A nitrogen-doped carbon-based oxygen reduction reaction catalyst and its preparation method and application

Through the two-stage pyrolysis reaction of cyclodextrin-based metal organic framework materials and ammonium salts, a nitrogen-doped carbon-based oxygen reduction catalyst with a high specific surface area is prepared, which solves the problem of strong acid in the preparation process of carbon-based oxygen reduction catalysts in the existing technology. Or the problems of using strong base and regulating pore structure have achieved efficient oxygen reduction catalytic performance.

CN115117373BActive Publication Date: 2024-10-29BEIJING UNIV OF CHEM TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210517925.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-13
Publication Date
2024-10-29
Estimated Expiration
2042-05-13

AI Technical Summary

Technical Problem

The preparation process of existing carbon-based oxygen reduction catalysts requires strong acid or strong alkali, and the control of pore structure is cumbersome and risky, making it difficult to increase the specific surface area through a simple, efficient and green method.

Method used

A two-stage pyrolysis reaction between cyclodextrin-based metal-organic framework materials and ammonium salts is adopted. Through in-situ doping of NH3 and decomposition of ammonium salts, NH3 is generated and reacts with cyclodextrin-based metal-organic framework materials to form nitrogen-doped carbon materials. , combined with inert gas or nitrogen atmosphere for pyrolysis, and washing to remove the hard template to increase the specific surface area.

Benefits of technology

A nitrogen-doped carbon-based oxygen reduction catalyst with rich recessed and porous structures was prepared, which significantly improved the catalytic activity and specific surface area and reduced the cost. It is suitable for fuel cells and metal-air batteries, and its performance is close to that of commercial Pt/C catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115117373B_ABST
    Figure CN115117373B_ABST
Patent Text Reader

Abstract

The present invention discloses a nitrogen-doped carbon-based oxygen reduction reaction catalyst, a preparation method and an application thereof. The nitrogen-doped carbon-based oxygen reduction reaction catalyst provided by the present invention is prepared by mixing a cyclodextrin-based metal organic framework material and an ammonium salt to obtain a mixture A, placing the mixture A in an inert gas or nitrogen atmosphere for a two-stage pyrolysis reaction to obtain a reaction product B, and washing and drying the reaction product B. The present invention also provides a preparation method and an application of the nitrogen-doped carbon-based oxygen reduction reaction catalyst. The nitrogen-doped carbon-based oxygen reduction catalyst provided by the present invention is a nitrogen-doped carbon material having a large number of concave structures on the surface, a large specific surface area, a hierarchical micropore and mesoporous structure, and the doping of nitrogen atoms increases the oxygen reduction active sites, so the electrocatalytic oxygen reduction performance is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrocatalyst preparation, and more specifically, to a nitrogen-doped carbon-based oxygen reduction reaction catalyst, a preparation method and application thereof. Background Art

[0002] The continuous consumption of traditional fossil fuels has caused a series of environmental pollution problems such as global warming and acid rain. Clean renewable energy technology has attracted widespread attention. In order to meet this growing energy demand and solve the environmental pollution problems caused by fossil fuels, renewable energy and clean energy have received widespread attention. Among many renewable energy and clean energy conversion technologies, metal-air batteries and fuel cells are the most promising. Fuel cells and metal-air batteries are a clean energy technology that directly converts chemical energy into electrical energy. However, the oxygen reduction reaction at the cathode during the discharge process has a slow kinetic rate, which restricts the development of such energy devices. Catalysts are urgently needed to accelerate the oxygen reduction reaction.

[0003] At present, platinum-based catalysts are the most effective commercial oxygen reduction catalysts, but platinum metal is expensive, has low reserves, poor stability and is easily poisoned. In recent years, carbon-based metal-free catalysts have been widely studied by scholars due to their low cost, excellent resistance to poisoning and high stability. By doping nitrogen into the carbon skeleton and increasing the specific surface area of ​​the carbon material, its oxygen reduction catalytic performance can be significantly improved, but how to regulate the pore structure of carbon materials and increase the specific surface area through simple, efficient and green methods remains to be solved. Hard templates such as silica and porous alumina can effectively regulate the pore structure of carbon materials and increase the specific surface area of ​​carbon materials. However, during the preparation process, the template agent and the catalyst precursor need to be evenly mixed, and strong acid or strong base is generally required to remove the template. The preparation process is cumbersome, highly dangerous and environmentally unfriendly.

[0004] Therefore, the present invention provides a nitrogen-doped carbon-based oxygen reduction reaction catalyst and a preparation method and application thereof, which at least solves one of the above problems. Summary of the invention

[0005] The first object of the present invention is to provide a nitrogen-doped carbon-based oxygen reduction reaction catalyst.

[0006] The second object of the present invention is to provide a method for preparing a nitrogen-doped carbon-based oxygen reduction reaction catalyst.

[0007] The third object of the present invention is to provide an application of a nitrogen-doped carbon-based oxygen reduction reaction catalyst.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] The invention provides a nitrogen-doped carbon-based oxygen reduction reaction catalyst, which is prepared by mixing a cyclodextrin-based metal organic framework material and an ammonium salt to obtain a mixture A, placing the mixture A in an inert gas or nitrogen atmosphere for a two-stage pyrolysis reaction to obtain a reaction product B, and washing and drying the reaction product B.

[0010] The nitrogen-doped carbon-based oxygen reduction catalyst provided by the present invention is a nitrogen-doped carbon material having a large number of recessed structures on its surface. The recessed structures have abundant defects and porous structures, which are more likely to expose active sites. Among them, defects are considered to be active sites for oxygen reduction reactions, and abundant defects are beneficial to improving catalytic activity. The porous structure is beneficial to the transmission of reactants and accelerates the reaction.

[0011] As another aspect of the present invention, the present invention also provides a method for preparing a nitrogen-doped carbon-based oxygen reduction reaction catalyst, comprising the following steps:

[0012] A cyclodextrin-based metal organic framework material and an ammonium salt are mixed to obtain a mixture A, the mixture A is placed in an inert gas or nitrogen atmosphere for a two-stage pyrolysis reaction to obtain a reaction product B, and the reaction product B is washed and dried to obtain the nitrogen-doped carbon-based oxygen reduction reaction catalyst.

[0013] The present invention uses a mixture of a cyclodextrin-based metal organic framework material and an ammonium salt as a precursor. The ammonium salt used will decompose during the heating process to produce NH3, and NH3 can undergo a dehydration condensation reaction with the carboxyl group in the cyclodextrin-based metal organic framework material (CD-MOF1), thereby in situ incorporating N atoms into the material; the ammonium salt simultaneously serves as a nitrogen source and a pore-forming agent, which not only facilitates the incorporation of nitrogen elements, but also increases the specific surface area of ​​the material; the cyclodextrin-based metal organic framework material used has highly ordered porous channels on the one hand, which has advantages for preparing hierarchical porous carbon materials (the ligands of other framework materials themselves do not have nano-scale cavities, and it is difficult to prepare hierarchical porous carbon materials through other framework materials); on the other hand, the potassium ions uniformly present in the cyclodextrin-based metal organic framework material are pyrolyzed to generate relatively uniformly distributed potassium salts and potassium oxides as hard templates, which play a role in regulating the morphology and pore structure of the material; in addition, after washing to remove the hard template, the specific surface area of ​​the material can be further increased, thereby improving the electrocatalytic performance of the catalyst.

[0014] The present invention also creatively adopts a two-stage pyrolysis reaction to solve the problem that ammonium salts decompose rapidly at high temperatures, resulting in the inability of the decomposed NH3 to fully contact and react with the cyclodextrin-based metal organic framework material, thereby affecting the doping of nitrogen atoms.

[0015] Preferably, the mass ratio of the cyclodextrin-based metal organic framework material to the ammonium salt is 1:1-10.

[0016] Preferably, in the two-stage heating reaction, the conditions for the first stage pyrolysis reaction are: 1-10°C·min -1 The heating rate is raised to 300-400°C and kept at this temperature for 0.1-2h. Furthermore, in some specific embodiments, the heating rate of the first stage pyrolysis reaction is 1-5°C·min -1 、5~10℃·min -1 etc., more preferably 5℃·min -1 ; The insulation temperature is 300-350°C, 350-400°C, etc., more preferably 350°C; the insulation time is 0.1-0.5h, 0.1-1h, 0.5-1h, 0.5-2h, 1-2h, etc., more preferably 0.5h.

[0017] Preferably, in the two-stage pyrolysis reaction, the conditions for the second stage pyrolysis reaction are: 1-10°C·min -1 The heating rate is raised to 800-1100°C and kept at this temperature for 1-4 hours; further, in some specific embodiments, the heating rate of the second stage pyrolysis reaction is 1-5°C·min -1 、5~10℃·min -1 etc., more preferably 5℃·min -1 ; The insulation temperature is 800-1000°C, 1000-1100°C, etc., more preferably 1000°C; the insulation time is 1-3h, 3-4h, etc., more preferably 3h.

[0018] The ammonium salt in the present application decomposes relatively slowly before 300-400°C (especially 350°C), and needs to stay for 0.1-2h (more preferably 0.5h) to allow the ammonium salt to fully and slowly decompose, so that NH3 and cyclodextrin-based metal organic framework materials react more fully and promote the doping of nitrogen atoms; secondary heating to 800-1100°C (preferably 1000°C) can allow the precursor to be fully carbonized into carbon material, increasing the conductivity of the material; if a one-time heating is adopted, or the first heating to 800-1100°C, the ammonium salt will quickly decompose at high temperature to produce NH3 and quickly escape, reducing the contact time and reaction time of NH3 and cyclodextrin-based metal organic framework materials, which is not conducive to nitrogen atom doping.

[0019] Preferably, the solvent used for washing the reaction product B is selected from one or more of deionized water, methanol, ethanol and isopropanol. In the present invention, the process of removing impurities from the reaction product B is near neutral conditions, without the need to use strong acid or strong base solutions, which reduces corrosion to the reaction equipment and is conducive to large-scale production.

[0020] Preferably, the reaction product B is dried after washing under the following conditions: vacuum drying at 40°C to 80°C for at least 24 hours; further, in some specific embodiments, the drying temperature is more preferably 60°C.

[0021] Preferably, the inert gas is argon.

[0022] Preferably, the cyclodextrin-based metal organic framework material is prepared by mixing cyclodextrin and potassium salt to obtain a mixture C, dissolving the mixture C in an inorganic solvent and placing the mixture in a closed space containing anhydrous methanol to carry out a coordination reaction to obtain a reaction product D, and washing and drying the reaction product D.

[0023] The -OCCO- unit in the cyclodextrin molecule used in the present application can be connected with a metal cation (K+) to form a cyclodextrin-based metal-organic framework material. This metal-organic framework material has a cyclodextrin-based metal-organic framework material with highly ordered porous channels, which has advantages in preparing hierarchical porous carbon materials.

[0024] The anhydrous methanol used in the present application has a low boiling point. At room temperature, the anhydrous methanol will evaporate, filling the enclosed space with methanol gas, which further diffuses into the mixed solution of cyclodextrin and potassium salt. If it is an open environment, the anhydrous methanol will evaporate into the environment, which is not conducive to the further diffusion of the anhydrous methanol gas into the mixed solution of cyclodextrin and potassium salt.

[0025] Preferably, the mass ratio of the cyclodextrin to the potassium salt is 1-2:0.1-1.

[0026] Preferably, the cyclodextrin is selected from one or more of α-cyclodextrin, β-cyclodextrin and γ-cyclodextrin. Compared with other carbon sources for preparing carbon materials (such as glucose), the preferred α-cyclodextrin, β-cyclodextrin, γ-cyclodextrin, etc. in this application contain a cavity structure and are ideal porous carbon source materials.

[0027] Preferably, the potassium salt is selected from one or more of potassium hydroxide, potassium chloride, potassium sulfate, potassium carbonate and potassium oxide.

[0028] Preferably, the inorganic solvent is water. The present application prefers water as the solvent, because on the one hand, it can remove potassium salt without affecting the product, and on the other hand, it is low in cost and is a green solvent.

[0029] Preferably, the mass ratio of the mixture C to the inorganic solvent is 1:5-15.

[0030] Preferably, the solvent used for washing the reaction product D is selected from one or more of deionized water, methanol, ethanol and isopropanol.

[0031] Preferably, the reaction product D is washed at least three times to ensure that impurities are completely removed.

[0032] Preferably, the reaction product D is dried after washing by vacuum drying at 40°C to 80°C for at least 24 hours; further, in some specific embodiments, the drying temperature is more preferably 60°C.

[0033] Preferably, the ammonium salt is one or more of ammonium chloride, ammonium sulfate, ammonium nitrate, ammonium fluoride and ammonium phosphate.

[0034] As another aspect of the present invention, the present invention also provides an application of a nitrogen-doped carbon-based oxygen reduction reaction catalyst in the preparation of a zinc-air battery. The efficiency of the oxygen reduction reaction affects the performance of the zinc-air battery.

[0035] The nitrogen-doped carbon-based oxygen reduction reaction catalyst provided by the present invention exhibits excellent oxygen reduction electrocatalytic performance, is expected to replace commercial Pt / C catalysts in the field of zinc-air batteries, and has good application prospects.

[0036] In addition, unless otherwise specified, any range described in the present invention includes the end value and any numerical value between the end values ​​and any sub-range formed by the end value or any numerical value between the end values.

[0037] The beneficial effects of the present invention are as follows:

[0038] (1) The nitrogen-doped carbon-based oxygen reduction catalyst provided by the present invention is a nitrogen-doped carbon material having a large number of concave structures on the surface, a large specific surface area, a hierarchical micropore and mesoporous structure, and the doping of nitrogen atoms increases the oxygen reduction active sites, so the electrocatalytic oxygen reduction performance is high.

[0039] (2) Compared with the existing preparation methods, the preparation method of the nitrogen-doped carbon-based oxygen reduction catalyst provided by the present invention is simple and convenient, and the raw materials are cheap, which effectively reduces the cost of the cathode oxygen reduction catalyst of the fuel cell and the metal-air battery; the ammonium salt used therein is used as both a nitrogen source and a pore-forming agent, which not only helps to incorporate the nitrogen element, but also increases the specific surface area of ​​the material; the potassium ions uniformly present in the cyclodextrin-based metal organic framework material used are pyrolyzed to generate relatively uniformly distributed potassium salts and potassium oxides as hard templates, and after washing and removing the hard template, the specific surface area of ​​the material can be further increased, thereby improving the electrocatalytic performance of the catalyst. In addition, the hard template removal process is a near-neutral condition, and there is no need to use strong acid or strong base solutions, which reduces the corrosion of the reaction equipment and is conducive to large-scale production.

[0040] (3) The nitrogen-doped carbon-based oxygen reduction catalyst provided by the present invention exhibits good electrocatalytic performance and high commercial value. In an oxygen-saturated 0.1 M KOH solution, the oxygen reduction reaction starting potential can reach 0.97 V (vs. RHE) and the current density can reach 5.87 mA cm -2, the half-wave potential can reach 0.835V, which is close to the performance of commercial 20% Pt / C catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0042] Figure 1 The low-magnification microscopic morphology of NC-1000 prepared in Example 1 under a scanning electron microscope is shown;

[0043] Figure 2 The high-magnification microscopic morphology of NC-1000 prepared in Example 1 in a transmission electron microscope is shown;

[0044] Figure 3 The low-magnification microscopic morphology of N-CD-1000 prepared in Comparative Example 1 under a scanning electron microscope is shown;

[0045] Figure 4 The low-magnification microscopic morphology of C-1000 prepared in Comparative Example 2 under a scanning electron microscope is shown;

[0046] Figure 5 The pore size distribution diagram of NC-1000 prepared in Example 1 is shown;

[0047] Figure 6 The nitrogen adsorption-desorption curves and specific surface areas of NC-1000, N-CD-1000 and C-1000 prepared in Example 1, Comparative Example 1 and Comparative Example 2 are shown;

[0048] Figure 7 The X-ray diffraction patterns of NC-1000, N-CD-1000 and C-1000 prepared in Example 1, Comparative Example 1 and Comparative Example 2 are shown;

[0049] Figure 8 The Raman curves of NC-1000, N-CD-1000 and C-1000 prepared in Example 1, Comparative Example 1 and Comparative Example 2 are shown;

[0050] Fig. 9 The linear sweep voltammetric curves obtained from Test Example 1, Comparative Test Example 1, Comparative Example Test 2 and Comparative Example Test 3 are shown respectively;

[0051] Fig.10 The linear sweep voltammetric curves obtained in test example 1, test example 2, test example 3 and test example 4 are shown respectively;

[0052] Fig.11 The 40000s chronoamperometry stability test curves obtained in test example 1 and comparative test example 3 are shown respectively;

[0053] Fig.12 The power density curves of the zinc-air batteries obtained in Test Example 5 and Comparative Test Example 4 are shown respectively. DETAILED DESCRIPTION

[0054] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0055] In the present invention, the preparation methods are conventional methods unless otherwise specified. The raw materials used are available from public commercial sources unless otherwise specified, and the percentages are by mass unless otherwise specified.

[0056] Example 1

[0057] This embodiment provides a method for preparing a nitrogen-doped carbon-based oxygen reduction catalyst, comprising the following steps:

[0058] (1) 1.30 g of γ-cyclodextrin and 0.45 g of potassium hydroxide were dissolved in 20 mL of deionized water and placed in a closed space filled with 50 mL of anhydrous methanol. After 7 days, the precipitated colorless crystals were collected, washed with anhydrous methanol for at least three times, and then vacuum dried at 60° C. for 24 h to obtain a cyclodextrin-based metal organic framework material;

[0059] (2) The cyclodextrin-based metal organic framework material and ammonium chloride were ground evenly in a mass ratio of 1:5, and the mixture was placed in an alumina porcelain boat and heated at 5 °C min under an argon atmosphere. -1 The temperature was raised to 350℃ at a rate of 5℃·min and then kept at this temperature for 0.5h. -1 The temperature was raised to 1000°C at a heating rate and then kept warm for 3 hours; the carbonized material was then collected, washed with deionized water for at least six times, and vacuum dried at 60°C for 24 hours to obtain a nitrogen-doped carbon-based oxygen reduction catalyst (NC-1000).

[0060] Figure 1 This is a scanning electron microscope image (SEM) of the nitrogen-doped carbon-based oxygen reduction reaction catalyst obtained in Example 1. The nitrogen-doped carbon-based oxygen reduction reaction catalyst has a large number of depressions. This morphology increases the specific surface area of ​​the material.

[0061] Figure 2 This is a transmission electron microscope (TEM) image of the nitrogen-doped carbon-based oxygen reduction reaction catalyst obtained in Example 1. The lattice fringe spacing of the nitrogen-doped carbon-based oxygen reduction reaction catalyst is about 0.353 nm.

[0062] Figure 5This is a pore size distribution diagram of the nitrogen-doped carbon-based oxygen reduction reaction catalyst obtained in Example 1. The nitrogen-doped carbon-based oxygen reduction reaction catalyst has a hierarchical microporous and mesoporous structure.

[0063] Figure 6 The nitrogen adsorption-desorption curve and specific surface area of ​​the nitrogen-doped carbon-based oxygen reduction reaction catalyst obtained in Example 1 are shown in Figure 1. The nitrogen-doped carbon-based oxygen reduction reaction catalyst has a higher adsorption amount at a relatively low pressure, indicating that the material has a microporous structure and a large specific surface area (555.5 cm 3 g -1 ).

[0064] Figure 7 The X-ray diffraction pattern of the nitrogen-doped carbon-based oxygen reduction reaction catalyst obtained in Example 1 is contained in the figure. The nitrogen-doped carbon-based oxygen reduction reaction catalyst exhibits broad and weak bulging peaks near 25.0° and 44.0°, corresponding to the (002) and (101) diffraction characteristic peaks of graphite carbon, respectively.

[0065] Figure 8 The Raman spectrum of the nitrogen-doped carbon-based oxygen reduction reaction catalyst obtained in Example 1 is shown in FIG. D / I G The value is about 0.99.

[0066] Example 2

[0067] This embodiment provides a method for preparing a nitrogen-doped carbon-based oxygen reduction catalyst, comprising the following steps:

[0068] (1) 1.30 g of γ-cyclodextrin and 0.45 g of potassium hydroxide were dissolved in 20 mL of deionized water and placed in a closed space filled with 50 mL of anhydrous methanol. After 7 days, the precipitated colorless crystals were collected, washed with anhydrous methanol for at least three times, and then vacuum dried at 60° C. for 24 h to obtain a cyclodextrin-based metal organic framework material;

[0069] (2) The cyclodextrin-based metal organic framework material and ammonium chloride were ground evenly in a mass ratio of 1:5, and the mixture was placed in an alumina porcelain boat and heated at 5 °C min under an argon atmosphere. -1 The temperature was raised to 350℃ at a rate of 5℃·min and then kept at this temperature for 0.5h. -1 The temperature was raised to 800°C at a heating rate and then kept warm for 3 hours; the carbonized material was then collected, washed with deionized water for at least six times, and vacuum dried at 60°C for 24 hours to obtain a nitrogen-doped carbon-based oxygen reduction catalyst (NC-800).

[0070] Example 3

[0071] This embodiment provides a method for preparing a nitrogen-doped carbon-based oxygen reduction catalyst, comprising the following steps:

[0072] (1) 1.30 g of γ-cyclodextrin and 0.45 g of potassium hydroxide were dissolved in 20 mL of deionized water and placed in a closed space filled with 50 mL of anhydrous methanol. After 7 days, the precipitated colorless crystals were collected, washed with anhydrous methanol for at least three times, and then vacuum dried at 60° C. for 24 h to obtain a cyclodextrin-based metal organic framework material;

[0073] (2) The cyclodextrin-based metal organic framework material and ammonium chloride were ground evenly in a mass ratio of 1:5, and the mixture was placed in an alumina porcelain boat and heated at 5 °C min under an argon atmosphere. -1 The temperature was raised to 350℃ at a rate of 5℃·min and then kept at this temperature for 0.5h. -1 The temperature was raised to 900°C at a heating rate and then kept at this temperature for 3 hours; the carbonized material was then collected, washed with deionized water for at least six times, and vacuum dried at 60°C for 24 hours to obtain a nitrogen-doped carbon-based oxygen reduction catalyst (NC-900).

[0074] Example 4

[0075] This embodiment provides a method for preparing a nitrogen-doped carbon-based oxygen reduction catalyst, comprising the following steps:

[0076] (1) 1.30 g of γ-cyclodextrin and 0.45 g of potassium hydroxide were dissolved in 20 mL of deionized water and placed in a closed space filled with 50 mL of anhydrous methanol. After 7 days, the precipitated colorless crystals were collected, washed with anhydrous methanol for at least three times, and then vacuum dried at 60° C. for 24 h to obtain a cyclodextrin-based metal organic framework material;

[0077] (2) The cyclodextrin-based metal organic framework material and ammonium chloride were ground evenly in a mass ratio of 1:5, and the mixture was placed in an alumina porcelain boat and heated at 5 °C min under an argon atmosphere. -1 The temperature was raised to 350℃ at a rate of 5℃·min and then kept at this temperature for 0.5h. -1 The temperature was raised to 1100°C at a heating rate and then kept at this temperature for 3 hours; the carbonized material was then collected, washed with deionized water for at least six times, and vacuum dried at 60°C for 24 hours to obtain a nitrogen-doped carbon-based oxygen reduction catalyst (NC-1100).

[0078] Comparative Example 1

[0079] This comparative example provides a method for preparing an oxygen reduction reaction catalyst, comprising the following steps:

[0080] γ-cyclodextrin and ammonium chloride were ground evenly in a mass ratio of 1:5, and the mixture was placed in an alumina porcelain boat and heated at 5 °C min under an argon atmosphere.-1 The temperature was raised to 350℃ at a rate of 5℃·min and then kept at this temperature for 0.5h. -1 The temperature was raised to 1000°C at a heating rate and kept at that temperature for 3 hours. After cooling, an oxygen reduction reaction catalyst (N-CD-1000) was obtained.

[0081] Compared with Example 1, Comparative Example 1 uses γ-cyclodextrin instead of cyclodextrin-based metal organic framework material, so the specific surface area of ​​the obtained product is smaller. Figure 3 As shown in Figure 2, N-CD-1000 exhibits the morphology of large carbon blocks and a relatively flat surface. Figure 6 As shown, the specific surface area of ​​N-CD-1000 is significantly smaller than that of NC-1000 obtained in Example 1.

[0082] Comparative Example 2

[0083] This comparative example provides a method for preparing an undoped oxygen reduction reaction catalyst, comprising the following steps:

[0084] (1) 1.30 g of γ-cyclodextrin and 0.45 g of potassium hydroxide were dissolved in 20 mL of deionized water and placed in a closed space filled with 50 mL of anhydrous methanol. After 7 days, the precipitated colorless crystals were collected, washed with anhydrous methanol for at least three times, and then vacuum dried at 60° C. for 24 h to obtain a cyclodextrin-based metal organic framework material;

[0085] (2) The cyclodextrin-based metal organic framework material was placed in an alumina porcelain boat and heated at 5°C min under an argon atmosphere. -1 The temperature was raised to 350℃ at a rate of 5℃·min and then kept at this temperature for 0.5h. -1 The temperature was raised to 1000°C at a heating rate and then kept at this temperature for 3 hours; the carbonized material was then collected, washed with deionized water for at least six times, and vacuum dried at 60°C for 24 hours to obtain an undoped oxygen reduction reaction catalyst (C-1000).

[0086] Compared with Example 1, Comparative Example 2 did not use ammonium salt, so the specific surface area of ​​the obtained product was smaller. Figure 4 As shown in Figure 2, C-1000 exhibits the morphology of irregular large carbon blocks; Figure 6 As shown, the specific surface area of ​​C-1000 is significantly smaller than that of NC-1000 obtained in Example 1.

[0087] Test Example 1

[0088] This test example provides an oxygen reduction electrochemical performance test method, using a three-electrode system to test the oxygen reduction performance, using the CHI760E electrochemical workstation and rotating disk electrode (RDE) device system of Shanghai Chenhua Instrument Co., Ltd. to test the application of catalyst materials in the electrocatalytic oxygen reduction reaction, including the following steps:

[0089] (1) 5 mg of the nitrogen-doped carbon-based oxygen reduction reaction catalyst prepared in Example 1 and 10 μL of Nafion solution were dispersed in a mixed solution of 495 μL of isopropanol and 495 μL of deionized water, followed by ultrasonic treatment for 30 min to form a uniform catalyst ink;

[0090] (2) 10 μL of catalyst ink was added to the RDE, and the catalyst loading was 0.25 mg / cm 2 After natural air drying, RDE was used as the working electrode, and the oxygen reduction electrochemical performance test was carried out in a three-electrode test system; in the three-electrode system, the catalyst-loaded RDE was used as the working electrode, the carbon rod was used as the counter electrode, and Ag / AgCl was used as the reference electrode;

[0091] (3) The working electrode prepared in step (2) was subjected to an oxygen reduction electrochemical performance test using a three-electrode system in a 0.1 M KOH electrolyte, and a linear voltammetric scan was performed at a scan rate of 10 mV / s. The resulting linear scan voltammetric curve was plotted as shown in FIG. Fig. 9 and Fig.10 shown.

[0092] (4) The stability of the working electrode prepared in step (2) is evaluated by chronoamperometry in a three-electrode system. In a saturated oxygen solution continuously supplied with oxygen, the working electrode is subjected to a long-term current test at a fixed potential (half-wave potential), and the current variation curve over time is recorded. The smaller the degree of current variation over time, the better the stability.

[0093] like Fig. 9 and Fig.10 As shown in Figure 1, in an oxygen-saturated 0.1 M KOH solution, the oxygen reduction reaction starting potential of the nitrogen-doped carbon-based oxygen reduction reaction catalyst prepared in Example 1 reached 0.97 V (vs. RHE) and the limiting current density reached 5.87 mA cm -2, the half-wave potential reaches 0.835V (vs.RHE), which is close to the performance of commercial 20% Pt / C catalyst. Compared with the catalyst prepared in Example 1, the catalysts prepared in Example 2, Example 3 and Example 4 have lower oxygen reduction reaction starting potential, half-wave potential and limiting current density, and the oxygen reduction catalytic performance is significantly inferior to that of the catalyst prepared in Example 1. The catalysts of Example 2, Example 3 and Example 4 are prepared at 800°C, 900°C and 1100°C, respectively. The temperature has a significant effect on the conductivity of the nitrogen-doped carbon-based oxygen reduction catalyst, the doping amount of the nitrogen element, etc.: the higher the temperature, the higher the degree of graphitization of the nitrogen-doped carbon-based oxygen reduction catalyst, the better the conductivity, and the more conducive to obtaining a highly active oxygen reduction catalyst. Therefore, the catalyst of Example 1 (prepared at 1000°C) performs better than the catalysts prepared in Example 2 (prepared at 800°C) and Example 3 (prepared at 900°C). However, as the catalyst temperature further increases, the nitrogen doping content in the catalyst prepared in Example 4 (prepared at 1100° C.) is significantly reduced, which is not conducive to further improving the oxygen reduction activity. Therefore, the performance of the catalyst prepared in Example 4 is also inferior to that of the catalyst prepared in Example 1.

[0094] Fig.11 The stability evaluation of the catalyst prepared in Example 1 by chronoamperometry is shown. After 40,000 seconds, the catalyst still retains 84% ​​of its catalytic performance, and its stability and durability are better than those of the commercial 20% Pt / C catalyst.

[0095] Test Example 2

[0096] The test method of this test example is the same as that of test example 1, except that in step (1), the nitrogen-doped carbon-based oxygen reduction catalyst NC-800 prepared in Example 2 is used instead of the nitrogen-doped carbon-based oxygen reduction catalyst NC-1000 prepared in Example 1.

[0097] Test Example 3

[0098] The test method of this test example is the same as that of test example 1, except that in step (1), the nitrogen-doped carbon-based oxygen reduction catalyst NC-900 prepared in Example 3 is used instead of the nitrogen-doped carbon-based oxygen reduction catalyst NC-1000 prepared in Example 1.

[0099] Test Example 4

[0100] The test method of this test example is the same as that of test example 1, except that in step (1), the nitrogen-doped carbon-based oxygen reduction catalyst NC-1100 prepared in Example 4 is used instead of the nitrogen-doped carbon-based oxygen reduction catalyst NC-1100 prepared in Example 1.

[0101] Test Example 5

[0102] This test example provides a test method for a zinc-air battery. The zinc-air battery is assembled with a zinc sheet as a negative electrode, carbon paper loaded with a catalyst as a positive electrode, 6 mol / L KOH as an electrolyte, and nickel foam as a current collector. The specific test includes the following steps:

[0103] (1) 5 mg of the nitrogen-doped carbon-based oxygen reduction reaction catalyst prepared in Example 1 and 10 μL of Nafion solution were dispersed in a mixed solution of 495 μL of isopropanol and 495 μL of deionized water, followed by ultrasonic treatment for 30 min to form a uniform catalyst slurry;

[0104] (2) Take 200 μL of catalyst and spread it evenly on a 1 cm 2 The catalyst loading on the carbon paper was 1 mg / cm 2 , after natural air drying, the carbon paper loaded with the catalyst was used as the positive electrode;

[0105] (3) Grinding the zinc sheet with sandpaper to remove the surface oxide layer, then performing ultrasonic treatment to remove surface impurities, and drying it to use as the negative electrode for later use;

[0106] (4) After the zinc-air battery is assembled, the power density curve of the zinc-air battery can be obtained by testing the polarization curve.

[0107] like Fig.12 As shown in Figure 1, the peak power density of the nitrogen-doped carbon-based oxygen reduction reaction catalyst prepared in Example 1 applied to zinc-air batteries reached 198.4 mW cm 2 , the battery performance is slightly better than commercial 20% Pt / C.

[0108] Comparative test example 1

[0109] The test method of this comparative test example is the same as that of Test Example 1, except that in step (1), the oxygen reduction reaction catalyst N-CD-1000 prepared in Comparative Example 1 is used instead of the nitrogen-doped carbon-based oxygen reduction catalyst NC-1000 prepared in Example 1.

[0110] Comparative test example 2

[0111] The test method of this comparative test example is the same as that of Test Example 1, except that in step (1), the undoped oxygen reduction reaction catalyst C-1000 prepared in Comparative Example 2 is used instead of the nitrogen-doped carbon-based oxygen reduction catalyst NC-1000 prepared in Example 1.

[0112] Comparative test example 3

[0113] The test method of this comparative test example is the same as that of Test Example 1, except that in step (1), a commercial 20% Pt / C catalyst is used instead of the nitrogen-doped carbon-based oxygen reduction catalyst NC-1000 prepared in Example 1.

[0114] Comparative test example 4

[0115] The test method of this comparative test example is the same as that of Test Example 5, except that commercial 20% Pt / C is used in step (1) instead of the nitrogen-doped carbon-based oxygen reduction catalyst prepared in Example 1.

[0116] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A nitrogen-doped carbon-based oxygen reduction reaction catalyst, characterized in that: The nitrogen-doped carbon-based oxygen reduction reaction catalyst is prepared by mixing a cyclodextrin-based metal organic framework material and an ammonium salt to obtain a mixture A, placing the mixture A in an inert gas or nitrogen atmosphere for a two-stage pyrolysis reaction to obtain a reaction product B, and washing and drying the reaction product B; in, The cyclodextrin-based metal organic framework material is prepared by mixing cyclodextrin and potassium salt to obtain a mixture C, dissolving the mixture C in an inorganic solvent and placing the mixture in a closed space containing anhydrous methanol to perform a coordination reaction to obtain a reaction product D, and washing and drying the reaction product D; In the two-stage pyrolysis reaction, the conditions for the first stage heating reaction are: 1-10°C·min -1 The heating rate is raised to 300-400℃ and kept at this temperature for 0.1-2h. The conditions for the second stage pyrolysis reaction are: 1-10℃·min -1 The heating rate is increased to 800-1100°C and kept warm for 1-4h.

2. The nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 1, characterized in that: The mass ratio of the cyclodextrin-based metal organic framework material to the ammonium salt is 1:1-10.

3. The nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 1, characterized in that: The ammonium salt is selected from one or more of ammonium chloride, ammonium sulfate, ammonium nitrate, ammonium fluoride and ammonium phosphate.

4. The nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 1, characterized in that: The solvent used for washing the reaction product B is selected from one or more of deionized water, methanol, ethanol and isopropanol.

5. The nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 1, characterized in that: The mass ratio of the cyclodextrin to the potassium salt is 1-2:0.1-1.

6. The nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 1, characterized in that: The mass ratio of the mixture C to the inorganic solvent is 1:5-15.

7. The nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 1, characterized in that: The potassium salt is selected from one or more of potassium hydroxide, potassium chloride, potassium sulfate, potassium carbonate and potassium oxide.

8. The nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 1, characterized in that: The cyclodextrin is selected from one or more of α-cyclodextrin, β-cyclodextrin and γ-cyclodextrin.

9. A method for preparing a nitrogen-doped carbon-based oxygen reduction reaction catalyst as claimed in claim 1, characterized in that: The method comprises the following steps: mixing a cyclodextrin-based metal organic framework material and an ammonium salt to obtain a mixture A, placing the mixture A in an inert gas or nitrogen atmosphere for a two-stage pyrolysis reaction to obtain a reaction product B, and washing and drying the reaction product B to obtain the nitrogen-doped carbon-based oxygen reduction reaction catalyst; in, The cyclodextrin-based metal organic framework material is prepared by mixing cyclodextrin and potassium salt to obtain a mixture C, dissolving the mixture C in an inorganic solvent and placing the mixture in a closed space containing anhydrous methanol to perform a coordination reaction to obtain a reaction product D, and washing and drying the reaction product D; In the two-stage pyrolysis reaction, the conditions for the first stage heating reaction are: 1-10°C·min -1 The heating rate is raised to 300-400℃ and kept at this temperature for 0.1-2h. The conditions for the second stage pyrolysis reaction are: 1-10℃·min -1 The heating rate is increased to 800-1100°C and kept warm for 1-4h.

10. The method for preparing a nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 9, characterized in that: The mass ratio of the cyclodextrin-based metal organic framework material to the ammonium salt is 1:1-10.

11. The method for preparing a nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 9, characterized in that: The ammonium salt is selected from one or more of ammonium chloride, ammonium sulfate, ammonium nitrate, ammonium fluoride and ammonium phosphate.

12. The method for preparing a nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 9, characterized in that: The solvent used for washing the reaction product B is selected from one or more of deionized water, methanol, ethanol and isopropanol.

13. The method for preparing a nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 9, characterized in that: The mass ratio of the cyclodextrin to the potassium salt is 1-2:0.1-1.

14. The method for preparing a nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 9, characterized in that: The mass ratio of the mixture C to the inorganic solvent is 1:5-15.

15. The method for preparing a nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 9, characterized in that: The potassium salt is selected from one or more of potassium hydroxide, potassium chloride, potassium sulfate, potassium carbonate and potassium oxide.

16. The method for preparing a nitrogen-doped carbon-based oxygen reduction reaction catalyst according to claim 9, characterized in that: The cyclodextrin is selected from one or more of α-cyclodextrin, β-cyclodextrin and γ-cyclodextrin.

17. Use of the nitrogen-doped carbon-based oxygen reduction reaction catalyst as claimed in claim 1 in the preparation of a zinc-air battery.

Citation Information

Patent Citations

  • ZIF-67 template method for preparing cobalt-platinum core-shell particle / porous carbon composite material and catalytic application of composite material in cathode of fuel cell

    CN106328960A

  • Superfine M-N-C non-noble metal carbon-based oxygen reduction catalyst, and preparation method and application thereof

    CN111987326A