An antibacterial and rapidly water-soluble thermosetting material and preparation method thereof

By introducing a quaternary ammonium salt structure and the reaction of a binary haloester and a trivalent tertiary amine into a thermosetting material, an antibacterial and rapidly water-soluble thermosolid system material is formed, which solves the problems of difficult degradation of the material and insufficient antibacterial performance, and achieves Rapid hydrolysis of the material and broad-spectrum antibacterial effect.

CN115108909BActive Publication Date: 2024-10-29ZHEJIANG UNIV OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210778553.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-30
Publication Date
2024-10-29
Estimated Expiration
2042-06-30

AI Technical Summary

Technical Problem

Existing thermoset materials are difficult to degrade, resulting in increased environmental pressure, and there is a lack of effective antibacterial materials to deal with the threat of microbial pathogens.

Method used

By introducing a quaternary ammonium salt structure, a three-dimensional cross-linked network is formed by the reaction of a binary haloester and a trivalent tertiary amine, forming an antibacterial and rapidly water-soluble thermosolid system material. The Quaternary ammonium group is used to make the ester bond easy to hydrolyze and combine. Rigid groups such as benzene rings increase material hardness and antibacterial properties.

Benefits of technology

It achieves rapid hydrolytic degradation of thermosetting materials, has good antibacterial properties and hardness, and the degradation products are biofriendly zwitterionic ions, which broadens the application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003722683720000011
    Figure HDA0003722683720000011
  • Figure HDA0003722683720000021
    Figure HDA0003722683720000021
  • Figure HDA0003722683720000031
    Figure HDA0003722683720000031
Patent Text Reader

Abstract

The invention discloses an antibacterial thermosetting system material that can be quickly dissolved in water and a preparation method thereof. The preparation method specifically comprises the following steps: adding diol, halogenated acid, toluene and p-toluenesulfonic acid, stirring to obtain a mixed solution; using an alkaline solution to adjust the Ph of the mixed solution, then washing with water and separating the liquids; taking the upper layer solution after separation and drying it; then performing rotary evaporation and reduced pressure distillation to obtain a diol halogenated ester; then mixing the diol halogenated ester with a tertiary amine, and curing to obtain an antibacterial thermosetting system material that can be quickly dissolved in water. The thermosetting system material prepared by the invention has many advantages such as good antibacterial performance and excellent mechanical properties, and can be quickly dissolved in water, and is environmentally friendly and pollution-free. Its degradation products are bio-friendly zwitterions and diols with antibacterial and antifungal effects, which broadens its application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of antibacterial fast-hydrolyzing materials, and in particular to an antibacterial fast-water-soluble thermosetting system material and a preparation method thereof. Background Art

[0002] Thermosetting materials generally have good formability and excellent mechanical properties, but they are generally difficult to degrade, which puts great pressure on the environment. At present, sustainable development is deeply rooted in people's hearts, and the degradation of degradable polymers into simpler compounds or polymers in stages has attracted widespread attention. Ester bonds, as a chemical bond that can break and degrade quickly, have also begun to attract more and more attention.

[0003] In addition, microbial pathogens have long been the culprit for endangering human health, and countless people or animals die every year due to bacterial or viral infections. Quaternary ammonium salts have excellent antibacterial properties and are widely used in antibacterial materials.

[0004] The invention provides a method for synthesizing an antibacterial and rapidly water-soluble thermosetting system, wherein a quaternary ammonium salt structure is introduced into the system, and a three-dimensional cross-linked network is formed by the reaction of a dibasic halogenated ester and a ternary tertiary amine. The introduction of the quaternary ammonium salt increases the antibacterial performance of the system, and the presence of the quaternary ammonium group causes the ester bond to be easily hydrolyzed, thereby ensuring that the cross-linking points of the thermosetting material are easily broken when exposed to water; the presence of a large number of cross-linking points and the presence of rigid groups such as benzene rings ensure that the material has good hardness and fracture strength in a dry state. Summary of the invention

[0005] The purpose of the present invention is to provide an antibacterial, rapidly water-soluble thermosetting material and a preparation method thereof in view of the deficiencies of the prior art.

[0006] The object of the present invention is achieved through the following technical scheme: a method for preparing an antibacterial and rapidly water-soluble thermosetting material, comprising the following steps:

[0007] Step 1: add diol, halogenated acid, toluene and p-toluenesulfonic acid, stir at 50-160° C. for 1-24 hours to obtain a mixed solution; use an alkaline solution to adjust the pH of the mixed solution to 9.0-11.0, then wash with water until the pH is 7.0 and separate the liquids; after separation, take the upper layer solution and dry it with anhydrous magnesium sulfate for 3-48 hours; perform rotary evaporation at 60° C. in a rotary evaporator until no liquid is evaporated, and perform reduced pressure distillation at 120-200° C. until no liquid is evaporated to obtain diol halogenated ester;

[0008] The molar ratio of the diol, the halogenated acid, toluene and p-toluenesulfonic acid is 1:2-3:3-10:0.1-0.3;

[0009] Step 2: Mix the diol halogenated ester prepared in step 1 with the ternary tertiary amine in a molar ratio of 1:0.5-2; cure at 10-160° C. for 1-24 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material.

[0010] Preferably, the diol is ethylene glycol, propylene glycol, butylene glycol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol or decanediol.

[0011] Preferably, the halogenated acid is chloroacetic acid, chloropropionic acid, chlorobutyric acid, chlorovaleric acid, chlorohexanoic acid, chloroheptanoic acid, chlorooctanoic acid, chlorononanoic acid, chlorodecanoic acid, bromoacetic acid, bromopropionic acid, bromobutyric acid, bromovalic acid, bromohexanoic acid, bromoheptanoic acid, bromooctanoic acid, bromononanoic acid, bromodecanoic acid, iodoacetic acid, iodopropionic acid, iodobutyric acid, iodovaleric acid, iodohexanoic acid, iodoheptanoic acid, iodooctanoic acid, iodononanoic acid or iododecanoic acid.

[0012] Preferably, the tertiary amine is pentamethyldiethylenetriamine or pentamethyldipropylenetriamine or 2,4,6-tris(dimethylaminomethyl)phenol.

[0013] The present invention also provides an antibacterial and rapidly water-soluble thermosetting system material prepared by the method.

[0014] The beneficial effects of the present invention are as follows: quaternary ammonium salt and ester bond are introduced into the system, and a three-dimensional cross-linked network is formed through the reaction of dibasic halogenated ester and tertiary amine. The introduction of quaternary ammonium salt increases the antibacterial property of the system. Due to the presence of quaternaryammonium group, the ester bond is easily hydrolyzed, ensuring that the cross-linking points of the thermosetting material are easily broken when exposed to water; the presence of a large number of cross-linking points and the presence of rigid groups such as benzene rings ensure that the material has good hardness and fracture strength in a dry state. In addition, its degradation products are bio-friendly zwitterions and diols with antibacterial and antifungal effects, which broadens its application prospects. . BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 is the infrared spectrum of hexanediol chloroacetate;

[0016] Figure 2 is the H NMR spectrum of hexanediol chloroacetate;

[0017] Figure 3 This is an infrared spectrum of an antibacterial, fast-soluble, water-soluble thermosetting material.

[0018] Figure 4 is the degradation process diagram, where Figure 4 (a) is a schematic diagram of an antibacterial, rapidly water-soluble thermosetting material. Figure 4 (b) is the degradation diagram at time 0h, Figure 4 (c) is the degradation diagram at 0.2h. Figure 4 (b) is the degradation diagram at a time of 0.5 h;

[0019] Figure 5 This is a comparison chart of antibacterial fluorescent staining. Figure 5 (a) is the antibacterial fluorescence staining comparison diagram of the blank control group. Figure 5 (b) is a comparison of antibacterial fluorescence staining of the experimental group. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0021] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0022] Example 1

[0023] A method for preparing an antibacterial and rapidly water-soluble thermosetting material comprises the following steps:

[0024] Step 1: add 1g hexanediol, 2.4g chloroacetic acid, 11ml toluene solution and 0.2g p-toluenesulfonic acid into a 50ml flask, stir at 120°C for 12h to obtain a mixed solution, wherein the toluene solution is used as a solvent and the p-toluenesulfonic acid is used as a catalyst; use sodium hydroxide solution to alkaline wash the mixed solution to pH = 10.0, the concentration of the sodium hydroxide solution is 1mol / L, and the excess chloroacetic acid and p-toluenesulfonic acid are neutralized to form salts with sodium hydroxide solution; then wash with water to pH = 7.0 and then separate the liquids, and wash with water to remove the salts in the mixed solution; after separation, take the upper layer solution and dry it with anhydrous magnesium sulfate for 24h, and filter to remove the anhydrous magnesium sulfate that has absorbed water; then perform rotary evaporation at 60°C in a rotary evaporator until no liquid is rotated out, and toluene is removed during the rotary evaporation process; perform reduced pressure distillation at 175°C until no liquid is evaporated to obtain hexanediol chloroacetate;

[0025] Step 2: Mix 1.53 g of hexanediol chloroacetate prepared in step 1 and 1 g of 2,4,6-tris(dimethylaminomethyl)phenol in a beaker, stir for 15 seconds, pour the mixture into a mold made of silica gel, and cure it at 60°C for 12 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material. The antibacterial, rapidly water-soluble thermosetting system material has high hardness and good broad-spectrum antibacterial properties and can be rapidly dissolved in water.

[0026] The hexanediol chloroacetate prepared in step 1 of Example 1 was subjected to infrared spectroscopy test to obtain an infrared spectrum as shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the hexanediol chloroacetate prepared in step 1 of Example 1 has an average wavelength of 1755 cm -1 The left and right sides are the stretching vibrations of C=O in the ester bond, 1470 cm -1 The left and right are stretching vibrations of the COC bond. There is no ester bond in the raw material, indicating that the product to be tested in step 1 is the target product, that is, hexanediol chloroacetate.

[0027] The H NMR spectrum of hexanediol chloroacetate prepared in step 1 of Example 1 is obtained, as shown in FIG. Figure 2 shown; from Figure 2 It can be seen that the spectral position of hydrogen in hexanediol chloroacetate is consistent with expectations, indicating that the product is hexanediol chloroacetate.

[0028] The antibacterial and rapidly water-soluble thermosetting material prepared in Example 1 was subjected to infrared spectroscopy testing, and the infrared spectrum was as follows: Figure 3 As shown. Figure 3 It can be seen that at 909cm -1 It is a quaternary ammonium salt peak, and the raw materials do not contain quaternary ammonium salt substances, indicating that hexanediol chloroacetate and 2,4,6-tris(dimethylaminomethyl)phenol are cross-linked in step 2 to generate the target product, which is an antibacterial, rapidly water-soluble thermosetting system material.

[0029] Since the mixture is poured into a mold made of silica gel in step 2, the antibacterial and rapidly water-soluble thermosetting material prepared in Example 1 is in the shape of a cylinder, such as Figure 4 (a) As shown. The antibacterial and rapidly water-soluble thermosetting system material prepared in Example 1 was placed in water to obtain its degradation process. The antibacterial and rapidly water-soluble thermosetting system material prepared in Example 1 was just placed in water, as shown. Figure 4 (b) When degraded in water for 0.2h, Figure 4 As shown in (c), it can be seen that the material has begun to degrade; when it degrades in water for 0.25h, Figure 4 As shown in (d), it can be seen that the material has been completely degraded.

[0030] The antibacterial and rapidly water-soluble thermosetting system material prepared in Example 1 was used to conduct an antibacterial experiment on Staphylococcus aureus. The antibacterial and rapidly water-soluble thermosetting system material prepared in Example 1 was added to the experimental group, and nothing was added to the blank control group. After 0.3 h of treatment, an antibacterial fluorescent staining comparison chart was obtained, as shown in FIG. Figure 5 shown. Figure 5(a) is the antibacterial fluorescence staining comparison diagram of the blank control group. Figure 5 (b) is a comparison of antibacterial fluorescence staining of the experimental group. Figure 5 It can be seen that the number of Staphylococcus aureus treated with the antibacterial, rapidly water-soluble thermosetting material prepared in Example 1 is significantly reduced.

[0031] Example 2

[0032] A method for preparing an antibacterial and rapidly water-soluble thermosetting material comprises the following steps:

[0033] Step 1: add 1g hexanediol, 2.4g chloroacetic acid, 11ml toluene solution and 0.2g p-toluenesulfonic acid into a 50ml flask, stir at 120°C for 12h to obtain a mixed solution, wherein the toluene solution is used as a solvent and the p-toluenesulfonic acid is used as a catalyst; use a sodium hydroxide solution to alkaline wash the mixed solution to pH = 10.0, and the concentration of the sodium hydroxide solution is 1 mol / L; then wash with water to pH = 7.0 and then separate the liquids, and wash with water to remove the salt in the mixed solution; after separation, take the upper layer solution and dry it with anhydrous magnesium sulfate for 24h, and filter to remove the anhydrous magnesium sulfate that has absorbed water; then perform rotary evaporation at 60°C in a rotary evaporator until no liquid is rotated out, and perform reduced pressure distillation at 175°C until no liquid is evaporated to obtain hexanediol chloroacetate;

[0034] Step 2: Mix 2.04 g of hexanediol chloroacetate prepared in step 1 and 1 g of pentamethyldipropylenetriamine in a beaker, stir for 15 seconds, pour the mixture into a silicone mold, and cure it at 60° C. for 12 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material. The antibacterial, rapidly water-soluble thermosetting system material has high hardness and good broad-spectrum antibacterial properties, and can be quickly dissolved in water.

[0035] Example 3

[0036] A method for preparing an antibacterial and rapidly water-soluble thermosetting material comprises the following steps:

[0037] Step 1: add 1g propylene glycol, 3g chloroacetic acid, 12ml toluene solution and 0.2g p-toluenesulfonic acid into a 50ml flask, stir at 120°C for 12h to obtain a mixed solution, wherein the toluene solution is used as a solvent and the p-toluenesulfonic acid is used as a catalyst; use a sodium hydroxide solution to alkaline wash the mixed solution to pH = 10.0, and the concentration of the sodium hydroxide solution is 1mol / L; then wash with water to pH = 7.0 and then separate the liquids, and wash with water to remove the salt in the mixed solution; after separation, take the upper layer solution and dry it with anhydrous magnesium sulfate for 24h, and filter to remove the anhydrous magnesium sulfate that has absorbed water; then perform rotary evaporation at 60°C in a rotary evaporator until no liquid is rotated out, and perform reduced pressure distillation at 175°C until no liquid is evaporated to obtain propylene glycol chloroacetate;

[0038] Step 2: Mix 1.24 g of propylene glycol chloroacetate prepared in step 1 and 1 g of 2,4,6-tris(dimethylaminomethyl)phenol in a beaker, stir for 15 seconds, pour the mixture into a silicone mold, and cure it at 60°C for 12 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material. The antibacterial, rapidly water-soluble thermosetting system material has high hardness and good broad-spectrum antibacterial properties and can be rapidly dissolved in water.

[0039] Example 4

[0040] A method for preparing an antibacterial and rapidly water-soluble thermosetting material comprises the following steps:

[0041] Step 1: add 1g propylene glycol, 3g chloroacetic acid, 12ml toluene solution and 0.2g p-toluenesulfonic acid into a 50ml flask, stir at 120°C for 12h to obtain a mixed solution, wherein the toluene solution is used as a solvent and the p-toluenesulfonic acid is used as a catalyst; use a sodium hydroxide solution to alkaline wash the mixed solution to pH = 10.0, and the concentration of the sodium hydroxide solution is 1mol / L; then wash with water to pH = 7.0 and then separate the liquids, and wash with water to remove the salt in the mixed solution; after separation, take the upper layer solution and dry it with anhydrous magnesium sulfate for 24h, and filter to remove the anhydrous magnesium sulfate that has absorbed water; then perform rotary evaporation at 60°C in a rotary evaporator until no liquid is rotated out, and perform reduced pressure distillation at 175°C until no liquid is evaporated to obtain propylene glycol chloroacetate;

[0042] Step 2: Mix 1.63 g of propylene glycol chloroacetate prepared in step 1 and 1 g of pentamethyldipropylenetriamine in a beaker, stir for 15 seconds, pour the mixture into a silicone mold, and cure it at 60° C. for 12 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material. The antibacterial, rapidly water-soluble thermosetting system material has high hardness and good broad-spectrum antibacterial properties, and can be quickly dissolved in water.

[0043] Example 5

[0044] A method for preparing an antibacterial and rapidly water-soluble thermosetting material comprises the following steps:

[0045] Step 1: add 1g hexanediol, 2.4g chloroacetic acid, 11ml toluene solution and 0.2g p-toluenesulfonic acid into a 50ml flask, stir at 120°C for 12h to obtain a mixed solution, wherein the toluene solution is used as a solvent and the p-toluenesulfonic acid is used as a catalyst; use a sodium hydroxide solution to alkaline wash the mixed solution to pH = 10.0, and the concentration of the sodium hydroxide solution is 1 mol / L; then wash with water to pH = 7.0 and then separate the liquids, and wash with water to remove the salt in the mixed solution; after separation, take the upper layer solution and dry it with anhydrous magnesium sulfate for 24h, and filter to remove the anhydrous magnesium sulfate that has absorbed water; then perform rotary evaporation at 60°C in a rotary evaporator until no liquid is rotated out, and perform reduced pressure distillation at 175°C until no liquid is evaporated to obtain hexanediol chloroacetate;

[0046] Step 2: Mix 1.46 g of hexanediol chloroacetate prepared in step 1 and 1 g of 2,4,6-tris(dimethylaminomethyl)phenol in a beaker, stir for 15 seconds, pour the mixture into a silicone mold, and cure it at 60°C for 12 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material. The antibacterial, rapidly water-soluble thermosetting system material has high hardness and good broad-spectrum antibacterial properties and can be rapidly dissolved in water.

[0047] Example 6

[0048] A method for preparing an antibacterial and rapidly water-soluble thermosetting material comprises the following steps:

[0049] Step 1: add 1g hexanediol, 2.4g chloroacetic acid, 11ml toluene solution and 0.2g p-toluenesulfonic acid into a 50ml flask, stir at 120°C for 12h to obtain a mixed solution, wherein the toluene solution is used as a solvent and the p-toluenesulfonic acid is used as a catalyst; use a sodium hydroxide solution to alkaline wash the mixed solution to pH = 10.0, and the concentration of the sodium hydroxide solution is 1 mol / L; then wash with water to pH = 7.0 and then separate the liquids, and wash with water to remove the salt in the mixed solution; after separation, take the upper layer solution and dry it with anhydrous magnesium sulfate for 24h, and filter to remove the anhydrous magnesium sulfate that has absorbed water; then perform rotary evaporation at 60°C in a rotary evaporator until no liquid is rotated out, and perform reduced pressure distillation at 175°C until no liquid is evaporated to obtain hexanediol chloroacetate;

[0050] Step 2: Mix 1.92 g of hexanediol chloroacetate prepared in step 1 and 1 g of pentamethyldipropylenetriamine in a beaker, stir for 15 seconds, pour the mixture into a silicone mold, and cure it at 60° C. for 12 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material. The antibacterial, rapidly water-soluble thermosetting system material has high hardness and good broad-spectrum antibacterial properties, and can be quickly dissolved in water.

[0051] Example 7

[0052] A method for preparing an antibacterial and rapidly water-soluble thermosetting material comprises the following steps:

[0053] Step 1: add 1g propylene glycol, 3.0g chloroacetic acid, 12ml toluene solution and 0.2g p-toluenesulfonic acid into a 50ml flask, stir at 120°C for 12h to obtain a mixed solution, wherein the toluene solution is used as a solvent and the p-toluenesulfonic acid is used as a catalyst; use a sodium hydroxide solution to alkaline wash the mixed solution to pH = 10.0, and the concentration of the sodium hydroxide solution is 1mol / L; then wash with water to pH = 7.0 and then separate the liquids, and wash with water to remove the salt in the mixed solution; after separation, take the upper solution and dry it with anhydrous magnesium sulfate for 24h, and filter to remove the anhydrous magnesium sulfate that has absorbed water; then perform rotary evaporation at 60°C in a rotary evaporator until no liquid is rotated out, and perform reduced pressure distillation at 175°C until no liquid is evaporated to obtain propylene glycol chloroacetate;

[0054] Step 2: Mix 1.17 g of propylene glycol chloroacetate prepared in step 1 and 1 g of 2,4,6-tris(dimethylaminomethyl)phenol in a beaker, stir for 15 seconds, pour the mixture into a silicone mold, and cure at 60°C for 12 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material. The antibacterial, rapidly water-soluble thermosetting system material has high hardness and good broad-spectrum antibacterial properties and can be rapidly dissolved in water.

[0055] Example 8

[0056] A method for preparing an antibacterial and rapidly water-soluble thermosetting material comprises the following steps:

[0057] Step 1: add 1g propylene glycol, 3.0g chloroacetic acid, 12ml toluene solution and 0.2g p-toluenesulfonic acid into a 50ml flask, stir at 120°C for 12h to obtain a mixed solution, wherein the toluene solution is used as a solvent and the p-toluenesulfonic acid is used as a catalyst; use a sodium hydroxide solution to alkaline wash the mixed solution to pH = 10.0, and the concentration of the sodium hydroxide solution is 1mol / L; then wash with water to pH = 7.0 and then separate the liquids, and wash with water to remove the salt in the mixed solution; after separation, take the upper solution and dry it with anhydrous magnesium sulfate for 24h, and filter to remove the anhydrous magnesium sulfate that has absorbed water; then perform rotary evaporation at 60°C in a rotary evaporator until no liquid is rotated out, and perform reduced pressure distillation at 175°C until no liquid is evaporated to obtain propylene glycol chloroacetate;

[0058] Step 2: Mix 1.55 g of propylene glycol chloroacetate prepared in step 1 and 1 g of pentamethyldipropylenetriamine in a beaker, stir for 15 seconds, pour the mixture into a silicone mold, and cure it at 60° C. for 12 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material. The antibacterial, rapidly water-soluble thermosetting system material has high hardness and good broad-spectrum antibacterial properties and can be rapidly dissolved in water.

[0059] Example 9

[0060] A method for preparing an antibacterial and rapidly water-soluble thermosetting material comprises the following steps:

[0061] Step 1: add 1g hexanediol, 2.4g chloroacetic acid, 11ml toluene solution and 0.2g p-toluenesulfonic acid into a 50ml flask, stir at 120°C for 12h to obtain a mixed solution, wherein the toluene solution is used as a solvent and the p-toluenesulfonic acid is used as a catalyst; use a sodium hydroxide solution to alkaline wash the mixed solution to pH = 10.0, and the concentration of the sodium hydroxide solution is 1 mol / L; then wash with water to pH = 7.0 and then separate the liquids, and wash with water to remove the salt in the mixed solution; after separation, take the upper layer solution and dry it with anhydrous magnesium sulfate for 24h, and filter to remove the anhydrous magnesium sulfate that has absorbed water; then perform rotary evaporation at 60°C in a rotary evaporator until no liquid is rotated out, and perform reduced pressure distillation at 175°C until no liquid is evaporated to obtain hexanediol chloroacetate;

[0062] Step 2: Mix 1.34 g of hexanediol chloroacetate prepared in step 1 and 1 g of 2,4,6-tris(dimethylaminomethyl)phenol in a beaker, stir for 15 seconds, pour the mixture into a silicone mold, and cure it at 60°C for 12 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material. The antibacterial, rapidly water-soluble thermosetting system material has high hardness and good broad-spectrum antibacterial properties and can be rapidly dissolved in water.

[0063] Example 10

[0064] A method for preparing an antibacterial and rapidly water-soluble thermosetting material comprises the following steps:

[0065] Step 1: add 1g hexanediol, 2.4g chloroacetic acid, 11ml toluene solution and 0.2g p-toluenesulfonic acid into a 50ml flask, stir at 120°C for 12h to obtain a mixed solution, wherein the toluene solution is used as a solvent and the p-toluenesulfonic acid is used as a catalyst; use a sodium hydroxide solution to alkaline wash the mixed solution to pH = 10.0, and the concentration of the sodium hydroxide solution is 1 mol / L; then wash with water to pH = 7.0 and then separate the liquids, and wash with water to remove the salt in the mixed solution; after separation, take the upper layer solution and dry it with anhydrous magnesium sulfate for 24h, and filter to remove the anhydrous magnesium sulfate that has absorbed water; then perform rotary evaporation at 60°C in a rotary evaporator until no liquid is rotated out, and perform reduced pressure distillation at 175°C until no liquid is evaporated to obtain hexanediol chloroacetate;

[0066] Step 2: Mix 1.8 g of hexanediol chloroacetate prepared in step 1 and 1 g of pentamethyldipropylenetriamine in a beaker, stir for 15 seconds, pour the mixture into a silicone mold, and cure it at 60° C. for 12 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material. The antibacterial, rapidly water-soluble thermosetting system material has high hardness and good broad-spectrum antibacterial properties and can be rapidly dissolved in water.

[0067] Embodiment 11

[0068] A method for preparing an antibacterial and rapidly water-soluble thermosetting material comprises the following steps:

[0069] Step 1: add 1g propylene glycol, 3.0g chloroacetic acid, 12ml toluene solution and 0.2g p-toluenesulfonic acid into a 50ml flask, stir at 120°C for 12h to obtain a mixed solution, wherein the toluene solution is used as a solvent and the p-toluenesulfonic acid is used as a catalyst; use a sodium hydroxide solution to alkaline wash the mixed solution to pH = 10.0, and the concentration of the sodium hydroxide solution is 1mol / L; then wash with water to pH = 7.0 and then separate the liquids, and wash with water to remove the salt in the mixed solution; after separation, take the upper solution and dry it with anhydrous magnesium sulfate for 24h, and filter to remove the anhydrous magnesium sulfate that has absorbed water; then perform rotary evaporation at 60°C in a rotary evaporator until no liquid is rotated out, and perform reduced pressure distillation at 175°C until no liquid is evaporated to obtain propylene glycol chloroacetate;

[0070] Step 2: Mix 1.09 g of propylene glycol chloroacetate prepared in step 1 and 1 g of 2,4,6-tris(dimethylaminomethyl)phenol in a beaker, stir for 15 seconds, pour the mixture into a silicone mold, and cure at 60°C for 12 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material. The antibacterial, rapidly water-soluble thermosetting system material has high hardness and good broad-spectrum antibacterial properties and can be rapidly dissolved in water.

[0071] Embodiment 11

[0072] A method for preparing an antibacterial and rapidly water-soluble thermosetting material comprises the following steps:

[0073] Step 1: add 1g propylene glycol, 3.0g chloroacetic acid, 12ml toluene solution and 0.2g p-toluenesulfonic acid into a 50ml flask, stir at 120°C for 12h to obtain a mixed solution, wherein the toluene solution is used as a solvent and the p-toluenesulfonic acid is used as a catalyst; use a sodium hydroxide solution to alkaline wash the mixed solution to pH = 10.0, and the concentration of the sodium hydroxide solution is 1mol / L; then wash with water to pH = 7.0 and then separate the liquids, and wash with water to remove the salt in the mixed solution; after separation, take the upper solution and dry it with anhydrous magnesium sulfate for 24h, and filter to remove the anhydrous magnesium sulfate that has absorbed water; then perform rotary evaporation at 60°C in a rotary evaporator until no liquid is rotated out, and perform reduced pressure distillation at 175°C until no liquid is evaporated to obtain propylene glycol chloroacetate;

[0074] Step 2: Mix 1.44 g of propylene glycol chloroacetate prepared in step 1 and 1 g of pentamethyldipropylenetriamine in a beaker, stir for 15 seconds, pour the mixture into a silicone mold, and cure it at 60° C. for 12 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material. The antibacterial, rapidly water-soluble thermosetting system material has high hardness and good broad-spectrum antibacterial properties and can be rapidly dissolved in water.

[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing an antibacterial, rapidly water-soluble thermosetting material, characterized in that: The following steps are involved: Step 1: add diol, halogenated acid, toluene and p-toluenesulfonic acid, stir at 50-160° C. for 1-24 hours to obtain a mixed solution; use an alkaline solution to adjust the pH of the mixed solution to 9.0-11.0, then wash with water until the pH is 7.0 and separate the liquids; after separation, take the upper layer solution and dry it with anhydrous magnesium sulfate for 3-48 hours; perform rotary evaporation at 60° C. in a rotary evaporator until no liquid is evaporated, and perform reduced pressure distillation at 120-200° C. until no liquid is evaporated to obtain diol halogenated ester; The molar ratio of the diol, the halogenated acid, toluene and p-toluenesulfonic acid is 1:2-3:3-10:0.1-0.3; The diol is ethylene glycol, propylene glycol, butylene glycol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol or decanediol; The halogenated acid is chloroacetic acid, chloropropionic acid, chlorobutyric acid, chlorovaleric acid, chlorohexanoic acid, chloroheptanoic acid, chlorooctanoic acid, chlorononanoic acid, chlorodecanoic acid, bromoacetic acid, bromopropionic acid, bromobutyric acid, bromovaleric acid, bromohexanoic acid, bromoheptanoic acid, bromooctanoic acid, bromononanoic acid, bromodecaneic acid, iodoacetic acid, iodopropionic acid, iodobutyric acid, iodovaleric acid, iodohexanoic acid, iodoheptanoic acid, iodooctanoic acid, iodononanoic acid or iododecanoic acid; Step 2: Mix the diol halogenated ester prepared in step 1 with the ternary tertiary amine in a molar ratio of 1:0.5-2; and cure at 10-160° C. for 1-24 hours to obtain an antibacterial, rapidly water-soluble thermosetting system material; The tertiary amine is pentamethyldiethylenetriamine or pentamethyldipropylenetriamine or 2,4,6-tris(dimethylaminomethyl)phenol.

2. An antibacterial, rapidly water-soluble thermosetting material prepared by the method of claim 1.

Citation Information

Patent Citations

  • Synthetic method of epoxy resin cured product capable of being hydrolyzed under alkalescence