A preparation method and application of perovskite film

By using conductive composite materials and perovskite precursor solutions in the preparation of perovskite films, combined with the anti-solvent effect of fluorobenzene, the problems of film unevenness and many holes are solved, and perovskite devices are significantly improved performance and stability.

CN115000334BActive Publication Date: 2024-11-22EAST CHINA NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210720755.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-24
Publication Date
2024-11-22
Estimated Expiration
2042-06-24

AI Technical Summary

Technical Problem

The existing perovskite film preparation methods are difficult to achieve flat and poreless film formation, which limits device performance.

Method used

The polymer layer was prepared by spin-coating the dispersed aqueous solution of conductive composite materials, and mixed in dimethyl sulfoxide by lead bromide, cesium bromide, 2-phenethylamine chloride perovskite precursor solutions to combine with dynamic distribution Spin coating and antisolvent fluorobenzene are used, spin coating and annealing are performed to prepare low-pore and high flatness perovskite films.

Benefits of technology

The high flatness and low pore characteristics of the perovskite film are achieved, the device performance is improved, and the stability and integrity of the film are enhanced through the passivation of anti-solvent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 220623104115
    Figure 220623104115
  • Figure 220623104119
    Figure 220623104119
  • Figure 220623104124
    Figure 220623104124
Patent Text Reader

Abstract

The present invention discloses a preparation method and application of a perovskite film. The present invention mainly examines how to use the method of step-by-step spin coating and anti-solvent dissolution to improve the stability of the perovskite film. The present invention innovatively uses a new anti-solvent fluorobenzene. The anti-solvent fluorinated benzene not only plays a role in reducing the solubility of perovskite and precipitating and purifying it, but also forms a protective layer through the passivation of the fluorine functional group, so that the perovskite layer maintains a more complete shape. The experimental results show that on the perovskite surface treated with the anti-solvent and the passivating agent fluorobenzene, the voids visible to the naked eye are significantly reduced, and the thin layer of perovskite becomes more uniform, and the situation where the perovskite cannot be covered is greatly alleviated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of perovskite film production, and in particular relates to a preparation method and application of a perovskite film. Background Art

[0002] The microstructure of perovskite crystals is a three-dimensional skeleton composed of an octahedral array connected by vertices, in which metal cations are located at the body center, halogen anions are located at the face center, and organic or inorganic cations are located in the gaps of the octahedron, forming a coordination effect with the surrounding 12 ions. Perovskite is a material that can generate electricity and emit light, with low preparation cost, high fluorescence quantum efficiency, high color purity, and adjustable color.

[0003] In the production process, the preparation of a flat, high-coverage, and low-pore perovskite film is the basis for achieving high-efficiency light-emitting devices. At present, the most commonly used method for preparing perovskite films is the drop coating method, which is to drop the perovskite precursor solution onto a glass or plastic substrate to obtain a relatively thin perovskite film. This method is easy to operate, low in cost, and has low requirements for the production test environment.

[0004] The quality of perovskite film is a key parameter that affects the photovoltaic performance of the device. The existing methods for preparing perovskite film make it difficult to achieve the rapid, uniform, and complete formation and growth of the wet film formed after the perovskite solution is coated. In the conventional perovskite film preparation process, due to problems such as process techniques, the prepared perovskite film may have many defects, thereby limiting the device performance. Therefore, how to prepare low-pore, high-flatness perovskite film is the key to improving the performance of perovskite devices. Summary of the invention

[0005] The present invention overcomes the defects of the existing perovskite drop coating technology, provides a method for preparing a low-pore, high-flatness perovskite film, obtains higher device performance, and has high repeatability and high adaptability.

[0006] The purpose of the present invention is to solve the problem of unevenness and many holes in the preparation process of perovskite film.

[0007] To achieve the above purpose, the present invention discloses the following technical contents:

[0008] A method for preparing a perovskite film is characterized by the following steps:

[0009] (1) preparing a polymer layer by spin coating a dispersed aqueous solution of a conductive composite material on a substrate; the conductive composite material refers to a hole transport layer material; the dispersed aqueous solution is an aqueous solution of a composite material of poly(ethylenedioxythiophene) (PEDOT) and polystyrene sulfonate anion (PSS); the molar ratio of poly(ethylenedioxythiophene) to polystyrene sulfonate anion is 2:1;

[0010] (2) Lead bromide (PbBr 2 ), cesium bromide (CsBr), 2-phenylethylammonium chloride (PEACl) perovskite precursors are dispersed in dimethyl sulfoxide solvent to obtain a perovskite precursor solution; that is, by mixing 53 mg CsBr and 91.3 mg PbBr in 1 mL dimethyl sulfoxide (DMSO) 2 CsPbBr 3 Solution: PEACl solution was prepared by mixing 39.5 mg PEACl in 1 mL DMSO to obtain CsPbBr 3 The solution was mixed with the PEACl solution in a ratio of 1:1;

[0011] (3) Spin coating the precursor solution obtained in step 2) onto the polymer layer obtained in step (1);

[0012] (4) During step 3), a relatively stable perovskite film is obtained by spin coating using a dynamic distribution spin coating method and an anti-solvent addition method; the anti-solvent is: 200 μl of fluorobenzene (C 6 H 5 F);

[0013] (5) The obtained perovskite film is annealed at 90-120° C. for 20 min to remove excess organic solvent and obtain a perovskite film.

[0014] Before the preparation of step (1), the clean substrate needs to be treated in ultraviolet ozone for 15 minutes. The spin coating in step (1) is a two-step spin coating; the first step is 300-500r / s for 1-2s, and the second step is 3500-4500r / s for 30-40s. After the spin coating is completed, the obtained polymer film is heated on a hot plate at 100-130°C for 20min to obtain a polymer layer. The spin coating in step (3) is a two-step spin coating: the first step is 300-500r / s for 2-5s, and the second step is 3500-5000r / s for 30-40s. Further, 20 seconds after the start of spin coating, the anti-solvent in step (4) is dripped onto the rotating perovskite film.

[0015] The present invention further discloses the application of the perovskite film prepared by the method in improving the performance of perovskite devices; wherein the improved performance of the perovskite device refers to: the perovskite device has low porosity and high flatness. Experimental results show that fluorobenzene can simultaneously act as an antisolvent and a passivating agent, dissolving electron-deficient metal cation complexes, inhibiting the holes overflowing from the surface, and generating a passivating layer, thereby improving the overall integrity of the surface of the perovskite film.

[0016] The present invention is described in more detail as follows:

[0017] (1) preparing a polymer layer by spin coating a dispersed aqueous solution of a conductive composite material on a substrate;

[0018] (2) Lead bromide (PbBr 2 ), cesium bromide (CsBr), 2-phenylethylammonium chloride (PEACl) perovskite precursors are dispersed in a solvent, and the solvent is preferably dimethyl sulfoxide (DMSO).

[0019] (3) Spin coating the precursor solution obtained in step 2) onto the polymer layer obtained in step 1);

[0020] (4) During step 3), a relatively stable perovskite film is obtained by spin coating using a dynamic distribution spin coating method and an anti-solvent addition method.

[0021] (5) The obtained perovskite film is annealed to remove and evaporate excess organic solvent, thereby obtaining a preferred perovskite film.

[0022] Note: Before step 1), the cleaned substrate needs to be treated in UV ozone for 15 minutes.

[0023] Furthermore, in step 1), the dispersed aqueous solution of the conductive composite material is an aqueous solution of a composite material of poly(ethylenedioxythiophene) (PEDOT) and polystyrene sulfonate anion (PSS). The aqueous solution generally uses the Al4083 parameter standard. The spin coating of the polymer dispersion is a two-step spin coating, the first step is at a rotation speed of 300-500r / s, the time is 1-2s, and the second step is at 3500-4500r / s, the time is 30-40s. After the spin coating is completed, the obtained polymer film needs to be heated on a hot plate at 100-130°C for 20 minutes to obtain a polymer layer.

[0024] Furthermore, the precursor solution of perovskite in step 2) is prepared by mixing 53 mg CsBr and 91.3 mg PbBr in 1 mL dimethyl sulfoxide (DMSO). 2 CsPbBr 3 Solution. CsPbBr 3The solution needs to be filtered before use. Prepare PEACl solution by mixing 39.5 mg PEACl in 1 mL DMSO. The resulting CsPbBr 3 The solution was mixed with PEACl solution in a 1:1 ratio.

[0025] The spin coating in step 3) is also a two-step spin coating, the first step is at a speed of 300-500 r / s for 2-5 s, and the second step is at a speed of 3500-5000 r / s for 30-40 s. Further, 20 seconds after the start of spin coating, the anti-solvent in step 4) is dropped onto the rotating perovskite film. The anti-solvent refers to 200 microliters of fluorobenzene (C 6 H 5 F).

[0026] In step 5), the annealing time is 90-120° C. for 20 min.

[0027] The present invention mainly examines how to use the step-by-step spin coating and anti-solvent dissolution method to improve the stability of the perovskite film. The difficulty of the invention lies in how to improve the properties of the perovskite itself through solubility and chemical growth regulation. The innovation of the present invention lies in the use of a new anti-solvent, a new perovskite solution composition and a new composition ratio.

[0028] The positive effects of the anti-solvent type and spin coating disclosed in the present invention compared with the prior art are: the method mentioned in this patent has universal operability and high controllability; the anti-solvent fluorinated benzene in this method not only plays a role in reducing the solubility of perovskite and precipitating and purifying it, but also forms a protective layer through the passivation effect of the fluorine functional group, so that the perovskite layer maintains a more complete shape.

[0029] The original CsPbBr 3 Thin film samples will show a large number of dark spots visible to the naked eye, which are equivalent to holes. This will be due to the non-radiative recombination of electron and hole pairs in the holes and the non-radiative recombination of electrons and holes in the pinhole defects. 6 H 5 F) is added to CsPbBr 3 When the film surface is exposed to the sun, the black spots associated with the pinholes disappear in large numbers. 6 H 5 F) Treated CsPbBr 3 Although pinholes can be found on the film surface, the number is much smaller. This is because fluorobenzene (C 6 H 5 F) antisolvent and the surface passivation effect of fluorination. Fluorobenzene (C 6 H 5F) The treatment modified the top surface of CsPbBr3 to form CsPbF with a larger bandgap energy level. 3 Protective layer.

[0030] Figure 1 The image shows a surface scan of an untreated perovskite film. It can be clearly seen that a large number of holes visible to the naked eye are formed on the surface of the untreated perovskite, and the thin layer of perovskite is extremely uneven, with many areas where the perovskite cannot cover.

[0031] Figure 2 The surface scanned image of the treated perovskite film prepared in Example 1 is shown. It can be clearly seen in the figure that on the surface of the perovskite treated with the antisolvent and the passivating agent fluorobenzene, the voids visible to the naked eye are significantly reduced, and the thin layer of the perovskite becomes more uniform, and the situation where the perovskite cannot be covered is greatly alleviated;

[0032] Figure 3 The perovskite light-emitting diode device prepared in Example 4 has a light-emitting area of ​​0.1 square centimeters, an external voltage of 3.0 volts, and a light-emitting wavelength of 488 nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a surface scan image of the prepared untreated perovskite film;

[0034] Figure 2 This is a surface scanning image of the treated perovskite film prepared in Example 1;

[0035] Figure 3 This is a picture of a light-emitting diode made of the treated perovskite film prepared in Example 4 being powered on and lit up. DETAILED DESCRIPTION

[0036] The present invention is described below by specific embodiments. Unless otherwise specified, the technical means used in the present invention are methods known to those skilled in the art. In addition, the embodiments should be understood as illustrative rather than limiting the scope of the present invention, and the essence and scope of the present invention are limited only by the claims. For those skilled in the art, various changes or modifications to the material composition and dosage in these embodiments, without departing from the essence and scope of the present invention, also belong to the protection scope of the present invention. The raw materials and reagents used in the present invention are all commercially available.

[0037] Example 1

[0038] The substrate (size 2×2cm 2ITO glass) was ultrasonically cleaned with deionized water, acetone, ethanol and isopropanol solvents in turn, and then dried in a drying oven for 6 hours before being taken out. The substrate was then subjected to UV ozone hydrophilization treatment for 15 minutes. The substrate was placed in a glove box for operation. The PEDOT:PSS (AI 4083) aqueous solution dispersion was spin-coated in two steps: the first step was at a speed of 500r / s for 2s; the second step was at a speed of 3500r / s for 30s. After the end, it was immediately placed on a hot plate at a temperature of 130°C and heated for 20 minutes to obtain a PEDOT:PSS thin layer. With CsBr, PbBr 2 With PEACl as solute and a mixed solvent composed of dimethyl sulfoxide as solvent, a saturated precursor solution with a total volume of 2 mL is prepared and ultrasonically dissolved for 20 minutes. After the dissolution is completed, the solution is filtered. Spin coating is performed under two-step speed conditions: speed of 400r / s, time of 2s, speed of 4000r / s, time of 40s; 200 microliters of fluorobenzene is added to the spin coating at the 20th second of spin coating. Immediately after the end, it is placed on a hot plate at a temperature of 90°C and heated for 20 minutes to obtain a perovskite thin layer, at which the thickness of the perovskite thin layer is 69.8nm.

[0039] Example 2

[0040] The substrate (size 2×2cm 2 ITO glass) was ultrasonically cleaned with deionized water, acetone, ethanol and isopropanol solvents in turn, and then dried in a drying oven for 6 hours before being taken out. The substrate was then subjected to UV-ozone hydrophilization treatment for 15 minutes. The substrate was placed in a glove box for operation. The PEDOT:PSS (AI 4083) aqueous solution dispersion was spin-coated in two steps: the first step was at a speed of 300r / s for 2s; the second step was at a speed of 3500r / s for 30s. After the end, it was immediately placed on a hot plate at 120°C and heated for 20 minutes to obtain a PEDOT:PSS thin layer. With CsBr, PbBr 2 With PEACl as solute and a mixed solvent composed of dimethyl sulfoxide as solvent, a saturated precursor solution with a total volume of 2 mL is prepared and ultrasonically dissolved for 20 minutes. After the dissolution is completed, the solution is filtered. Spin coating is performed under two-step speed conditions: speed of 300r / s, time of 2s, speed of 4000r / s, time of 40s; 200 microliters of fluorobenzene is added to the spin coating at the 20th second of spin coating. Immediately after the end, it is placed on a hot plate at a temperature of 100°C and heated for 20 minutes to obtain a perovskite thin layer, at which the thickness of the perovskite thin layer is 73.2nm.

[0041] Example 3

[0042] The substrate (size 2×2cm 2ITO glass) was ultrasonically cleaned with deionized water, acetone, ethanol and isopropanol solvents in turn, and then dried in a drying oven for 6 hours before being taken out. The substrate was then subjected to UV-ozone hydrophilization treatment for 15 minutes. The substrate was placed in a glove box for operation. The PEDOT:PSS (AI 4083) aqueous solution dispersion was spin-coated in two steps: the first step was at a speed of 400r / s for 3s; the second step was at a speed of 4000r / s for 30s. After the end, it was immediately placed on a hot plate at a temperature of 110°C and heated for 20 minutes to obtain a PEDOT:PSS thin layer. With CsBr, PbBr 2 and PEACl as solutes, a mixed solvent consisting of dimethyl sulfoxide as solvent, a total volume of 2mL of saturated precursor solution is prepared, and ultrasonic dissolution is performed for 20 minutes. After the dissolution is completed, the solution is filtered. Spin coating is performed under two-step speed conditions: speed of 500r / s, time of 2s, speed of 4500r / s, time of 40s; 200 microliters of fluorobenzene is added to the spin coating at the twentieth second of spin coating. Immediately after the end, it is placed on a hot plate at a temperature of 110°C and heated for 20 minutes to obtain a perovskite thin layer, at which the thickness of the perovskite thin layer is 70.2nm.

[0043] Example 4

[0044] The substrate (ITO glass with a size of 2×2cm2) was ultrasonically cleaned in deionized water, acetone, ethanol and isopropanol solvents in turn, and then dried in a drying oven for 6 hours before being taken out. The substrate was then subjected to UV ozone hydrophilization treatment for 15 minutes. The substrate was placed in a glove box for operation. The PEDOT:PSS (AI 4083) aqueous solution dispersion was spin-coated in two steps: the first step was 300r / s for 2s; the second step was 3500r / s for 30s. After the end, it was immediately placed on a hot plate at a temperature of 125℃ for 20 minutes to obtain a PEDOT:PSS thin layer. With CsBr, PbBr2 and PEACl as solutes and a mixed solvent composed of dimethyl sulfoxide as solvent, a saturated precursor solution with a total volume of 2mL was prepared and ultrasonically dissolved for 20 minutes. After the dissolution was completed, the solution was filtered. The spin coating was performed under two-step rotation speed conditions: 300 r / s for 2 s, and 4000 r / s for 40 s; 200 μl of fluorobenzene was added to the spin coating at the 20th second of the spin coating. Immediately after the spin coating was completed, the film was placed on a hot plate at 90°C and heated for 20 minutes to obtain a perovskite thin layer, at which the thickness of the perovskite thin layer was 70.1 nm.

[0045] The perovskite thin layer prepared in this example, CsPbBr 3The film becomes denser while maintaining the average grain size. Then, through thermal evaporation, the hole blocking material TPBI with a thickness of 40nm, lithium fluoride with a thickness of less than 1nm, and aluminum electrode with a thickness of 100nm are sequentially covered to complete the manufacture of the original perovskite light-emitting diode. The light-emitting diode area is 0.1 square centimeters. Figure 3 As shown in the figure, under an external voltage of 3.5 volts, a luminescent wavelength of 488 nm was measured, and the luminescence can be continuously and stably emitted for at least 100 minutes. It can be seen that the perovskite thin layer prepared by this method has higher stability and better luminescence ability.

[0046] After the preferred embodiments are described in detail, those familiar with the technology can clearly understand that various changes and modifications can be made without departing from the scope and spirit of the above patent application, and any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention are within the scope of the technical solution of the present invention. The present invention is not limited to the example implementation methods given in the specification.

Claims

1. A method for preparing a perovskite film, characterized in that Proceed as follows: (1) preparing a polymer layer by spin coating a dispersed aqueous solution of a conductive composite material on a substrate; the conductive composite material is a hole transport layer material; the dispersed aqueous solution is an aqueous solution of a composite material of poly(dioxyethylthiophene) and polystyrene sulfonate anions; wherein the molar ratio of poly(dioxyethylthiophene) to polystyrene sulfonate anions is 2:1; (2) dispersing lead bromide, cesium bromide, and 2-phenylethylammonium chloride perovskite precursors in a dimethyl sulfoxide solvent to obtain a perovskite precursor solution; that is, a CsPbBr3 solution prepared by mixing 53 mg of CsBr and 91.3 mg of PbBr2 in 1 mL of dimethyl sulfoxide; and a PEACL solution prepared by mixing 39.5 mg of PEACL in 1 mL of DMSO, and the obtained CsPbBr3 solution and the PEACL solution were mixed in a ratio of 1:1; (3) spin coating the precursor solution obtained in step (2) onto the polymer layer obtained in step (1); (4) During step (3), a relatively stable perovskite film is obtained by spin coating using a dynamic distribution spin coating method and an anti-solvent addition method; the anti-solvent is 200 μl of fluorobenzene; (5) The obtained perovskite film is annealed at 90-120° C. for 20 min to remove and evaporate excess organic solvent, thereby obtaining a perovskite film.

2. The preparation method according to claim 1, wherein before the preparation in step (1), the clean substrate needs to be treated in ultraviolet ozone for 15 minutes.

3. The preparation method according to claim 1, wherein the spin coating in step (1) is a two-step spin coating; the first step is at a rotation speed of 300-500 r / s for 1-2 s, and the second step is at 3500-4500 r / s for 30-40 s. After the spin coating, the obtained polymer film is heated on a hot plate at 100-130°C for 20 min to obtain a polymer layer.

4. The preparation method according to claim 1, wherein the spin coating in step (3) is a two-step spin coating: the first step has a rotation speed of 300-500 r / s and a time of 2-5 s, and the second step has a rotation speed of 3500-5000 r / s and a time of 30-40 s. Furthermore, 20 seconds after the start of spin coating, the anti-solvent in step (4) is dripped onto the rotating perovskite film.

5. An application of a perovskite film prepared by the method of claim 1 to improve the performance of a perovskite device, wherein the improved performance of the perovskite device is: the perovskite film has low porosity and high flatness.