A method for manufacturing a double-sided tape with TPU as a substrate

By matching a suitable adhesive layer on the TPU substrate, the problem of bonding between low-surface energy materials and common plastics is solved, high adhesion and durability are achieved, and it is suitable for the bonding needs of long-term wearing equipment.

CN115109534BActive Publication Date: 2024-11-26SUZHOU LINGHUI MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210695067.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-20
Publication Date
2024-11-26
Estimated Expiration
2042-06-20

AI Technical Summary

Technical Problem

Existing glues or tapes are difficult to firmly bond and fix low-surface energy materials such as TPU, silicone rubber and common plastics, especially when long-term wear and maintain stretched and bent state, and are tolerated to the environment. insufficient.

Method used

Double-sided tape using TPU as the substrate is used to ensure adhesion and durability by making TPU base layer, low-surface energy-supply adhesive layer and medium- and high-surface energy-supply adhesive layer, combined with specific adhesive layer components and process flow.

Benefits of technology

It realizes stable bonding to low-surface energy materials, provides high adhesion and repeatable tear-off functions, meeting long-term use and environmental tolerance requirements, especially in applications in wearable devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115109534B_ABST
    Figure CN115109534B_ABST
Patent Text Reader

Abstract

The present application provides a method for making a double-sided tape with TPU as the base material, the method comprising the following steps: (A) making a TPU base layer; (B) making a low surface energy applicable adhesive layer and laminating it on the TPU base layer; (C) making a medium and high surface energy applicable adhesive layer and laminating it on the TPU base layer, the thickness of the TPU base layer is 30 to 250um, the tensile strength is 5 to 95MPa, and the elongation at break is 450% to 1500%. The novel TPU double-sided tape solves the problem of bonding low surface energy TPU foam or silicone rubber on common plastic materials by innovatively introducing a TPU base material and combining low surface energy applicable adhesive and polyacrylic resin on both sides suitable for different surface energies, and has the advantages of elasticity and weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of adhesive tapes, and in particular to a method for manufacturing a double-sided adhesive tape with TPU as a substrate. Background Art

[0002] The description in this section merely provides background information related to the present disclosure and does not constitute prior art.

[0003] As consumer electronics products become increasingly wearable, the hardware of smart watches, bracelets, and emerging VR devices (including head-mounted and wristbands, handheld controllers, etc.) will be designed to be suitable for long-term wear, that is, the wearing material is more skin-friendly, the overall weight is lighter, and the battery life is longer. Among them, skin-friendly materials include not only hardness and touch, but also whether they can be as waterproof as possible, oil-free, dust-free, and other hygiene and health considerations. Therefore, in some places that come into contact with human skin for a long time, such as the straps of smart watches and bracelets, the headbands of VR headsets, and the foam pads of bracelets, some loose, porous, lightweight, chemically inert, and low surface energy silicone rubber or TPU materials that are not stained with water, oil, or dust are used.

[0004] Therefore, when assembling electronic devices, it is difficult to bond and fix these low surface energy materials with conventional glue or tape, because these external materials usually need to be fixed to the internal structural frame or electronic components. Single-material glue (including adhesives coated on the surface of tape products) is difficult to bond and fix low surface energy materials and common plastics such as PC, PS and other materials at the same time. At the same time, because these skin-friendly materials are mostly lightweight, porous and elastic, they need to be stretched and bent to fit the human body contour after the finished product is assembled, which also increases the difficulty of firm and snug bonding. In addition, due to long-term wear, the bonding of these materials will also be affected by or come from external conditions (such as direct sunlight outdoors) and the heat caused by the continuous operation of the machine, and a certain tolerance to the environment is required.

[0005] It should be noted that the above introduction to the technical background is only for the convenience of providing a clear and complete description of the technical solutions of the present invention and for the convenience of understanding by those skilled in the art. It cannot be considered that the above technical solutions are well known to those skilled in the art simply because these solutions are described in the background technology section of the present invention. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a double-sided tape with TPU as the base material and a method for making the same, which can solve the problem of long-term and stable bonding of porous, elastic, low-surface-energy silicone rubber or TPU materials on the surfaces of conventional materials such as PC, PS, metal, etc. in the above-mentioned situation. In order to solve the above-mentioned technical problem, the present application provides a method for making a double-sided tape with TPU as the base material, and the said method for making the same comprises the following steps: (A) making a TPU base layer; (B) making a low-surface-energy applicable adhesive layer and attaching it to the TPU base layer; (C) making a medium- and high-surface-energy applicable adhesive layer and attaching it to the TPU base layer, and the said TPU base layer has a thickness of 30 to 250 um, a tensile strength of 5 to 95 MPa, and an elongation at break of 450% to 1500%.

[0007] Preferably, the low surface energy applicable adhesive layer has a surface adhesion of more than 20N / in to low surface energy materials with a bonding surface energy of <30, and the medium and high surface energy applicable adhesive layer has a surface adhesion of more than 20N / in to medium and high surface energy materials with a bonding surface energy of >38.

[0008] Preferably, step (A) comprises: (A1) taking polyether TPU particles and polyester TPU particles, the mass ratio of the polyether TPU particles to the polyester TPU particles is between 4:1-7:1, dissolving them with a solvent to obtain a TPU mixed solution with a solid content in the range of 25-35%; (A2) taking a release film or release paper with a release agent coated on the surface, coating the TPU solution thereon, heating and baking after coating to volatilize the solvent, and removing the release film or release paper after curing to obtain a TPU base layer.

[0009] Preferably, step (B) comprises: (B1) mixing silicone or rubber with a molecular weight of 800,000 to 1,000,000 and vinyl silicone oil with a molecular weight of 10,000 to 30,000 in a ratio of 1:2-2:1, adding silicone oil and additives after mixing and dissolving with a solvent; (B2) coating the solution obtained by (B1) on the TPU base layer obtained by (A2); (B3) using a gradually increasing temperature method to volatilize the solvent to obtain a low surface energy applicable adhesive layer covering the TPU base layer, and after curing, laminating a layer of release film or release paper on the low surface energy applicable adhesive layer as surface protection,

[0010] The specific test method for the adhesion of the low surface energy applicable adhesive layer to low surface energy materials is: on the surface of low surface energy materials (surface energy of the bonding surface <30), the adhesion test result reaches 20N / in or more, and the above is tested according to the test standard ASTM D3330 or GB / T 2792-2014. The low surface energy applicable adhesive layer has the effect of being repeatedly torn off and pasted again. The judgment method is: after pasting the adhesive layer on the surface of standard 304 stainless steel, it can be torn off without residual adhesive, the adhesive surface is not damaged, and it can be pasted again. Specifically, according to the test standard ASTM D3330 or GB / T 2792-2014, 2kg roller pressure is applied and left to stand for 20 minutes. After standing, the adhesive surface is peeled off. The peeling process is smooth, and there is no residual adhesive or damage on the stainless steel plate and the adhesive surface. The pasting test can be repeated again, and this can be repeated for 10 times or more.

[0011] Preferably, step (C) comprises: (C1) taking an acrylic copolymer, mixing it with an isocyanate curing agent in a mass ratio of 60:1-100:1, dissolving it with a solvent, and obtaining an acrylate-isocyanate copolymer solution; (C2) taking a release film or release paper with a release agent coated on the surface, coating the acrylate-isocyanate copolymer solution thereon, heating and baking after coating to evaporate the solvent and form a polyacrylate adhesive layer; (C3) laminating the polyacrylate adhesive layer with the release film or release paper to the surface of the TPU base layer described in step (B3), the polyacrylate layer contacts the TPU surface, removing the release film or release paper, and obtaining a polyacrylate adhesive layer laminated to the TPU substrate layer. The design standard adhesion test is carried out by the following test method: testing is carried out on the surface of a standard 304 stainless steel plate according to the test standard ASTM D3330 or GB / T 2792-2014.

[0012] Preferably, in step (A1), the polyether TPU particles and the polyester TPU particles are both OH-terminated, the solution in step (A1) is a mixed solvent of polar and non-polar solvents, the mass ratio of non-polar to polar solvents is 1.2:1-1.6:1, and the total mass of the solvent to the total mass of the TPU particles is 3.5:1-4:1. Furthermore, the solvent can be a mixed solvent of toluene and DMF or a mixed solvent of other polar and non-polar solvents; in step (A2), the release agent is a silicone-based release agent or a fluoride release agent, the release film is one of PET material, PE material, and PP material, and the heating and baking temperature range is 50-120°C.

[0013] Preferably, in step (B1), the silicone or rubber is vinyl-modified silicone or rubber, the solvent is a medium-polarity aromatic hydrocarbon solvent, the total mass of the silicone oil is 1-3% of the silicone or rubber, the silicone oil is a mixture of hydrogenated silicone oil and epoxy-modified silicone oil, the mass ratio of the hydrogenated silicone oil to the epoxy-modified silicone oil is 1:1-2:1, and 2% of platinum by mass of polymerized silicone or rubber is added as a catalyst, and further, the solvent can be toluene; in step (B3), after curing, the residual solvent content in the low surface energy applicable adhesive layer is <0.1%, and the gradually heating operation refers to starting from 40-50°C and gradually rising to 150-160°C;

[0014] Preferably, the solvent in step (C1) is a mixture of acrylate and one or two medium-grade solvents, the mass ratio of the acrylate to the medium-grade solvent is 11:10-15:10, and further, the solvent is ethyl acetate or a mixed solvent of ethyl acetate and toluene; in step (C2), after curing, the residual solvent content in the polyacrylate adhesive layer is <0.1%, the release agent is a silicone-based release agent or a fluoride release agent, the release film is made of PET, PE, or PP, and the heating and baking temperature starts at 40-50° C. and gradually rises to 100-110° C. until the solvent evaporates.

[0015] The beneficial effects of the present invention are as follows:

[0016] (1) The thickness of the TPU base layer of the present application is 40-100um, the solid content is about 25-35%, the material modulus reaches 30MPa, and it has a breaking elongation of 700% to 1000%. It has excellent elasticity and ductility, and can reduce the stress caused by the different degrees of deformation on both sides of the bonding after stretching. In addition, the chemical properties of this TPU finished product are stable and it has good resistance to ultraviolet and temperature.

[0017] (2) The conventional surface adhesion of the polyacrylate adhesive layer of the double-sided tape of the present application can reach more than 20 N / in according to the test standard ASTM D3330 or GB / T 2792-2014 and other equivalent standards.

[0018] (3) Low surface energy material adaptation The surface adhesion of the adhesive layer to low surface energy materials (surface dyne value <= 30) is above 20N / in according to the test standard ASTM D3330 or GB / T 2792-2014 and other equivalent standards. At the same time, due to its high cohesive force, it can be removed after bonding and then repeatedly bonded to meet the needs of repeated positioning in some assembly processes.

[0019] In summary, this new TPU double-sided tape solves the bonding problem of low surface energy TPU foam or silicone rubber on common plastic materials by innovatively introducing TPU substrate and matching it with double-sided low surface energy adhesive and polyacrylic resin suitable for different surface energies. It also has the advantages of elasticity and weather resistance, and is an ideal solution to solve the difficulties of this type of application. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram of the structure of the double-sided tape of the present application.

[0021] Among them: 1, 5, release film or release paper; 2. Low surface energy applicable adhesive layer; 3. TPU substrate surface layer; 4. Polyacrylate adhesive layer. DETAILED DESCRIPTION

[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1

[0024] (A) Preparation of TPU base layer: (A1) Take 4 parts by mass of OH-terminated polyether TPU particles, mix with 1 part of polyester TPU particles, use 18 parts by mass of toluene and 11 parts by mass of DMF as solvents to form a TPU mixed solution; (A2) Use PET release film as a supporting base, apply the TPU mixture on the PET release film, bake at 50°C to evaporate the solvent, and form a TPU base layer. The thickness of this TPU product is 30um, the solid content is about 25%, the material modulus reaches 30MPa, the elongation at break is 450%, and the tensile strength is 5MPa. It has excellent elasticity and ductility, and can reduce the stress caused by the different degrees of deformation on both sides of the bonding after stretching. In addition, the chemical properties of this TPU product are stable and it has good resistance to ultraviolet and temperature.

[0025] (B) Preparation of low surface energy applicable adhesive layer: (B1) taking silica gel with a molecular weight of 800,000 to 1,000,000 and vinyl silicone oil with a molecular weight of 10,000 to 30,000, mixing them in a ratio of 1:2, adding silicone oil and additives after mixing and dissolving them with a solvent, wherein the silica gel is vinyl modified silica gel, the solvent is a medium polar aromatic hydrocarbon solvent, the total mass of the silicone oil is 1% of the silica gel or rubber, the silicone oil is a mixture of hydrogenated silicone oil and epoxy modified silicone oil, the mass ratio of the hydrogenated silicone oil to the epoxy modified silicone oil is 1:1, and 2% of platinum by mass of the polymerized silica gel or rubber is added as a catalyst; (B2) coating the silica gel mixture on the TPU base layer formed in step (A2); (B3) using a gradually increasing temperature method to volatilize the solvent to obtain a low surface energy applicable adhesive layer covering the TPU base layer, and after curing, laminating a layer of release film or release paper on the low surface energy applicable adhesive layer as surface protection, wherein the gradually increasing temperature method is specifically, starting from 40°C and gradually increasing to 150°C.

[0026] (C) Preparation of adhesive layers suitable for medium and high surface energy: (C1) Take an acrylic copolymer, mix it with an isocyanate curing agent in a mass ratio of 60:1, and dissolve it in a solvent to obtain an acrylate-isocyanate copolymer solution; (C2) Take a release film with a release agent coated on the surface, coat the acrylate-isocyanate copolymer solution on it, heat and bake it after coating to evaporate the solvent, and form a polyacrylate adhesive layer. After curing, the residual solvent content in the polyacrylate adhesive layer is <0.1%. The release agent is a silicone-based release agent, and the release film is made of PET. The heating and baking temperature starts from 40°C and gradually rises to 100°C until the solvent evaporates; (C3) The polyacrylate adhesive layer with the release film is laminated to the surface of the TPU base layer in step (B3), so that the polyacrylate layer contacts the TPU surface, and the release film is removed to obtain a polyacrylate adhesive layer laminated to the TPU substrate layer.

[0027] Example 2

[0028] (A) Preparation of TPU base layer: (A1) Take 7 parts by mass of OH-terminated polyether TPU particles, mix with 1 part of polyester TPU particles, use 18 parts by mass of toluene and 11 parts by mass of DMF as solvents to form a TPU mixed solution; (A2) Use PET release film as a supporting base, apply the TPU mixture on the PET release film, bake at 120°C to evaporate the solvent, and form a TPU base layer. The thickness of this TPU product is 250um, the solid content is about 25%, the material modulus reaches 30MPa, the elongation at break is 1500%, the tensile strength is 95MPa, it has excellent elasticity and ductility, and can reduce the stress caused by the different degrees of deformation on both sides of the bonding after stretching. In addition, the chemical properties of this TPU finished product are stable and it has good resistance to ultraviolet and temperature.

[0029] (B) Preparation of low surface energy applicable adhesive layer: (B1) Rubber with a molecular weight of 800,000 to 1,000,000 and vinyl silicone oil with a molecular weight of 10,000 to 30,000 are mixed in a ratio of 2:1, silicone oil and additives are added after mixing and dissolved with a solvent, wherein the rubber is a vinyl modified rubber, the solvent is a medium polar aromatic hydrocarbon solvent, the total mass of the silicone oil is 3% of the silicone or rubber, the silicone oil is a mixture of hydrogenated silicone oil and epoxy modified silicone oil, the mass ratio of the hydrogenated silicone oil to the epoxy modified silicone oil is 2:1, and 2% of platinum by mass of the polymerized silicone or rubber is added as a catalyst; (B2) The silicone mixture is coated on the TPU base layer formed in step (A2); (B3) The solvent is volatilized by a gradually increasing temperature method to obtain a low surface energy applicable adhesive layer covering the TPU base layer, and after curing, a layer of release film or release paper is attached to the low surface energy applicable adhesive layer as surface protection, wherein the gradually increasing temperature method is specifically, starting from 50°C and gradually increasing to 160°C.

[0030] (C) Preparation of medium and high surface energy suitable adhesive layer: (C1) Take an acrylic copolymer, mix it with an isocyanate curing agent in a mass ratio of 100:1, and use a solvent to dissolve it to obtain an acrylate-isocyanate copolymer solution; (C2) Take a release paper with a release agent coated on the surface, coat the acrylate-isocyanate copolymer solution on it, heat and bake after coating to evaporate the solvent to form a polyacrylate adhesive layer, after curing, the residual solvent content in the polyacrylate adhesive layer is <0.1%, the release agent is a silicone-based release agent, and the release paper is made of PE material. The heating and baking temperature starts from 50°C and gradually rises to 110°C until the solvent evaporates; (C3) The polyacrylate adhesive layer with the release paper is laminated to the surface of the TPU base layer in step (B3), the polyacrylate layer is in contact with the TPU surface, and the release paper is removed to obtain a polyacrylate adhesive layer laminated to the TPU substrate layer.

[0031] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A method for preparing a double-sided tape with TPU as a substrate, characterized in that: The manufacturing method comprises the following steps: (A) manufacturing a TPU base layer; (B) manufacturing a low surface energy applicable adhesive layer and laminating it on the TPU base layer; (C) manufacturing a medium and high surface energy applicable adhesive layer and laminating it on the TPU base layer. The thickness of the TPU base layer is 30-250um, the tensile strength is 5-95MPa, and the elongation at break is 450%-1500%. The low surface energy applicable adhesive layer has a surface adhesion of more than 20N / in to low surface energy materials with a bonding surface energy of <30, and the medium and high surface energy applicable adhesive layer has a surface adhesion of more than 20N / in to medium and high surface energy materials with a bonding surface energy of >38. Step (A) comprises, (A1) taking polyether TPU particles and polyester TPU particles, wherein the mass ratio of the polyether TPU particles to the polyester TPU particles is between 4:1 and 7:1, dissolving them in a solvent to obtain a TPU mixed solution having a solid content in the range of 25% to 35%; (A2) taking a release film or release paper coated with a release agent, coating the TPU solution thereon, heating and baking after coating to evaporate the solvent, and removing the release film or release paper after curing to obtain a TPU base layer. Step (B) comprises, (B1) Mixing silicone or rubber with a molecular weight of 800,000 to 1,000,000 and vinyl silicone oil with a molecular weight of 10,000 to 30,000 in a ratio of 1:2 to 2:1, adding silicone oil and additives after mixing and dissolving with a solvent; (B2) coating the solution obtained from (B1) on the TPU base layer obtained from (A2); (B3) The solvent is evaporated by gradually increasing the temperature to obtain a low surface energy applicable adhesive layer covering the TPU base layer. After curing, a release film or release paper is attached to the low surface energy applicable adhesive layer as a surface protection. Step (C) comprises, (C1) taking an acrylic copolymer, mixing it with an isocyanate curing agent in a mass ratio of 60:1-100:1, dissolving it in a solvent to obtain an acrylate - isocyanate copolymer solution; (C2) taking a release film or release paper having a release agent coated on the surface, coating an acrylate-isocyanate copolymer solution thereon, and heating and baking after coating to evaporate the solvent to form a polyacrylate adhesive layer; (C3) laminating a polyacrylate adhesive layer with a release film or release paper to the surface of the TPU base layer in step (B3), with the polyacrylate layer in contact with the TPU surface, removing the release film or release paper, and obtaining a polyacrylate adhesive layer laminating to the TPU base layer. In step (A1), both the polyether TPU particles and the polyester TPU particles have OH endcapping. The solution in step (A1) is a mixed solvent of polar and non-polar solvents, the mass ratio of the non-polar solvent to the polar solvent is 1.2:1-1.6:1, and the total mass ratio of the solvent to the total mass of the TPU particles is 3.5:1-4:1; In step (A2), the release agent is a silicone-based release agent or a fluoride release agent, the release film is made of PET, PE, or PP, and the heating and baking temperature ranges from 50 to 120°C. In step (B1), the silicone or rubber is vinyl-modified silicone, the solvent is a medium-polarity aromatic hydrocarbon solvent, the total mass of the silicone oil is 1-3% of the silicone or rubber, the silicone oil is a mixture of hydrogenated silicone oil and epoxy-modified silicone oil, the mass ratio of the hydrogenated silicone oil to the epoxy-modified silicone oil is 1:1-2:1, and platinum is added as a catalyst in an amount of 2% of the mass of the silicone or rubber; In step (B3), after curing, the residual solvent content in the low surface energy applicable adhesive layer is less than 0.1%, and the gradually increasing temperature operation refers to starting from 40-50°C and gradually increasing to 150-160°C. The solvent in step (C1) is a mixture of acrylate and one or two medium-grade solvents, and the mass ratio of the acrylate to the medium-grade solvent is 11:10-15:10; In step (C2), after curing, the residual solvent content in the polyacrylate adhesive layer is less than 0.1%, the release agent is a silicone-based release agent or a fluoride release agent, the release film is made of PET, PE, or PP, and the heating and baking temperature starts at 40-50°C and gradually rises to 100-110°C until the solvent evaporates.