A hydrophilic channel with a high proportion of Fe-N 4 Nitrogen-doped porous carbon material and preparation method and application thereof

By forming a high proportion of Fe-N4 active sites in porous carbon materials, the problems of low catalyst pore utilization and easy loss of metal load are solved, and efficient catalytic decomposition of ozone and pollutants are achieved, which significantly improves the treatment efficiency and stability sex.

CN115041214BActive Publication Date: 2024-12-03ZHEJIANG UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210707530.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-21
Publication Date
2024-12-03
Estimated Expiration
2042-06-21

AI Technical Summary

Technical Problem

The existing catalytic ozone carbon and nitrogen materials have low pore utilization rates and are prone to loss of metal loads, making it difficult to effectively degrade new organic pollutants that are difficult to degrade in water.

Method used

Using high-proportion Fe-N4 nitrogen-doped porous carbon material in hydrophilic pores, the ozone catalytic capacity is enhanced by forming Fe-N4 active sites in the ammonia pressurization and calcination process. The Fe and N doping are transferred into the pore through ultrasonic and negative pressure vacuum evacuation, etc., to enhance the hydrophilicity and catalytic efficiency of the pore.

Benefits of technology

The stability and catalytic performance of the catalyst are significantly improved, the treatment efficiency of organic pollutants is improved, and the active Fe-N4 sites are not easily lost, achieving efficient catalytic decomposition of ozone and pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115041214B_ABST
    Figure CN115041214B_ABST
Patent Text Reader

Abstract

The present invention discloses a porous carbon material with a high proportion of Fe-N4 nitrogen doped in a hydrophilic channel, and a preparation method and application thereof. The material is obtained by vacuuming porous carbon loaded with iron elements, pressurizing it with ammonia, and then calcining it in an atmosphere containing ammonia. The present invention presses ammonia into the channels of porous carbon by vacuuming the porous carbon and pressurizing it with ammonia, while maintaining a certain proportion of NH3 during the calcination process, so that Fe and N are loaded in the channels together, and a large number of Fe-N4 active sites are formed after calcination, and the proportion of Fe-N4 active sites generating N doping is significantly increased. The Fe-N4 active sites in the channels can not only enhance the ozone catalytic ability, but also are not easy to lose. In addition, the present invention transfers Fe and N doping to the porous carbon channels and strengthens the hydrophilicity of the channels, so that pollutants and ozone can easily enter the porous carbon channels for catalytic reactions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to nanomaterials and water treatment technology, and specifically relates to a method for loading a high proportion of Fe-N in a hydrophilic pore. 4 Nitrogen-doped porous carbon material, preparation method thereof and application in catalytic decomposition of ozone. Background Art

[0002] In recent years, new organic pollutants such as pesticides and antibiotics have been frequently detected in aquatic environments. Due to their easy entry into soil and water bodies and their difficulty in being degraded, they are extremely easy to enter water bodies and spread to all parts of the world with the global water cycle. The continuous input of new pollutants into the environment leads to the rapid accumulation of pollutants in water, and causes acute or chronic damage to aquatic organisms, aquatic products and humans through the food chain. Therefore, the development of water technology that can stably and effectively remove or decompose organic pollutants in agricultural wastewater or urban wastewater to eliminate the harm of these pollutants to aquatic organisms and humans has become an urgent problem to be solved. At present, the water treatment methods for degrading new organic pollutants in water bodies include physical methods, chemical methods, biological methods and physical and chemical methods.

[0003] Ozone catalytic oxidation is an advanced oxidation method in chemical methods. It is a common treatment method for effectively removing new organic pollutants in water. The use of catalysts to catalyze ozone to produce highly oxidizing free radicals can effectively degrade most new organic pollutants in water.

[0004] In recent years, metal-doped carbon-nitrogen materials have attracted extensive attention from researchers due to their good catalytic degradation effects. However, the pore utilization rate of common catalytic ozone carbon-nitrogen catalysts is low, and the metal loaded on the surface is easy to lose. Summary of the invention

[0005] The present invention aims to provide a simple and easy-to-operate method for loading a high proportion of Fe-N in hydrophilic channels. 4 The invention discloses a preparation method and application of nitrogen-doped porous carbon materials. The prepared catalyst exhibits excellent catalytic performance to ozone and can be used to catalyze the degradation of refractory organic pollutants by ozone.

[0006] In the first aspect, the present invention provides a hydrophilic channel with a high proportion of Fe-N 4 The nitrogen-doped porous carbon material is obtained by evacuating porous carbon loaded with iron elements, pressurizing it with ammonia, and then calcining it in an atmosphere containing ammonia.

[0007] Preferably, the porous carbon loaded with iron is prepared by mixing the porous carbon and Fe(NO 3 ) 3 Obtained by ultrasound in water.

[0008] Preferably, the porous carbon is kept for 1 h-10 h after vacuuming.

[0009] Preferably, after the vacuum maintenance is completed, the porous carbon is pressurized to 0.2 MPa-0.5 MPa using ammonia gas.

[0010] In a second aspect, the present invention provides the aforementioned hydrophilic pores loaded with a high proportion of Fe-N 4 The preparation method of nitrogen-doped porous carbon material comprises the following specific steps:

[0011] Step 1: Porous carbon and Fe(NO 3 ) 3 Place them together in ultrapure water for ultrasonic treatment.

[0012] Step 2: Dry the solid phase product after the treatment in step 1, heat it in an oil bath and evacuate it under negative pressure. Keep the vacuum for more than 1 hour.

[0013] Step 3: introduce ammonia gas and pressurize it to above 0.2 MPa, and cool the solid phase product to room temperature for more than 1 hour.

[0014] Step 4: Use liquid nitrogen to freeze the product obtained in step 3, and freeze the obtained solid particles under N 2 and NH 3 Calcination was performed under a low temperature atmosphere to obtain a high proportion of Fe-N loaded in the hydrophilic pores. 4 Nitrogen-doped porous carbon materials.

[0015] Preferably, in step 1, the Fe(NO 3 ) 3 The weight ratio of porous carbon to water is (0.1-10):100; the mass ratio of porous carbon to water is 0.1-1:10;

[0016] Preferably, in step 1, the ultrasonic time is 1 h to 6 h.

[0017] Preferably, in step 2, the drying temperature is 80°C to 120°C;

[0018] Preferably, in step 2, the oil bath heating temperature is 100°C to 200°C.

[0019] Preferably, in step 2, the negative pressure vacuuming is maintained for 1 h to 10 h after being evacuated to a vacuum.

[0020] Preferably, in step three, the pressure is increased to 0.3 MPa with ammonia and maintained for 1 h to 6 h.

[0021] Preferably, in step 4, the calcination condition is N 2 :NH 3 =1:1, raise the temperature to 550℃ at 5℃ per minute, calcine for 2 hours, and then cool naturally.

[0022] In a third aspect, the present invention provides a method for loading a high proportion of Fe-N in the hydrophilic pores. 4 Application of nitrogen-doped porous carbon materials in catalytic ozone decomposition of organic pollutants in water.

[0023] Preferably, the water body is agricultural wastewater or urban sewage.

[0024] Compared with the prior art, the present invention has the following advantages:

[0025] 1. The present invention uses ammonia to pressurize the porous carbon and then evacuate the porous carbon to pressurize the ammonia into the pores of the porous carbon, and at the same time maintains a certain proportion of NH 3 The Fe and N are loaded in the pores together, and a large amount of Fe-N is formed after calcination. 4 active sites and significantly increased the Fe-N 4 The ratio of N doping in the active site. 4 The active sites not only enhance the ozone catalytic ability but are also not easily lost.

[0026] 2. The present invention transfers Fe and N doping into the porous carbon channels and enhances the hydrophilicity of the channels, so that pollutants and ozone can easily enter the porous carbon channels for catalytic reaction, thereby improving the treatment efficiency of pollutants.

[0027] 3. The present invention utilizes the confinement effect of the pores during the preparation of porous materials to make it easier for Fe in the pores to react with N to form Fe-N 4 , instead of forming surface FeOx. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The hydrophilic channels prepared by the present invention are loaded with a high proportion of Fe-N 4 Scanning electron micrograph of nitrogen-doped porous carbon materials;

[0029] Figure 2 The hydrophilic pores provided by the invention are loaded with a high proportion of Fe-N 4 Comparison of the performance of nitrogen-doped porous carbon materials and other materials as catalysts for degrading the organic pollutant ATZ;

[0030] Figure 3 The hydrophilic pores provided by the invention are loaded with a high proportion of Fe-N 4 Comparison of outlet ozone concentrations during ATZ process when nitrogen-doped porous carbon materials and other materials are used as catalysts to degrade organic pollutants. DETAILED DESCRIPTION

[0031] The content of the present invention is further illustrated below in conjunction with specific examples, but it should not be construed as limiting the present invention. Without departing from the spirit and substance of the present invention, simple modifications or replacements made to the inventive method, steps or conditions all belong to the scope of the present invention. Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art.

[0032] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0033] Example 1

[0034] A hydrophilic channel with a high proportion of Fe-N 4 Nitrogen-doped porous carbon materials, using porous carbon as a carrier, 4 The material is loaded in the pores of porous carbon and has a spherical shape with a particle size of 20nm to 50nm.

[0035] Example 2

[0036] A hydrophilic channel with a high proportion of Fe-N 4 The preparation method of nitrogen-doped porous carbon material, the specific process is as follows:

[0037] Step 1: Porous carbon and Fe(NO 3 ) 3 Put them together in deionized water and ultrasonically treat. 3 ) 3 The mass ratio of porous carbon to deionized water is 1:100.

[0038] Step 2: After filtering and drying the porous carbon, place it in a pressure cooker and heat it in an oil bath and evacuate it under negative pressure. Continue to introduce NH 3 The mixture is cooled to room temperature, and then ammonia is introduced under pressure. After the pressure of the autoclave is released to normal pressure, liquid nitrogen is added for rapid freezing to obtain solid particles. The temperature of the porous carbon filtration and drying is not more than 120°C.

[0039] Step 3: Place the obtained solid particles into a tube furnace and heat them in N 2 and NH 3 Calcination was performed under a low temperature atmosphere to obtain a high proportion of Fe-N loaded in the hydrophilic pores. 4 Nitrogen-doped porous carbon materials.

[0040] Example 3

[0041] The difference between this embodiment and embodiment 2 is that the ultrasonic time described in step 1 is limited to 1h-6h.

[0042] Example 4

[0043] The difference between this embodiment and one of the embodiments 2 or 3 is that the oil bath heating temperature described in step 2 is limited to 100-200°C.

[0044] Example 5

[0045] The difference between this embodiment and any one of embodiments 2 to 4 is that the holding time after the negative pressure vacuuming described in step 2 is limited to 1-10 hours.

[0046] Example 7

[0047] The difference between this comparative example and any one of Examples 2 to 10 is that the pressure after the ammonia gas is introduced in step 2 is maintained at 0.2 MPa.

[0048] Example 8

[0049] The difference between this comparative example and any one of Examples 2 to 10 is that the pressure after the ammonia gas is introduced in step 2 is maintained at 0.3 MPa.

[0050] Example 9

[0051] The difference between this comparative example and any one of Examples 2 to 10 is that the pressure after the ammonia gas is introduced in step 2 is maintained at 0.4 MPa.

[0052] Example 10

[0053] The difference between this comparative example and any one of Examples 2 to 10 is that the pressure after the ammonia gas is introduced in step 2 is maintained at 0.5 MPa.

[0054] Embodiment 11

[0055] The difference between this embodiment and any one of embodiments 2 to 7 is that the calcination atmosphere in step 3 is limited to pure NH 3 .

[0056] Example 12

[0057] The difference between this embodiment and any one of embodiments 2 to 8 is that the calcination temperature in step 3 is limited to 500°C-600°C.

[0058] Example 13

[0059] The difference between this embodiment and any one of embodiments 2 to 9 is that the calcination time in step 3 is limited to 1-6 hours.

[0060] Comparative Example 1

[0061] The difference between this comparative example and any one of Examples 2 to 10 is that the calcination atmosphere in step 3 is limited to pure N 2 .

[0062] Comparative Example 2

[0063] The difference between this comparative example and any one of Examples 2 to 10 is that there is no vacuuming and pressurizing step in step 2.

[0064] The effect of the present invention is verified by the following test:

[0065] Experiment 1: This experiment is a hydrophilic channel with a high proportion of Fe-N 4 The preparation experiment of nitrogen-doped porous carbon material is carried out according to the following steps:

[0066] 0.1 g Fe(NO 3 ) 3 10.0 g of porous carbon was added to 100 mL of deionized water and ultrasonicated for 1 h in an ultrasonic machine at room temperature. The ultrasonic machine was operated at 40 kHz and 200 W. The porous carbon was filtered and dried in an 80 ° C drying oven for 12 h. The porous carbon was then placed in a pressure autoclave and heated to 150 ° C in an oil bath. The negative pressure was evacuated to vacuum and then maintained for 2 h. NH was continuously introduced. 3 , cool the autoclave to room temperature, seal it, and then 3 The pressure was increased to 0.3 MPa and maintained for 1 hour. The gas was vented to normal pressure and liquid nitrogen was quickly added to rapidly freeze the porous carbon. Finally, the porous carbon was placed in a tube furnace and heated under N 2 :NH 3 =1:1 atmosphere, the temperature was raised to 550℃ at 5℃ per minute for 2 hours, and then the temperature was naturally cooled to obtain a high proportion of Fe-N loaded in the hydrophilic pores. 4 Nitrogen-doped porous carbon materials.

[0067] The prepared hydrophilic channels are loaded with a high proportion of Fe-N 4 SEM images of nitrogen-doped porous carbon materials are shown in Figure 2. Figure 1 shown; from Figure 1 It can be seen that the obtained material has a spherical morphology and a particle size of 20nm-50nm.

[0068] Experiment 2: High Fe-N ratio loaded in hydrophilic channels 4 Nitrogen-doped porous carbon materials were simulated and applied to the catalytic ozone efficient degradation of organic pollutant atrazine (ATZ) experiment. ATZ was dissolved in 1L deionized water to a concentration of 10μmol / L, and the resulting solution was loaded into the ozone catalytic reaction device. Then, the hydrophilic channels prepared in the first experiment were loaded with a high proportion of Fe-N 4 Nitrogen-doped porous carbon material was put into the solution of the ozone catalytic reaction device, the catalyst dosage was 0.03g / L, and the total dosage was 30mg. Ozone was continuously aerated into the reactor, and the ozone concentration was detected at the reactor outlet. Samples were taken at regular intervals to monitor the concentration of ATZ in the simulated wastewater as the experimental group.

[0069] Six control groups were set up. The difference between control group 1 and the experimental group was that no catalyst was added. The difference between control group 2 and the experimental group was that a high proportion of Fe-N was added into the hydrophilic pores. 4 The nitrogen-doped porous carbon material was replaced with the material obtained in Comparative Example 1 (N 2 NH 3 The atmosphere was replaced with pure N 2 atmosphere); the difference between the control group 3 and the experimental group is that a high proportion of Fe-N 4 The nitrogen-doped porous carbon material was replaced by the material prepared in Comparative Example 2 (without vacuuming and pressurizing steps); the differences between the control groups 4, 5, and 6 and the experimental groups were as follows: 4 The nitrogen-doped porous carbon material was replaced with the materials prepared in Examples 7, 9 and 10 (the pressures of pressurized ammonia gas were 0.2, 0.4 and 0.5 MPa, respectively).

[0070] The results of the test group and four control groups on ATZ degradation are as follows: Figure 2 and 3 shown.

[0071] Figure 2 It shows that after 30 minutes of reaction time, in the control group 1 without catalyst, ozone oxidized 45.6% of ATZ: 2 In the control group 2 of the material fired under the atmosphere, 76.2% of ATZ was catalytically oxidized by ozone; in the control group 3 without vacuum and pressure conditions, 49.3% of ATZ was catalytically oxidized by ozone; in the control groups 4, 5, and 6 of the materials prepared under different pressures (0.2, 0.4, and 0.5 MPa), 79.2%, 89.0%, and 85.5% of ATZ were catalytically oxidized by ozone, respectively. 4 In the experimental group of nitrogen-doped porous carbon materials, ATZ was almost completely decomposed, and more than 95.0% of ATZ was catalytically oxidized within 5 minutes.

[0072] exist Figure 3 In the figure, ■ represents the ozone outlet concentration when no catalyst is added (control group 1), and ▲ represents the N 2 The ozone outlet concentration of the material fired under the atmosphere (control group 2), ◆ represents the ozone outlet concentration of the material prepared under no vacuum and pressurization conditions (control group 3), △, ▽ and ○ represent the ozone outlet concentration of the material prepared under different pressurization conditions (0.2, 0.4 and 0.5 MPa) (control groups 4, 5, 6), and ● represents the ozone outlet concentration of the material loaded with a high proportion of Fe-N in the hydrophilic pores prepared in Experiment 1. 4 Ozone outlet concentration when nitrogen-doped porous carbon materials.

[0073] Figure 3 This indicates that a high proportion of Fe-N is loaded in the hydrophilic pores. 4 Nitrogen-doped porous carbon materials can catalyze the decomposition of ozone to produce free radicals. According to ICP-OES test, the amount of iron ions dissolved in the simulated wastewater after the reaction was only 0.005 mg / L, which is extremely low, indicating that the hydrophilic pores are loaded with a high proportion of Fe-N 4 Nitrogen-doped porous carbon materials have high stability.

Claims

1. A porous carbon material doped with Fe-N4 with a high proportion of hydrophilic pores, characterized in that: The porous carbon loaded with iron elements is obtained by evacuating the porous carbon, pressurizing it with ammonia, and then calcining it in an atmosphere containing ammonia; the porous carbon is kept for 1h-10h after evacuating the porous carbon; after the vacuum is maintained, the porous carbon is pressurized to 0.2MPa-0.5MPa with ammonia.

2. The hydrophilic pores of the porous carbon material with a high proportion of Fe-N4 nitrogen doped therein according to claim 1, characterized in that: The porous carbon loaded with iron element is obtained by ultrasonicating the porous carbon and Fe(NO3)3 in water.

3. The method for preparing a porous carbon material doped with Fe-N4 with a high proportion of hydrophilic channels as claimed in claim 1, characterized in that: Step 1, placing porous carbon and Fe(NO3)3 in ultrapure water for ultrasonic treatment; Step 2: Dry the solid phase product after the treatment in step 1, heat it in an oil bath and evacuate it under negative pressure; keep it for more than 1 hour after evacuation; Step 3: introducing ammonia gas and pressurizing it to above 0.2 MPa, and cooling the solid phase product to room temperature for more than 1 hour; Step 4: Use liquid nitrogen to freeze the product obtained in step 3, and calcine the obtained solid particles under N2 and NH3 atmosphere to obtain a porous carbon material doped with Fe-N4 with a high proportion of hydrophilic channels.

4. The preparation method according to claim 3, characterized in that: In step 1, the weight ratio of Fe(NO3)3 to porous carbon is (0.1-10):100; the mass ratio of porous carbon to water is 0.1-1:10; and the ultrasonic time is 1h-6h.

5. The preparation method according to claim 3, characterized in that: In step 2, the drying temperature is 80°C to 120°C; the oil bath heating temperature is 100°C to 200°C; the negative pressure vacuuming is maintained for 1h to 10h after being evacuated to vacuum; in step 3, ammonia is used to increase the pressure to 0.3MPa and maintain it for 1h to 6h.

6. The preparation method according to claim 3, characterized in that: In step 4, the calcination condition is N2: NH3 = 1: 1, the temperature is increased to 550°C at 5°C per minute, calcined for 2 hours, and then cooled naturally.

7. Use of the nitrogen-doped porous carbon material with a high proportion of Fe-N4 loaded in the hydrophilic pores as claimed in claim 1 or 2 in catalyzing ozone decomposition of organic pollutants in water.

8. The use according to claim 7, characterized in that: The water body is agricultural wastewater or urban sewage.

Citation Information

Patent Citations

  • Advanced redox water treatment technology based on nitrogen-doped iron-carbon material with core-shell structure and for magnetic field recovery

    CN108940335A

  • Supported monatomic metal catalyst and preparation method and application thereof

    CN111036261A

  • Method for degrading organic pollutants in water by using nitrogen-doped porous carbon anchored monatomic cobalt catalyst to activate persulfate

    CN112408577A

  • Preparation and application of iron-nitrogen co-doped porous carbon material

    CN114053998A

  • Iron-nitrogen co-doped porous carbon prepared by using ferrate as iron source as well as preparation method and application of iron-nitrogen co-doped porous carbon

    CN114082432A