A cesium copper iodine blue light nanocrystal and its preparation method and use
By using bifunctional silane coupling agent as ligand in cesium copper iodine blue light nanocrystals, the core-shell-like structure is formed through anti-solvent method and hydrolysis, the dispersion and water-blocking problems of nanocrystals are solved, and its in-photoelectric field is improved Application performance.
Patent Information
- Application Number
- CN202210787558.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-07-04
AI Technical Summary
The prior art is difficult to achieve uniform dispersion and high water resistance in cesium copper iodine blue light nanocrystals, resulting in low fluorescence efficiency and instability in photoelectric component applications.
A bifunctional silane coupling agent is used as a ligand to prepare cesium copper-iodine blue light nanocrystals by anti-solvent method, and a core-shell-like structure is formed by hydrolysis to inhibit agglomeration and enhance dispersion and water-blocking properties.
It significantly improves the dispersion and water resistance of cesium copper iodine blue light nanocrystals, improves the fluorescence efficiency, and reduces the fluorescence efficiency attenuation after soaking in water, and is suitable for the field of photoelectricity.
Smart Images

Figure CN115074113B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of perovskite luminescent materials and relates to a cesium copper iodine blue light nanocrystal and a preparation method and application thereof. Background Art
[0002] Lead halide perovskite is considered one of the most promising materials in the field of optoelectronics due to its high quantum efficiency and adjustable band gap. However, its popularity in certain fields is limited by its small Stokes shift, susceptibility to "self-absorption", instability, and lead toxicity. In recent years, cesium copper iodide, as a perovskite material with good stability and luminescence properties, has attracted extensive attention in the field of detection and luminescence due to its wide spectral range and large Stokes shift, and almost negligible self-absorption.
[0003] However, cesium copper iodide obtained by the prior art is mostly bulk material, and its large size makes it difficult to achieve uniform dispersion in solvents or films, thus restricting its application and development in optoelectronic components.
[0004] Some current preparation methods have many disadvantages. (1) The hot injection method requires high temperature and atmosphere protection. The heating and cooling process is slow during large-scale production, making it difficult to ensure a uniform reaction environment and, therefore, the uniformity of the product. (2) The cesium copper iodine nanocrystals prepared by the general anti-solvent method are severely agglomerated and have low fluorescence efficiency, which limits their application in micro optoelectronic components. (3) The muffle furnace calcination method takes a long time to prepare and produces a large powder particle size. There is also the problem of decomposition and failure in a humid environment.
[0005] For example, CN110117024A discloses a method for preparing zero-dimensional lead-free cesium copper iodine perovskite blue light nanocrystals. The precursor solution is heated and dissolved and then injected into an organic solvent, and the cesium copper iodine nanocrystals are obtained by centrifugal washing. The sample prepared by this method has low fluorescence efficiency and serious nanocrystal agglomeration, and poor water barrier performance. Zhang et al. used hot injection to prepare Cs3Cu2I5 nanocrystals with good dispersibility (DOI: 10.1002 / adfm.202105771), but this method requires high temperature and atmosphere protection, which is difficult to scale up industrially. Huang et al. used a muffle furnace to calcine cesium copper iodine blue phosphor (DOI: 10.1016 / j.mtchem.2020.100288), but the preparation method is time-consuming, the powder particle size is large and difficult to disperse, and it will fail and decompose in a humid environment. Although many such methods can obtain cesium copper iodine materials with good stability, their water barrier and dispersibility are still far from practical applications.
[0006] Therefore, how to improve the water resistance and dispersibility of cesium copper iodine blue light nanocrystals while ensuring that their fluorescence efficiency is not affected is a technical problem that needs to be solved urgently. Summary of the invention
[0007] The purpose of the present invention is to provide a cesium copper iodine blue light nanocrystal and its preparation method and use. The present invention adopts a bifunctional silane coupling agent as a ligand, prepares the cesium copper iodine blue light nanocrystal by an anti-solvent method, and forms a core-shell structure by hydrolysis, and forms a cross-linked bifunctional silane coupling agent on its surface, which inhibits the agglomeration of the material, increases the water barrier performance of the material, greatly improves the dispersibility and water barrier performance of the cesium copper iodine blue light nanocrystal, and further improves its fluorescence efficiency.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing cesium copper iodine blue light nanocrystals, the preparation method comprising the following steps:
[0010] Mixing a bifunctional silane coupling agent ligand, a cesium copper iodine perovskite nanocrystal precursor and a first solvent, adding a second solvent to perform an anti-solvent reaction, and hydrolyzing the reacted substance to obtain the cesium copper iodine blue light nanocrystal;
[0011] The first solvent and the second solvent have different polarities.
[0012] In the present invention, the first solvent and the second solvent have different polarities, that is, the two solvents can achieve the role of anti-solvents. When the first solvent is a good solvent, the second solvent is an anti-solvent, and when the first solvent is an anti-solvent, the second solvent is a good solvent.
[0013] The present invention adopts a bifunctional silane coupling agent as a ligand, prepares cesium copper iodine blue light nanocrystals by an anti-solvent method, and forms a core-shell structure by hydrolysis, and forms a cross-linked bifunctional silane coupling agent on its surface, which inhibits the agglomeration of the material, increases the water barrier performance of the material, greatly improves the dispersibility and water barrier of the cesium copper iodine blue light nanocrystals, and further improves its fluorescence efficiency. In addition, the preparation method provided by the present invention does not require high temperature and controls the reaction atmosphere, and is easy to scale up production.
[0014] In the present invention, by introducing a bifunctional silane coupling agent ligand during the anti-solvent method, on the one hand, the size of the cesium copper iodine nanocrystal is limited to achieve a spatial confinement effect, prevent the nanocrystals from agglomerating, and improve the dispersibility of the nanocrystals in the solvent and the film; on the other hand, through the hydrolysis reaction after the anti-solvent method, the ligand forms a core-shell structure on the surface of the cesium copper iodine nanocrystal through cross-linking, thereby forming a dense surface protective layer, which reduces the problem of decomposition failure when exposed to water; in addition, the type of ligand can be flexibly adjusted to adapt to solvents and films in different polar environments, thereby greatly improving its applicability.
[0015] In the present invention, if hydrolysis is not performed after the anti-solvent reaction, cross-linking cannot be performed on the surface of the cesium copper iodine nanocrystals to form a core-shell structure, thereby failing to solve the problems of water resistance and dispersibility of the cesium copper iodine nanocrystals.
[0016] Preferably, the cesium copper iodide perovskite nanocrystal precursor is mixed with a good solvent.
[0017] In the present invention, the cesium copper iodide perovskite nanocrystal precursor can be better dissolved in a good solvent, but it does not mean that it cannot be dissolved in an anti-solvent.
[0018] Preferably, the bifunctional silane coupling agent ligand includes any one of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-bromopropyltrimethoxysilane, 3-aminopropyldimethylmethoxysilane, 3-[2-(2-aminoethylamino)ethylamino]propyl-trimethoxysilane or 3-aminopropyldimethoxymethylsilane, or a combination of at least two thereof, preferably 3-aminopropyltrimethoxysilane.
[0019] Preferably, the mixing comprises co-mixing or stepwise mixing, preferably co-mixing.
[0020] In the present invention, when the first solvent is a good solvent, the effect of mixing together is better.
[0021] Preferably, the co-mixing is adding and mixing the bifunctional silane coupling agent ligand, the cesium copper iodide perovskite nanocrystal precursor and the first solvent.
[0022] Preferably, the step-by-step mixing is to first mix the bifunctional silane coupling agent ligand with the first solvent, and then add the cesium copper iodide perovskite nanocrystal precursor.
[0023] In the present invention, it is not the case that step-by-step mixing can be more uniform as proposed in conventional methods. On the contrary, mixing together can better achieve the coordination of anions and cations, thereby improving the size uniformity, dispersibility and stability of cesium copper iodide perovskite nanocrystals.
[0024] Preferably, the cesium copper iodide perovskite nanocrystal precursor comprises cesium iodide and cuprous iodide.
[0025] Preferably, the molar ratio of the cesium iodide to the bifunctional silane coupling agent ligand is 1:(1-1.5), for example, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4 or 1:1.5.
[0026] In the present invention, if the molar ratio of the bifunctional silane coupling agent ligand to cesium iodide is too small, that is, too little ligand is added, incomplete coordination will occur, and the crystallization rate of the ions not participating in the coordination will be too fast, resulting in the problem of too large grains. If the molar ratio is too large, that is, too much ligand is added, the ion mobility will be seriously affected, and then the lattice integrity will be affected.
[0027] Preferably, the molar ratio of the bifunctional silane coupling agent ligand to the first solvent is 1:(10-20), for example, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19 or 1:20, etc.
[0028] In the present invention, if the molar ratio of the bifunctional silane coupling agent ligand to the first solvent is too large, that is, the solvent is too little, resulting in incomplete dissolution, while if the molar ratio is too large, that is, the solvent is too much, resulting in increased costs.
[0029] In the present invention, the amount of the second solvent added is not limited, and it only needs to be added to obtain precipitation of nanocrystals.
[0030] Preferably, the method of mixing comprises stirring.
[0031] Preferably, the stirring time is 2 to 5 hours, such as 2 hours, 3 hours, 4 hours or 5 hours.
[0032] Preferably, the first solvent and the second solvent each independently comprise a good solvent and an anti-solvent.
[0033] Preferably, the good solvent includes any one of dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, n-hexane or dichloromethane, or a combination of at least two thereof.
[0034] Preferably, the anti-solvent comprises any one of isopropanol, toluene or chloroform, or a combination of at least two thereof.
[0035] Preferably, the reaction is carried out under ice bath ultrasound.
[0036] Preferably, the reaction is followed by centrifugation and washing.
[0037] Preferably, the hydrolysis process comprises:
[0038] The reacted material is dissolved in a solvent, and water is added under ultrasonic conditions for hydrolysis.
[0039] Preferably, the molar ratio of the bifunctional silane coupling agent ligand to water is 1:(4-7), for example, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5 or 1:7, etc.
[0040] In the hydrolysis process of the present invention, if the molar ratio of the ligand to water is too large, that is, too little water is added, it will lead to incomplete hydrolysis and incomplete cross-linking, while if the molar ratio is too large, the cesium copper iodine nanocrystal lattice will be directly dissociated.
[0041] As a preferred technical solution, the preparation method comprises the following steps:
[0042] Adding a bifunctional silane coupling agent ligand, cesium iodide, cuprous iodide and a first solvent at a molar ratio of cesium iodide to bifunctional silane coupling agent ligand of 1:(1-1.5) together and stirring for 2-5 hours, adding a second solvent to carry out an anti-solvent reaction under ice bath ultrasound, centrifuging, washing, dissolving the washed substance in a solvent, adding water to hydrolyze, and obtaining the cesium copper iodine blue light nanocrystals;
[0043] Among them, the polarity of the first solvent is different from that of the second solvent, and the first solvent and the second solvent each independently include a good solvent and an anti-solvent; the molar ratio of the bifunctional silane coupling agent ligand to the first solvent is 1:(10-20); the molar ratio of the bifunctional silane coupling agent ligand to water is 1:(4-7).
[0044] In a second aspect, the present invention provides a cesium copper iodine blue light-emitting nanocrystal, which is prepared by the cesium copper iodine blue light-emitting nanocrystal preparation method as described in the first aspect, and the surface of the cesium copper iodine blue light-emitting nanocrystal is cross-linked with a bifunctional silane coupling agent.
[0045] In a third aspect, the present invention further provides a use of cesium copper iodine blue light-emitting nanocrystals, which includes using the cesium copper iodine blue light-emitting nanocrystals as described in the second aspect in the field of optoelectronics.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] In the present invention, by introducing a bifunctional silane coupling agent ligand during the anti-solvent method, on the one hand, the size of the cesium copper iodine nanocrystal is limited to achieve a spatial confinement effect, prevent the nanocrystals from agglomerating, and improve the dispersibility of the nanocrystals in the solvent and the film; on the other hand, through the hydrolysis reaction after the anti-solvent method, the ligand forms a core-shell structure on the surface of the cesium copper iodine nanocrystal through cross-linking, thereby forming a dense surface protective layer, which reduces the problem of decomposition failure when exposed to water; in addition, the type of ligand can be flexibly adjusted to adapt to solvents and films in different polar environments, thereby greatly improving its applicability. The cesium copper iodine blue light nanocrystal provided by the present invention, after adjusting the molar ratio of the bifunctional silane coupling agent ligand to cesium iodide and water, is excited under 300nm excitation light, and its fluorescence efficiency before soaking in water can reach more than 86.54%, and the fluorescence efficiency after soaking in water can reach more than 75.32%, and the fluorescence efficiency before and after soaking in water only decays by 14.5% or even lower. When the bifunctional silane coupling agent ligand is 3-aminopropyltrimethoxysilane, its fluorescence efficiency before soaking in water can reach more than 93.62%, and the fluorescence efficiency after soaking in water can reach more than 83.03%, and the fluorescence efficiency before and after soaking in water only decays by 11.6% or even lower, which can be as low as less than 5.3%. In addition, the preparation method does not require high temperature and controls the reaction atmosphere, and is easy to scale up production. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 It is a schematic diagram of the process of the preparation method in a specific embodiment of the present invention.
[0049] Figure 2 This is a comparison chart of the dispersion effects of cesium copper iodine blue light nanocrystals on PS glue films provided by Example 1 and Comparative Example 1.
[0050] Figure 3 This is a comparison chart of the dispersion effects of cesium copper iodine blue light nanocrystals on PS glue films provided by Example 2 and Comparative Example 1.
[0051] Figure 4 This is a comparative diagram of the fluorescence efficiency of the cesium copper iodine blue light nanocrystals provided in Example 1 and Comparative Example 1 before being soaked in water.
[0052] Figure 5 This is a comparative diagram of the fluorescence efficiency of the cesium copper iodine blue light nanocrystals provided in Example 1 and Comparative Example 1 after being soaked in water. DETAILED DESCRIPTION
[0053] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0054] In a specific embodiment, the present invention provides a method for preparing cesium copper iodine blue light nanocrystals, such as Figure 1As shown in the schematic diagram of the preparation process, the preparation method comprises the following steps:
[0055] Mixing a bifunctional silane coupling agent ligand, a cesium copper iodine perovskite nanocrystal precursor and a first solvent, adding a second solvent to perform an anti-solvent reaction, and hydrolyzing the reacted substance to obtain the cesium copper iodine blue light nanocrystal;
[0056] The first solvent and the second solvent have different polarities, and the first solvent and the second solvent each independently include a good solvent and an antisolvent; and the cesium copper iodide perovskite nanocrystal precursor includes cesium iodide and cuprous iodide.
[0057] Example 1
[0058] This embodiment provides a method for preparing cesium copper iodine blue light nanocrystals. Based on the preparation method of the above specific implementation method, a more specific preparation method is as follows:
[0059] (1) Weigh 0.7171 g of 3-aminopropyltrimethoxysilane (0.004 mol), 0.7794 g of cesium iodide (0.003 mol), and 0.3809 g of cuprous iodide and dissolve them in 4 mL (0.056 mol) of dimethyl sulfoxide. Stir at room temperature for 3 h to form a homogeneous clear light yellow mixed solution.
[0060] (2) 1 mL of the mixed solution was slowly added dropwise to 10 mL of isopropanol under ice bath ultrasound conditions. A white precipitate was precipitated during the addition. After the addition was completed, centrifugation was performed at a speed of 10,000 rpm for 10 minutes. After the centrifugation was completed, a white precipitate was obtained at the bottom, which was the crude cesium copper iodine nanocrystal. Then, 10 mL of isopropanol was added and centrifuged twice for washing;
[0061] (3) Under ultrasonic conditions, 0.4 mL (molar weight 0.02 mol) of deionized water was added dropwise to 10 mL of cesium copper iodine isopropanol dispersion. After the addition was completed, ultrasonic treatment was performed for 10 minutes. Finally, the white precipitate was vacuum dried for 12 hours to obtain cesium copper iodine blue light nanocrystals with a core-shell structure (cross-linked aminopropyltrimethoxysilane was formed on the surface).
[0062] Example 2
[0063] The difference between this embodiment and embodiment 1 is that the ligand in step (1) of this embodiment is 0.8855 g of 3-aminopropyltriethoxysilane (0.004 mol).
[0064] The rest of the preparation methods and parameters were the same as those in Example 1.
[0065] Example 3
[0066] The difference between this embodiment and embodiment 1 is that the ligand in step (1) of this embodiment is 0.7653 g of 3-aminopropylmethyldiethoxysilane (0.004 mol).
[0067] The rest of the preparation methods and parameters were the same as those in Example 1.
[0068] Example 4
[0069] The difference between this example and Example 1 is that the ligand in step (1) of this example is 0.9727 g of 3-bromopropyltrimethoxysilane (0.004 mol).
[0070] The rest of the preparation methods and parameters were the same as those in Example 1.
[0071] Example 5
[0072] The difference between this embodiment and embodiment 1 is that in step (1) of this embodiment, the mass of 3-aminopropyltrimethoxysilane is 0.5378 g (molar weight is 0.003 mol), and the molar ratio of cesium iodide to the bifunctional silane coupling agent ligand is 1:1.
[0073] The rest of the preparation methods and parameters were the same as those in Example 1.
[0074] Example 6
[0075] The difference between this embodiment and embodiment 1 is that in step (1) of this embodiment, the mass of 3-aminopropyltrimethoxysilane is 0.8067 (molar amount is 0.0045 mol), and the molar ratio of cesium iodide to the bifunctional silane coupling agent ligand is 1:1.5.
[0076] The rest of the preparation methods and parameters were the same as those in Example 1.
[0077] Example 7
[0078] The difference between this embodiment and embodiment 1 is that the mass of 3-aminopropyltrimethoxysilane in step (1) of this embodiment is 1.0757 g (molar weight is 0.0.006 mol), that is, the molar ratio of cesium iodide to the bifunctional silane coupling agent ligand is 1:2.
[0079] The rest of the preparation methods and parameters were the same as those in Example 1.
[0080] Example 8
[0081] The difference between this embodiment and embodiment 1 is that the solvent in step (1) of this embodiment is isopropanol, and the solvent in step (2) is dimethyl sulfoxide.
[0082] The rest of the preparation methods and parameters were the same as those in Example 1.
[0083] Example 9
[0084] The difference between this embodiment and embodiment 1 is that in step (1) of this embodiment, 3-aminopropyltrimethoxysilane is first dissolved in dimethyl sulfoxide for dispersion, and then cesium iodide and cuprous iodide are added.
[0085] The rest of the preparation methods and parameters were the same as those in Example 1.
[0086] Example 10
[0087] The difference between this embodiment and embodiment 1 is that in step (3) of this embodiment, the amount of deionized water added is 0.3 mL (molar weight 0.016 mol), that is, the molar ratio of ligand to water is 1:4.25.
[0088] The rest of the preparation methods and parameters were the same as those in Example 1.
[0089] Embodiment 11
[0090] The difference between this embodiment and embodiment 1 is that in step (3) of this embodiment, the amount of deionized water added is 0.5 mL (molar weight 0.028 mol), that is, the molar ratio of ligand to water is 1:7.
[0091] The rest of the preparation methods and parameters were the same as those in Example 1.
[0092] Example 12
[0093] The difference between this embodiment and embodiment 1 is that in step (3) of this embodiment, the amount of deionized water added is 0.58 mL (molar weight 0.032 mol), that is, the molar ratio of ligand to water is 1:8.
[0094] The rest of the preparation methods and parameters were the same as those in Example 1.
[0095] Embodiment 13
[0096] The difference between this embodiment and embodiment 1 is that in step (3) of this embodiment, the amount of deionized water added is 0.2 mL (molar weight 0.012 mol), that is, the molar ratio of ligand to water is 1:3.
[0097] The rest of the preparation methods and parameters were the same as those in Example 1.
[0098] Comparative Example 1
[0099] The difference between this comparative example and Example 1 is that 3-aminopropyltrimethoxysilane is not added in step (1) of this comparative example.
[0100] The rest of the preparation methods and parameters were the same as those in Example 1.
[0101] Figure 2The figure shows the dispersion effect comparison of cesium copper iodine blue light nanocrystals provided by Example 1 and Comparative Example 1 on PS glue film. Figure 3 The figure shows the dispersion effect comparison of cesium copper iodine blue light nanocrystals provided in Example 2 and Comparative Example 1 on PS glue film. Figure 2 and Figure 3 (Left) is the dispersion of cesium copper iodine blue light nanocrystals in comparative example 1. Figure 2 and Figure 3 (Right) The dispersion conditions of the cesium copper iodine blue light-emitting nanocrystals in Example 1 and Example 2, respectively. From the figures, it can be clearly seen that the addition of the bifunctional silane coupling agent ligand of the present invention during the preparation process greatly improves the dispersion of the cesium copper iodine blue light-emitting nanocrystals without agglomeration.
[0102] Figure 4 The fluorescence efficiency comparison diagram of the cesium copper iodine blue light nanocrystals provided in Example 1 and Comparative Example 1 before being soaked in water is shown. Figure 4 It can be seen that after the bifunctional silane coupling agent ligand of the present invention is added into the preparation method, the fluorescence efficiency of the cesium copper iodine blue light nanocrystals is also significantly improved.
[0103] Figure 5 The fluorescence efficiency comparison diagram of the cesium copper iodine blue light nanocrystals after being soaked in water provided by Example 1 and Comparative Example 1 is shown. Figure 5 It can be seen that after the cesium copper iodine blue light nanocrystals provided by the present invention are soaked in water, the fluorescence efficiency stability is good, indicating that the material obtained by the preparation method of the present invention has good water barrier properties.
[0104] Comparative Example 2
[0105] The difference between this comparative example and Example 1 is that step (3) is not performed in this comparative example, and the material after washing in step (2) is directly dried.
[0106] The rest of the preparation methods and parameters were the same as those in Example 1.
[0107] The cesium copper iodine blue light nanocrystals provided in Example 1-13 and Comparative Example 1-2 were used to prepare PS adhesive films. The fluorescence efficiency of the PS adhesive films provided in Example 1-13 and Comparative Example 1-2 was tested before and after soaking in water. The test conditions were to use 300nm excitation light to excite the film samples at room temperature, and the blank reference curve and the film sample curve were integrally calculated. The results are shown in Table 1.
[0108] Table 1
[0109]
[0110]
[0111] From the data results of Examples 1-4, it can be seen that 3-aminopropyltrimethoxysilane has a better water-blocking effect.
[0112] It can be seen from the data results of Example 1 and Examples 5-7 that adding too much bifunctional silane coupling agent ligand is not conducive to the lattice integrity of the nanocrystals, thereby affecting the water barrier properties.
[0113] From the data results of Example 1 and Example 8, it can be seen that whether the anti-solvent or the good solvent is added first, cesium copper iodine blue light nanocrystals with good dispersibility and water barrier properties can be obtained.
[0114] From the data results of Example 1 and Example 9, it can be seen that the stepwise addition of the raw materials in step (1) will affect the dispersibility and water barrier properties of the cesium copper iodine nanocrystals.
[0115] From the data results of Example 1 and Examples 10-13, it can be seen that if too much water is added during the hydrolysis process, the cesium copper iodine nanocrystal lattice will be directly dissociated, resulting in poor water barrier properties. If too little water is added, the hydrolysis will be incomplete and the cross-linking will not be thorough, which will affect the formation of a good water barrier material.
[0116] From the data results of Examples 1-4 and Comparative Example 1, it can be seen that without adding the bifunctional silane coupling agent ligand, the obtained cesium copper iodine blue light nanocrystals have obvious agglomeration and extremely poor water barrier properties.
[0117] From the data results of Example 1 and Comparative Example 2, it can be seen that after the anti-solvent reaction, no hydrolysis reaction is carried out, and cesium copper iodine nanocrystals with good water barrier properties cannot be obtained.
[0118] In summary, the present invention adopts a bifunctional silane coupling agent as a ligand to prepare cesium copper iodine blue light-emitting nanocrystals by an anti-solvent method, and at the same time forms a core-shell structure through hydrolysis, and forms a cross-linked bifunctional silane coupling agent on its surface, which inhibits the agglomeration of the material, increases the water barrier performance of the material, greatly improves the dispersibility and water barrier properties of the cesium copper iodine blue light-emitting nanocrystals, and further improves its fluorescence efficiency. The cesium copper iodine blue light nanocrystal provided by the present invention, after adjusting the molar ratio of the bifunctional silane coupling agent ligand to cesium iodide and water, is excited under 300nm excitation light, and its fluorescence efficiency before soaking in water can reach more than 86.54%, and the fluorescence efficiency after soaking in water can reach more than 75.32%, and the fluorescence efficiency before and after soaking in water only decays by 14.5% or even lower, when the bifunctional silane coupling agent ligand is 3-aminopropyltrimethoxysilane, its fluorescence efficiency before soaking in water can reach more than 93.62%, and the fluorescence efficiency after soaking in water can reach more than 83.03%, and the fluorescence efficiency before and after soaking in water only decays by 11.6% or even lower, which can be as low as less than 5.3%. In addition, the preparation method provided by the present invention does not require high temperature and controls the reaction atmosphere, and is easy to scale up production.
[0119] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing cesium copper iodine blue light nanocrystals, characterized in that: The preparation method comprises the following steps: The bifunctional silane coupling agent ligand, the cesium copper iodine perovskite nanocrystal precursor and the first solvent are mixed, the second solvent is added to carry out an anti-solvent reaction under ice bath ultrasound conditions, and the reacted substance is hydrolyzed to obtain the cesium copper iodine blue light nanocrystal; The hydrolysis process comprises: The reacted substance is dissolved in a solvent, and water is added under ultrasonic conditions for hydrolysis; after hydrolysis, a cross-linked bifunctional silane coupling agent is formed on the surface of the cesium copper iodine blue light nanocrystal; wherein the first solvent and the second solvent have different polarities; The molar ratio of the bifunctional silane coupling agent ligand to water is 1:(4-7); The bifunctional silane coupling agent ligand includes any one of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-bromopropyltrimethoxysilane, 3-aminopropyldimethylmethoxysilane, 3-[2-(2-aminoethylamino)ethylamino]propyl-trimethoxysilane or 3-aminopropyldimethoxymethylsilane, or a combination of at least two thereof; The first solvent and the second solvent each independently include a good solvent and an anti-solvent.
2. The method for preparing cesium copper iodine blue light nanocrystals according to claim 1, characterized in that: The bifunctional silane coupling agent ligand is 3-aminopropyltrimethoxysilane.
3. The method for preparing cesium copper iodine blue light nanocrystals according to claim 1, characterized in that: The mixing includes mixing together or mixing in steps.
4. The method for preparing cesium copper iodine blue light nanocrystals according to claim 3, characterized in that: The mixing is co-mixing.
5. The method for preparing cesium copper iodine blue light nanocrystals according to claim 3, characterized in that: The co-mixing is to add and mix the bifunctional silane coupling agent ligand, the cesium copper iodide perovskite nanocrystal precursor and the first solvent together.
6. The method for preparing cesium copper iodine blue light nanocrystals according to claim 3, characterized in that: The step-by-step mixing is to first mix the bifunctional silane coupling agent ligand with the first solvent, and then add the cesium copper iodide perovskite nanocrystal precursor.
7. The method for preparing cesium copper iodine blue light nanocrystals according to claim 1, characterized in that: The cesium copper iodide perovskite nanocrystal precursor comprises cesium iodide and cuprous iodide.
8. The method for preparing cesium copper iodine blue light nanocrystals according to claim 7, characterized in that: The molar ratio of the cesium iodide to the bifunctional silane coupling agent ligand is 1:(1-1.5).
9. The method for preparing cesium copper iodine blue light nanocrystals according to claim 1, characterized in that: The molar ratio of the bifunctional silane coupling agent ligand to the first solvent is 1:(10-20).
10. The method for preparing cesium copper iodine blue light nanocrystals according to claim 1, characterized in that: The mixing method includes stirring.
11. The method for preparing cesium copper iodine blue light nanocrystals according to claim 10, characterized in that: The stirring time is 2 to 5 hours.
12. The method for preparing cesium copper iodine blue light nanocrystals according to claim 1, characterized in that: The good solvent includes any one of dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, n-hexane or dichloromethane, or a combination of at least two thereof.
13. The method for preparing cesium copper iodine blue light nanocrystals according to claim 1, characterized in that: The anti-solvent includes any one of isopropanol, toluene or chloroform, or a combination of at least two of them.
14. The method for preparing cesium copper iodine blue light nanocrystals according to claim 1, characterized in that: The reaction is followed by centrifugation and washing.
15. The method for preparing cesium copper iodine blue light nanocrystals according to claim 1, characterized in that: The preparation method comprises the following steps: Adding a bifunctional silane coupling agent ligand, cesium iodide, cuprous iodide and a first solvent at a molar ratio of cesium iodide to bifunctional silane coupling agent ligand of 1: (1-1.5) together and stirring for 2-5 hours, adding a second solvent to carry out an anti-solvent reaction under ice bath ultrasound, centrifuging, washing, dissolving the washed substance in a solvent, adding water to hydrolyze, and obtaining the cesium copper iodine blue light nanocrystals; The first solvent and the second solvent have different polarities, and the first solvent and the second solvent each independently include a good solvent and an antisolvent; the molar ratio of the bifunctional silane coupling agent ligand to the first solvent is 1:(10-20); and the molar ratio of the bifunctional silane coupling agent ligand to water is 1:(4-7).
Citation Information
Patent Citations
Zero-dimensional lead-free caesium copper iodine perovskite blue nanocrystal and preparation method thereof
CN110117024A
Organic-inorganic hybrid perovskite quantum dot and preparation method thereof
CN106634961A
Core-shell perovskite quantum dot and preparation method thereof
CN109678728A
Preparation method of silica-coated all-inorganic perovskite core-shell structure quantum dots
CN111205853A
Method for growing copper-based lead-free perovskite single crystal by low-temperature solvent method
CN112853466A