A formula and preparation method of soft magnetic composite material
Through the combination of modified zinc stearate and nano-inorganic oxides, the bonding problem of soft magnetic composite materials during the mold release process is solved, the non-stickness and insulation quality of the finished product are improved, the preparation process is simplified, and the production is improved efficiency.
Patent Information
- Application Number
- CN202210807781.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-11
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-07-11
AI Technical Summary
The existing soft magnetic composite materials have bonding phenomena during the demolding process, and the overall activity is low, which affects the quality and production efficiency of the finished product.
Modified zinc stearate as a mold release agent, and the lubrication effect is improved by reaction with aluminum hydroxide and zinc stearate, and the insulation treatment of nanoinorganic oxides and electrically insulating inorganic nanofillers is formed to form double insulation. Structure, avoid bonding and improve insulation quality.
It effectively avoids bonding during mold release, improves the non-stickness and insulation quality of the finished product, simplifies the preparation process, and improves the overall performance and production efficiency of the finished product.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of soft magnetic composite material preparation, and specifically relates to a formula and a preparation method of a soft magnetic composite material. Background Art
[0002] Soft magnetic composite materials are a type of functional material widely used in the field of power electronics, mainly used in various magnetic devices such as high-power inductors and transformers. Because such materials have high saturation magnetization and large resistivity, they are widely used in high-power electronic systems in the kilohertz frequency band.
[0003] In the preparation of soft magnetic composite materials, zinc stearate is used as a release agent. Although this material can achieve the effect of lubrication and demolding, in actual use, there is still a phenomenon of local bonding, which affects the quality of the finished product and also has a certain impact on production. At the same time, in the later preparation, only a single insulation treatment is used, which has low cost and quality in the later stage, and there are also many shortcomings. Summary of the invention
[0004] The purpose of the present invention is to provide a formula and a preparation method of a soft magnetic composite material to solve the problem that the existing release agent used in the above background technology still has a bonding phenomenon and low overall activity.
[0005] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a formula of a soft magnetic composite material, specifically comprising the following formula: 30-40wt% FeSiAl powder core, 20-30wt% FeSi powder core, 10-20wt% FeSiCr powder core, 10-40wt% strontium ferrite powder, 20-40wt% barium ferrite powder and 5-8wt% modified zinc stearate, wherein the modified zinc stearate can improve demolding efficiency and quality.
[0006] As a preferred technical solution of the present invention, the preparation method of the modified zinc stearate is as follows:
[0007] S1: Weigh 8-14 g of aluminum hydroxide and add 100-186 mL of water to prepare a slurry with a mass fraction of 4-7%;
[0008] S2: Add 130-160g zinc stearate to the slurry, heat and stir to speed up the reaction rate;
[0009] S3: After constant temperature reaction for 3 to 5 hours, filter and wash to remove impurities, and dry at 90 to 110° C. to obtain modified zinc stearate.
[0010] As a preferred technical solution of the present invention, in S2, the heating rate is 5-8°C / min, the initial temperature is 20-22°C, and an efficient and comprehensive reaction can be achieved by gradually heating up. The maximum temperature is 100-110°C, and the stirring speed is 30-60r / min.
[0011] A method for preparing a soft magnetic composite material comprises the following steps:
[0012] Step 1: Powdering, dispersing nano inorganic oxides into silane hydrolyzate to obtain an insulating dispersion, then adding FeSiAl powder cores, FeSi powder cores, FeSiCr powder cores, strontium ferrite powders, and barium ferrite powders into the insulating dispersion, stirring and mixing, then taking out, washing, and drying to obtain insulating soft magnetic powders;
[0013] Step 2: Insulation treatment, coating the insulating soft magnetic powder obtained in step 1 with two or more layers of electrically insulating inorganic nanofillers to form double insulation with the insulation treatment in step 1, thereby forming insulating ferromagnetic powder;
[0014] Step 3: Bonding: coating the surface of the ferromagnetic powder with modified zinc stearate to facilitate demoulding in the later stage;
[0015] Step 4: Pressing and heat treatment, pressing and heat treating the product in step 3.
[0016] As a preferred technical solution of the present invention, the stirring rate in step 1 is 60-100 r / min, and the stirring time is 20-40 min.
[0017] As a preferred technical solution of the present invention, the pressing time in step 4 is 20 to 30 minutes, the pressing pressure is 700 to 2000 MPa, and the shaping process is achieved. The heat treatment temperature is 400 to 800°C.
[0018] As a preferred technical solution of the present invention, the drying temperature in step 1 is 300-600° C., and the drying time is 30-50 min.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The modified zinc stearate designed by the present invention can improve the lubrication effect during demoulding, avoid the phenomenon of sticking, improve the non-stickiness, and ensure the quality of the finished product. At the same time, the preparation method is very simple and easy to use. In the powder making of the later preparation, the preliminary insulation treatment can be achieved, and the insulation quality can be improved in combination with the later insulation treatment, so that the quality of the finished product is also improved. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0022] Example 1
[0023] The invention provides a technical solution: a formula of a soft magnetic composite material, specifically comprising the following formula: 30wt% of FeSiAl powder core, 20wt% of FeSi powder core, 10wt% of FeSiCr powder core, 10wt% of strontium ferrite powder, 20wt% of barium ferrite powder and 5wt% of modified zinc stearate.
[0024] In this embodiment, the preparation method of modified zinc stearate is as follows:
[0025] S1: Weigh 8-14 g of aluminum hydroxide and add 100 mL of water to prepare a slurry with a mass fraction of 4%;
[0026] S2: Add 130g zinc stearate to the slurry, heat and stir;
[0027] S3: After constant temperature reaction for 3 hours, filtering, washing, and drying at 90°C, the modified zinc stearate is obtained. The designed modified zinc stearate can improve the lubrication effect during demoulding, avoid adhesion, improve the non-stickiness, and ensure the quality of the finished product.
[0028] In this embodiment, in S2, the heating rate is 5°C / min, the initial temperature is 20°C, the maximum temperature is 100°C, and the stirring speed is 30r / min.
[0029] A method for preparing a soft magnetic composite material comprises the following steps:
[0030] Step 1: Powdering, dispersing nano inorganic oxides into silane hydrolyzate to obtain an insulating dispersion, then adding FeSiAl powder cores, FeSi powder cores, FeSiCr powder cores, strontium ferrite powders, and barium ferrite powders into the insulating dispersion, stirring and mixing, then taking out, washing, and drying to obtain insulating soft magnetic powders. In the later preparation of powdering, preliminary insulation treatment can be achieved, and with the later insulation treatment, the insulation quality can be improved;
[0031] Step 2: Insulation treatment, coating the insulating soft magnetic powder obtained in step 1 with two or more layers of electrically insulating inorganic nanofillers to form insulating ferromagnetic powder;
[0032] Step 3: bonding, coating the surface of the ferromagnetic powder with modified zinc stearate;
[0033] Step 4: Pressing and heat treatment, pressing and heat treating the product in step 3.
[0034] In this embodiment, the stirring rate in step 1 is 60 r / min and the stirring time is 20 min.
[0035] In this embodiment, the pressing time in step 4 is 20 minutes, the pressing pressure is 700 MPa, and the heat treatment temperature is 400°C.
[0036] In this embodiment, the drying temperature in step 1 is 300° C. and the drying time is 30 min.
[0037] Example 2
[0038] The difference from Example 1 is that the present invention provides a technical solution: a formula of a soft magnetic composite material, specifically including the following formula: 30wt% FeSiAl powder core, 20wt% FeSi powder core, 10wt% FeSiCr powder core, 20wt% strontium ferrite powder, 20wt% barium ferrite powder and 8wt% modified zinc stearate.
[0039] In this embodiment, the preparation method of modified zinc stearate is as follows:
[0040] S1: Weigh 14g aluminum hydroxide and add 186mL water to prepare a slurry with a mass fraction of 7%;
[0041] S2: Add 160g zinc stearate to the slurry, heat and stir;
[0042] S3: After constant temperature reaction for 5 hours, filtering, washing, and drying at 110°C, the modified zinc stearate is obtained. The designed modified zinc stearate can improve the lubrication effect during demoulding, avoid adhesion, improve the non-stickiness, and ensure the quality of the finished product.
[0043] In this embodiment, in S2, the heating rate is 8°C / min, the initial temperature is 22°C, the maximum temperature is 110°C, and the stirring speed is 60r / min.
[0044] A method for preparing a soft magnetic composite material comprises the following steps:
[0045] Step 1: Powdering, dispersing nano inorganic oxides into silane hydrolyzate to obtain an insulating dispersion, then adding FeSiAl powder cores, FeSi powder cores, FeSiCr powder cores, strontium ferrite powders, and barium ferrite powders into the insulating dispersion, stirring and mixing, then taking out, washing, and drying to obtain insulating soft magnetic powders. In the later preparation of powdering, preliminary insulation treatment can be achieved, and with the later insulation treatment, the insulation quality can be improved;
[0046] Step 2: Insulation treatment, coating the insulating soft magnetic powder obtained in step 1 with two or more layers of electrically insulating inorganic nanofillers to form insulating ferromagnetic powder;
[0047] Step 3: bonding, coating the surface of the ferromagnetic powder with modified zinc stearate;
[0048] Step 4: Pressing and heat treatment, pressing and heat treating the product in step 3.
[0049] In this embodiment, the stirring rate in step 1 is 100 r / min and the stirring time is 40 min.
[0050] In this embodiment, the pressing time in step 4 is 30 minutes, the pressing pressure is 2000 MPa, and the heat treatment temperature is 800°C.
[0051] In this embodiment, the drying temperature in step 1 is 600° C. and the drying time is 50 min.
[0052] Example 3
[0053] The difference from the above embodiment is that: the present invention provides a technical solution: a formula of a soft magnetic composite material, specifically including the following formula: 30wt% FeSiAl powder core, 20wt% FeSi powder core, 10wt% FeSiCr powder core, 15wt% strontium ferrite powder, 20wt% barium ferrite powder and 5wt% modified zinc stearate.
[0054] In this embodiment, the preparation method of modified zinc stearate is as follows:
[0055] S1: Weigh 10g aluminum hydroxide and add 156mL water to prepare a slurry with a mass fraction of 5%;
[0056] S2: Add 140g zinc stearate to the slurry, heat and stir;
[0057] S3: After constant temperature reaction for 4 hours, filtering, washing, and drying at 100°C, the modified zinc stearate is obtained. The designed modified zinc stearate can improve the lubrication effect during demoulding, avoid adhesion, improve the non-stickiness, and ensure the quality of the finished product.
[0058] In this embodiment, in S2, the heating rate is 7°C / min, the initial temperature is 21°C, the maximum temperature is 105°C, and the stirring speed is 40r / min.
[0059] A method for preparing a soft magnetic composite material comprises the following steps:
[0060] Step 1: Powdering, dispersing nano inorganic oxides into silane hydrolyzate to obtain an insulating dispersion, then adding FeSiAl powder cores, FeSi powder cores, FeSiCr powder cores, strontium ferrite powders, and barium ferrite powders into the insulating dispersion, stirring and mixing, then taking out, washing, and drying to obtain insulating soft magnetic powders. In the later preparation of powdering, preliminary insulation treatment can be achieved, and with the later insulation treatment, the insulation quality can be improved;
[0061] Step 2: Insulation treatment, coating the insulating soft magnetic powder obtained in step 1 with two or more layers of electrically insulating inorganic nanofillers to form insulating ferromagnetic powder;
[0062] Step 3: bonding, coating the surface of the ferromagnetic powder with modified zinc stearate;
[0063] Step 4: Pressing and heat treatment, pressing and heat treating the product in step 3.
[0064] In this embodiment, the stirring rate in step 1 is 80 r / min and the stirring time is 30 min.
[0065] In this embodiment, the pressing time in step 4 is 25 minutes, the pressing pressure is 1500 MPa, and the heat treatment temperature is 700°C.
[0066] In this embodiment, the drying temperature in step 1 is 400° C. and the drying time is 40 minutes.
[0067] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A soft magnetic composite material, characterized in that: Specifically, the formula includes: 30-40wt% FeSiAl powder, 20-30wt% FeSi powder, 10-20wt% FeSiCr powder, 10-40wt% strontium ferrite powder, 20-40wt% barium ferrite powder and 5-8wt% modified zinc stearate; The preparation method of the modified zinc stearate is as follows: S1: weigh 8-14g of aluminum hydroxide, add 100-186mL of water to prepare a slurry with a mass fraction of 4-7%; S2: add 130-160g of zinc stearate to the slurry, heat and stir; S3: after constant temperature reaction for 3-5h, filter and wash, and dry at 90-110°C to obtain the modified zinc stearate; in S2, the heating rate is 5-8°C / min, the initial temperature is 20-22°C, the maximum temperature is 100-110°C, and the stirring speed is 30-60r / min; The preparation method of the soft magnetic composite material comprises the following steps: step 1: powder preparation, dispersing nano inorganic oxide into silane hydrolyzate to obtain insulating dispersion liquid, then adding FeSiAl powder, FeSi powder, FeSiCr powder, strontium ferrite powder and barium ferrite powder into the insulating dispersion liquid, stirring and mixing, then taking out, washing and drying to obtain insulating soft magnetic powder; step 2: insulation treatment, coating the insulating soft magnetic powder obtained in step 1 with two or more layers of electrically insulating inorganic nano fillers to form insulating ferromagnetic powder; step 3: Bonding, coating the surface of the ferromagnetic powder with modified zinc stearate; step four: pressing and heat treatment, pressing and heat treating the product in step three; the stirring rate in the step one is 60-100r / min, and the stirring time is 20-40min; the pressing time in the step four is 20-30min, the pressing pressure is 700-2000MPa, and the heat treatment temperature is 400-800°C; the drying temperature in the step one is 300-600°C, and the drying time is 30-50min.