A low dielectric glass fiber composition and its application
By optimizing the composition and preparation process of glass fiber, we solve the problems of signal loss and low production efficiency of existing glass fiber in high-frequency signal transmission, and prepare low-dielectric glass fiber with excellent dielectric properties, which reduces manufacturing costs and improves efficiency. improve production efficiency.
Patent Information
- Application Number
- CN202210726068.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-06-23
AI Technical Summary
The signal loss of existing glass fibers increases significantly during high-frequency signal transmission, and the high viscosity in the high-temperature molten state leads to low production efficiency and easy generation of bubbles, which affects the drawing process.
A low-dielectric glass fiber composition composed of SiO2 50-58.5%, Al2O3 8-16%, B2O3 17-26%, etc. is used to reduce the melting temperature and viscosity of the glass liquid through a specific heating and drawing molding process to prepare the media. Glass fiber with lower electrical constant and dielectric loss.
It significantly reduces the manufacturing cost of glass fiber, improves production efficiency and product quality, optimizes dielectric properties, and is suitable for high-speed, low-loss transmission of high-frequency signals.
Smart Images

Figure BDA0003711011210000051 
Figure BDA0003711011210000061 
Figure BDA0003711011210000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass fibers, in particular to a low-dielectric glass fiber composition and application thereof. Background Art
[0002] The main components of glass fiber include silicon dioxide, aluminum oxide, calcium oxide, boron oxide, magnesium oxide, sodium oxide, etc. According to the alkali content in the glass, it can be divided into alkali-free glass fiber, medium-alkali glass fiber and high-alkali glass fiber. E glass, also known as alkali-free glass, is a borosilicate glass and is currently the most widely used type of glass fiber. However, the dielectric constant and loss tangent of E glass are relatively high. D glass, also known as low-dielectric glass, has a lower dielectric constant and loss tangent. It is mainly used to produce low-dielectric glass fibers with better dielectric strength. However, the melting temperature of D glass is higher and its machinability is poor.
[0003] B2O3-P2O5-SiO2 alkali-free glass has a smaller dielectric constant and lower loss tangent when the frequency is above 10GHz. However, the SiO2 content in this alkali-free glass is relatively high, which leads to its high viscosity in the high-temperature molten state, poor clarification effect, and difficulty in escaping bubbles in the glass liquid. At the same time, the glass fiber drawing temperature of this glass exceeds 1400℃, which not only seriously affects the production efficiency of the glass fiber, but also easily generates bubbles or stripes during the drawing process, which in turn causes broken wires. In addition, as the signal transmission frequency increases, the signal loss of existing glass fibers increases significantly, which is not conducive to high-speed, low-loss transmission of high-frequency signals.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The object of the present invention is to provide a low dielectric glass fiber composition and its application. The low dielectric glass fiber composition has a low drawing temperature, a relatively low dielectric constant and a relatively low dielectric loss, and also has a significant improvement effect on the insertion loss.
[0006] The invention provides a low dielectric glass fiber composition, comprising the following components by mass: SiO2 50-58.5%, Al2O3 8-16%, B2O3 17-26%, CaO 0-1.0%, ZnO 0-5.0%, BaO 0.5-6.0%, SrO0.5-3.0%, TiO2 0.1-5.0%, F2 0.1-1.8% and Na2O+K2O+Li2O 0.05-0.5%.
[0007] Further, the low dielectric glass fiber composition of the present invention comprises the following components by mass content: SiO2 52-58%, Al2O3 8-13.5%, B2O3 21-25%, CaO 0-1.0%, ZnO 0-4.5%, BaO 0.5-6.0%, SrO0.5-3.0%, TiO2 0.5-4.0%, F2 0.5-1.8% and Na2O+K2O+Li2O 0.05-0.3%.
[0008] Further, the low dielectric glass fiber composition of the present invention comprises the following components by mass content: SiO2 53.6-57.2%, Al2O3 8.5-11.9%, B2O3 21.5-23.8%, CaO 0-0.5%, ZnO 0-4.2%, BaO 1.6-5.9%, SrO 1.6-2.9%, TiO2 1.1-3.1%, F2 0.8-1.7% and Na2O+K2O+Li2O 0.1-0.2%.
[0009] The present invention also provides a method for preparing low dielectric glass fiber, comprising the following steps:
[0010] S1: preparing ingredients according to the composition of the above-mentioned low dielectric glass fiber composition;
[0011] S2: mixing and homogenizing the prepared raw materials, and then heating them to melt and clarify them to obtain glass liquid;
[0012] S3: Drawing the glass liquid into a wire to obtain low dielectric glass fiber.
[0013] In step S2, the heating rate is 4-6°C / min, and the heating time is 4-5h; the melting and clarification temperature is 1550-1620°C, and the time is 4-7h.
[0014] In step S3, the diameter of the low dielectric glass fiber is 3-15 μm.
[0015] The present invention also provides a low-dielectric glass fiber, which is prepared according to the above preparation method.
[0016] The low dielectric glass fiber of the present invention has a dielectric constant of ≤4.5 and a dielectric constant of ≤6×10 -4 Specifically, the dielectric constant of low dielectric glass fiber at a frequency of 1 GHz is 4.33-4.48, and the dielectric loss tangent is 3.69×10 -4 to 5.20×10 -4 .
[0017] The low dielectric glass fiber of the present invention has a dielectric constant of ≤4.4 and a dielectric constant of ≤2×10-3 Specifically, the dielectric constant of low dielectric glass fiber at a frequency of 10 GHz is 4.23-4.35, and the dielectric loss tangent is 1.38×10 -3 to 1.58×10 -3 .
[0018] The low dielectric glass fiber of the present invention has a glass viscosity of 1340-1390°C, and further 1344-1381°C at 1000P.
[0019] The present invention also provides a product comprising the above-mentioned low dielectric glass fiber, and the product is not strictly limited. For example, it can be a printed circuit board, a woven fabric, a non-woven fabric, a unidirectional fabric, a chopped strand, a chopped strand mat, a composite material, a communication signal transmission medium, etc.
[0020] The implementation of the present invention has at least the following advantages:
[0021] 1. The low dielectric glass fiber composition of the present invention significantly reduces the glass viscosity at 1000P. Due to the reduction in high temperature viscosity, the drawing temperature and the requirements for kiln equipment are reduced, which greatly reduces the manufacturing cost of glass fiber and improves the efficiency of large-scale manufacturing;
[0022] 2. The low dielectric glass fiber of the present invention has a low drawing temperature, few bubbles, good processability, and improved product output and production yield; at the same time, the low dielectric glass fiber has a lower dielectric constant and dielectric loss, excellent dielectric properties, a wider range of product applications, and higher economic benefits;
[0023] 3. The water resistance of the low dielectric glass fiber of the present invention is improved, which increases the service life of the product under complex conditions; in addition, the low dielectric glass fiber has a significant improvement effect on insertion loss, which is particularly beneficial for high-speed, low-loss transmission of high-frequency signals. DETAILED DESCRIPTION
[0024] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0025] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0026] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Examples 1-8
[0028] The low dielectric glass fiber compositions of Examples 1-8 include the following components by mass: SiO2 50-58.5%, Al2O3 8-16%, B2O3 17-26%, CaO 0-1.0%, ZnO 0-5.0%, BaO 0.5-6.0%, SrO0.5-3.0%, TiO2 0.1-5.0%, F2 0.1-1.8% and Na2O+K2O+Li2O 0.05-0.5%; the specific compositions of the low dielectric glass fiber compositions of Examples 1-8 are shown in Table 1.
[0029] The preparation method of the low dielectric glass fiber of Examples 1-8 comprises the following steps:
[0030] S1: Mixing ingredients according to the low dielectric glass fiber composition;
[0031] S2: mixing and homogenizing the prepared raw materials, and then heating them to melt and clarify them to obtain glass liquid;
[0032] S3: Drawing the glass liquid into a wire to obtain a low dielectric glass fiber;
[0033] In step S2, the heating rate is 4-6°C / min, and the heating time is 4-5h; the melting and clarifying temperature is 1550-1620°C, and the time is 4-7h. The specific parameters in the preparation process of the low dielectric glass fiber composition of Examples 1-8 can be determined according to the respective components, as long as the composition of the prepared low dielectric glass fiber composition meets Table 1.
[0034] The performance test is carried out using the following method:
[0035] Dielectric properties (D k , D f ): The experimental sample was cut and ground to produce a sample of 80 mm × 3 mm × 1 mm. The obtained sample was dried at 110°C for 24 hours and stored in a constant temperature and humidity chamber at 23°C and 60% humidity for 24 hours. Subsequently, the dielectric constant D of the above sample at 1 GHz and 10 GHz was measured using the cavity resonant cavity dielectric performance test device of Japan AET Co., Ltd. in accordance with JIS C2565:1992. k and dielectric loss tangent Df .
[0036] Liquidus temperature T L :Put a glass sample to be tested with a size of 10×10×10mm into a gradient furnace that has been heated to 800-1300℃, heat treat for 8 hours, then take it out and cool it to room temperature to obtain a cooled glass. Use a polarizing microscope to observe the crystallization inside the cooled glass: if there is crystallization within 2 mm from the surface of the cooled glass, it is determined that the temperature of the melting treatment is lower than the liquidus temperature of the glass sample to be tested; if there is no crystallization inside the cooled glass, it is determined that the temperature of the melting treatment is higher than the liquidus temperature of the glass sample to be tested; if there is no crystallization within 2 mm from the surface of the cooled glass, but there is crystallization within 2 mm from the surface of the cooled glass, the temperature of this position in the gradient furnace is taken as the liquidus temperature T of the glass sample to be tested. L .
[0037] T3 temperature test: After the glass to be tested is broken into appropriate particle sizes, 100 grams are weighed and placed in a platinum crucible, and then the platinum crucible is placed in a high-temperature heating furnace, and the position of the platinum rotor is adjusted to the center of the platinum crucible, and heating is started according to the program. After the temperature rises to a high temperature, it is kept warm for a period of time, and then cooled according to the program. The torque of the rotor is recorded every time the set temperature is reached, and it is converted into the corresponding glass viscosity value at this temperature. The T3 temperature refers to the temperature corresponding to the viscosity equal to 1000 poise.
[0038] The test results are shown in Table 2.
[0039] Table 1 Composition of low dielectric glass fiber composition of each example (wt%)
[0040]
[0041]
[0042] Comparative Example 1
[0043] This comparative example uses E glass, which is widely used in industry, as a control, and its composition is as follows:
[0044] SiO2 54.8%, Al2O3 14.3%, B2O3 6.3%, CaO 22.6%, MgO 1.4% and F2 0.6%; the preparation method and the test method refer to Example 1.
[0045] Comparative Example 2
[0046] This comparative example uses NE glass fiber as a control, and its composition is as follows:
[0047] SiO2 54.7%, Al2O3 14.9%, B2O3 19.9%, CaO 4.0%, MgO 4.0%, TiO2 2.0% and F2 0.5%; the preparation method and the test method refer to Example 1.
[0048] Comparative Example 3
[0049] The composition of the glass fiber composite of this comparative example is as follows:
[0050] SiO2 53.6%, Al2O3 12.4%, B2O3 22.7%, CaO 3.1%, MgO 1.0%, SrO 4.1%, TiO2 2.1% and F2 1.0%; the preparation method and the test method refer to Example 1.
[0051] Comparative Example 4
[0052] The composition of the glass fiber composite of this comparative example is as follows:
[0053] SiO2 57.72%, Al2O3 11.33%, B2O3 23.98%, CaO 5.82% and F2 1.15%; the preparation method and the test method refer to Example 1.
[0054] Comparative Example 5
[0055] The composition of the glass fiber composite of this comparative example is as follows:
[0056] SiO2 50.73%, B2O3 24.57%, Al2O3 17.07%, P2O5 3.96%, CaO 3.30%, MgO0.04%, TiO2 0.01%, Fe2O3 0.03%, Na2O 0.04%, K2O 0.01% and SnO2 0.22%; the preparation method and test method refer to Example 1.
[0057] Table 2 Performance test results of various low dielectric glass fibers
[0058]
[0059] Note: "E-04" in Table 2 means "×10 -4 ", "E-03" means "×10 -3 ”.
[0060] Test Example 1
[0061] The loss performance test boards were prepared by using low loss grade boards and the glass fibers of Examples 1-8 and Comparative Examples 1-5, respectively. The corresponding loss values were tested by the FD method using a vector network analyzer. The results are shown in Table 3.
[0062] Table 3 Insertion loss changes of PCB signals with various glass fibers at different frequencies (dB / cm)
[0063]
[0064] It can be seen from Table 3 that, compared with E glass fiber, NE glass fiber and other glass fibers, the low dielectric glass fibers of the embodiments of the present invention can reduce signal loss to a certain extent; at the same time, the higher the signal transmission frequency, the more obvious the improvement of the insertion loss by each low dielectric glass fiber.
[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A low dielectric glass fiber composition, characterized in that: It is composed of the following components in mass content: SiO2 50-58.5%, Al2O3 8-16%, B2O3 17-26%, CaO 0-1.0%, ZnO 0-5.0%, BaO 0.5-6.0%, SrO 0.5-3.0%, TiO2 0.1-5.0%, F2 0.1-1.8% and Na2O+K2O+Li2O 0.05-0.5%.
2. The low dielectric glass fiber composition according to claim 1, characterized in that It is composed of the following components in mass content: SiO2 52-58%, Al2O3 8-13.5%, B2O3 21-25%, CaO 0-1.0%, ZnO 0-4.5%, BaO 0.5-6.0%, SrO 0.5-3.0%, TiO2 0.5-4.0%, F2 0.5-1.8% and Na2O+K2O+Li2O 0.05-0.3%.
3. A method for preparing low dielectric glass fiber, characterized in that: The steps include: S1: The composition of the low dielectric glass fiber composition according to claim 1 or 2; S2: mixing and homogenizing the prepared raw materials, and then heating them to melt and clarify them to obtain glass liquid; S3: Drawing the glass liquid into a wire to obtain low dielectric glass fiber.
4. The preparation method according to claim 3, characterized in that: The heating rate is 4-6°C / min, and the heating time is 4-5h; the melting and clarification temperature is 1550-1620°C, and the time is 4-7h.
5. The preparation method according to claim 3, characterized in that: The diameter of low dielectric glass fibers is 3-15 μm.
6. A low dielectric glass fiber, characterized in that: Prepared according to any one of the preparation methods of claims 3-5.
7. The low dielectric glass fiber according to claim 6, characterized in that: The low dielectric glass fiber has a dielectric constant of ≤4.5 and a dielectric constant of ≤6×10 -4 The dielectric loss tangent.
8. The low dielectric glass fiber according to claim 6, characterized in that: The low dielectric glass fiber has a dielectric constant of ≤4.4 and a dielectric constant of ≤2×10 -3 The dielectric loss tangent.
9. The low dielectric glass fiber according to claim 6, characterized in that: The low dielectric glass fiber has a glass temperature of 1340-1390°C at 1000P.
10. A product comprising the low dielectric glass fiber according to any one of claims 6 to 9, characterized in that: The product is a printed circuit board, a woven fabric, a nonwoven fabric, a chopped strand, a chopped strand mat, a composite material, or a communication signal transmission medium.
Citation Information
Patent Citations
Glass with low dielectric constant
CN101033114A