A self-adhesive label and its production process

By using modified film layers made of raw materials such as polyvinyl alcohol and stearic acid, combined with seaweed polysaccharide and wollastonite, the problem of non-degradation of polyvinyl chloride is solved, and the biodegradation and mechanical properties of self-adhesive labels are improved. , reducing environmental pollution.

CN115100943BActive Publication Date: 2024-11-08ZHEJIANG HAOYUAN PACKAGING PRODUCTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210761056.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-30
Publication Date
2024-11-08
Estimated Expiration
2042-06-30

AI Technical Summary

Technical Problem

The existing PVC films with self-adhesive labels are non-degradable, resulting in environmental pollution problems.

Method used

The film layer made of raw materials such as polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant and stabilizer can improve water resistance and compatibility through the esterification reaction, and add algae polysaccharide and wollastonite to enhance Tensile strength and degradation properties.

Benefits of technology

The biodegradation of self-adhesive labels is achieved, reducing environmental pollution, and improving the water resistance and mechanical properties of the film layer, ensuring that the label is not easy to tear when used.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003724064000000041
    Figure BDA0003724064000000041
  • Figure BDA0003724064000000081
    Figure BDA0003724064000000081
Patent Text Reader

Abstract

This application relates to a self-adhesive label and its manufacturing process, falling within the field of labels. A self-adhesive label comprises a release paper layer, an adhesive layer, a face paper layer, and a film layer arranged sequentially. The film layer is made from raw materials including polyvinyl alcohol, stearic acid, modified wood flour fiber, a dispersant, and a stabilizer. The manufacturing process for the self-adhesive label includes the following steps: S1, preparing coating particles; S2, melting the coating particles and coating them onto the surface of the face paper layer to form a film layer; S3, mixing starch, water, polyhydroxyalkanoates, calcium hydroxide, zinc sulfate, boric acid, and an antibacterial agent evenly to obtain an adhesive; S4, applying the adhesive to the side of the face paper layer away from the film layer to form an adhesive layer; S5, attaching the release paper to the side of the adhesive layer away from the film layer in step S3 and pressing them together to obtain the self-adhesive label. This application enables the film on the self-adhesive label to degrade, reducing environmental pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of labels, and in particular to a self-adhesive label and a production process thereof. Background Art

[0002] Self-adhesive label is a common type of label. It is also called self-adhesive label, instant sticker, pressure-sensitive paper, etc. It is a composite material with paper, film or special material as the fabric, adhesive on the back, and silicon-coated base paper as protective paper. It becomes a finished label after printing, die-cutting and other processing.

[0003] A Chinese patent with application number 201620031947.3 discloses a waterproof self-adhesive label, including a polyvinyl chloride film, coated paper, an adhesive and a silicon-coated protective paper. The side of the polyvinyl chloride film is coated with lotus leaf latex paint. The polyvinyl chloride film is transparent and has a groove. The coated paper is embedded in the polyvinyl chloride film. The adhesive is located in the groove. The silicon-coated protective paper is located below the adhesive. The silicon-coated protective paper is detachably connected to the adhesive. The waterproof self-adhesive label has an excellent waterproof effect.

[0004] Regarding the above-mentioned related technologies, the inventors believe that the following defects exist: the film is made of polyvinyl chloride, which is a non-degradable polymer material. Therefore, after the label is separated from glass and other sticking materials, it still cannot be completely recycled, which will cause pollution to the environment. Summary of the invention

[0005] In order to enable the film on the self-adhesive label to be degraded and reduce environmental pollution, the present application provides a self-adhesive label and a production process thereof.

[0006] In the first aspect, the present application provides a self-adhesive label, which adopts the following technical solution:

[0007] A self-adhesive label, comprising a release paper layer, an adhesive layer, a surface paper layer and a film layer arranged in sequence;

[0008] The film layer is made of the following raw materials in parts by weight: 80-90 parts of polyvinyl alcohol, 10-20 parts of stearic acid, 15-28 parts of modified wood powder fiber, 1-2 parts of dispersant and 1-2 parts of stabilizer.

[0009] By adopting the above technical scheme, polyvinyl alcohol has the characteristics of biodegradation, and the final hydrolysis products are carbon dioxide and water, which is a good environmentally friendly material; since polyvinyl alcohol is rich in hydroxyl groups, it has poor water resistance, but stearic acid and polyvinyl alcohol undergo an esterification reaction to esterify some of the hydroxyl groups in the polyvinyl alcohol, thereby improving the water resistance of the film layer; at the same time, stearic acid can also improve the compatibility of various raw materials, which is beneficial to improving the stability of the system.

[0010] Wood powder fiber is a plant fiber with low price and can be biodegraded by itself, which is beneficial to environmental protection. In addition, wood powder fiber filled in polyvinyl alcohol can improve the tensile strength of the film layer. At the same time, the modified wood powder fiber can not only make the compatibility between wood powder fiber and other raw materials better, but also can further enhance the connection strength between wood powder fiber and polyvinyl alcohol, thereby further enhancing the tensile strength of the film layer.

[0011] Optionally, the preparation method of the modified wood powder fiber is: 1) dissolving 10-15 parts of maleic anhydride in 20-30 parts of dimethyl sulfoxide, adding 5-10 parts of hydroquinone and stirring to mix evenly to obtain a modified solution; 2) adding 30-35 parts of wood powder fiber to the modified solution, reacting at 40-50°C for 30-50 minutes, filtering to obtain a first wood powder fiber; 3) pouring the first wood powder fiber into 45-55 parts of acetone, letting it stand for 2-3 hours, filtering to obtain a second fiber; 4) drying the second fiber at 60-70°C for 9-11 hours to obtain a modified wood powder fiber.

[0012] By adopting the above technical solution, maleic anhydride and wood powder fiber undergo esterification reaction, reducing the polarity and hygroscopicity of the wood powder fiber, thereby enhancing the compatibility between the wood powder fiber and polyvinyl alcohol, and making the adhesion between the polyvinyl alcohol and the wood powder fiber stronger.

[0013] Optionally, in step 2), the wood powder fiber is first added to 50-60 parts of 0.05-1 mol / L acetic acid solution and stirred for reaction for 0.5-1 h, filtered, and then added to the modified solution.

[0014] By adopting the above technical solution, acetic acid can react with impurities such as pectin in the wood powder fiber, thereby removing part of the pectin and impurities, improving the adhesion between the wood part of the wood powder fiber and polyvinyl alcohol, and thus improving the mechanical properties of the film layer.

[0015] Optionally, 20-30 parts by weight of seaweed polysaccharide are also included.

[0016] By adopting the above technical solution, seaweed polysaccharide has good biodegradability and adhesion, so it can maintain good film-forming properties after the raw materials in the film layer are mixed. At the same time, seaweed polysaccharide has good hydrophilicity and can accelerate the degradation of the film layer.

[0017] Optionally, 10-15 parts by weight of wollastonite is also included.

[0018] By adopting the above technical solution, wollastonite is a natural mineral fiber that can improve the tensile strength and thermal stability of the film layer. At the same time, stearic acid can react with wollastonite to modify the surface of wollastonite, thereby enhancing the compatibility between wollastonite and polyvinyl alcohol, so that wollastonite can be better dispersed in the film layer system.

[0019] Optionally, 5-10 parts by weight of acetic anhydride is also included.

[0020] By adopting the above technical solution, acetic anhydride is easily hydrolyzed to generate acetic acid, forming acidic conditions and thus accelerating the degradation rate of the film layer.

[0021] Optionally, the dispersant is polyethylene glycol.

[0022] By adopting the above technical solution, polyethylene glycol can improve the compatibility between various raw materials such as polyvinyl alcohol and modified wood powder fiber.

[0023] Optionally, the stabilizer is a rare earth stabilizer.

[0024] By adopting the above technical solution, the rare earth stabilizer can make the structure of the film layer denser, thereby improving the mechanical strength of the film layer, and can also purify impurities to make the film layer clearer and more transparent.

[0025] In a second aspect, the present application provides a production process for a self-adhesive label, which adopts the following technical solution:

[0026] A production process for a self-adhesive label comprises the following steps:

[0027] S1, mixing polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant and stabilizer uniformly, extruding and granulating to obtain coated particles;

[0028] S2, melting the coated particles and coating them on the surface of the surface paper layer to form a film layer;

[0029] S3, weighing 20-60 parts of starch, 90-110 parts of water, 30-50 parts of polyhydroxyalkanoate, 0.5-20 parts of calcium hydroxide, 0.5-10 parts of zinc sulfate, 0.1-5 parts of boric acid and 0.1-5 parts of antibacterial agent by weight, and then stirring and mixing starch, water, polyhydroxyalkanoate, calcium hydroxide, zinc sulfate, boric acid and antibacterial agent to obtain viscose;

[0030] S4, applying adhesive on the side of the surface paper layer away from the film layer to form an adhesive layer;

[0031] S5, attaching the release paper to the side of the adhesive layer away from the film layer in step S3, and pressing the release paper to obtain a self-adhesive label.

[0032] By adopting the above technical solution, the prepared self-adhesive label can be biodegraded after being discarded, thus protecting the environment. At the same time, the film layer can also have good mechanical properties, so that the self-adhesive label is not easy to be torn and is easy to use.

[0033] In summary, the present application includes at least one of the following beneficial technical effects:

[0034] 1. Polyvinyl alcohol has the characteristics of biodegradation, and the final hydrolysis products are carbon dioxide and water, which is a good environmentally friendly material; because polyvinyl alcohol is rich in hydroxyl groups, it has poor water resistance, but stearic acid and polyvinyl alcohol undergo esterification reaction, so that part of the hydroxyl groups in polyvinyl alcohol are esterified, thereby improving the water resistance of the film layer; at the same time, stearic acid can also improve the compatibility of various raw materials, which is beneficial to improve the stability of the system;

[0035] 2. Wood powder fiber is a plant fiber with low price and can be biodegraded by itself, which is beneficial to environmental protection. In addition, wood powder fiber filled in polyvinyl alcohol can improve the tensile strength of the film layer. At the same time, the modified wood powder fiber can not only make the compatibility between wood powder fiber and other raw materials better, but also further enhance the connection strength between wood powder fiber and polyvinyl alcohol, thereby further enhancing the tensile strength of the film layer;

[0036] 3. Acetic acid can react with impurities such as pectin in wood powder fiber, thereby removing part of the pectin and impurities, improving the adhesion between the wood part of the wood powder fiber and polyvinyl alcohol, and thus improving the mechanical properties of the film layer. DETAILED DESCRIPTION

[0037] The present application is further described in detail below in conjunction with the examples. It should be noted that if no specific conditions are specified in the following examples, the reaction is carried out according to conventional conditions or conditions recommended by the manufacturer. All raw materials in the following examples can be obtained from common commercial sources unless otherwise specified.

[0038] Example

[0039] Example 1

[0040] This embodiment discloses a self-adhesive label, the component contents of which are shown in Table 1:

[0041] Table 1 Component dosage of the self-adhesive label of Examples 1-3

[0042]

[0043] The dispersant is polyethylene glycol, and the stabilizer is a rare earth stabilizer;

[0044] The preparation method of the modified wood powder fiber is as follows: 1) dissolving 10g of maleic anhydride in 20g of dimethyl sulfoxide, adding 5g of hydroquinone and stirring and mixing evenly to obtain a modified solution; 2) adding 30g of wood powder fiber to the modified solution, reacting at 40°C for 50min, filtering, and obtaining a first wood powder fiber; 3) pouring the first wood powder fiber into 45g of acetone, standing for 2h, filtering, and obtaining a second fiber; 4) drying the second fiber at 60°C for 11h to obtain a modified wood powder fiber;

[0045] This embodiment also discloses a production process of a self-adhesive label, comprising the following steps:

[0046] S1, mixing polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant and stabilizer uniformly, extruding and granulating to obtain coated particles;

[0047] S2, melting the coated particles and coating them on the surface of the surface paper layer to form a film layer;

[0048] S3, weighing 20g of starch, 90g of water, 30g of polyhydroxyalkanoate, 0.5g of calcium hydroxide, 0.5g of zinc sulfate, 0.1g of boric acid and 0.1g of antibacterial agent (the antibacterial agent is a special antibacterial agent for starch glue) by weight, and then stirring and mixing starch, water, polyhydroxyalkanoate, calcium hydroxide, zinc sulfate, boric acid and antibacterial agent to obtain viscose;

[0049] S4, applying adhesive on the side of the surface paper layer away from the film layer to form an adhesive layer;

[0050] S5, attaching the release paper to the side of the adhesive layer away from the film layer in step S3, and pressing the release paper to obtain a self-adhesive label.

[0051] Example 2

[0052] This embodiment discloses a self-adhesive label, the component contents of which are shown in Table 1;

[0053] The dispersant is polyethylene glycol, and the stabilizer is a rare earth stabilizer;

[0054] The preparation method of the modified wood powder fiber is as follows: 1) dissolving 15g of maleic anhydride in 30g of dimethyl sulfoxide, adding 10g of hydroquinone and stirring and mixing evenly to obtain a modified solution; 2) adding 35g of wood powder fiber to the modified solution, reacting at 50°C for 30min, filtering, and obtaining a first wood powder fiber; 3) pouring the first wood powder fiber into 55g of acetone, standing for 3h, filtering, and obtaining a second fiber; 4) drying the second fiber at 70°C for 9h to obtain a modified wood powder fiber;

[0055] This embodiment also discloses a production process of a self-adhesive label, comprising the following steps:

[0056] S1, mixing polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant and stabilizer uniformly, extruding and granulating to obtain coated particles;

[0057] S2, melting the coated particles and coating them on the surface of the surface paper layer to form a film layer;

[0058] S3, weighing 60g of starch, 110g of water, 50g of polyhydroxyalkanoate, 20g of calcium hydroxide, 10g of zinc sulfate, 5g of boric acid and 5g of antibacterial agent (the antibacterial agent is a special antibacterial agent for starch glue) by weight, and then stirring and mixing starch, water, polyhydroxyalkanoate, calcium hydroxide, zinc sulfate, boric acid and antibacterial agent to obtain viscose;

[0059] S4, applying adhesive on the side of the surface paper layer away from the film layer to form an adhesive layer;

[0060] S5, attaching the release paper to the side of the adhesive layer away from the film layer in step S3, and pressing the release paper to obtain a self-adhesive label.

[0061] Example 3

[0062] This embodiment discloses a self-adhesive label, the component contents of which are shown in Table 1;

[0063] The dispersant is polyethylene glycol, and the stabilizer is a rare earth stabilizer;

[0064] The preparation method of the modified wood powder fiber is as follows: 1) dissolving 13g of maleic anhydride in 26g of dimethyl sulfoxide, adding 8g of hydroquinone and stirring and mixing evenly to obtain a modified solution; 2) adding 33g of wood powder fiber to the modified solution, reacting at 45°C for 42min, filtering, and obtaining a first wood powder fiber; 3) pouring the first wood powder fiber into 50g of acetone, standing for 2.4h, filtering, and obtaining a second fiber; 4) drying the second fiber at 66°C for 10h to obtain a modified wood powder fiber;

[0065] This embodiment also discloses a production process of a self-adhesive label, comprising the following steps:

[0066] S1, mixing polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant and stabilizer uniformly, extruding and granulating to obtain coated particles;

[0067] S2, melting the coated particles and coating them on the surface of the surface paper layer to form a film layer;

[0068] S3, weighing 40g of starch, 85g of water, 42g of polyhydroxyalkanoate, 4g of calcium hydroxide, 2g of zinc sulfate, 1g of boric acid and 1g of antibacterial agent (the antibacterial agent is a special antibacterial agent for starch glue) by weight, and then stirring and mixing starch, water, polyhydroxyalkanoate, calcium hydroxide, zinc sulfate, boric acid and antibacterial agent to obtain viscose;

[0069] S4, applying adhesive on the side of the surface paper layer away from the film layer to form an adhesive layer;

[0070] S5, attaching the release paper to the side of the adhesive layer away from the film layer in step S3, and pressing the release paper to obtain a self-adhesive label.

[0071] Example 4

[0072] The difference between this embodiment and embodiment 3 is that in step 2) of the preparation method of modified wood powder fiber, 33g of wood powder fiber is first added to 50g of 0.05mol / L acetic acid solution and stirred for reaction for 1h, filtered, and then added to the modified solution.

[0073] Example 5

[0074] The difference between this embodiment and embodiment 3 is that in step 2) of the preparation method of modified wood powder fiber, 33g of wood powder fiber is first added to 60g of 1mol / L acetic acid solution and stirred for reaction for 0.5h, filtered, and then added to the modified solution.

[0075] Example 6

[0076] The difference between this embodiment and embodiment 3 is that in step 2) of the preparation method of modified wood powder fiber, 33g of wood powder fiber is first added to 56g of 0.8mol / L acetic acid solution and stirred for reaction for 0.7h, filtered, and then added to the modified solution.

[0077] Example 7

[0078] The difference between this embodiment and embodiment 6 is that: a self-adhesive label further contains 20g of seaweed polysaccharide;

[0079] A production process for self-adhesive labels, in step S1, polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant, stabilizer and seaweed polysaccharide are stirred and mixed evenly, and extruded and granulated to obtain coated particles.

[0080] Example 8

[0081] The difference between this embodiment and embodiment 7 is that: a self-adhesive label further contains 30 g of seaweed polysaccharide.

[0082] Example 9

[0083] The difference between this embodiment and embodiment 7 is that: a self-adhesive label further contains 23 g of seaweed polysaccharide.

[0084] Example 10

[0085] The difference between this embodiment and embodiment 9 is that: a self-adhesive label further contains 10 g of wollastonite;

[0086] A production process for self-adhesive labels, in step S1, polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant, stabilizer, seaweed polysaccharide and wollastonite are stirred and mixed evenly, and extruded and granulated to obtain coated particles.

[0087] Embodiment 11

[0088] The difference between this embodiment and embodiment 9 is that: a self-adhesive label further contains 15 g of wollastonite;

[0089] A production process for self-adhesive labels, in step S1, polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant, stabilizer, seaweed polysaccharide and wollastonite are stirred and mixed evenly, and extruded and granulated to obtain coated particles.

[0090] Example 12

[0091] The difference between this embodiment and embodiment 9 is that: a self-adhesive label further contains 13 g of wollastonite;

[0092] A production process for self-adhesive labels, in step S1, polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant, stabilizer, seaweed polysaccharide and wollastonite are stirred and mixed evenly, and extruded and granulated to obtain coated particles.

[0093] Embodiment 13

[0094] The difference between this embodiment and embodiment 12 is that: a self-adhesive label further contains 5 g of acetic anhydride;

[0095] A production process for self-adhesive labels, in step S1, polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant, stabilizer, seaweed polysaccharide, wollastonite and acetic anhydride are stirred and mixed evenly, and extruded and granulated to obtain coated particles.

[0096] Embodiment 14

[0097] The difference between this embodiment and embodiment 12 is that: a self-adhesive label further contains 10 g of acetic anhydride;

[0098] A production process for self-adhesive labels, in step S1, polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant, stabilizer, seaweed polysaccharide, wollastonite and acetic anhydride are stirred and mixed evenly, and extruded and granulated to obtain coated particles.

[0099] Embodiment 15

[0100] The difference between this embodiment and embodiment 12 is that: a self-adhesive label further contains 8 g of acetic anhydride;

[0101] A production process for self-adhesive labels, in step S1, polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant, stabilizer, seaweed polysaccharide, wollastonite and acetic anhydride are stirred and mixed evenly, and extruded and granulated to obtain coated particles.

[0102] Comparative Example

[0103] Comparative Example 1

[0104] The difference between this comparative example and Example 1 is that no modified wood powder fiber is added.

[0105] Comparative Example 2

[0106] The difference between this comparative example and Example 1 is that the same mass of wood powder fiber as the modified wood powder fiber is added, but the wood powder fiber is not modified.

[0107] Comparative Example 3

[0108] The difference between this comparative example and Example 1 is that stearic acid is not added.

[0109] Performance testing

[0110] 1. Degradation performance test

[0111] According to GB / T20197-2006, the self-adhesive labels prepared in Examples 1-15 and Comparative Examples 1-3 were subjected to degradation detection tests, and the results were recorded as shown in Table 2;

[0112] 2. Tensile performance test

[0113] According to GB / T1040, the draw cord strength and elongation at break of the self-adhesive labels prepared in Examples 1-15 and Comparative Examples 1-3 were measured, and the results were recorded as shown in Table 2.

[0114] Table 2 Test result record

[0115]

[0116] Combining Examples 1-3, Comparative Example 1 and Table 2, it can be seen that adding modified wood powder fiber to the components of the film layer of the self-adhesive label is beneficial to increasing the degradation rate of the film layer, and is also beneficial to increasing the tensile strength and elongation at break of the film layer, thereby improving the practicality of the self-adhesive label, indicating that the modified wood powder fiber is beneficial to enhancing the connection strength between the components; the appropriate amount of each component in the film layer will accelerate the degradation rate of the film layer, thereby improving the degradation performance of the self-adhesive label, and at the same time can ensure the mechanical strength of the self-adhesive label when in use, making it difficult to be torn and more convenient to use;

[0117] Combining Example 1, Comparative Examples 1-3 and Table 2, it can be seen that the degradation rate of the self-adhesive label obtained without modifying the wood powder fiber is significantly reduced, and stearic acid is beneficial to improving the tensile strength and elongation at break of the self-adhesive label film layer, indicating that the product generated by the reaction of stearic acid and polyvinyl alcohol can be better mixed with other components and is not easy to separate. Stearic acid and polyvinyl alcohol have a synergistic effect that can improve the degradation rate and mechanical properties of the film layer;

[0118] Combining the analysis of Examples 3-6 and Table 2, it can be seen that the use of acetic acid to treat the wood powder fiber before modification is beneficial to both increasing the degradation rate of the self-adhesive label and increasing the tensile strength and elongation at break of the film layer, indicating that acetic acid is beneficial to the degradation of the wood powder fiber after removing pectin and impurities in the wood powder fiber, and is also beneficial to increasing the connection strength between polyvinyl alcohol and the wood powder fiber;

[0119] Combining the analysis of Examples 6-9 and Table 2, it can be concluded that seaweed polysaccharide is beneficial to enhancing the connection force of the components in the self-adhesive label film layer, thereby improving the mechanical properties of the film layer. At the same time, seaweed polysaccharide replacing part of polyvinyl alcohol is beneficial to accelerating the degradation of the film layer.

[0120] Combining the analysis of Examples 9-12 and Table 2, it can be concluded that adding wollastonite as a mineral fiber filler to polyvinyl alcohol can not only accelerate the degradation of the film layer, but also help to improve the tensile strength and elongation at break of the film layer;

[0121] Combining the analysis of Examples 12-15 and Table 2, it can be seen that acetic anhydride is beneficial for ensuring the mechanical strength of the film layer while also providing an acidic environment when the film layer is degraded, thereby accelerating the degradation rate of the film layer.

[0122] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A self-adhesive label, characterized in that: It includes a release paper layer, an adhesive layer, a surface paper layer and a film layer arranged in sequence; The film layer is made of the following raw materials in parts by weight: 80-90 parts of polyvinyl alcohol, 10-20 parts of stearic acid, 15-28 parts of modified wood powder fiber, 1-2 parts of dispersant and 1-2 parts of stabilizer; The preparation method of the modified wood powder fiber is as follows: 1) dissolving 10-15 parts of maleic anhydride in 20-30 parts of dimethyl sulfoxide, adding 5-10 parts of hydroquinone, stirring and mixing evenly to obtain a modified solution; 2) Add 30-35 parts of wood powder fiber to the modified solution, react at 40-50°C for 30-50 minutes, filter, and obtain the first wood powder fiber; 3) Pour the first wood powder fiber into 45-55 parts of acetone, let stand for 2-3 hours, filter, and obtain the second fiber; 4) Dry the second fiber at 60-70°C for 9-11 hours to obtain the modified wood powder fiber; In step 2), the wood powder fiber is first added to 50-60 parts of 0.05-1 mol / L acetic acid solution and stirred for 0.5-1h, filtered, and then added to the modified solution; It also includes 5-10 parts by weight of acetic anhydride.

2. The self-adhesive label according to claim 1, characterized in that: The invention also comprises 20-30 parts by weight of seaweed polysaccharide.

3. The self-adhesive label according to claim 1, characterized in that: Also included is 10-15 parts by weight of wollastonite.

4. The self-adhesive label according to claim 1, characterized in that: The dispersant is polyethylene glycol.

5. The self-adhesive label according to claim 1, characterized in that: The stabilizer is a rare earth stabilizer.

6. A process for producing a self-adhesive label according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, mixing polyvinyl alcohol, stearic acid, modified wood powder fiber, dispersant and stabilizer uniformly, extruding and granulating to obtain coated particles; S2, melting the coated particles and coating them on the surface of the surface paper layer to form a film layer; S3, weighing 20-60 parts of starch, 90-110 parts of water, 30-50 parts of polyhydroxyalkanoate, 0.5-20 parts of calcium hydroxide, 0.5-10 parts of zinc sulfate, 0.1-5 parts of boric acid and 0.1-5 parts of antibacterial agent by weight, and then stirring and mixing starch, water, polyhydroxyalkanoate, calcium hydroxide, zinc sulfate, boric acid and antibacterial agent to obtain viscose; S4, applying adhesive on the side of the surface paper layer away from the film layer to form an adhesive layer; S5, attaching the release paper to the side of the adhesive layer away from the film layer in step S3, and pressing the release paper to obtain a self-adhesive label.