture (the second step), LiOH and a composite oxide (Ni 0.91 Al 0.04 Co 0.05 O2), Sr(OH)2, and Ba(OH)2 are mixed in a manner such that the total amount of Li, Ni, Al, and Co, and the molar ratio of Sr and Ba become 1.03:1:0.0015:0.000009 to obtain a mixture, and the positive electrode active material is obtained in the same manner as in Example 4 except that
[0100] <Comparative Example 8>
[0101] A positive electrode active material was obtained in the same manner as in Example 4 except that Sr(OH) 2 and Ba(OH) 2 were not added in the step of obtaining the mixture (second step).
[0102] <Comparative Example 9>
[0103] A positive electrode active material was obtained in the same manner as in Example 4 except that Sr(OH) 2 was not added in the step of obtaining the mixture (second step).
[0104] <Comparative Example 10>
[0105] A positive electrode active material was obtained in the same manner as in Example 4 except that Ba(OH) 2 was not added in the step of obtaining the mixture (second step).
[0106] <Comparative Example 11>
[0107] A positive electrode active material was obtained in the same manner as in Example 5 except that Ba(OH) 2 was not added in the step of obtaining the mixture (second step).
[0108] <Example 6>
[0109] Use [Ni 0.91 Al 0.055 Co 0.035 ](OH)2 gives a composite hydroxide (Ni 0.91 Al 0.055 Co 0.035 O2), LiOH, the composite oxide, Sr(OH)2, and Ba(OH)2 were mixed in a manner such that the total amount of Li, Ni, Al, and Co, and the molar ratio of Sr and Ba were 1.03:1:0.0007:0.00001 to obtain a mixture, and the positive electrode active material was obtained in the same manner as in Example 1. The composition of the obtained positive electrode active material is LiNi 0.91 Al 0.055 Co 0.035 Sr 0.0007 Ba β O2. This was used as the positive electrode active material of Example 6. As in Example 1, it was confirmed that Ba was contained in the positive electrode active material, but the content β of Ba was too small to be quantified. It was estimated from the added amount that β was about 0.00001.
[0110] <Example 7>
[0111] A positive electrode active material was obtained in the same manner as in Example 6 except that Ca(OH) 2 was added in place of Sr(OH) 2 in the step of obtaining the mixture (second step).
[0112] <Comparative Example 12>
[0113] A positive electrode active material was obtained in the same manner as in Example 6 except that Sr(OH) 2 and Ba(OH) 2 were not added in the step of obtaining the mixture (second step).
[0114] <Comparative Example 13>
[0115] A positive electrode active material was obtained in the same manner as in Example 6 except that Sr(OH) 2 was not added in the step of obtaining the mixture (second step).
[0116] <Comparative Example 14>
[0117] A positive electrode active material was obtained in the same manner as in Example 6 except that Ba(OH) 2 was not added in the step of obtaining the mixture (second step).
[0118] <Comparative Example 15>
[0119] A positive electrode active material was obtained in the same manner as in Example 6 except that Ca(OH) 2 was added instead of Sr(OH) 2 in the step of obtaining the mixture (second step) and Ba(OH) 2 was not added.
[0120] <Example 8>
[0121] Use [Ni 0.91 Al 0.05 Mn 0.04 ](OH)2 gives a composite hydroxide (Ni 0.91 Al 0.05 Mn 0.04 O2), LiOH, the composite oxide, Sr(OH)2, and Ba(OH)2 were mixed in a manner such that the total amount of Li, Ni, Al, and Co, and the molar ratio of Sr and Ba were 1.03:1:0.0015:0.000004 to obtain a mixture, and the positive electrode active material was obtained in the same manner as in Example 1. The composition of the obtained positive electrode active material is LiNi 0.91 Al 0.05 Mn 0.04 Sr 0.0015 Ba β O2. This was used as the positive electrode active material of Example 8. As in Example 1, it was confirmed that Ba was contained in the positive electrode active material, but the content β of Ba was too small to be quantified. Based on the added amount, β was estimated to be about 0.000004.
[0122] <Comparative Example 16>
[0123] A positive electrode active material was obtained in the same manner as in Example 8 except that Sr(OH) 2 and Ba(OH) 2 were not added in the step of obtaining the mixture (second step).
[0124] <Comparative Example 17>
[0125] A positive electrode active material was obtained in the same manner as in Example 8 except that Sr(OH) 2 was not added in the step of obtaining the mixture (second step).
[0126] <Comparative Example 18>
[0127] A positive electrode active material was obtained in the same manner as in Example 8 except that Ba(OH) 2 was not added in the step of obtaining the mixture (second step).
[0128] <Example 9>
[0129] Use [Ni 0.925 Al 0.05 Mn 0.025 ](OH)2 gives a composite hydroxide (Ni 0.925 Al 0.05 Mn 0.025 O2), LiOH, the composite oxide, Sr(OH)2, and Ba(OH)2 were mixed in a manner such that the total amount of Li, Ni, Al, and Co, and the molar ratio of Sr and Ba were 1.03:1:0.0018:0.000003 to obtain a mixture, and the positive electrode active material was obtained in the same manner as in Example 1. The composition of the obtained positive electrode active material is LiNi 0.925 Al 0.05 Mn 0.025 Sr 0.0018 Ba β O2. This was used as the positive electrode active material of Example 9. As in Example 1, it was confirmed that Ba was contained in the positive electrode active material, but the content β of Ba was too small to be quantified. It was estimated from the added amount that β was about 0.000003.
[0130] <Comparative Example 19>
[0131] A positive electrode active material was obtained in the same manner as in Example 9 except that Sr(OH) 2 and Ba(OH) 2 were not added in the step of obtaining the mixture (second step).
[0132] <Comparative Example 20>
[0133] A positive electrode active material was obtained in the same manner as in Example 9 except that Sr(OH) 2 was not added in the step of obtaining the mixture (second step).
[0134] <Comparative Example 21>
[0135] A positive electrode active material was obtained in the same manner as in Example 9 except that Ba(OH) 2 was not added in the step of obtaining the mixture (second step).
[0136] <Reference Example 1>
[0137] Use [Ni 0.595 Co 0.21 Mn0.195 ](OH)2 gives a composite hydroxide (Ni 0.595 Co 0.21 Mn 0.195 O2), LiOH, the composite oxide, Sr(OH)2, and Ba(OH)2 were mixed in a manner such that the total amount of Li, Ni, Al, and Co, and the molar ratio of Sr and Ba were 1.03:1:0.0007:0.00001 to obtain a mixture, and the positive electrode active material was obtained in the same manner as in Example 1. The composition of the obtained positive electrode active material is LiNi 0.595 Co 0.21 Mn 0.195 Sr 0.0007 Ba β O2. This was used as the positive electrode active material of Reference Example 1. As in Example 1, it was confirmed that Ba was contained in the positive electrode active material, but the Ba content β was too small to be quantified. It was estimated from the added amount that β was about 0.00001.
[0138] <Reference Example 2>
[0139] A positive electrode active material was obtained in the same manner as in Reference Example 1 except that Sr(OH) 2 and Ba(OH) 2 were not added in the step of obtaining the mixture (second step).
[0140] <Reference Example 3>
[0141] A positive electrode active material was obtained in the same manner as in Reference Example 1 except that Sr(OH) 2 was not added in the step of obtaining a mixture (second step).
[0142] <Reference Example 4>
[0143] A positive electrode active material was obtained in the same manner as in Reference Example 1 except that Ba(OH) 2 was not added in the step of obtaining a mixture (second step).
[0144] <Reference Example 5>
[0145] A positive electrode active material was obtained in the same manner as in Reference Example 1 except that Ca(OH) 2 was added in place of Sr(OH) 2 in the step of obtaining a mixture (second step).
[0146] The reaction resistance and capacity retention rate of the examples, comparative examples, and reference examples are shown in Tables 1 to 7, respectively. In addition, the results of ICP analysis are summarized for the obtained positive electrode active materials in Tables 1 to 7. The reaction resistance and capacity retention rate of the test battery cells of Example 1 and Comparative Examples 2 and 3 shown in Table 1 are values relatively expressed with the reaction resistance and capacity retention rate of the test battery cell of Comparative Example 1 being 100.
[0147] The reaction resistance and capacity retention rate of the test cells of Examples 2 and 3 and Comparative Examples 5 to 7 shown in Table 2 are values expressed relatively with the reaction resistance and capacity retention rate of the test cell of Comparative Example 4 being 100.
[0148] The reaction resistance and capacity retention rate of the test cells of Examples 4 and 5 and Comparative Examples 9 to 11 shown in Table 3 are values expressed relatively with the reaction resistance and capacity retention rate of the test cell of Comparative Example 8 being 100.
[0149] The reaction resistance and capacity retention rate of the test cells of Examples 6 and 7 and Comparative Examples 13 to 15 shown in Table 4 are values expressed relatively with the reaction resistance and capacity retention rate of the test cell of Comparative Example 12 being 100.
[0150] The reaction resistance and capacity retention rate of the test cells of Example 8 and Comparative Examples 17 and 18 shown in Table 5 are values expressed relatively with the reaction resistance and capacity retention rate of the test cell of Comparative Example 16 being 100.
[0151] The reaction resistance and capacity retention rate of the test cells of Example 9 and Comparative Examples 20 and 21 shown in Table 6 are values expressed relatively with the reaction resistance and capacity retention rate of the test cell of Comparative Example 19 being 100.
[0152] The reaction resistance and capacity retention rate of the test cells of Reference Examples 1 and 3 to 5 shown in Table 7 are values expressed relatively with the reaction resistance and capacity retention rate of the test cell of Reference Example 2 being 100.
[0153] [Table 1]
[0154]
[0155] [Table 2]
[0156]
[0157] [Table 3]
[0158]
[0159] [Table 4]
[0160]
[0161] [Table 5]
[0162]
[0163] [Table 6]
[0164]
[0165] [Table 7]
[0166]
[0167] In any one of Tables 1 to 6, the examples containing Sr and Ba in the surface modification layer have lower reaction resistance and higher capacity retention rate than the comparative examples not containing at least one of Sr and Ba in the surface modification layer. It should be noted that in Table 7, in any one of Reference Examples 1 to 5, the lithium transition metal composite oxide does not contain Al, so the reaction resistance and capacity retention rate do not change when Sr and Ba are added or not.
[0168] Description of Reference Numerals
[0169] 10 Non-aqueous electrolyte secondary battery
[0170] 11 Positive electrode
[0171] 12 Negative electrode
[0172] 13 Divider
[0173] 14 Electrode body
[0174] 15 Battery housing
[0175] 16 Outer can
[0176] 17 Sealing body
[0177] 18, 19 Insulation board
[0178] 20 positive electrode tab
[0179] 21. Negative electrode tab
[0180] 22 Groove
[0181] 23 Base Plate
[0182] 24 Lower valve core
[0183] 25 Insulation components
[0184] 26 Upper valve core
[0185] 27 Cover
[0186] 28 Pad
[0187] 30 Positive electrode collector
[0188] 31. Positive electrode active material layer
[0189] 40 Negative electrode collector
[0190] 41 Negative electrode active material layer
Claims
1. A positive electrode active material for a non-aqueous electrolyte secondary battery, comprising: A lithium transition metal composite oxide having secondary particles formed by aggregation of primary particles, and a surface modification layer formed on the surface of the primary particles of the lithium transition metal composite oxide, The lithium transition metal composite oxide contains at least Al and 80 mol % or more of Ni relative to the total molar number of metal elements other than Li, The surface modification layer contains at least one of Sr and Ca, and Ba.
2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein The surface modification layer further contains Al.
3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein The lithium transition metal composite oxide is represented by the general formula Li a Ni x Al y Co z M w O 2-b wherein 0.95 < a < 1.05, 0.8 ≤ x ≤ 0.96, 0 < y ≤ 0.10, 0 ≤ z ≤ 0.15, 0 ≤ w ≤ 0.1, 0 ≤ b < 0.05, x + y + z + w = 1, and M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo, and Zn.
4. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein The ratio of Sr and Ca in the surface modification layer is 0.05 mol % to 0.25 mol % relative to the total molar number of metal elements other than Li in the lithium transition metal composite oxide.
5. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein The ratio of Ni is 90 mol % or more relative to the total number of moles of metal elements other than Li in the lithium transition metal composite oxide. 6 . A non-aqueous electrolyte secondary battery comprising: a positive electrode containing the positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 , a negative electrode, and a non-aqueous electrolyte.