Polarizer and organic electroluminescent display device

By setting a specific sequence of pigment compound layer and ultraviolet absorber layer in the polarizer, the problem of phase retardation film and polarizer degradation caused by heat generation of ultraviolet absorber layer is solved, and long-term quality protection of organic electroluminescent display device is achieved.

CN115151848BActive Publication Date: 2024-11-15KONICA MINOLTA INC
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202180016241.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-02-28
Filing Date
2021-02-02
Publication Date
2024-11-15
Estimated Expiration
2041-02-02

AI Technical Summary

Technical Problem

In the prior art, in organic electroluminescent display devices, the heating of the ultraviolet absorber layer caused by the polarizer leads to the deterioration of the phase retardation film and the polarizer, affecting the long-term performance of the display device.

Method used

In a polarizer, a layer containing an ultraviolet absorber and a layer containing a pigment compound are provided. The pigment compound layer is located on the visible side, which absorbs short-wavelength light and protects the display element, prevents heat accumulation, and suppresses the deterioration of the phase retardation film and the polarizer.

Benefits of technology

It effectively protects display elements from external light, suppresses the degradation of phase retardation film and polarizer, and improves the long-term performance of organic electroluminescent display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115151848B_ABST
    Figure CN115151848B_ABST
Patent Text Reader

Abstract

A polarizing plate, which has a hard coating layer, a protective film, a polarizer and a phase difference film in order from the visible side, at least one of the hard coating layer and the protective film contains a pigment compound whose maximum absorption wavelength exists in the range of more than 380nm and less than 430nm in the absorption spectrum in the wavelength region of 300 to 460nm, at least one of the protective film and the phase difference film contains an ultraviolet absorber, and the layer containing the pigment compound is located on the visible side compared with the layer containing the ultraviolet absorber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polarizing plate and an organic electroluminescent display device. More specifically, the present invention relates to a polarizing plate that can protect a display element from external light when used in a display device, especially an organic electroluminescent display device, and can suppress degradation of a retardation film and a polarizer due to heat, and an organic electroluminescent display device having the polarizing plate and suppressing degradation of quality during long-term use. Background Art

[0002] In recent years, display devices such as smartphones are often used under strong external light. In order to improve visibility under external light, the use of organic electroluminescence (EL) elements in light sources has increased, and with this, the problem of organic EL elements being degraded by external light has arisen. Therefore, in organic EL display devices, the following technology is known: a component such as a polarizer disposed on the visible side of the organic EL element contains an ultraviolet absorber and a pigment compound that absorbs light on the longer wavelength side than the ultraviolet absorber, thereby suppressing the degradation of the organic EL element caused by external light.

[0003] For example, Patent Document 1 describes an organic EL display device having an organic EL element and an optical laminate having a polarizer, a phase difference film, and at least one other layer, such as a pressure-sensitive adhesive layer, laminated on its visible side. Patent Document 1 describes the following technology: by providing a layer containing the above-mentioned pigment compound and a layer containing an ultraviolet absorber in the optical laminate, the layer containing the pigment compound is located closer to the organic EL element than the layer containing the ultraviolet absorber, thereby suppressing the degradation of the organic EL element. Patent Document 1 describes that by arranging the layers in such a specific order, the above-mentioned pigment compound can be prevented from being degraded by exposure to ultraviolet rays.

[0004] However, in the configuration of patent document 1, the layer containing ultraviolet absorber absorbs ultraviolet rays and generates heat, and then the pigment compound absorbs light and generates heat in its inner side. Here, it is clear that the layer containing ultraviolet absorber absorbs short-wavelength light and generates more heat than the pigment compound, thus hindering the heat dissipation from the heat generated by the pigment compound to the outside of the display device. In the configuration of patent document 1, in order to become the above-mentioned specific order, the pigment compound is included in the phase difference film or the pressure-sensitive adhesive layer present in the organic EL element side. Therefore, it is believed that: due to the heat generated from the pigment compound, the temperature rise of the phase difference film is caused, and the optical values ​​such as phase difference change due to the size change of the phase difference film, resulting in light leakage of reflected light. In addition, it is believed that: due to the heat generated from the pigment compound, the polarizer shrinks, resulting in poor contrast of the display device.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2017-168430 Summary of the invention

[0008] Problems to be solved by the invention

[0009] The present invention is made in view of the above problems and situations, and the problem to be solved is to provide a polarizing plate which can protect a display element from external light when used in a display device, especially an organic EL display device, and can suppress the degradation of a retardation film and a polarizer caused by heat. In addition, an organic EL display device having the polarizing plate and the quality degradation suppressed during long-term use is provided.

[0010] Means for solving problems

[0011] In order to solve the above-mentioned problems, the inventors have studied the causes of the above-mentioned problems and found that by providing a layer containing an ultraviolet absorber (layer containing an ultraviolet absorber) and a layer containing a pigment compound that absorbs light in a specified wavelength region on the longer wavelength side than the ultraviolet absorber (layer containing a pigment compound) in the layers constituting the polarizer, and forming a structure in which the layer containing the above-mentioned pigment compound is arranged on the visible side compared with the layer containing the above-mentioned ultraviolet absorber, it is possible to protect the display element from the influence of external light, and at the same time obtain a polarizer capable of suppressing the degradation of the phase difference film and the polarizer caused by heat, thereby completing the present invention.

[0012] That is, the above-mentioned problems according to the present invention are solved by the following means.

[0013] 1. A polarizing plate comprising, in order from a visible side, a hard coating layer, a protective film, a polarizer and a phase difference film, wherein at least one of the hard coating layer and the protective film contains a pigment compound having a maximum absorption wavelength in a range of more than 380 nm and less than 430 nm in an absorption spectrum in a wavelength region of 300 to 460 nm, at least one of the protective film and the phase difference film contains an ultraviolet absorber, and a layer containing the pigment compound is located on a visible side compared to a layer containing the ultraviolet absorber.

[0014] 2. The polarizing plate according to item 1, wherein the pigment compound is contained in the hard coat layer, and the ultraviolet absorber is contained in the protective film.

[0015] 3. The polarizing plate according to item 1 or 2, wherein the pigment compound contains a compound having a structure represented by the following general formula (1).

[0016] [Chemistry 1]

[0017] General formula (1)

[0018]

[0019] (In the general formula (1), Z represents a heteroaryl group which may have a substituent and contains at least one nitrogen atom as a heteroatom.)

[0020] 4. The polarizing plate according to any one of items 1 to 3, wherein a pressure-sensitive adhesive layer is provided on the side opposite to the visible side of the retardation film.

[0021] 5. An organic electroluminescent display device comprising the polarizing plate according to any one of items 1 to 4 on a visible side.

[0022] Effects of the Invention

[0023] By means of the present invention, a polarizing plate can be provided, which can protect the display element from the influence of external light when used in a display device, especially an organic EL display device, and can suppress the degradation of the phase difference film and the polarizer caused by heat. In addition, by using the polarizing plate, an organic EL display device in which the quality degradation during long-term use is suppressed can be provided.

[0024] Although the manifestation mechanism and action mechanism of the effect of the present invention are not clearly understood, they are presumed as follows.

[0025] The polarizing plate of the present invention comprises, in order from the visible side, a hard coating layer, a protective film, a polarizer and a phase difference film, and is characterized in that at least one of the hard coating layer and the protective film contains a pigment compound (hereinafter also referred to as "pigment compound (D)") having a maximum absorption wavelength in the range of more than 380 nm and less than 430 nm in the absorption spectrum in the wavelength region of 300 to 460 nm, at least one of the protective film and the phase difference film contains an ultraviolet absorber, and the layer containing the pigment compound is located on the visible side compared with the layer containing the ultraviolet absorber.

[0026] The polarizing plate of the present invention is configured such that, when used in a display device, particularly an organic EL display device, a layer containing a pigment compound (D) is arranged closer to the visible side than a layer containing an ultraviolet absorber. The ultraviolet absorber is a compound having a maximum absorption wavelength within the range of 300 to 380 nm in an absorption spectrum within a wavelength range of 300 to 460 nm.

[0027] The polarizing plate of the present invention is used in combination with a layer containing a pigment compound and a layer containing an ultraviolet absorber, so that, for example, light with a wavelength shorter than the light-emitting region of an organic EL element (wavelength longer than 430 nm) can be fully absorbed, thereby protecting display elements such as organic EL elements from the influence of external light.

[0028] The polarizer of the present invention further configures the layer containing the pigment compound and the layer containing the ultraviolet absorber in the above-mentioned specific order, so that the heat generated from the pigment compound (D) will not be hindered by the heating of the layer containing the ultraviolet absorber, and can be released from the surface of the display device to the outside. According to the relationship between wavelength and energy, the ultraviolet absorber is larger than the pigment compound in terms of the heat generated by the absorption of light, and the temperature of the layer containing the ultraviolet absorber is higher than that of the layer containing the pigment compound. As in the polarizer of the present invention, in the structure where the low-temperature layer (the layer containing the pigment compound) is located outside the high-temperature layer (the layer containing the ultraviolet absorber), heat dissipation will not be hindered, and heat is dissipated to the outside in the order from the high-temperature layer to the low-temperature layer. Thus, it is inferred that the degradation of the optical value of the phase difference film caused by the heating of the pigment compound (D) and the degradation of the shrinkage of the polarizer can be suppressed.

[0029] In addition, in an organic EL display device having a polarizer of the present invention, it is presumed that the temperature difference between the polarizer that shows a small temperature rise due to light emission from the inside of the organic EL element and the temperature near the visible side surface of the polarizer that shows a small temperature rise due to heat generation of the pigment compound (D) can be suppressed to be small, and the thermal stress of the entire display device is relaxed, and deformation of the components can be suppressed. The polarizer suppresses deformation caused by heat in this way, and the pigment compound (D) and ultraviolet absorber contained in the polarizer have the function of protecting the organic EL element from the influence of external light, so that the degradation of the quality of the organic EL display device having the polarizer during long-term use is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a cross-sectional view showing a configuration example of the polarizing plate of the present invention.

[0031] Figure 2 It is a cross-sectional view showing another structural example of the polarizing plate of the present invention.

[0032] Figure 3 It is a cross-sectional view showing a configuration example of the organic EL display device of the present invention.

[0033] Figure 4 It is a plan view schematically showing the general structure of a production apparatus for an obliquely stretched film.

[0034] Figure 5 It is schematically indicated Figure 41 is a plan view of an example of a track pattern of a stretching section included in the manufacturing apparatus for a diagonally stretched film shown. DETAILED DESCRIPTION

[0035] The polarizing plate of the present invention is a polarizing plate having a hard coating layer, a protective film, a polarizer and a phase difference film in order from the visible side, characterized in that at least one of the hard coating layer and the protective film contains a pigment compound (pigment compound (D)) whose maximum absorption wavelength exists in the range of more than 380nm and less than 430nm in the absorption spectrum in the wavelength region of 300 to 460nm, and at least one of the protective film and the phase difference film contains an ultraviolet absorber, and the layer containing the pigment compound is located on the visible side compared with the layer containing the ultraviolet absorber. This feature is a technical feature common to the following embodiments.

[0036] As an embodiment of the present invention, from the viewpoint of suppressing deterioration of the retardation film and the polarizing plate due to heat generation, it is preferred that the dye compound (D) is contained in the hard coat layer and the ultraviolet absorber is contained in the protective film.

[0037] As an embodiment of the present invention, from the viewpoint of suppressing deterioration of the retardation film and the polarizer due to heat generation, it is preferred that the dye compound (D) contains a compound having a structure represented by the above formula (1).

[0038] The polarizing plate of the present invention may also be provided with a pressure-sensitive adhesive layer on the side opposite to the visible side of the retardation film. This improves workability when manufacturing an organic EL display device in which the polarizing plate is arranged on the visible side of an organic EL element.

[0039] The organic EL display device of the present invention is characterized by comprising the polarizing plate of the present invention on the visible side. Thus, the organic EL display device is an organic EL display device in which quality degradation during long-term use is suppressed.

[0040] Hereinafter, the present invention and its constituent elements, as well as the forms and methods for implementing the present invention are described in detail. It should be noted that in the present application, "~" is used to include the numerical values ​​recorded before and after it as the lower limit and upper limit. In this specification, the compound with the structure shown in the general formula (1) is referred to as compound (1). Similarly, the group with the structure shown in the formula (Z1) is referred to as group (Z1). It is the same in other compounds and groups.

[0041] In this specification, "ultraviolet absorber" refers to a compound whose maximum absorption wavelength exists in the range of 300 to 380 nm in the absorption spectrum of the wavelength region of 300 to 460 nm. In addition, the "maximum absorption wavelength" in the absorption spectrum of a specific wavelength region refers to the absorption maximum wavelength showing the maximum absorbance when there are multiple absorption maxima in the spectral absorption spectrum of the specific wavelength region. Furthermore, the absorption spectrum of various compounds is the absorption spectrum measured by dissolving the compound in dichloromethane and using a spectrophotometer.

[0042] [Overview of the polarizing plate of the present invention]

[0043] The polarizing plate of the present invention is a polarizing plate having a hard coating layer, a protective film, a polarizer and a phase difference film in order from the visible side, characterized in that at least one of the hard coating layer and the protective film contains a pigment compound (D), at least one of the protective film and the phase difference film contains an ultraviolet absorber, and the layer containing the pigment compound (D) is located on the visible side compared to the layer containing the ultraviolet absorber.

[0044] The polarizer of the present invention can also be a mode in which a pressure-sensitive adhesive layer is provided on the side opposite to the visible side of the above-mentioned phase difference film. The polarizer of the present invention can also arbitrarily have other layers as required within the range that does not damage the effect of the present invention. As other layers, a primer layer arranged on one or both sides of the protective film according to the material of the protective film, an adhesive layer arranged between the protective film and the polarizer and between the phase difference film and the polarizer, etc. can be cited.

[0045] Hereinafter, constituent elements of the present invention will be described in detail with reference to the accompanying drawings. Figure 1 This is a cross-sectional view showing a configuration example of a polarizing plate 10A of the present invention including a hard coat layer 1, a protective film 2, a polarizer 3, and a retardation film 4 in this order from the visible side. Figure 2 This is a cross-sectional view showing a configuration example of a polarizing plate 10B of the present invention having a hard coat layer 1, a protective film 2, a polarizer 3, a retardation film 4, and a pressure-sensitive adhesive layer 5 in this order from the visible side.

[0046] The polarizing plate of the present invention is described as an example using the polarizing plate 10B. Figure 3 As in the organic EL display device 20 shown in the cross-sectional view in FIG, the pressure-sensitive adhesive layer 5 is disposed on the visible side surface of the organic EL element 11 for use.

[0047] The polarizing plate of the present invention will be described below mainly by taking the polarizing plate 10A as an example, but the present invention is not limited thereto. In the present invention, the polarizing plate 10A is configured to satisfy the following conditions (1) to (3).

[0048] (1) At least one of the hard coat layer 1 and the protective film 2 contains the dye compound (D).

[0049] (2) At least one of the protective film 2 and the retardation film 4 contains an ultraviolet absorber.

[0050] (3) The layer containing the dye compound (D) of (1) above is located on the visible side relative to the layer containing the ultraviolet absorber of (2) above.

[0051] If the polarizing plate 10A satisfying all of the above (1) to (3) is shown in Table I, it is possible to exemplify Configurations 1 to 5. In Table I, "(D)" indicates that the layer or film on the left column of Table I contains the pigment compound (D), and "UVA" indicates that the layer or film on the left column of Table I contains an ultraviolet absorber.

[0052] [Table 1]

[0053] Table I

[0054]

[0055] In the polarizing plate 10A, from the viewpoint of ease of adjustment of optical characteristics and ease of manufacture, it is preferred that the layers containing the pigment compound (D) and the ultraviolet absorber are each one layer, that is, configuration 1, configuration 2, and configuration 3. In addition, from the viewpoint of ease of heat dissipation to the outside and protection of the substrate and polarizer 3 on which the polarizing plate 10A is provided, it is preferred that the pigment compound (D) is contained in the hard coat layer 1 and the ultraviolet absorber is contained in the protective film 2, that is, configuration 1 and configuration 4, and configuration 1 is particularly preferred.

[0056] (Pigment compound (D))

[0057] The pigment compound (D) used in the present invention is not particularly limited as long as the maximum absorption wavelength in the absorption spectrum in the wavelength region of 300 to 460 nm is present in the compound exceeding 380 nm and below 430 nm. Below, as long as there is no special explanation, the maximum absorption wavelength of various compounds refers to the maximum absorption wavelength in the absorption spectrum in the wavelength region of 300 to 460 nm.

[0058] The maximum absorption wavelength of the pigment compound (D) is more preferably present in the wavelength region of 390 to 420 nm. The pigment compound (D) can protect the display element, especially the organic EL element, from the influence of external light and inhibit degradation by having the above-mentioned light absorption characteristics. The pigment compound (D) is not particularly limited as long as it has the above-mentioned light absorption characteristics, but preferably does not have fluorescence and phosphorescence performance (photoluminescence) that hinder the display of the organic EL element.

[0059] Pigment compound (D) is as long as having above-mentioned light absorption characteristic, and its structure etc. are not particularly limited.As pigment compound (D), for example, can enumerate organic pigment compound, inorganic pigment compound.Pigment compound (D) is included in hard coat and / or protective film, from the viewpoint of maintaining the dispersibility and transparency in the resin components such as the base polymer as the film-forming component of these layers or film, preferably organic pigment compound.

[0060] Examples of the organic pigment compound include azomethine compounds, indole compounds, cinnamic acid compounds, pyrimidine compounds, porphyrin compounds, and dicyanomethine compounds.

[0061] As the above-mentioned organic pigment compound, commercially available products can be preferably used. Specifically, as indole compounds, BONASORB UA3911 (trade name, maximum absorption wavelength: 398nm, manufactured by Orient Chemical Industry Co., Ltd.) and BONASORB UA3912 (trade name, maximum absorption wavelength: 386nm, manufactured by Orient Chemical Industry Co., Ltd.) can be listed. As cinnamic acid compounds, SOM-5-0106 (trade name, maximum absorption wavelength: 416nm, manufactured by Orient Chemical Industry Co., Ltd.) can be listed. As porphyrin compounds, FDB-001 (trade name, maximum absorption wavelength: 420nm, manufactured by Yamada Chemical Industry Co., Ltd.) and FDB-009 (trade name, maximum absorption wavelength: 402nm, manufactured by Yamada Chemical Industry Co., Ltd.) can be listed.

[0062] Since the pigment compound (D) is contained in the layer on the visible side compared with the layer containing the ultraviolet absorber, it is preferably weather-resistant to light of a wavelength below 380 nm. As such a pigment compound (D), for example, a compound (1) having a structure shown in the following general formula (1) can be cited. Compound (1) is a compound belonging to a dicyanomethene-based compound.

[0063] [Chemistry 2]

[0064] General formula (1)

[0065]

[0066] (In the general formula (1), Z represents a heteroaryl group which may have a substituent and contains at least one nitrogen atom as a heteroatom.)

[0067] In the general formula (1), the heteroaryl group represented by Z is a group generated by removing one hydrogen atom from any ring atom of the heteroaryl ring possessed by the heteroaromatic hydrocarbon compound. The number of members of the heteroaryl ring possessed by Z is 5 to 30, preferably 5 to 9. The heteroaryl ring may be a monocyclic ring or a condensed ring (polycyclic ring). The number of rings possessed by the heteroaryl ring is preferably 1 or 2. Each ring constituting the monocyclic ring and the condensed ring is preferably a 5-membered ring or a 6-membered ring.

[0068] As the hetero atom that Z has in the heteroaromatic ring, at least one nitrogen atom is contained. The heteroaromatic ring may contain nitrogen atoms in the range of, for example, 1 to 10. The number of nitrogen atoms contained in the heteroaromatic ring is preferably 1 or 2. In addition, the heteroaromatic ring may have hetero atoms other than nitrogen atoms in addition to nitrogen atoms. Examples of hetero atoms other than nitrogen atoms include sulfur atoms and oxygen atoms, preferably sulfur atoms. The number of hetero atoms other than nitrogen atoms is preferably 1 or 2, more preferably 1. When the heteroaromatic ring is a condensed ring, any ring may have hetero atoms.

[0069] The heteroaryl group in Z may have a substituent. The heteroaryl group having a substituent means that a hydrogen atom bonded to a ring atom of the heteroaryl ring is substituted with a substituent. Examples of such a substituent include an alkyl group, an alkoxy group, an alkynyl group, an amino group, an alkyl-substituted amino group, and an aryloxy group.

[0070] The number of carbon atoms in the alkyl group in the above-mentioned alkyl group, alkoxy group, alkynyl group, and alkyl-substituted amino group is preferably 1 to 20, and more preferably 1 to 10. The alkyl group in the above-mentioned alkyl group, alkoxy group, or alkyl-substituted amino group may be in the form of a straight chain, a branched chain, a cyclic shape, or a combination thereof. The number of carbon atoms in the aryloxy group may be 5 to 30. The aryl group in the aryloxy group may have a heteroatom. In addition, the aromatic ring in the aryl group may be a monocyclic ring or a condensed ring. Examples of the aryloxy group include phenoxy, naphthoxy, 2-methylphenoxy, and the like.

[0071] Specific examples of Z in the general formula (1) include groups (Z1) to (Z3) having structures represented by the following formulas (Z1) to (Z3), respectively. 1 , R 2 , R 11 ~R 16 , and R 21 ~R 23 Each represents a hydrogen atom, an alkyl group or an alkynyl group having 1 to 20 carbon atoms, an amino group, an alkyl-substituted amino group (wherein the alkyl group has 1 to 20 carbon atoms), or an aryloxy group. Examples of the aryloxy group include the same groups as described above. * in formula (Z1) to formula (Z3) represents a linking site.

[0072] [Chemistry 3]

[0073]

[0074] From the viewpoint of weather resistance, Z is preferably a group (Z1) or a group (Z2). When Z is a group (Z1), R 1 , preferably a hydrogen atom and an amino group, more preferably a hydrogen atom. 2 , preferably a hydrogen atom, an alkyl-substituted amino group and an alkoxy group. As the alkyl-substituted amino group, preferably a dimethylamino group.

[0075] When Z is a group (Z2), as R 11 ~R 16 , preferably a hydrogen atom and an alkyl group having 1 to 10 carbon atoms. Examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, and the like. As group (Z2), preferably R 11 Methyl, R 12 isobutyl, R 13 ~R 16 A group of hydrogen atoms.

[0076] The abbreviations of compound (1) based on the type of Z are shown in Table II. In Table II, "Me" represents a methyl group and "i-Bu" represents an isobutyl group. In Table II, the compound abbreviation (1)-1 is referred to as compound (1)-1. The same applies to other compounds. For example, compound (1)-1 is described as follows: Z in formula (1) is a group (Z1), R 1 is a hydrogen atom, R 2 The maximum absorption wavelength and weather resistance of each compound (1) are shown. The weather resistance is evaluated by the following method.

[0077] (Weather resistance evaluation method)

[0078] A hard coating layer containing compound (1) was formed on a substrate film, such as a cycloolefin film, and evaluated. The hard coating layer was a layer formed by photocuring a resin composition containing a urethane acrylate of compound (1), such as U-4H (product name, manufactured by Shin-Nakamura Chemical Industry Co., Ltd.), wherein the content of compound (1) was 5% by mass and the thickness was 5 μm.

[0079] The hard coating layer of the substrate film with a hard coating layer prepared above was continuously irradiated with a xenon lamp (60 W / m 2 ) light, and the absorbance of the substrate film with the hard coating layer before irradiation (0 hours) and after irradiation was measured with a spectrophotometer, and the pigment residual rate was measured according to the following formula (3). It should be noted that the substrate film used has no difference in absorbance at the maximum absorption wavelength of the compound (1) before and after irradiation with light.

[0080] Pigment residual rate (%) = {(A1) / (A0)}×100 Formula (3)

[0081] [Where A0 is the absorbance before xenon lamp irradiation, and A1 is the absorbance after xenon lamp irradiation.]

[0082] In addition, "absorbance" indicates the absorbance at the maximum absorption wavelength of each compound (1), and the higher the residual pigment ratio, the more difficult the compound (1) is to be decomposed by light, indicating higher weather resistance. Weather resistance was evaluated according to the following criteria.

[0083] A: Pigment residual rate is more than 65%

[0084] B: Pigment residual rate is 40% or more and less than 65%

[0085] C: Pigment residual rate is 10% or more and less than 40%

[0086] D: Pigment residual rate is less than 10%

[0087] [Table 2]

[0088] Table II

[0089]

[0090] Compound (1) can be produced by a conventionally known method. The following is a method for producing Compound (1)-1 and Compound (1)-2.

[0091] (Compound (1)-1)

[0092] Compound (1)-1 can be prepared from a raw material compound (A1) whose structure is represented by (A1) in the following formula. Specifically, a weighed raw material compound (A1) and malononitrile are introduced into a 3-necked flask, and toluene is added as a solvent to dissolve. Then, morpholine is added dropwise, the temperature is raised, and the mixture is heated to reflux. After the reaction is completed, the solvent is removed under reduced pressure, methanol is added, and the mixture is stirred in a suspended state, and the reaction product is precipitated by recrystallization. The obtained precipitate is filtered and dried to obtain a powder of compound (1)-1. The structure can be confirmed by NMR.

[0093] [Chemistry 4]

[0094]

[0095] (Compound (1)-2)

[0096] Compound (1)-2 can be manufactured from a raw material compound (A2) whose structure is shown by (A2) in the following formula. Specifically, a weighed raw material compound (A2) and malononitrile are introduced into a 3-necked flask, and toluene is added as a solvent to dissolve. Then, morpholine is added dropwise, the temperature is raised, and the mixture is heated to reflux. After the reaction is completed, the solvent is removed under reduced pressure, methanol is added, and the mixture is stirred in a suspended state, and the reaction product is precipitated by recrystallization. The obtained precipitate is filtered and dried to obtain a powder of compound (1)-2. The structure can be confirmed by NMR.

[0097] [Chemistry 5]

[0098]

[0099] The pigment compound (D) may be used alone or in combination of two or more thereof. The content of the pigment compound (D) in the layer containing the pigment compound (D) is expressed as the mass parts of the pigment compound (D) relative to 100 mass parts of the film-forming component, ie, the resin component, in each layer.

[0100] For example, in the case of the above-mentioned configurations 1, 2 and 4 in which the pigment compound (D) is contained only in the hard coat layer, the content of the pigment compound (D) relative to 100 parts by mass of the constituent resin of the hard coat layer is preferably in the range of 0.01 to 50 parts by mass, and more preferably in the range of 0.02 to 30 parts by mass.

[0101] In addition, in the case of the composition 3 in which the pigment compound (D) is contained only in the protective film, the content of the pigment compound (D) relative to 100 parts by mass of the constituent resin of the protective film is preferably in the range of 0.01 to 10 parts by mass, and more preferably in the range of 0.02 to 8 parts by mass. In the case of the above-mentioned composition 5 in which both the hard coat layer and the protective film contain the pigment compound (D), the total content of the pigment compound (D) in each layer is preferably in the range of 0.01 to 10 parts by mass, and more preferably in the range of 0.02 to 8 parts by mass, relative to 100 parts by mass of the total amount of the constituent resin in each layer.

[0102] By setting the content of the dye compound (D) to the above range, when the polarizing plate of the present invention is used in an organic EL display device, light in a region that does not affect the emission of the organic EL element can be sufficiently absorbed, and degradation of the organic EL element can be suppressed, which is preferred.

[0103] (Ultraviolet light absorber)

[0104] The ultraviolet absorber is not particularly limited as long as it is an ultraviolet absorber having a maximum absorption wavelength in the wavelength range of 300 to 380 nm.

[0105] Examples of the ultraviolet absorber include triazine ultraviolet absorbers, benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, hydroxybenzophenone ultraviolet absorbers, salicylate ultraviolet absorbers, and cyanoacrylate ultraviolet absorbers. These may be used alone or in combination of two or more.

[0106] Among them, triazine-based ultraviolet absorbers and benzotriazole-based ultraviolet absorbers are preferred, and at least one ultraviolet absorber selected from triazine-based ultraviolet absorbers having two or less hydroxyl groups in one molecule and benzotriazole-based ultraviolet absorbers having one benzotriazole skeleton in one molecule is preferred. These ultraviolet absorbers are preferably preferred because they have good solubility in resin components such as base polymers that are film-forming components of protective films and / or phase difference films containing the ultraviolet absorbers. Furthermore, these ultraviolet absorbers have high ultraviolet absorption capacity near a wavelength of 380nm, so they are preferred.

[0107] Specific examples of triazine-based ultraviolet absorbers having two or less hydroxyl groups in one molecule include 2,4-bis-[{4-(4-ethylhexyloxy)-4-hydroxy}-phenyl]-6-(4-methoxyphenyl)-1,3,5-triazine (Tinosorb S, manufactured by BASF), 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine (Tinubin 460, manufactured by BASF), reaction product of 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-hydroxyphenyl and [(C10-C16 (mainly C12-C13) alkoxy)methyl]ethylene oxide (Tinubin 400, manufactured by BASF), 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol) , reaction product of 2-(2,4-dihydroxyphenyl)-4,6-bis-(2,4-dimethylphenyl)-1,3,5-triazine and (2-ethylhexyl)-glycidate (Tinubin 405, manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol (Tinubin 1577, manufactured by BASF), 2-(2-hydroxyphenyl)-benzotriazole (Tinubin 970, manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]-phenol (ADKSTAB LA46, manufactured by ADEKA Co., Ltd.), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (Thunubin 479, manufactured by BASF), 6,6',6"-(1,3,5-triazine-2,4,6-triyl)tris(3-hexyloxy-2-methylphenol) (LA-F70, manufactured by ADEKA Co., Ltd.), etc.

[0108] In addition, examples of benzotriazole-based ultraviolet absorbers having one benzotriazole skeleton in one molecule include 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (Tinubin 928, manufactured by BASF), 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole (Tinubin PS, manufactured by BASF), phenylpropionic acid, and an ester compound of 3-(2H-benzotriazole-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy (C7-9 side chain and linear alkyl) (Tinubin 928, manufactured by BASF). 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate / polyethylene glycol 300 reaction product (Tinubin 1130, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-p-cresol (Tinubin P, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (Tinubin 900, manufactured by BASF), methyl-3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate / polyethylene glycol 300 reaction product (Tinubin 1130, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-p-cresol (Tinubin P, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol Phenol (Tinubin 234, manufactured by BASF), 2-[5-chloro(2H)-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol (Tinubin 326, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6-di-tert-amylphenol (Tinubin 328, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (Tinubin 329, manufactured by BASF), methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate and poly(vinyl alcohol) Reaction product of ethylene glycol 300 (Thunbine 213, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol (Thunbine 571, manufactured by BASF), 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole (Sumisorb 250, manufactured by Sumitomo Chemical Co., Ltd.), 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole (SeeSorb 703, manufactured by Dipro Chemicals, Ltd., or Kemisorb 73, manufactured by Dipro Chemicals, Ltd.), etc.

[0109] Examples of the benzophenone-based ultraviolet absorbers (benzophenone-based compounds) and hydroxybenzophenone-based ultraviolet absorbers (hydroxybenzophenone-based compounds) include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid (anhydrous and trihydrate), 2-hydroxy-4-octyloxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 4-benzyloxy-2-hydroxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone (SeeSorb 106, manufactured by Dipro Chemicals Co., Ltd.), 2,2'-dihydroxy-4-methoxybenzophenone (KEMISORB 111, manufactured by Chemipro Chemicals Co., Ltd.), etc.

[0110] Examples of the salicylate ultraviolet absorber (salicylate compound) include phenyl-2-acryloyloxybenzoate, phenyl-2-acryloyloxy-3-methylbenzoate, phenyl-2-acryloyloxy-4-methylbenzoate, phenyl-2-acryloyloxy-5-methylbenzoate, phenyl-2-acryloyloxy-3-methoxybenzoate, phenyl-2-hydroxybenzoate, phenyl-2-hydroxy-3-methylbenzoate, phenyl-2-hydroxy-4-methylbenzoate, phenyl-2-hydroxy-5-methylbenzoate, phenyl 2-hydroxy-3-methoxybenzoate, and 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate (Thunubin 120, manufactured by BASF).

[0111] Examples of the cyanoacrylate ultraviolet absorber (cyanoacrylate compound) include alkyl-2-cyanoacrylate, cycloalkyl-2-cyanoacrylate, alkoxyalkyl-2-cyanoacrylate, alkenyl-2-cyanoacrylate, and alkynyl-2-cyanoacrylate.

[0112] The ultraviolet absorber may be used alone or in combination of two or more. The content of the ultraviolet absorber in the layer containing the ultraviolet absorber is expressed as parts by mass of the ultraviolet absorber relative to 100 parts by mass of the resin component which is the film-forming component in each layer.

[0113] For example, in the case of the above-mentioned structure 1 containing a UV absorber only in the protective film, the content of the UV absorber relative to 100 parts by mass of the constituent resin of the protective film is preferably in the range of 0.1 to 8 parts by mass, and more preferably in the range of 0.5 to 5 parts by mass. The same is true for the cases of structures 2, 3, and 5 containing a UV absorber only in the phase difference film, and the content of the UV absorber relative to 100 parts by mass of the constituent resin of the phase difference film is preferably in the same range as above. In the case of the above-mentioned structure 4 containing a UV absorber in both the protective film and the phase difference film, the content of the pigment compound (D) in each layer is preferably in the same range as above.

[0114] By making the content of the ultraviolet absorber within the above range, the layer containing the ultraviolet absorber can fully exert the ultraviolet absorption function, so it is preferred. Moreover, when the polarizing plate of the present invention is used in an organic EL display device, the layer containing the above-mentioned pigment compound (D) and the layer containing the ultraviolet absorber function to protect the organic EL element from the influence of external light, thereby maintaining the quality of the organic EL display device for a long time.

[0115] Hereinafter, each layer constituting the polarizing plate 10A will be described in order from the visible side. It should be noted that the hard coat layer 1 is a layer formed on the obtained protective film 2 after the protective film 2 is produced, and therefore will be described together with the protective film 2 .

[0116] [Protective film]

[0117] The protective film 2 is a film made of, for example, a thermoplastic resin and is provided to protect the polarizer 3. The protective film 2 is preferably formed of a thermoplastic resin material having excellent transparency, mechanical strength, thermal stability, moisture blocking properties, isotropy, and the like.

[0118] Examples of the thermoplastic resin used to form the protective film 2 include cellulose ester resins, polyester resins, polycarbonate resins, polyarylate resins, acrylic resins, polystyrene resins, acrylonitrile-styrene copolymers (AS resins), polyamide resins, polyimide resins, polysulfone resins, polyethersulfone resins, polyolefin resins, cycloolefin resins, polyvinyl chloride resins, polyvinyl alcohol resins, polyvinyl butyral resins, epoxy resins, norbornene resins, and fluororesins.

[0119] Thermoplastic resins may be used alone or in combination of two or more. In addition to the above-mentioned thermoplastic resins, the protective film 2 may also contain thermoplastic elastomers, rubber polymers, organic particles, inorganic particles, etc. as film-forming components within a range that does not impair the effects of the present embodiment. It should be noted that the organic particles include rubber particles described in the acrylic resin described later.

[0120] The protective film 2 may contain a pigment compound (D) or a UV absorber according to the above-mentioned configurations 1 to 5 of the polarizer 10A, or may not contain any of these. When the protective film 2 contains a pigment compound (D) or a UV absorber, the types and contents of these additives are as described above. In addition to the pigment compound (D) or the UV absorber, the protective film 2 may also contain other additives such as an antioxidant, a plasticizer, an antistatic agent, a stripping agent, and a thickener within the range that does not impair the effect of the present embodiment.

[0121] The protective film 2 may be a single layer or a laminated film of more than two layers. When the protective film 2 is a laminated film and contains a pigment compound (D) or an ultraviolet absorber, the amount of addition in each layer may be adjusted in the manner described above so that the content of these additives as the protective film 2 as a whole is adjusted. It should be noted that when the protective film 2 is a laminated film, the thermoplastic resin used in the formation of each layer may be the same or different. As a method for manufacturing a laminated film, a conventionally known method may be applied without particular limitation.

[0122] As the thermoplastic resin used for forming the protective film 2, cycloolefin resin, cellulose ester resin and acrylic resin are preferred from the viewpoints of transparency, mechanical strength, etc. Among them, a particularly preferred thermoplastic resin is a cycloolefin resin which is not easily affected by moisture due to its low polarity and whose refractive index is not easily changed by wavelength.

[0123] (Cycloolefin resin)

[0124] Examples of the cycloolefin resin used in the present invention include (co)polymers having a structure represented by the following general formula (2).

[0125] [Chemistry 6]

[0126] General formula (2)

[0127]

[0128] In the general formula (2), R 1 ~R 4 Each is independently a hydrogen atom, a hydrocarbon group, a halogen atom, a hydroxyl group, an ester group, an alkoxy group, a cyano group, an amide group, an imide group, a silyl group, or a hydrocarbon group substituted by a polar group (i.e., a halogen atom, a hydroxyl group, an ester group, an alkoxy group, a cyano group, an amide group, an imide group, or a silyl group). 1 ~R 4 Two or more may be bonded to each other to form an unsaturated bond, a monocyclic ring or a polycyclic ring. The monocyclic ring or polycyclic ring may have a double bond or may form an aromatic ring. 1 and R 2 , or R 3 and R 4 p and m are integers greater than 0.

[0129] In the above general formula (2), R 1 and R 3 It is a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, more preferably 1 to 4 carbon atoms, and particularly preferably 1 or 2 carbon atoms. 2 and R 4 is a hydrogen atom or a monovalent organic group, R 2 and R 4 At least one of the monomers is a polar group other than a hydrogen atom and a hydrocarbon group. m is an integer of 0 to 3, p is an integer of 0 to 3, more preferably m+p=0 to 4, further preferably 0 to 2, and particularly preferably m=1 and p=0. The specific monomer in which m=1 and p=0 is preferred in that the obtained cycloolefin resin has a high glass transition temperature and excellent mechanical strength.

[0130] As the polar group of the above-mentioned specific monomer, carboxyl, hydroxyl, alkoxycarbonyl, allyloxycarbonyl, amino, amide, cyano, etc. can be mentioned, and these polar groups can be bonded via connecting groups such as methylene. In addition, carbonyl, ether, silyl ether, thioether, imino, etc., which have polar divalent organic groups, become connecting groups and bonded hydrocarbon groups, etc. are also mentioned as polar groups. Among them, carboxyl, hydroxyl, alkoxycarbonyl or allyloxycarbonyl is preferred, and alkoxycarbonyl or allyloxycarbonyl is particularly preferred.

[0131] Furthermore, R 2 and R 4 At least one of the following is of the formula -(CH2) n The monomer of the polar group represented by COOR is preferred in that the obtained cycloolefin resin has a high glass transition temperature and low hygroscopicity, and has excellent adhesion to various materials. In the formula related to the above-mentioned specific polar group, R is a hydrocarbon group having 1 to 12 carbon atoms, more preferably 1 to 4 carbon atoms, and particularly preferably 1 to 2 carbon atoms, and is preferably an alkyl group.

[0132] Specific examples of the copolymerizable monomer include cycloolefins such as cyclobutene, cyclopentene, cycloheptene, cyclooctene, and dicyclopentadiene. The number of carbon atoms in the cycloolefin is preferably within a range of 4 to 20, more preferably 5 to 12.

[0133] In the present embodiment, the cycloolefin resin may be used alone or in combination of two or more.

[0134] The preferred molecular weight of the cycloolefin resin of the present embodiment is 0.2 to 5 dL / g, more preferably 0.3 to 3 dL / g, and particularly preferably 0.4 to 1.5 dL / g in terms of intrinsic viscosity [η]inh, the number average molecular weight (Mn) in terms of polystyrene measured by gel permeation chromatography (GPC) is 8,000 to 100,000, more preferably 10,000 to 80,000, and particularly preferably 12,000 to 50,000, and the weight average molecular weight (Mw) is in the range of 20,000 to 300,000, more preferably 30,000 to 250,000, and particularly preferably 40,000 to 200,000.

[0135] When the intrinsic viscosity [η]inh, the number average molecular weight, and the weight average molecular weight are within the above ranges, the heat resistance, water resistance, chemical resistance, and mechanical properties of the cycloolefin resin and the moldability of the cycloolefin film of the present embodiment become good.

[0136] The glass transition temperature (Tg) of the cycloolefin resin of the present embodiment is usually 110°C or higher, preferably 110 to 350°C, more preferably 120 to 250°C, and particularly preferably 120 to 220°C. When Tg is 110°C or higher, deformation due to use under high temperature conditions or secondary processing such as coating and printing is not likely to occur, so it is preferred. On the other hand, by making Tg 350°C or lower, it is possible to avoid the situation where molding becomes difficult, and the possibility of resin degradation due to heat during molding can be suppressed.

[0137] In addition, as the cycloolefin resin, commercially available products can be preferably used. Commercially available products are sold by JSR (Strain) under the trade names of Arton (registered trademark) G (G7810, etc.), Arton F, Arton R, and Arton RX, and by Zeon (Strain) Japan under the trade names of Zeonor (registered trademark) ZF14, ZF16, Zeonex (registered trademark) 250, or Zeonex 280, and these can be used.

[0138] (Cellulose ester resin)

[0139] Examples of the cellulose ester resin used in the present invention include triacetyl cellulose, cellulose acetate propionate, cellulose diacetate, cellulose acetate butyrate, etc. In addition, polyester resins such as polyethylene terephthalate and polyethylene naphthalate, polycarbonate resins, polyolefin resins such as polyethylene and polypropylene, norbornene resins, fluororesins, cycloolefin resins, etc. may be used in combination with the cellulose ester resin.

[0140] Commercially available products of cellulose ester resin films (cellulose ester films) include, for example, Conika Minolta KC8UX, KC4UX, KC8UY, KC4UY, KC6UA, KC4UA, KC2UA, KC4UE, KC4UZ, KC4CT1, and KC2CT1 (all manufactured by Conika Minolta Co., Ltd.). The refractive index of the cellulose ester film is preferably 1.45 to 1.55. The refractive index can be measured in accordance with JIS K7142-2008.

[0141] The cellulose ester used in the protective film of the present invention is preferably a carboxylic acid ester having about 2 to 22 carbon atoms, and may be an ester of an aromatic carboxylic acid, preferably a lower fatty acid ester of cellulose. Here, the "lower fatty acid" in the lower fatty acid ester of cellulose refers to a fatty acid having 6 or less carbon atoms.

[0142] In addition, the acyl group bonded to the hydroxyl group of the glucose unit constituting the cellulose ester may be a straight-chain hydrocarbon group, a branched hydrocarbon group, or a hydrocarbon group of a cyclic structure, and the acyl group may be substituted with other substituents. When the degree of substitution of the substituent bonded to the hydroxyl group of the cellulose ester is the same, if the carbon number of the lower fatty acid exceeds 7, the birefringence decreases, so the carbon number of the acyl group bonded to the hydroxyl group of the glucose unit constituting the cellulose ester is preferably 2 to 6, more preferably 2 to 4, and even more preferably 2 to 3.

[0143] In the present invention, cellulose ester may also use an acyl group derived from a mixed acid, preferably an acyl group having 2 and 3 carbon atoms, or an acyl group having 2 and 4 carbon atoms. As specific examples of such cellulose ester, a mixed fatty acid ester of cellulose having a propionate group or a butyrate group bonded to it in addition to an acetyl group, such as cellulose acetate propionate, cellulose acetate butyrate, or cellulose acetate propionate butyrate, may be used. It should be noted that the butyryl group forming the butyrate may be linear or branched. Cellulose ester is preferably cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, or cellulose acetate phthalate.

[0144] The retardation value of the protective film 2 can be appropriately controlled by the type of acyl group contained in the cellulose ester, the degree of substitution of the acyl group on the pyranose ring of the cellulose resin skeleton, and the like.

[0145] The substituent bonded to the hydroxyl group of the glucose unit constituting the cellulose ester used for the protective film 2 preferably satisfies the following formula (4) and formula (5) at the same time.

[0146] Formula (4): 2.0≤X+Y≤3.0

[0147] Formula (5): 0≤Y≤2.0

[0148] In the above formula (4), X is the degree of substitution of acetyl groups, and in formula (4) and formula (5), Y is the degree of substitution of propionyl groups or butyryl groups. By satisfying the above two formulas, a protective film 2 showing excellent optical properties can be manufactured. Among the above cellulose esters, triacetyl cellulose and cellulose acetate propionate are preferably used. Cellulose acetate propionate preferably has a degree of substitution X of acetyl groups of 1.0≤X≤2.5, 0.1≤Y≤1.5, and 2.0≤X+Y≤3.0.

[0149] The degree of substitution of the acyl group can be determined according to ASTM-D817-96. When the degree of substitution of the acyl group is too low, the unreacted portion becomes large relative to the hydroxyl group of the pyranose ring constituting the skeleton of the cellulose resin, and a large amount of the hydroxyl group remains. Therefore, the retardation value of the protective film 2 changes depending on the humidity, which is not preferred, and the ability to protect the polarizer as a polarizing plate protective film is reduced, which is not preferred.

[0150] The number average molecular weight of the cellulose ester is preferably 60000 to 300000, more preferably 70000 to 200000. By using cellulose ester having such a number average molecular weight, it is possible to improve the mechanical strength of the protective film 2. The number average molecular weight of the cellulose ester is a value measured by high performance liquid chromatography under the following conditions.

[0151] Solvent: Acetone

[0152] Column: MPW × 1 (manufactured by Tosoh Corporation)

[0153] Sample concentration: 0.2 (mass / volume)%

[0154] Flow rate: 1.0mL / min

[0155] Sample injection volume: 300μL

[0156] Standard sample: Standard polystyrene Temperature: 23°C

[0157] The cellulose used as the raw material of cellulose ester is not particularly limited, and examples thereof include cotton linter, wood pulp, kenaf, etc. Cellulose esters obtained from these materials may be used by mixing them in any proportion.

[0158] When using an acid anhydride such as acetic anhydride, propionic anhydride, or butyric anhydride as the acylating agent for the cellulose raw material, an organic acid such as acetic acid or an organic solvent such as dichloromethane and a protic catalyst such as sulfuric acid are used for the reaction. When using an acyl chloride (CH3COCl, C2H5COCl, or C3H7COCl) as the acylating agent, an alkaline compound such as amine is used as a catalyst. The acylation of the cellulose raw material can be synthesized by the method described in Japanese Patent Application Laid-Open No. 10-45804.

[0159] In the above-mentioned cellulose ester, the average degree of substitution of the acyl group at the 6th position of the glucose unit is preferably 0.5 to 0.9. The hydroxyl group at the 6th position of the glucose unit constituting the cellulose ester has a primary hydroxyl group that is more reactive than the hydroxyl groups at the 2nd and 3rd positions. The primary hydroxyl group preferentially forms a sulfate ester in the production process of cellulose ester using sulfuric acid as a catalyst. Therefore, in the esterification reaction of cellulose, by increasing the amount of sulfuric acid added as a catalyst, a cellulose ester having a higher average degree of substitution of the hydroxyl groups at the 2nd and 3rd positions of the glucose unit can be obtained compared to conventional cellulose esters.

[0160] In addition, in order to increase the average degree of substitution of the hydroxyl groups at positions 2 and 3, the cellulose ester can be tritylized as needed. The hydroxyl group at position 6 of the glucose unit constituting the cellulose ester is selectively protected by tritylization, thereby enabling the hydroxyl groups at positions 2 and 3 of the glucose unit to be concentratedly esterified. Moreover, after the hydroxyl groups at positions 2 and 3 of the glucose unit are esterified, the trityl group (protecting group) protecting the hydroxyl group at position 6 of the glucose unit is detached, thereby enabling the average degree of substitution of the hydroxyl groups at positions 2 and 3 to be increased compared to the hydroxyl group at position 6 of the glucose unit. As such an esterification method, it is preferred to use a cellulose ester manufactured by the method described in Japanese Patent Application Laid-Open No. 2005-281645.

[0161] When using acetylcellulose as cellulose ester, in order to increase the acetylation rate of acetylcellulose, it is necessary to extend the time of acetylation reaction. However, if the reaction time of acetylation reaction is extended, it will cause the severance of cellulose chain and decomposition of acetyl group, so it is not preferred. Therefore, in order to suppress the decomposition of acetylcellulose while increasing the acetylation rate of acetylcellulose, it is preferred to set the reaction time of acetylation reaction to a specific range. However, the preferred numerical range of reaction time varies greatly depending on the reaction device, reaction equipment, other reaction conditions, etc., and it is difficult to uniformly stipulate.

[0162] Therefore, it is preferred to use the value of weight average molecular weight (Mw) / number average molecular weight (Mn) as an indicator of the degree of reaction instead of the above reaction time. As the decomposition of cellulose ester progresses, the molecular weight distribution becomes wider, similar to the decomposition of ordinary polymers. Therefore, the degree of decomposition of cellulose ester can be grasped based on the value of weight average molecular weight (Mw) / number average molecular weight (Mn). For example, by determining the degree of reaction using weight average molecular weight (Mw) / number average molecular weight (Mn), in the process of acetylation of cellulose triacetate, it is possible to prevent the reaction time of acetylation from being too long and the decomposition of cellulose triacetate from being excessive, and to ensure sufficient reaction time required for acetylation. The Mw / Mn ratio of cellulose ester is preferably 1.4 to 5.0.

[0163] An example of a method for producing cellulose ester is shown below. 100 parts by mass of cotton linter (cotton linter) as a cellulose raw material is crushed, 40 parts by mass of acetic acid is added, and pre-treatment activation is performed at 36°C for 20 minutes. Then, 8 parts by mass of sulfuric acid, 260 parts by mass of acetic anhydride, and 350 parts by mass of acetic acid are added, and esterification is performed at 36°C for 120 minutes. After neutralization with 11 parts by mass of a 24% magnesium acetate aqueous solution, saponification and aging are performed at 63°C for 35 minutes to obtain acetyl cellulose. After stirring the acetyl cellulose at room temperature for 160 minutes using a 10-fold acetic acid aqueous solution (acetic acid: water = 1:1 (mass ratio)), the acetyl cellulose is filtered and dried to obtain a purified acetyl cellulose with an acetyl substitution degree of 2.75. The Mn of the acetyl cellulose is 92,000, the Mw is 156,000, and the Mw / Mn is 1.7. Similarly, by adjusting the esterification conditions (temperature, time, stirring) and hydrolysis conditions of cellulose ester, cellulose esters having different degrees of substitution and Mw / Mn ratios can be synthesized.

[0164] The cellulose ester synthesized by the above method is preferably purified to remove low molecular weight components, preferably by filtering to remove unacetylated or low acetylated components. In addition, when the cellulose ester is a mixed acid cellulose ester, it can be obtained by the method described in Japanese Patent Application Laid-Open No. 10-45804.

[0165] In addition, cellulose ester preferably does not contain metals such as iron (Fe), calcium (Ca), and magnesium (Mg). This is because these metal ions form insoluble cores by forming salts with polymer decomposition products containing organic acidic groups. These trace metal components are believed to be contained in cellulose esters from water used in the production process.

[0166] The iron content of the above-mentioned cellulose ester is preferably 1 ppm or less. The calcium content of the cellulose ester is preferably 60 ppm or less, and more preferably 0 to 30 ppm. Calcium sometimes forms complexes with acidic components such as carboxylic acids or sulfonic acids, and sometimes forms complexes with a large amount of ligands. Sometimes these complexes form scum (insoluble precipitation, turbidity) derived from insoluble calcium. The magnesium content of the cellulose ester is preferably 0 to 70 ppm, and more preferably 0 to 20 ppm. By setting the magnesium content to 70 ppm or less, the formation of insoluble components can be suppressed.

[0167] The above metal content is determined by decomposing absolutely dry cellulose ester with sulfuric acid and nitric acid using a micro-digestion wet decomposition device, pre-treating it by alkali melting, and analyzing the pre-treated cellulose ester using ICP-AES (inductively coupled plasma emission spectrometry).

[0168] (Acrylic resin)

[0169] The acrylic resin is a resin composed of a (co)polymer obtained by (co)polymerizing a monomer selected from (meth)acrylic acid and its derivatives. The unit derived from the monomer in the (co)polymer is referred to as a "structural unit".

[0170] It should be noted that in the present embodiment, "(meth)acrylic acid" means both "acrylic acid" and "methacrylic acid", "(meth)acrylate" means both "acrylate" and "methacrylate", and "(meth)acryloyl" means both "acryloyl" and "methacryloyl". For example, "urethane (meth)acrylate" means both "urethane acrylate" and "urethane methacrylate".

[0171] The acrylic resin used for the protective film 2 is selected from the type, combination, and monomer composition of the monomers according to the required physical properties. Hereinafter, from the perspective of adjusting the equilibrium moisture content of the protective film to within a specified range and improving brittleness, the acrylic resin is described by taking a molecularly designed acrylic resin as an example, but the acrylic resin used in the present invention is not limited thereto. The acrylic resin preferably includes, for example, a structural unit (U1) derived from methyl methacrylate, a structural unit (U2) derived from phenylmaleimide, and a structural unit (U3) derived from an alkyl acrylate.

[0172] The content of the structural unit (U1) derived from methyl methacrylate is preferably 50 to 95% by mass, more preferably 70 to 90% by mass, based on all the structural units constituting the acrylic resin.

[0173] The structural unit (U2) derived from phenylmaleimide has moderate polarity, and thus can improve affinity with water. In addition, since the structural unit (U2) derived from phenylmaleimide has a relatively large structure, it can have a small gap that can allow water to move in the resin matrix. Thus, the mobility and discharge of water in the protective film can be improved.

[0174] The content of the structural unit (U2) from phenylmaleimide is preferably 1 to 25% by mass relative to all the structural units constituting the acrylic resin. If the content of the structural unit (U2) from phenylmaleimide is more than 1% by mass, it has appropriate polarity, so it is not only easy to be compatible with water molecules, but also fully has a small gap in which water molecules can move, so it is easy to improve the equilibrium moisture content. If the content of the structural unit (U2) from phenylmaleimide is less than 25% by mass, the brittleness of the protective film 2 is not easily damaged. From the above viewpoint, the content of the structural unit (U2) from phenylmaleimide is more preferably 7 to 15% by mass.

[0175] The structural unit (U3) derived from an alkyl acrylate, for example, a polymer constituting the shell portion described below has good affinity with rubber particles containing structural units derived from butyl acrylate, and thus can improve the dispersibility of the rubber particles.

[0176] The alkyl acrylate is preferably one having an alkyl moiety with carbon atoms of 1 to 7, preferably 1 to 5. Examples of the alkyl acrylate include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-hydroxyethyl acrylate, hexyl acrylate, 2-ethylhexyl acrylate and the like.

[0177] The content of the structural unit (U3) from alkyl acrylate is preferably 1 to 25% by mass relative to all the structural units constituting the acrylic resin. If the content of the structural unit (U3) from alkyl acrylate is 1% by mass or more, the acrylic resin can be given appropriate flexibility, so the film will not become too brittle and will not break easily. If the content of the structural unit (U3) from alkyl acrylate is 25% by mass or less, the Tg of the acrylic resin will not be excessively reduced, so not only the heat resistance of the protective film 2 is not easily impaired, but also the mechanical strength is not easily impaired. From the above viewpoint, the content of the structural unit from alkyl acrylate is more preferably 5 to 15% by mass.

[0178] The ratio of the structural unit (U2) derived from phenylmaleimide to the total amount of the structural unit (U2) derived from phenylmaleimide and the structural unit (U3) derived from alkyl acrylate is preferably 20 to 70% by mass. If the ratio is 20% by mass or more, the heat resistance of the protective film 2 is easily improved, and if it is 70% by mass or less, the protective film 2 will not become too brittle.

[0179] The glass transition temperature (Tg) of the acrylic resin is preferably 110° C. or higher, more preferably 120 to 150° C. When the Tg of the acrylic resin is within the above range, the heat resistance of the protective film 2 is easily improved. In order to adjust the Tg of the acrylic resin, for example, it is preferable to adjust the content of the structural unit (U2) derived from phenylmaleimide and the structural unit (U3) derived from alkyl acrylate.

[0180] The weight average molecular weight (Mw) of the acrylic resin is preferably 500,000 or more. When the weight average molecular weight of the acrylic resin is 500,000 or more, the viscosity of the dope used in the solution casting will not become too low, so it is not only possible to suppress the aggregation of rubber particles, but also possible to suppress the reduction in the flatness of the surface of the protective film 2. Furthermore, if the weight average molecular weight of the acrylic resin is 500,000 or more, sufficient mechanical strength (toughness) can be imparted to the protective film 2. From the above viewpoints, the weight average molecular weight of the acrylic resin is more preferably 500,000 to 3,000,000, and further preferably 600,000 to 2,000,000. The weight average molecular weight can be measured by the same method as above.

[0181] The content of the acrylic resin is preferably 60% by mass or more, and more preferably 70% by mass or more, based on the protective film 2 .

[0182] When the protective film 2 is mainly composed of acrylic resin, it may also contain rubber particles that have the function of imparting toughness (softness) to the protective film 2. Rubber particles are particles containing rubber-like polymers. Rubber-like polymers are soft cross-linked polymers with a glass transition temperature of 20°C or less. Examples of such cross-linked polymers include butadiene-based cross-linked polymers, (meth)acrylic cross-linked polymers, and organosiloxane cross-linked polymers. Among them, from the viewpoint of having a small refractive index difference with acrylic resin and not being easy to damage the transparency of the protective film 2, (meth)acrylic cross-linked polymers are preferred, and acrylic cross-linked polymers (acrylic rubber-like polymers) are more preferred.

[0183] The rubber particles are preferably particles containing an acrylic rubber polymer. The acrylic rubber polymer is a cross-linked polymer containing a structural unit derived from an acrylic ester as a main component. The so-called containing as a main component means that the content of the structural unit derived from the acrylic ester is 40% by mass or more. The acrylic rubber polymer is preferably a cross-linked polymer containing a structural unit derived from an acrylic ester, a structural unit derived from other monomers copolymerizable therewith, and a structural unit derived from a multifunctional monomer having two or more free radical polymerizable groups (non-conjugated reactive double bonds) in one molecule.

[0184] The glass transition temperature (Tg) of the rubbery polymer is preferably 0° C. or lower, more preferably -10° C. or lower. When the glass transition temperature (Tg) of the rubbery polymer is 0° C. or lower, appropriate toughness can be imparted to the film. The glass transition temperature (Tg) of the rubbery polymer is measured by the same method as above.

[0185] The particles containing the acrylic rubber polymer may be core-shell particles having a core containing the acrylic rubber polymer and a shell covering the core. The shell preferably contains a methacrylic polymer containing a methacrylic acid ester-derived structural unit graft-bonded to the acrylic rubber polymer as a main component.

[0186] The average particle size of the rubber particles can be determined by measuring the dispersed particle size of the rubber particles in the dispersion using a zeta potential particle size measurement system (ELSZ-2000ZS manufactured by Otsuka Electronics Co., Ltd.). The average particle size of the rubber particles is preferably in the range of 100 to 300 nm. The content of the rubber particles is not particularly limited, but is preferably 5 to 25% by mass, more preferably 5 to 15% by mass, relative to the protective film 2.

[0187] (Manufacturing of protective film)

[0188] The protective film 2 can be produced by a known molding method such as melt casting, solution casting, calendar molding, etc. The melt casting method and solution casting method are preferably used, and the solution casting method is particularly preferred.

[0189] In order to manufacture the protective film 2 by the solution casting method, specifically, a manufacturing method including the following steps (1) to (3) can be used. Furthermore, the manufacturing method preferably includes the step (4).

[0190] (1) A step of obtaining a dope including a film-forming component containing a thermoplastic resin, a pigment compound (D) or an ultraviolet absorber added as needed depending on the structure of the polarizer 10A, and any additives, and a solvent.

[0191] (2) The process of casting the obtained slurry onto a support, drying and peeling it off to obtain a film-like product

[0192] (3) Step of drying the obtained film while stretching it as needed

[0193] (4) Step of winding the obtained protective film to obtain a roll

[0194] About the process of (1)

[0195] A film-forming component including a thermoplastic resin, a dye compound (D) or an ultraviolet absorber added as necessary depending on the structure of the polarizing plate 10A, and arbitrary additives are dissolved or dispersed in a solvent to prepare a dope.

[0196] The solvent used for the glue contains at least an organic solvent (good solvent) that can dissolve the thermoplastic resin. In the case of containing a pigment compound (D) or an ultraviolet absorber, it is preferred that the organic solvent also has high solubility for these additives. Examples of good solvents include chlorine-based organic solvents such as dichloromethane; non-chlorine-based organic solvents such as methyl acetate, ethyl acetate, acetone, and tetrahydrofuran. Among them, dichloromethane is preferred.

[0197] The solvent used for the glue may further contain a poor solvent. Examples of poor solvents include linear or branched aliphatic alcohols having 1 to 4 carbon atoms. If the ratio of alcohol in the glue increases, the film-like material is easily gelled and it becomes easy to peel off from the metal support. As linear or branched aliphatic alcohols having 1 to 4 carbon atoms, methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, and tert-butanol can be cited. Among them, ethanol is preferred from the perspectives of the stability of the glue, relatively low boiling point, and good drying properties.

[0198] Regarding the process of (2)

[0199] The obtained dope is cast on a support. The dope can be cast by discharging from a casting die.

[0200] Next, the solvent in the dope cast on the support is evaporated to dry the dope, and the dried dope is peeled off from the support to obtain a film-like object.

[0201] The residual solvent content of the dope when peeled from the support (the residual solvent content of the film when peeled) is preferably 20% by mass or more, more preferably 20 to 30% by mass. When the residual solvent content is 30% by mass or less, excessive elongation of the film caused by peeling can be easily suppressed.

[0202] The amount of residual solvent in the adhesive during peeling is defined by the following formula. The same applies to the following.

[0203] Residual solvent content of the adhesive (mass %) = (mass of the adhesive before heating treatment - mass of the adhesive after heating treatment) / mass of the adhesive after heating treatment × 100

[0204] In addition, the heat treatment in measuring the residual solvent amount means a heat treatment at 140° C. for 30 minutes.

[0205] The amount of residual solvent during peeling can be adjusted by adjusting the drying temperature and drying time of the adhesive on the support, the temperature of the support, and the like.

[0206] About the process of (3)

[0207] The obtained film is dried. Drying can be performed in one stage or in multiple stages. In addition, drying can be performed while stretching as needed.

[0208] For example, the film-drying step may include a step of pre-drying the film (pre-drying step), a step of stretching the film (stretching step), and a step of drying the stretched film (main drying step).

[0209] (Pre-drying process)

[0210] The pre-drying temperature (drying temperature before stretching) can be a temperature higher than the stretching temperature. Specifically, when the glass transition temperature of the thermoplastic resin is set to Tg, it is preferably (Tg-50) to (Tg+50)°C. If the pre-drying temperature is above (Tg-50)°C, it is easy to volatilize the solvent appropriately, so it is easy to improve the transportability (handling properties). If it is below (Tg+50)°C, the solvent will not volatilize excessively, so it is difficult to damage the stretchability in the subsequent stretching process. The initial drying temperature can be measured as an atmosphere temperature such as the temperature inside the stretching machine or the hot air temperature when (a) drying is performed by non-contact heating while conveying with a tenter stretching machine or rollers.

[0211] (Stretching process)

[0212] Stretching can be performed according to the required optical properties, such as retardation value, and is preferably performed in at least one direction. It can also be performed in two orthogonal directions (for example, biaxial stretching in the width direction (TD direction) of the film and the conveying direction (MD direction) orthogonal thereto).

[0213] The stretching ratio when producing the protective film B is preferably 5 to 100%, more preferably 20 to 100%. When biaxial stretching is performed, the stretching ratio in each direction is preferably within the above range.

[0214] The stretch ratio (%) is defined as (stretching direction size of the film after stretching - stretching direction size of the film before stretching) / (stretching direction size of the film before stretching)×100. When biaxial stretching is performed, the stretch ratios are preferably set for both the TD direction and the MD direction.

[0215] The stretching temperature (drying temperature during stretching) is the same as above. When the glass transition temperature of the thermoplastic resin is set to Tg, it is preferably Tg (°C) or above, and more preferably (Tg + 10) to (Tg + 50) °C. If the stretching temperature is above Tg (°C), preferably above (Tg + 10) °C, it is easy to volatilize the solvent appropriately, so it is easy to adjust the stretching tension to an appropriate range. If it is below (Tg + 50) °C, the solvent will not volatilize excessively, so the stretchability is not easily impaired. The stretching temperature during the manufacture of the protective film B can be set to, for example, 115 °C or above. The stretching temperature is the same as above, and it is preferably measured (a) The atmospheric temperature such as the temperature inside the stretching machine.

[0216] The amount of residual solvent in the film at the start of stretching is preferably about the same as the amount of residual solvent in the film at the time of peeling, for example, preferably 20 to 30% by mass, more preferably 25 to 30% by mass.

[0217] The stretching of the film in the TD direction (width direction) can be performed, for example, by fixing both ends of the film with clamps or needles and enlarging the interval between the clamps or needles in the running direction (tenter method). The stretching of the film in the MD direction can be performed, for example, by giving a peripheral speed difference to a plurality of rollers and utilizing the peripheral speed difference between the rollers (roller method).

[0218] (Formal drying process (main drying process))

[0219] From the viewpoint of further reducing the amount of residual solvent, the film obtained after stretching is preferably further dried. For example, the film obtained after stretching is preferably further dried while being conveyed by a roller or the like.

[0220] The main drying temperature (drying temperature in the case of non-stretching) is preferably (Tg-50) to (Tg-30)°C, more preferably (Tg-40) to (Tg-30)°C, when the glass transition temperature of the thermoplastic resin is set to Tg. If the post-drying temperature is (Tg-50)°C or higher, it is easy to fully volatilize and remove the solvent from the stretched film, and if it is (Tg-30)°C or lower, deformation of the film can be highly suppressed. The main drying temperature is preferably measured as the atmosphere temperature such as (a) hot air temperature as described above.

[0221] Regarding the process of (4)

[0222] The obtained protective film is preferably in a long strip shape. The long strip protective film is wound into a roll to form a roll body.

[0223] The length of the long protective film is not particularly limited, and may be, for example, about 100 to 10,000 m. The width of the protective film is preferably 1 m or more, and more preferably 1.3 to 4 m.

[0224] The thickness of the protective film 2 can be appropriately determined, but is usually preferably in the range of 1 to 500 μm from the perspectives of strength, workability such as handling, thin film properties, etc. The thickness of the protective film 2 is more preferably in the range of 5 to 50 μm, and further preferably in the range of 15 to 45 μm.

[0225] The polarizing plate 10A has a hard coating layer 1 on the visible side of the protective film 2, and a polarizer 3 on the opposite side of the visible side of the protective film 2. Although it depends on the type of resin as the main constituent material of the protective film, a primer layer can be provided on one side or both sides of the protective film 2. In particular, when the protective film 2 is formed with a cycloolefin resin as a main component, it is preferable to provide a primer layer. It is particularly preferable to provide a primer layer on the side of the protective film 2 on which the hard coating layer 1 is provided.

[0226] (Primer layer)

[0227] As the material constituting the primer layer, any material that can improve the adhesion and bonding between the protective film 2 and the hard coating layer 1 or the polarizer 3 can be used. In addition, as the characteristics of the material, in addition to the adhesion and bonding, it is also preferred that the transparency and thermal stability are excellent. As such a material, resins composed of polyurethane, polyolefin, polyester, polyvinylidene chloride, acrylic polymer, modified silicone polymer, styrene butadiene rubber, carbodiimide compound, isocyanate, etc. can be cited.

[0228] The above-mentioned primer layer can also contain any additive as required. As the specific example of additive, leveling agent, polymerization initiator, polymerization accelerator, viscosity modifier, slip agent, dispersant, plasticizer, heat stabilizer, light stabilizer, lubricant, antioxidant, flame retardant, colorant, antistatic agent, compatibility agent, crosslinking agent etc. can be enumerated. The type and amount of the additive used can be appropriately set according to the purpose. For example, relative to 100 mass parts of total solids in the primer layer, the usage amount of the additive is preferably below 30 mass parts, more preferably below 20 mass parts.

[0229] As the material constituting the above-mentioned primer layer, among the above-mentioned resins, it is preferred to use a material with polyurethane as the main component. As specific examples of polyurethane, DIC (Strain) has a product name of "Hidoran Series" AP-201, AP-40F, HW-140SF, WLS-202, Daiichi Kogyo Seiyaku (Strain) has a product name of "Superflex Series" SF-210, SF460, SF870, SF420, SF-420NS, Mitsui Chemicals (Strain) has a product name of "Takelac Series" W-615, W6010, W-6020, W-6061, W-405, W-5030, W-5661, W-512A-6, W-635, WPB-6601, WS-6021, WS-5000, WS-5100, WS-4000, WSA-5920, WF-764, ADEKA (Co., Ltd.), developed product "SPX-0882", etc. It should be noted that resins such as polyurethane having a carboxyl group in the side chain can be cross-linked with a cross-linking agent such as isocyanate, oxazoline, and carbodiimide to improve the strength of the primer layer.

[0230] Specific examples of polyolefins that can be used as a material constituting the primer layer include SB-1200, SE-1010, SE-1013N, SE-1030N, SD-1010, TC-4010, TD-4010 manufactured by Unichika Co., Ltd., S3148, S3121, S8512, P-5060N, P-9018 manufactured by Toho Chemical Co., Ltd., and P-5060N, P-9018 manufactured by Mitsui Chemicals. Co., Ltd., brand name "Typical Series" S-120, S-75N, V100, H-200, H-300, EV210H, Mitsui Chemical Co., Ltd., brand name "Chemipearl Series" XHP- 400. Manufactured by Sumitomo Seika Co., Ltd., trade name "ザイクセン series"ザイクセンA, "ザイクセンL", Toyobo Co., Ltd., trade name "Hydron Series" NZ-1004, NZ-1005, NZ-1022, etc.

[0231] Specific examples of acrylic polymers that can be used as a material constituting the primer layer include WS-700, a product of Nippon Shokubai Co., Ltd., and CP-0101, a product of Shin-Nakamura Chemical Co., Ltd., under the trade name "Newcoat series".

[0232] Specific examples of the modified silicone polymer that can be used as a material constituting the primer layer include "Selanet Series" WSA1060 and WSA1070 manufactured by DIC Corporation, and H7620, H7630, and H7650 manufactured by Asahi Kasei Chemicals Corporation.

[0233] Specific examples of polyesters that can be used as a material constituting the above-mentioned primer layer include Toyobo Co., Ltd., trade names "Bilonal Series" MD1400, MD1480, MD1245, MD1500, and Huying Chemical Industry Co., Ltd., trade names "Plastic Code Series" Z-221, Z-561, Z-730, RZ-142, Z-687, etc.

[0234] Specific examples of the styrene butadiene rubber that can be used as a material constituting the primer layer include NIPOL LX415, NIPOL LX407, NIPOL V1004, NIPOL MH8101, and SX1105 manufactured by Nippon Zeon Co., Ltd.

[0235] Specific examples of polyvinylidene chloride that can be used as a material constituting the primer layer include "SARAN Emulsion Series" L509, a product of Asahi Kasei Corporation.

[0236] Specific examples of the carbodiimide compound that can be used as a material constituting the primer layer include Nisshinbo Chemical Co., Ltd., trade names of "Carbodiimide Series" V-02, V-02-L2, SV-02, V-04, E-02, and the like.

[0237] As the isocyanate compound that can be used as the material constituting the above-mentioned primer layer, various compounds containing two or more isocyanate groups in one molecule can be used. For example, hexamethylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, xylylene diisocyanate, etc. can be listed. In addition, isocyanate can also be subjected to masking processing using a blocking agent.

[0238] In order to impart anti-blocking property to the primer layer, any appropriate microparticles may be used. Specific examples of microparticles include Nippon Shokubai (Strain), "Series" KE-P20, KE-P30, development product KE-W20, "Series" MX100W, etc. The particle size of the microparticles is preferably 50 to 500 nm, more preferably 100 to 300 nm. If it is the above range, the transparency and anti-blocking property of the primer layer can be taken into account.

[0239] The glass transition temperature (Tg) of the primer layer is preferably -40 to +130° C., more preferably -30 to +50° C., and particularly preferably 0 to +20° C. The glass transition temperature can be measured by reading the maximum value of the loss tangent (tan δ) by dynamic viscoelasticity measurement.

[0240] Any thickness may be adopted as the thickness of the primer layer. The thickness of the primer layer is preferably 10 to 1000 nm, more preferably 20 to 500 nm, and most preferably 50 to 400 nm.

[0241] The primer layer is formed, for example, by applying a coating solution containing a thermoplastic resin such as the polyurethane at a predetermined ratio to the surface of the protective film 2 and drying the coating solution. Any appropriate method may be used to adjust the coating solution. For example, a commercially available solution or dispersion may be used, a solvent may be added to a commercially available solution or dispersion, or a solid component may be dissolved or dispersed in various solvents for use.

[0242] As the coating method of the coating solution, any method can be used. For example, the coating method using a gravure die or a coater can be used. It should be noted that the primer layer can be formed only on the single side of the protective film 2 as required, or it can be formed on both sides.

[0243] When the primer layer is applied to the protective film 2 , solvent modification, corona treatment, or plasma treatment may be performed on the surface of the protective film as a pretreatment for improving wettability.

[0244] The total solid content concentration of the coating solution may vary depending on the type, solubility, coating viscosity, wettability, thickness after coating, etc. of the primer layer forming material. In order to obtain a primer layer with high surface uniformity, the total solid content concentration is preferably 1 to 100 parts by mass, more preferably 1 to 50 parts by mass, of solid content relative to 100 parts by mass of the solvent.

[0245] As the viscosity of the coating liquid, any appropriate viscosity can be adopted within the range of coating. As the viscosity, the value measured at a shear rate of 1000 (1 / s) at 23° C. is preferably 1 to 50 (mPa·seconds), and more preferably 2 to 10 (mPa·seconds). If it is within the above range, a primer layer with excellent surface uniformity can be formed.

[0246] The protective film 2 laminated with the primer layer can also be stretched at any ratio as required. The stretching direction can be a uniaxial direction in the horizontal direction, vertical direction, or oblique direction relative to the conveying direction, or a biaxial direction. It should be noted that the stretching of the protective film 2 can be performed as required before or after the primer layer is applied, or it can be stretched once or more before or after the primer layer is applied. The stretching conditions are as described above.

[0247] [Hard coating]

[0248] The polarizer 10A has a hard coat layer 1 as the outermost layer on the visible side. By having the hard coat layer 1, the impact resistance and ease of handling of the polarizer 10A can be improved. The hard coat layer 1 appropriately contains a pigment compound (D) according to the above-mentioned configurations 1 to 5 of the polarizer 10A. When the hard coat layer 1 contains a pigment compound (D), the type and content of the pigment compound (D) are as described above.

[0249] The hard coating layer 1 preferably shows a hardness of "HB" or more in the pencil hardness test specified in JIS K5600-2014. In order to obtain this hardness, it is preferred to contain a cured product of an active ray curable resin. As an active ray curable resin, a component containing a monomer having an ethylenically unsaturated double bond is preferably used. As an active ray curable resin, ultraviolet curable resins and electron beam curable resins can be listed. From the perspective of excellent mechanical film strength (scratch resistance, pencil hardness), a resin cured by ultraviolet irradiation is preferred.

[0250] As the active radiation curable resin, acrylic materials are preferably used. As acrylic materials, monofunctional or multifunctional (meth)acrylate compounds such as (meth)acrylates of polyols, and multifunctional urethane (meth)acrylate compounds synthesized from diisocyanates, polyols, and hydroxy esters of (meth)acrylates can be used. In addition, polyether resins, polyester resins, epoxy resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiol polyene resins, etc. having acrylate functional groups can also be used.

[0251] It is particularly preferred to use UV-curable acrylate resins, UV-curable urethane acrylate resins, UV-curable polyester acrylate resins, UV-curable epoxy acrylate resins, UV-curable polyol acrylate resins, or UV-curable epoxy resins, among which UV-curable acrylate resins are preferred.

[0252] The hard coat layer 1 is formed, for example, using a hard coat layer forming composition containing an active radiation curable resin, a polymerization initiator, and, when the hard coat layer 1 contains a pigment compound (D), a pigment compound (D) and a solvent. As the solvent contained in the hard coat layer forming composition, it is preferred that the protective film 2 or, when the protective film 2 has a primer layer, the primer layer be dissolved or swelled. By dissolving or swelling the protective film 2 or the primer layer with the solvent, the hard coat layer forming composition easily penetrates from the surface of the protective film 2 or the primer layer to the inside, and the adhesion between the protective film 2 or the primer layer and the hard coat layer 1 can be improved.

[0253] In addition, near the surface of the protective film 2 or the primer layer, a layer is formed in which the resin components of the protective film 2 or the primer layer and the resin components of the hard coating layer are mixed. Through the action of this layer, the refractive index of the protective film 2 or the primer layer and the hard coating layer can be tilted, thereby preventing the occurrence of interference unevenness.

[0254] In addition, in the hard coat layer forming composition, conventionally known microparticles, dispersants, surfactants, antistatic agents, silane coupling agents, thickeners, anti-coloring agents, colorants (pigments, dyes), defoamers, leveling agents, flame retardants, adhesion-imparting agents, polymerization inhibitors, antioxidants, surface modifiers, etc. may be added for the purpose of improving the hardness of the hard coat layer, inhibiting curing shrinkage, preventing adhesion, controlling the refractive index, imparting anti-glare properties, controlling the properties of the hard coat layer surface, etc. In addition, the above-mentioned hard coat layer forming composition may contain a photosensitizer, and specific examples thereof include n-butylamine, triethylamine, and poly-n-butylphosphine.

[0255] It is particularly preferred that the hard coat layer contains microparticles. The content of microparticles is preferably microparticles: active radiation curable resin = 100:100 to 400:100. By containing microparticles in such a content, the dimensional variation of the hard coat layer can be reduced. The microparticles here are not particularly limited, and are preferably microparticles composed of metal oxides (hereinafter also referred to as "metal oxide particles"). Examples of the metal oxides here include silicon dioxide, aluminum oxide, zirconium oxide, titanium oxide, antimony pentoxide, and the like. Among them, the metal oxide particles are preferably composed of silicon dioxide. The silicon dioxide microparticles may also be hollow particles having a cavity formed inside.

[0256] The above-mentioned microparticles are preferably coated with a polymer silane coupling agent. By coating the surface of the microparticles with a polymer silane coupling agent, the microparticles can be uniformly dispersed in the hard coat forming composition. The average particle size of the microparticles coated with a polymer silane coupling agent is preferably 5 to 500 nm, more preferably 10 to 200 nm. By using microparticles with such an average particle size, the optical properties of the hard coat can be improved.

[0257] The polymer silane coupling agent is adjusted by reacting a polymerizable monomer with a silane coupling agent (reactive silane compound). As the polymerizable monomer, a monomer having an ethylenically unsaturated double bond can be cited, preferably a monomer selected from (meth) acrylic acid and its derivatives. As the reactive silane compound, a hydrolyzable silane compound having three alkoxy groups and one functional group bonded to the silicon atom is preferred. As the functional group bonded to the silicon atom, a group having one or more groups selected from (meth) acryloyloxy, epoxy (glycidyl), carbamate, amino, fluoro, and mercapto can be cited.

[0258] The polymer silane coupling agent can be prepared, for example, according to the method for preparing a reaction product of a polymerizable monomer and a reactive silane compound disclosed in Japanese Patent Application Laid-Open No. 11-116240. The number average molecular weight of the polymer silane coupling agent is preferably 2,000 to 150,000, more preferably 2,500 to 100,000 in terms of polystyrene.

[0259] The method for coating the surface of particles with a polymer silane coupling agent is described by taking silica particles as an example. First, a dispersion is prepared in which silica particles and a polymer silane coupling agent are dispersed in an organic solvent. A base is added to the dispersion to generate an OH group on the surface of the silica particles, so that the OH group adsorbs the polymer silane coupling agent. Alternatively, the OH group is bonded to the OH group of the polymer silane coupling agent by a dehydration reaction. Finally, the silica particles adsorbed or bonded with the polymer silane coupling agent are separated from the dispersion and dried to obtain silica particles coated with a polymer silane coupling agent.

[0260] The method for preparing the hard coating layer-forming composition is not particularly limited as long as the solid components contained in the hard coating layer can be uniformly mixed in the solvent. For example, the hard coating layer can be prepared by mixing or dissolving the solid components and the solvent using a known device such as a paint shaker, a bead mill, a kneader, or a mixer.

[0261] The hard coat forming composition is applied to the surface of the protective film 2 or the primer layer, and the active ray curable resin in the coating film is cured to form a hard coat 1. As a coating method for the hard coat forming composition, a previously known method can be applied without particular restriction. For example, in the case of forming a uniform thin film layer, a micro-gravure coating method is preferred, and in the case of needing to form a thick film layer, a die coating method is preferred. After removing the solvent from the coating film as needed, the active ray curable resin is cured by active ray irradiation to obtain a hard coat.

[0262] The thickness of the hard coat layer 1 is preferably in the range of 0.01 to 20 μm, more preferably in the range of 0.5 to 10 μm, as an average thickness.

[0263] [Polarizing filter]

[0264] The polarizer 3 is an element that allows only light of a polarization plane in a certain direction to pass through. Examples of the polarizer include: a polarizer formed by adsorbing a dichroic substance such as iodine or a dichroic dye on a hydrophilic polymer film such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, and a partially saponified film of an ethylene-vinyl acetate copolymer, and then uniaxially stretching the film; a polyene-based oriented film such as a dehydrated product of polyvinyl alcohol or a dehydrochlorinated product of polyvinyl chloride, etc. Among them, a polarizer composed of a polyvinyl alcohol film and a dichroic substance such as iodine is preferred. The thickness of these polarizers is not particularly limited, but is usually about 5 to 80 μm.

[0265] The polarizer formed by dyeing the polyvinyl alcohol film with iodine and uniaxially stretching can be made, for example, by immersing polyvinyl alcohol in an aqueous solution of iodine for dyeing and stretching to 3 to 7 times the original length. As needed, it can also be immersed in an aqueous solution of potassium iodide, which can contain boric acid, zinc sulfate, zinc chloride, etc. Furthermore, the polyvinyl alcohol film can be immersed in water and washed before dyeing as needed. By washing the polyvinyl alcohol film, in addition to cleaning the dirt and anti-adhesion agent on the surface of the polyvinyl alcohol film, it also has the effect of preventing uneven dyeing by swelling the polyvinyl alcohol film. Stretching can be carried out after dyeing with iodine, or it can be stretched while dyeing. In addition, it can also be dyed with iodine after stretching. It can also be stretched in an aqueous solution or water bath of boric acid, potassium iodide, etc.

[0266] In addition, in the present invention, a thin polarizer with a thickness of 10 μm or less may be used. From the viewpoint of thinning, the thickness is preferably 1 to 7 μm. Such a thin polarizer has less uneven thickness and excellent visibility. In addition, due to less dimensional change, it has excellent durability, and is also preferred in terms of achieving thinning of the thickness of the polarizing film.

[0267] As a thin polarizer, representative examples include thin polarizing films described in Japanese Patent Publication No. 51-069644, Japanese Patent Publication No. 2000-338329, International Publication No. 2010 / 100917, International Publication No. 2010 / 100917, Japanese Patent No. 4751481, and Japanese Patent Publication No. 2012-073563. These thin polarizing films can be obtained by a method including a step of stretching a polyvinyl alcohol resin (hereinafter also referred to as a PVA resin) layer and a stretching resin substrate in a laminated state and a step of dyeing. According to this method, even if the PVA resin layer is thin, it can be stretched without any undesirable conditions such as breakage caused by stretching by being supported by the stretching resin substrate.

[0268] As the above-mentioned thin polarizing film, in the manufacturing method including the steps of stretching in the state of a stack and the step of dyeing, from the aspect of being able to stretch at a high ratio to improve the polarization performance, it is preferred to use a thin polarizing film obtained by the method including the step of stretching in an aqueous boric acid solution as described in International Publication No. 2010 / 100917 Pamphlet, International Publication No. 2010 / 100917 Pamphlet, or Japanese Patent No. 4751481 Specification, and Japanese Patent Gazette No. 2012-073563. It is particularly preferred to use a polarizing film obtained by the method including the step of auxiliary aerial stretching before stretching in an aqueous boric acid solution as described in Japanese Patent No. 4751481 Specification and Japanese Patent Gazette No. 2012-073563.

[0269] [Phase difference film]

[0270] Any retardation film having a retardation and functioning as an optical compensation layer can be used as the retardation film 4. When a transparent protective film having a retardation is used, the retardation characteristics thereof can be appropriately adjusted to a value required for optical compensation.

[0271] As the phase difference film 4, for example, when the refractive index in the direction of the slow axis is set to nx, the refractive index in the direction of the fast axis in the plane is set to ny, and the refractive index in the thickness direction is set to nz, a film satisfying the relationship of nx=ny>nz, nx>ny>nz, nx>ny=nz, nx>nz>ny, nz=nx>ny, nz>nx>ny, nz>nx=ny is selected and used according to various uses. It should be noted that nx=ny includes not only the case where nx and ny are completely the same, but also the case where nx and ny are basically the same. In addition, ny=nz includes not only the case where ny and nz are completely the same, but also the case where ny and nz are basically the same.

[0272] When the polarizing plate 10A is used in an organic EL display device, the phase difference film 4 is preferably a 1 / 4 wavelength plate with a front retardation of 1 / 4 wavelength (about 100 to 170 nm). By stacking the polarizer 3 and the 1 / 4 wavelength plate (phase difference film) 4, it functions as a circular polarizing plate for anti-reflection of the organic EL display device, so it is preferred.

[0273] That is, the external light incident on the organic EL display device passes through the polarizer 3 and transmits only the linearly polarized light component. The linearly polarized light generally becomes elliptically polarized light when passing through the retardation film 4, and particularly becomes circularly polarized light when the retardation film 4 is a 1 / 4 wavelength plate and the angle formed with the polarization direction of the retardation film 4 is π / 4.

[0274] The circularly polarized light passes through the transparent substrate, transparent electrode, and organic film in the organic EL panel, is reflected by the metal electrode, passes through the organic film, transparent electrode, and transparent substrate again, and becomes linearly polarized light again at the phase difference film 4. Moreover, the linearly polarized light is orthogonal to the polarization direction of the polarizer 3, and therefore cannot pass through the polarizer 3. As a result, the mirror surface of the metal electrode can be completely shielded.

[0275] A stretched film obtained by stretching a film containing a thermoplastic resin as a film-forming component can be preferably used as the retardation film 4. As the thermoplastic resin, the same thermoplastic resin as described as the constituent material of the protective film 2 can be used.

[0276] The phase difference film 4 may contain an ultraviolet absorber according to the above-mentioned configurations 1 to 5 of the polarizing plate 10A. When the phase difference film 4 contains an ultraviolet absorber, the type and content of the ultraviolet absorber are as described above. In addition to the ultraviolet absorber, the phase difference film 4 may also contain other additives such as a phase difference adjusting agent, an antioxidant, a plasticizer, an antistatic agent, a release agent, and a thickener within a range that does not impair the effect of the present embodiment.

[0277] The phase difference film 4 may be a single layer or a laminated film of two or more layers. When the phase difference film 4 is a laminated film and contains an ultraviolet absorber, the amount of the ultraviolet absorber added in each layer may be adjusted as described above so that the content of the ultraviolet absorber as the entire phase difference film 4 is adjusted. It should be noted that when the phase difference film 4 is a laminated film, the thermoplastic resin used in the formation of each layer may be the same or different. As a method for manufacturing a laminated film, a conventionally known method may be applied without particular limitation.

[0278] As the thermoplastic resin used in the formation of the phase difference film 4, in addition to the above-mentioned cycloolefin resin, cellulose ester resin and acrylic resin, polycarbonate resin is preferably used. In particular, when manufacturing the oblique stretched film described later, polycarbonate resin is preferably used. When the phase difference film 4 is set as a laminated film, for example, a combination of a cellulose ester resin and a polycarbonate resin layer is preferably used.

[0279] (Polycarbonate resin)

[0280] The polycarbonate resin is not particularly limited, and various polycarbonate resins can be used. From the viewpoint of chemical properties and physical properties, aromatic polycarbonate resins are preferred, and polycarbonates having a fluorene skeleton and bisphenol A-based polycarbonate resins are particularly preferred. Among them, bisphenol A derivatives in which a benzene ring, a cyclohexane ring, an aliphatic hydrocarbon group, etc. are introduced into bisphenol A are more preferably used. Furthermore, it is particularly preferred to use a polycarbonate resin having a structure in which the anisotropy in the unit molecule is reduced by introducing the above-mentioned functional groups asymmetrically with respect to the central carbon of bisphenol A.

[0281] As such a polycarbonate resin, it is particularly preferable to use a product obtained by replacing two methyl groups of the central carbon of bisphenol A with benzene rings, or a product obtained by replacing hydrogen of the benzene ring of each bisphenol A with methyl groups, phenyl groups, etc. asymmetrically with respect to the central carbon. Specifically, it is a product obtained by the phosgene method or the transesterification method from 4,4'-dihydroxydiphenylalkane or a halogen-substituted product thereof, for example, 4,4'-dihydroxydiphenylmethane, 4,4'-dihydroxydiphenylethane, 4,4'-dihydroxydiphenylbutane, etc. In addition, if specific polycarbonate resins are specifically illustrated, for example, polycarbonate resins described in Japanese Patent Application Laid-Open Nos. 2006-215465, 2006-91836, 2005-121813, 2003-167121, 2009-126128, 2012-67300, and International Publication No. 2000 / 026705 can be cited.

[0282] (Manufacturing of Phase Difference Film)

[0283] The retardation film 4 can be produced by a known molding method such as melt casting, solution casting, or calendaring, similarly to the protective film 2 described above. The melt casting method or solution casting method is preferably used, and the solution casting method is particularly preferred.

[0284] As for the phase difference film 4, in the solution casting method described in the protective film 2, in the step of obtaining the slurry in (1), the additive is combined with the phase difference film 4, and according to the structure of the polarizer 10A, except for the ultraviolet absorber and any additives added as needed, it can be manufactured in the same way. In addition, in the solution casting method described in the protective film 2, the film obtained in the step (3) or (4) is used as a film substrate, and further oblique stretching is performed by the following method to produce the phase difference film 4.

[0285] In order to produce a long oblique stretched film using a film substrate, for example, Figure 4 and Figure 5 The device having a general structure is schematically shown in FIG. Figure 4 It is a plan view schematically showing the general structure of a production apparatus 80 for a diagonally stretched film. Figure 5 1 is a top view schematically showing an example of a track pattern of a stretching section provided in a manufacturing device 80 for obliquely stretched film. The manufacturing device 80 includes, in order from the upstream side in the conveying direction of the film substrate, a film unwinding section 81, a conveying direction changing section 82, a guide roller 83, a stretching section 84, a guide roller 85, a conveying direction changing section 86, and a film winding section 87.

[0286] The film unwinding section 81 unwinds the film substrate produced as described above and supplies it to the stretching section 84. The conveying direction changing section 82 changes the conveying direction of the film substrate delivered from the film unwinding section 81 to a direction toward the entrance of the stretching section 84, which is an oblique stretching tenter. In order to stabilize the trajectory of the film substrate during travel, at least one guide roller 83 is provided on the upstream side of the stretching section 84. In order to stabilize the trajectory of the film obliquely stretched in the stretching section 84 during travel, at least one guide roller 85 is provided on the downstream side of the stretching section 84. The conveying direction changing section 86 changes the conveying direction of the stretched film delivered from the stretching section 84 to a direction toward the film winding section 87. The film winding section 87 winds up the film delivered from the stretching section 84 via the conveying direction changing section 86.

[0287] based on Figure 5 The details of the stretching section 84 will be described. For example, the diagonally stretched film can be produced by using Figure 5 The tenter (oblique stretching machine) capable of oblique stretching as shown in the figure is used as the stretching section 84. The tenter is a device that heats the film substrate to an arbitrary temperature at which it can be stretched and performs oblique stretching, and is equipped with a heating zone Z, a pair of left and right rails Ri·Ro, and a plurality of holding tools Ci·Co (in Figure 5 In the figure, only one set of holding tools is shown. The details of the heating zone Z will be described later. The tracks Ri and Ro are respectively formed by connecting a plurality of track parts through a connecting part ( Figure 5 The white circle in FIG. 1 is an example of a connecting portion. The holding tool Ci·Co is composed of clamps for holding both ends of the film in the width direction.

[0288] exist Figure 5 In the drawing, the feeding direction D1 of the film substrate is different from the winding direction D2 of the stretched long obliquely stretched film, and forms a feeding angle θi with the winding direction D2. The feeding angle θi can be arbitrarily set to a desired angle within a range of more than 0° and less than 90°.

[0289] Since the delivery direction D1 is different from the winding direction D2, the track pattern of the tenter becomes a left-right asymmetric shape. Moreover, the track pattern can be adjusted manually or automatically according to the orientation angle θ, the stretching ratio, etc. given to the long oblique stretched film to be manufactured. In the oblique stretching machine used in the manufacturing method of this embodiment, it is preferred to freely set the positions of the various track parts and the track connecting parts constituting the track Ri·Ro, and the track pattern can be arbitrarily changed. Thus, the orientation angle of the film can be freely set.

[0290] In the stretching section 84, the film substrate is held at both ends by the left and right holding tools Ci·Co, and is transported in the heating zone Z as the holding tools Ci·Co move. The left and right holding tools Ci·Co are opposite to each other in a direction substantially perpendicular to the film's moving direction (delivery direction D1) at the entrance of the stretching section 84 (position A in the figure), and move on left and right asymmetric tracks Ri·Ro respectively, releasing the film held at the exit (position B in the figure) at the end of stretching. The film released from the holding tools Ci·Co is wound around the winding core by the film winding section 87 described above.

[0291] Since the orbit Ri·Ro is asymmetric, Figure 5 In the example, in the figure, the left and right gripping tools Ci·Co at the relative positions of A travel on the track Ri·Ro, and the gripping tool Ci traveling on the track Ri side (inner side) becomes in a positional relationship in which it precedes the gripping tool Co traveling on the track Ro side (outer side).

[0292] That is, when one of the holding tools Ci·Co at position A in the figure reaches position B at which the film stretching ends first, the straight line connecting the holding tools Ci·Co is tilted by an angle θL relative to the direction substantially perpendicular to the film winding direction D2. By the above actions, the film substrate is tilted and stretched at an angle θL relative to the width direction. Here, substantially perpendicular means in the range of 90±1°.

[0293] The heating zone Z of the stretching section 84 is composed of a preheating zone Z1, a stretching zone Z2, and a heat fixing zone Z3. In the stretching section 84, the film held by the holding tool Ci·Co passes through the preheating zone Z1, the stretching zone Z2, and the heat fixing zone Z3 in sequence. In this embodiment, the preheating zone Z1 and the stretching zone Z2 are divided by a partition, and the stretching zone Z2 and the heat fixing zone Z3 are divided by a partition.

[0294] The preheating zone Z1 is a zone in which the holding tools Ci·Co holding both ends of the film at the entrance of the heating zone Z travel with a constant interval between them (in the film width direction).

[0295] The stretching zone Z2 refers to the interval between the holding tools Ci·Co holding the two ends of the film until the interval becomes a predetermined interval. Thus, the above-mentioned oblique stretching is performed. That is, in the stretching zone Z2, the long film (film substrate) is stretched in an oblique direction inclined relative to the width direction and the length direction in the film surface, thereby performing an oblique stretching process for obtaining an obliquely stretched film. It should be noted that before and after the oblique stretching, longitudinal or transverse stretching can be performed as needed.

[0296] The heat fixing zone Z3 is a zone where the interval between the holding tools Ci·Co after the stretching zone Z2 becomes constant again, and refers to a zone where the holding tools Ci·Co at both ends travel while maintaining parallelism with each other. That is, in the heat fixing zone Z3, a heat fixing process is performed while conveying the oblique stretched film while maintaining a constant width.

[0297] It should be noted that the stretched film may also pass through a region (cooling zone) in which the temperature in the region is set to a range below the glass transition temperature Tg (°C) of the thermoplastic resin constituting the film after passing through the heat fixing zone Z3. At this time, the shrinkage of the film due to cooling may be considered to form a track pattern that narrows the interval between the holding tools Ci·Co that are previously opposite.

[0298] Relative to the glass transition temperature Tg of the thermoplastic resin, the temperature of the preheating zone Z1 is preferably set to Tg~Tg+30°C, the temperature of the stretching zone Z2 is preferably set to Tg~Tg+30°C, and the temperature of the heat fixing zone Z3 and the cooling zone is preferably set to Tg-30~Tg+20°C.

[0299] It should be noted that the lengths of the preheating zone Z1, the stretching zone Z2 and the heat fixing zone Z3 can be appropriately selected. Relative to the length of the stretching zone Z2, the length of the preheating zone Z1 is usually 100-150%, and the length of the heat fixing zone Z3 is usually 50-100%.

[0300] In addition, if the width of the film before stretching is set to Wo (mm) and the width of the film after stretching is set to W (mm), the stretching ratio R (W / Wo) in the stretching process is preferably 1.3 to 3.0, and more preferably 1.5 to 2.8. If the stretching ratio is within this range, the thickness unevenness in the width direction of the film becomes smaller, so it is preferred. In the stretching zone Z2 of the oblique stretching tenter, if a difference is given to the stretching temperature in the width direction, the thickness unevenness in the width direction can be further improved to a good level. It should be noted that the above-mentioned stretching ratio R is equal to the ratio (W2 / W1) when the interval W1 between the two ends of the clamp held at the entrance of the tenter becomes the interval W2 at the exit of the tenter.

[0301] The thickness of the retardation film 4 can be appropriately determined, and is generally preferably in the range of 1 to 500 μm from the perspectives of optical properties, strength, workability such as handling, thin film properties, etc. The thickness of the retardation film 4 is more preferably in the range of 5 to 100 μm, and further preferably in the range of 15 to 80 μm.

[0302] (Adhesive layer)

[0303] Preferably, the polarizer 3 and the protective film 2 and the polarizer 3 and the retardation film 4 are closely attached to each other, for example, via an adhesive layer. The adhesive layer may be a layer obtained by drying an aqueous adhesive or a cured layer of an active ray-curable adhesive. In addition, the adhesive layer may contain a metal compound filler.

[0304] As water-based adhesives, isocyanate adhesives, polyvinyl alcohol adhesives, gelatin adhesives, vinyl latex adhesives, water-based polyurethanes, water-based polyesters, etc. can be exemplified. As polyvinyl alcohol adhesives, specifically, fully saponified polyvinyl alcohol aqueous solutions (water pastes) can be cited. As active radiation-curable adhesives, ultraviolet-curable adhesives, electron beam-curable adhesives, etc. can be cited.

[0305] [Pressure-sensitive adhesive layer]

[0306] The pressure-sensitive adhesive layer is arbitrarily provided on the polarizing plate of the present invention. By providing the pressure-sensitive adhesive layer, the workability is improved when manufacturing an organic EL display device in which the polarizing plate is arranged on the visible side of the organic EL element. Figure 2The polarizing plate 10B shown in the cross-sectional view is an example of a polarizing plate having a pressure-sensitive adhesive layer. The polarizing plate 10B may include the same preferred aspects as the polarizing plate 10A, except that the pressure-sensitive adhesive layer 5 is provided on the side of the retardation film 4 opposite to the polarizer 3 .

[0307] The type of pressure-sensitive adhesive forming the pressure-sensitive adhesive layer 5 is not particularly limited, and examples thereof include rubber pressure-sensitive adhesives, acrylic pressure-sensitive adhesives, silicone pressure-sensitive adhesives, urethane pressure-sensitive adhesives, vinyl alkyl ether pressure-sensitive adhesives, polyvinyl alcohol pressure-sensitive adhesives, polyvinyl pyrrolidone pressure-sensitive adhesives, polyacrylamide pressure-sensitive adhesives, cellulose pressure-sensitive adhesives, etc. Among these pressure-sensitive adhesives, acrylic pressure-sensitive adhesives are preferably used from the perspective of excellent optical transparency, adhesive properties showing appropriate adhesion, cohesion, and adhesion, weather resistance, heat resistance, etc. In the present invention, acrylic pressure-sensitive adhesives containing (meth) acrylic polymers as base polymers are preferred.

[0308] The method for forming the pressure-sensitive adhesive layer 5 is not particularly limited, and the pressure-sensitive adhesive layer 5 may be formed by a method commonly used in the art. Specifically, a pressure-sensitive adhesive composition containing the pressure-sensitive adhesive or its raw material and a solvent may be applied to at least one side of the substrate, and dried to form a coating film formed of the pressure-sensitive adhesive composition, or irradiated with active rays such as ultraviolet rays. In the case of an acrylic adhesive, the pressure-sensitive adhesive composition contains a monomer that becomes a structural unit of a polymer, a polymerization initiator, and a solvent.

[0309] The substrate on which the pressure-sensitive adhesive composition is applied is, for example, a release film or a phase difference film 4. When the pressure-sensitive adhesive layer 5 is formed on the release film, the formed pressure-sensitive adhesive layer 5 is transferred to the phase difference film 4, and the release film is peeled off. It should be noted that the pressure-sensitive adhesive layer 5 may be protected by a release film before the polarizing plate 10B is put into practical use.

[0310] The thickness of the pressure-sensitive adhesive layer 5 is not particularly limited, but is preferably about 10 to 75 μm, more preferably about 12 to 50 μm.

[0311] [Polarizing plate]

[0312] The polarizing plate 10A is obtained by laminating the protective film 2 with the hard coating layer 1, the polarizer 3 and the phase difference film 4 prepared as described above so as to form the hard coating layer 1, the protective film 2, the polarizer 3 and the phase difference film 4 from the visible side. It should be noted that when laminating, the hard coating layer 1, the protective film 2 and the phase difference film 4 are selected so that the combination of the hard coating layer 1, the protective film 2 and the phase difference film 4 is any one of the above-mentioned structures 1 to 5. In addition, the protective film 2 and the polarizer 3 and the polarizer 3 and the phase difference film 4 are preferably bonded by an adhesive as described above.

[0313] The polarizing plate 10B is obtained by laminating the protective film 2 with the hard coating layer 1, the polarizer 3, the phase difference film 4, and the pressure-sensitive adhesive layer 5 prepared as described above. As with the polarizing plate 10A, when laminating, the hard coating layer 1, the protective film 2, and the phase difference film 4 are selected in such a way that the combination of the hard coating layer 1, the protective film 2, and the phase difference film 4 is any one of the above-mentioned structures 1 to 5. The protective film 2 and the polarizer 3 and the polarizer 3 and the phase difference film 4 are preferably bonded by an adhesive. When laminating, the pressure-sensitive adhesive layer 5 may be laminated with the phase difference film 4 in advance, or may be laminated as the pressure-sensitive adhesive layer 5 formed on the release film.

[0314] In the polarizing plate of the present invention, the transmittance of the layer containing the ultraviolet absorber or the pigment compound (D) and the transmittance of the polarizing plate are preferably in the following ranges.

[0315] (i) Transmittance of the layer containing the ultraviolet absorber

[0316] The transmittance of the layer containing the ultraviolet absorber at a wavelength of 380nm is preferably 9% or less, more preferably 7% or less, further preferably 5% or less, and particularly preferably 3% or less. When the transmittance at a wavelength of 380nm is within the above range, the region near the wavelength of the incident ultraviolet rays can be more highly blocked, and when used in an organic EL display device, the degradation of the organic EL element can be significantly suppressed.

[0317] In addition, the transmittance of the layer containing the ultraviolet absorber at a wavelength of 450nm is preferably 60% or more, preferably 70% or more, and more preferably 75% or more. When the transmittance at a wavelength of 450nm is within the above range, when used in an organic EL display device, the light emission of the organic EL element can be fully transmitted, and sufficient display performance can be ensured in the organic EL display device, so it is preferred.

[0318] (ii) Transmittance of the layer containing the dye compound (D)

[0319] About the transmittance of the layer containing the pigment compound (D), the transmittance at 400nm is preferably below 50%, preferably below 35%, and more preferably below 20%. By the transmittance at a wavelength of 400nm being the above range, the region near the wavelength in the incident ultraviolet light can be more highly blocked, and when used for an organic EL display device, the degradation of the organic EL element can be significantly suppressed.

[0320] In addition, the transmittance of the layer containing the above-mentioned pigment compound at a wavelength of 450nm is preferably 60% or more, preferably 70% or more, and more preferably 75% or more. When the transmittance at a wavelength of 450nm is within the above range, when used in an organic EL display device, the luminescence of the organic EL element can be fully transmitted, and sufficient display performance can be ensured in the organic EL display device, so it is preferred.

[0321] (iii) Transmittance of polarizer

[0322] In the polarizer of the present invention, the transmittance at a wavelength of 380nm is preferably 9% or less, more preferably 7% or less, further preferably 5% or less, and particularly preferably 3% or less. In addition, the transmittance at a wavelength of 400nm of the polarizer is preferably 20% or less, preferably 15% or less, and more preferably 10% or less.

[0323] By setting the transmittance of the polarizing plate at a wavelength of 380 nm and at a wavelength of 400 nm to the above range, incident ultraviolet rays can be blocked to a greater extent. Thus, when the polarizing plate is used in an organic EL display device, incident ultraviolet rays can be blocked to a greater extent.

[0324] In addition, the transmittance of the polarizing plate of the present invention at a wavelength of 450nm is preferably 25% or more, preferably 30% or more, and more preferably 33% or more. When the transmittance at a wavelength of 450nm is within the above range, when used in an organic EL display device, the light emission of the organic EL element can be fully transmitted, and sufficient display performance can be ensured in the organic EL display device, so it is preferred.

[0325] [Organic EL display device]

[0326] The polarizing plate of the present invention can be used in various display devices such as liquid crystal display devices (LCD), organic EL display devices (OELD), touch panels, etc. The polarizing plate of the present invention is particularly preferably used as a circular polarizing plate for an organic EL display device.

[0327] exist Figure 3 Detailed description of the invention A cross-sectional view showing a configuration example of an organic EL display device according to the present invention. Figure 3 The organic EL display device 20 shown in FIG. 1 has a polarizing plate 10B of the present invention between an organic EL element 11 and its visible side. The organic EL display element 11 has, for example, a light reflecting electrode, a light emitting layer, a transparent electrode layer, and a transparent plastic film substrate.

[0328] When electricity is supplied between the light-reflecting electrode and the transparent electrode layer of the organic EL display device 20, the light-emitting layer emits light, and an image can be displayed. Furthermore, all the light incident on the organic EL display device from the outside is absorbed by the polarizer 3 of the polarizing plate 10B, so even if it is reflected by the light-reflecting electrode of the organic EL element 11, it will not be emitted to the outside, and the reduction of display characteristics caused by the reflection of the background can be suppressed.

[0329] In the organic EL display device 20, the polarizer 10B is configured as follows: as in the above-mentioned configurations 1 to 5, at least one of the hard coating layer 1 and the protective film 2 contains a pigment compound (D), at least one of the protective film 2 and the phase difference film 4 contains an ultraviolet absorber, and the layer containing the pigment compound (D) is located on the visible side compared to the layer containing the ultraviolet absorber.

[0330] Thus, by arranging the polarizing plate 10B having the layer containing the pigment compound and the layer containing the ultraviolet absorber on the visible side of the organic EL element 11, the polarizing plate 10B can fully absorb the light of the wavelength shorter than the light emitting region (the wavelength longer than 430 nm) of the organic EL element 11, and protect the organic EL element 11 from the influence of external light. Furthermore, by arranging the layer containing the pigment compound and the layer containing the ultraviolet absorber in the above-mentioned specific order, the heat generated from the pigment compound (D) is not hindered by the heat generation of the layer containing the ultraviolet absorber, and can be discharged to the outside from the surface of the organic EL display device 20. Thus, the degradation such as the change of the optical value of the retardation film 4 and the degradation such as the shrinkage of the polarizer 3 caused by the heat generation of the pigment compound (D) can be suppressed.

[0331] Example

[0332] The present invention is specifically described below with reference to Examples, but the present invention is not limited to these Examples. It should be noted that "parts" or "%" are used in the Examples, but unless otherwise specified, they represent "parts by mass" or "mass %".

[0333] [Production of Compound (1)]

[0334] Compound (1)-1 and Compound (1)-2 were prepared as the dye compound (D) as follows and used for the production of the polarizing plate of the example.

[0335] (1) Preparation of compound (1)-1

[0336] In a 100mL three-necked flask, weigh 1.5g of the raw material compound (A1) and 0.697g of malononitrile, add 40mL of toluene and dissolve. Then, add 0.817g of morpholine dropwise, raise the temperature, and heat under reflux for 4 hours. After the reaction is completed, remove the solvent under reduced pressure, add 10mL of methanol, stir in a suspended state, and recrystallize to obtain a precipitate. The precipitate is filtered and dried to obtain 1.89g (yield 96%) of powder of compound (1)-1. The structure is confirmed by NMR.

[0337] (2) Preparation of compound (1)-2

[0338] In a 100mL three-necked flask, 1g of the raw material compound (A2) and 0.61g of malononitrile were measured, and 40mL of toluene was added and dissolved. Then, 0.554g of morpholine was added dropwise, the temperature was raised, and heated to reflux for 4 hours. After the reaction was completed, the solvent was removed under reduced pressure, 10mL of methanol was added and stirred, and recrystallization was performed to obtain a precipitate. The precipitate was filtered and dried to obtain 0.93g of powder of compound (1)-2 (yield 56%). The structure was confirmed by NMR.

[0339] [1]Manufacturing of protective films with hard coatings

[0340] (1) Production of Cycloolefin Resin Film with Hard Coat Layer

[0341] (1-1) Production of Cycloolefin Resin Film

[0342] (Adjustment of glue)

[0343] The components of Table III are placed in a sealed container, heated, and stirred to completely dissolve. Filter it using Azumi filter paper No. 24 manufactured by Azumi filter paper (co., Ltd.) to obtain a slurry (COP-1 to COP-4). It should be noted that as the cycloolefin resin in the table, Aton G7810 (manufactured by JSR Corporation) is used. In addition, LA-F70 is a respective ultraviolet absorber ("UVA" in the table) manufactured by ADEKA (co., Ltd.) with a maximum absorption wavelength of 355nm, Tinuvin 928 manufactured by ADEKA (co., Ltd.) and a maximum absorption wavelength of 349nm manufactured by BASF Japan (co., Ltd.). Compound (1)-1 is equivalent to the pigment compound (D) ("(D)" in the table).

[0344] [Table 3]

[0345] Table III

[0346]

[0347] (Film formation of protective film)

[0348] The obtained dope was kept at 30° C. and uniformly cast on a stainless steel belt as a metal support kept at 30° C. Then, the cast dope was dried until the residual solvent content reached 30% by mass and then peeled from the stainless steel belt to obtain a film.

[0349] Next, the obtained film was dried at 40°C until the residual solvent content became 10% by mass, and then stretched in the width direction at a stretching ratio of 1.4 times (40%). Then, the obtained film was further dried at 150°C while being conveyed by multiple rollers to obtain a protective film with a length of 3000m and a thickness of 20μm. The obtained protective films were designated as protective films COP-1 to COP-4 corresponding to the types of adhesive.

[0350] (1-2) Formation of primer layer

[0351] (Preparation of hard coat side primer layer coating solution)

[0352] 100 parts by mass of a thermosetting waterborne polyolefin resin (Alobe SB-1200 (trade name), solid content 25%, manufactured by Unichika Co., Ltd.) and 8 parts by mass of an oxazoline crosslinking agent (WS-700, manufactured by Nippon Shokubai Co., Ltd.) were diluted with a diluent (water / methanol = 30 / 70 (mass %)) to a solid content concentration of 5%, and then stirred at room temperature to prepare a primer layer coating liquid 1.

[0353] (Formation of primer layer on the hard coat side)

[0354] The prepared primer coating liquid 1 was applied to the hard coating layer side of the protective film having a thickness of 20 μm using a bar coater and dried in a drying oven at 80° C. for 40 seconds to prepare a hard coating layer side primer layer having a dry film thickness of 0.4 μm.

[0355] (Preparation of the polarizer side primer coating solution)

[0356] 100 parts by mass of a water-based polyurethane resin (HIDOLAN AP-40F (trade name), solid content 20%, manufactured by DIC Corporation) and 5 parts by mass of an oxazoline crosslinking agent (WS-700, trade name, manufactured by Nippon Shokubai Co., Ltd.) were diluted with a diluent (water / methanol = 30 / 70 (mass %)) to a solid content concentration of 5%, and then stirred at room temperature to prepare a primer layer coating liquid 2.

[0357] (Formation of Primer Layer on Polarizer Side)

[0358] The prepared primer coating liquid 2 was applied to the polarizer side surface of the protective film having a thickness of 20 μm using a bar coater and dried in a drying oven at 120° C. for 120 seconds to form a polarizer side primer layer having a film thickness of 0.5 μm.

[0359] (1-3) Formation of hard coating

[0360] (Preparation of Hard Coat Layer Forming Composition)

[0361] The materials were mixed in the ratios shown in Table IV to prepare the hard coating forming compositions (CHD-1 to CHD-5). It should be noted that as the hard coating resins in the table, urethane acrylate and UA-306H (trade name, manufactured by Kyoeisha Chemical Co., Ltd.) were used. In addition, Ilgakuya 184 (manufactured by BASF Japan Co., Ltd.) was a photopolymerization initiator, and KF-351A (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.) was a surfactant. As diluent solvents, propylene glycol monomethyl ether (PGME) and methyl acetate (MA) were used (solvent mass ratio; MA / PGME=60 / 40). Pigment compound 1 was BONASORB UA3912 (trade name, manufactured by Orient Chemical Co., Ltd.), and pigment compound 2 was FDB-009 (trade name, manufactured by Yamada Chemical Co., Ltd.). The pigment compounds 1 and 2, compound (1)-1 and compound (1)-2 correspond to the pigment compound (D).

[0362] [Table 4]

[0363] Table IV

[0364]

[0365] (Formation of hard coat layer)

[0366] On the primer layer on the hard coating side of the protective film with a primer layer prepared above, the hard coating forming composition prepared as shown in Table V was applied using a bar coater and dried in a drying oven at 50°C for 40 seconds to volatilize the solvent. Then, nitrogen was purged in this state so that the oxygen concentration was 1.0 volume % or less, and an ultraviolet lamp was used at an illumination of 100 mW / cm 2 , irradiation dose is 0.2J / cm 2 The applied layer was cured to prepare protective films with a hard coat layer having a hard coat layer with a film thickness of 3 μm (protective films with HD layer 1 to 7).

[0367] [Table 5]

[0368] Table V

[0369] Composition for forming hard coat layer Protective film With HD layer protective film 1 CHD-2 COP-2 With HD layer protective film 2 CHD-3 COP-2 With HD layer protective film 3 CHD-2 COP-3 With HD layer protective film 4 CHD-2 COP-1 With HD layer protective film 5 CHD-1 COP-4 With HD layer protective film 6 CHD-4 COP-2 With HD layer protective film 7 CHD-5 COP-2

[0370] (2) Production of Cellulose Ester Resin Film with Hard Coat Layer

[0371] (2-1) Production of cellulose ester resin film

[0372] (Preparation of glue)

[0373] A dope of the following composition was prepared. That is, first, dichloromethane and ethanol were added to a pressure dissolving tank. Then, cellulose ester was added to the pressure dissolving tank with the solvent added while stirring, and the cellulose ester was heated and completely dissolved while stirring.

[0374] Cellulose esters:

[0375] 100 parts by mass of triacetyl cellulose

[0376] Polycondensation ester compound N 2 parts by mass

[0377] Polycondensation ester compound M 7 parts by mass

[0378] Solvent:

[0379] 540 parts by mass of dichloromethane

[0380] Ethanol 35 parts by mass

[0381] additive:

[0382] Microparticles: 3 parts by mass of silica dispersion dilution

[0383] 2 parts by mass of ultraviolet absorber

[0384] Furthermore, the above-mentioned additive components were put into a sealed container, dissolved while stirring, and filtered using Azumi filter paper No. 244 manufactured by Azumi Filter Paper Co., Ltd. to prepare a dope.

[0385] The ester compound N, the ester compound M, and the silica dispersion dilution were prepared as follows: Thunibin 928 (trade name, manufactured by BASF Japan Co., Ltd.) was used as an ultraviolet absorber.

[0386] (Ester Compound N)

[0387] First, 251 g of 1,2-propylene glycol, 354 g of terephthalic acid, 680 g of p-toluic acid, and 0.191 g of tetraisopropyl titanate as an esterification catalyst were placed in a 2L four-necked flask equipped with a thermometer, a stirrer, and a reflux condenser (quick cooling tube). Then, a nitrogen stream was blown into the four-necked flask, and the solution was slowly heated while stirring until the temperature of the solution reached 230°C, and a dehydration condensation reaction was performed while observing the degree of polymerization. After the reaction was completed, unreacted 1,2-propylene glycol was removed by reduced pressure distillation at 200°C, thereby obtaining an ester compound N. The acid value of the ester compound N was 0.30 and the number average molecular weight was 400.

[0388] (Ester compound M)

[0389] First, 251g of 1,2-propylene glycol, 244g of phthalic anhydride, 103g of adipic acid, 610g of benzoic acid, and 0.191g of tetraisopropyl titanate as an esterification catalyst were placed in a 2L four-necked flask equipped with a thermometer, a stirrer, and a reflux condenser. Next, a nitrogen stream was blown into the four-necked flask, and the solution was stirred while slowly heating the solution until the temperature of the solution reached 230°C, thereby conducting a dehydration condensation reaction while observing the degree of polymerization. After the reaction was completed, unreacted 1,2-propylene glycol was removed by reduced pressure distillation at 200°C, thereby obtaining a polycondensation ester compound M. The ester compound M had an acid value of 0.10 and a number average molecular weight of 450.

[0390] (Silicon dioxide dispersion)

[0391] First, 10 parts by mass of Aerosil R812 (trade name, manufactured by Aerosil Co., Ltd., Japan) and 90 parts by mass of ethanol were stirred and mixed with a dissolver for 30 minutes, and then the silica was dispersed in the ethanol with Manton-Gallin. 88 parts by mass of dichloromethane was added to the dispersion while stirring, and the dispersion was diluted with a dissolver for 30 minutes. The diluted dispersion was filtered with a particle dispersion dilution filter (manufactured by Adbandek Toyo Co., Ltd.: polypropylene air drum filter TCW-PPS-1N), thereby obtaining a silica dispersion.

[0392] (Film formation of protective film)

[0393] The prepared dope was uniformly cast on a stainless steel belt support at 22°C and 1.8 m in width using a belt casting device. The solvent was evaporated until the residual solvent amount reached 20% using the stainless steel belt support, and the dope film (web) was peeled off from the stainless steel belt support.

[0394] Next, the peeled web was allowed to evaporate the solvent at 35° C., slit into 1.6 m width, and then stretched 1.1 times the original width in the width direction (TD direction) using a tenter stretching machine at a temperature of 160° C. At this time, the residual solvent content at the start of the stretching using the tenter was 4% by mass.

[0395] Then, the film was conveyed in a drying zone at 120°C and 140°C by multiple rollers while being dried, slit into 1.3m width, knurled at both ends with a width of 10mm and a height of 2.5μm, and then rolled up on a core to produce a protective film TAC-1. The protective film TAC-1 had a thickness of 25μm and a roll length of 6000m.

[0396] (2-2) Formation of hard coating

[0397] (Preparation of Hard Coat Layer Forming Composition)

[0398] The respective materials were mixed at the following ratio to prepare a hard coat layer-forming composition.

[0399] Hard coating resin:

[0400] Pentaerythritol tri / tetraacrylate (NK Ester A-TMM-3L, trade name, manufactured by Shin-Nakamura Chemical Industry Co., Ltd.) 100 parts by mass

[0401] Photopolymerization initiator:

[0402] 9 parts by mass of Urakurea 184 (trade name, manufactured by BASF Electronics Co., Ltd.)

[0403] Solvent:

[0404] Propylene glycol monomethyl ether 20 parts by mass

[0405] 30 parts by mass of methyl acetate

[0406] 70 parts by mass of methyl ethyl ketone

[0407] additive:

[0408] Surfactant: KF-351A (trade name, polyether-modified silicone oil, manufactured by Shin-Etsu Chemical Co., Ltd.) 2 parts by mass

[0409] Microparticles: Polymer silane coupling agent coated silica (1) 100 parts by mass

[0410] Pigment compound (D): Pigment compound 1 5 parts by mass

[0411] The above-mentioned polymer silane coupling agent coated silica (1) is prepared as follows. 30 mL of methyl methacrylate (manufactured by Kyoeisha Chemical Co., Ltd.: Light Esther M), 1 mL of 3-mercaptopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: KBM-803), 100 mL of tetrahydrofuran as a solvent, and 50 mg of azoisobutyronitrile (manufactured by Kanto Chemical Co., Ltd.: AIBN) as a polymerization initiator are added to a container, replaced with N2 gas, and heated at 80°C for 3 hours to prepare a polymer silane coupling agent. The molecular weight of the obtained polymer silane coupling agent is 16000. It should be noted that the molecular weight is measured by a gel permeation chromatography device.

[0412] Next, the silica sol (manufactured by JGC Catalysts & Chemicals Co., Ltd.: Si-45P, trade name, SiO2 concentration 30% by mass, average particle size 45 nm, dispersion medium: water) was subjected to ion exchange using an ion exchange resin, and the aqueous solvent was replaced with ethanol using an ultrafiltration membrane method to prepare 100 g of an ethanol dispersion of silica particles (SiO2 concentration 30% by mass).

[0413] 100 g of the silica fine particle ethanol dispersion and 1.5 g of a polymer silane coupling agent were dispersed in 20 g (25 mL) of acetone, 20 mg of 29.8 mass % ammonia water was added thereto, and the mixture was stirred at room temperature for 30 hours to allow the polymer silane coupling agent to adsorb to the silica fine particles.

[0414] Then, silica particles with an average particle size of 5 μm were added and stirred for 2 hours to allow the unabsorbed polymer silane coupling agent in the solution to be adsorbed on the silica particles. Then, the silica particles with an average particle size of 5 μm adsorbed with the unabsorbed polymer silane coupling agent were removed by centrifugal separation. 1000 g of ethanol was added to the silica particle dispersion adsorbed with the polymer silane coupling agent to allow the silica particles to settle. The silica particles were separated and dried under reduced pressure. Then, the mixture was dried at 25°C for 8 hours to obtain polymer silane coupling agent-coated silica (1). The average particle size of the obtained polymer silane coupling agent-coated silica (1) was 57 nm. The average particle size was measured by a laser particle size measuring device.

[0415] (Formation of hard coat layer)

[0416] The hard coat forming composition prepared above was applied to the visible side surface of the protective film prepared above by a bar coater, and dried in a drying oven at 50°C for 40 seconds to volatilize the solvent. Then, nitrogen was purged in this state so that the oxygen concentration was 1.0 volume % or less, and an ultraviolet lamp was used at the same time, and the illumination of the irradiated part was 100 mW / cm 2 , so that the irradiation amount is 0.2J / cm 2The coating layer was cured to prepare a protective film with a hard coating layer having a hard coating layer with a film thickness of 3 μm. The obtained hard coating layer is also referred to as “THD1”. In addition, the obtained protective film with a hard coating layer is also referred to as “protective film 21 with HD layer” hereinafter.

[0417] (3) Production of acrylic resin film with hard coat layer

[0418] (3-1) Production of acrylic resin film

[0419] (Preparation of glue)

[0420] Prepare a mortar with the following composition. First, add dichloromethane and ethanol to a pressure dissolving tank. Then, add resin to the pressure dissolving tank while stirring. Then, add the rubber particle dispersion prepared above and stir to completely dissolve it. Filter it using SHP150 manufactured by Rokitechno Co., Ltd. to obtain a mortar.

[0421]

[0422] The (meth)acrylic resin used above was a copolymer of methyl methacrylate (MMA) / phenylmaleimide (PMI) / butyl acrylate (BA) (80 / 10 / 10 mass ratio), Tg: 120° C., Mw: 2 million).

[0423] In addition, the glass transition temperature (Tg) of an acrylic resin is measured using DSC (Differential Scanning Calorimetry) according to JISK7121-2012.

[0424] In addition, the weight average molecular weight (Mw) of the acrylic resin was measured using a gel permeation chromatography (HLC8220GPC manufactured by Tosoh Corporation) and a column (TSK-GELG6000HXL-G5000HXL-G5000HXL-G4000HXL-G3000HXL manufactured by Tosoh Corporation in series). A sample of 20 mg ± 0.5 mg was dissolved in 10 mL of tetrahydrofuran and filtered with a 0.45 mm filter. 100 mL of the solution was injected into the column (temperature 40° C.), and the detector RI temperature was measured at 40° C., and the value converted to styrene was used.

[0425] The rubber particle dispersion used in the above was obtained as follows: 10 parts by mass of acrylic rubber particles M-210 (core: acrylic rubber polymer with a multilayer structure, shell: core-shell type rubber particles of a methacrylate polymer with methyl methacrylate as the main component, Tg of the acrylic rubber polymer: about -10°C, average particle size: 220 nm) and 190 parts by mass of dichloromethane were stirred and mixed in a dissolver for 50 minutes, and then dispersed in a Microdial Disperser (manufactured by Ohira Kiko Co., Ltd.) at 1500 rpm.

[0426] The average particle size of the rubber particles is obtained by measuring the dispersed particle size of the rubber particles in the dispersion using a zeta potential particle size measuring system (ELSZ-2000ZS manufactured by Otsuka Electronics Co., Ltd.).

[0427] (Film formation of protective film)

[0428] The dope was used to form a film. Specifically, an endless belt casting device was used to uniformly cast the dope on a stainless steel belt support at a temperature of 30°C and a width of 1800 mm. The temperature of the stainless steel belt was controlled at 28°C.

[0429] On the stainless steel belt support, the solvent was evaporated until the residual solvent content in the cast (cast) dope reached 30% by mass. Then, it was peeled off from the stainless steel belt support at a peeling tension of 128 N / m to obtain a film. The residual solvent content of the film at the time of peeling was 30% by mass.

[0430] Next, the film was stretched by 20% in the width direction (TD direction) at 140°C (Tg+20°C) using a tenter while conveying the peeled film with a plurality of rollers. Then, the film was further dried at 100°C (Tg-20°C) while conveying with rollers, and the end portion clamped by the tenter clamp was longitudinally cut and wound into a roll to obtain a protective film Ac-1 (roll) having a length of 3000 m, a width of 1.5 m, and a film thickness of 40 μm.

[0431] (3-2) Formation of Hard Coat Layer (Preparation of Hard Coat Layer Forming Composition)

[0432] The materials were mixed at the following ratios to prepare a hard coat layer-forming composition. The polymer silane coupling agent-coated silica (1) was obtained in the same manner as the polymer silane coupling agent-coated silica (1) prepared in the production of the cellulose ester resin film with a hard coat layer.

[0433] Hard coating resin:

[0434] Urethane acrylate (U-4H, trade name, manufactured by Shin-Nakamura Chemical Industry Co., Ltd.) 35 parts by mass

[0435] Photopolymerization initiator:

[0436] イルガキュア184 (trade name, manufactured by BASF Electronics Co., Ltd.) 5 parts by mass

[0437] Solvent:

[0438] Propylene glycol monomethyl ether 80 parts by mass

[0439] 20 parts by mass of methyl acetate

[0440] additive:

[0441] Surfactant: KF-642 (trade name, polyether-modified silicone oil, manufactured by Shin-Etsu Chemical Co., Ltd.) 2 parts by mass

[0442] Microparticles: Polymer silane coupling agent coated silica (1) 10 parts by mass

[0443] Pigment compound (D): Pigment compound 1 5 parts by mass

[0444] (Formation of hard coat layer)

[0445] The hard coating forming composition prepared above was applied to the surface of the protective film not in contact with the casting tape using an extrusion coater, and dried at a constant rate drying section temperature of 50°C and a decreasing rate drying section temperature of 50°C. Then, nitrogen was purged in such a way that the oxygen concentration became 1.0 volume % or less, and an ultraviolet lamp was used at a irradiation portion illumination of 100 mW / cm 2 , so that the irradiation amount is 0.25J / cm 2 The coating layer was cured to form a hard coating layer with a film thickness of 3 μm. The obtained hard coating layer is also referred to as “AHD1”. In addition, the obtained protective film with a hard coating layer is also referred to as “protective film 31 with HD layer” hereinafter.

[0446] [2] Manufacturing of polarizers

[0447] A polyvinyl alcohol film having a thickness of 25 μm was swollen in water at 35°C. The obtained film was immersed in an aqueous solution consisting of 0.075 g of iodine, 5 g of potassium iodide and 100 g of water for 60 seconds, and further immersed in an aqueous solution consisting of 3 g of potassium iodide, 7.5 g of boric acid and 100 g of water at 45°C. The obtained film was uniaxially stretched under the conditions of a stretching temperature of 55°C and a stretching ratio of 5 times. The uniaxially stretched film was washed with water and then dried to obtain a polarizer (1) having a thickness of 12 μm.

[0448] [3] Manufacturing of retardation films

[0449] (Phase difference film 1)

[0450] A polycarbonate resin film (PC film) was produced by the following production method (melt casting film forming method).

[0451] The polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and a reflux condenser controlled at 100°C. 9,9-[4-(2-hydroxyethoxy)phenyl]fluorene (BHEPF), isosorbide (ISB), diethylene glycol (DEG), diphenyl carbonate (DPC) and magnesium acetate tetrahydrate were charged in a molar ratio of BHEPF / ISB / DEG / DPC / magnesium acetate = 0.348 / 0.490 / 0.162 / 1.005 / 1.00×10-5. The reactor was fully purged with nitrogen (oxygen concentration 0.0005 to 0.001 vol%), heated with a heat medium, and stirring was started when the internal temperature reached 100°C. 40 minutes after the start of the temperature increase, the internal temperature reached 220°C, and the pressure was controlled so as to maintain the temperature, and the pressure was reduced to 13.3 kPa in 90 minutes after reaching 220°C. The phenol vapor produced as a by-product during the polymerization reaction was introduced into a reflux condenser at 100°C, a small amount of monomer components contained in the phenol vapor was returned to the reactor, and the uncondensed phenol vapor was introduced into a condenser at 45°C for recovery.

[0452] Nitrogen was introduced into the first reactor, and after temporarily returning to atmospheric pressure, the oligomerized reaction liquid in the first reactor was transferred to the second reactor. Next, the temperature and pressure reduction in the second reactor were started, and the internal temperature reached 240°C and the pressure reached 0.2 kPa in 50 minutes. After that, polymerization was carried out until the specified stirring power was reached. At the moment when the specified power was reached, nitrogen was introduced into the reactor for re-pressurization, and the reaction liquid was extracted in the form of a tow, and granulated with a rotary cutter to obtain a polycarbonate resin A with a copolymer composition of BHEPF / ISB / DEG=34.8 / 49.0 / 16.2 [mol %]. The reduced viscosity of the polycarbonate resin A was 0.430 dL / g, and the glass transition temperature was 138°C.

[0453] After the obtained polycarbonate resin A was vacuum dried at 80°C for 5 hours, a polycarbonate resin film (PC film 1) having a thickness of 130 μm was prepared as a roll (film roll) of a long film using a film-making apparatus equipped with a single-screw extruder (manufactured by Isuzu Chemical Machinery Co., Ltd., with a screw diameter of 25 mm and a barrel setting temperature of 220°C), a T-die (width 900 mm, setting temperature: 220°C), a cooling roller (setting temperature: 120-130°C) and a winder.

[0454] The roll of the PC film 1 prepared above (film roll) is placed in a manufacturing device 80 for an obliquely stretched film (see Figure 4 , Figure 5) and extract the PC film 1. Then, the PC film 1 is passed through the preheating zone Z1 of the stretching section to heat the PC film 1 to the preheating temperature, and then, it is passed through the stretching zone Z2 and obliquely stretched at a stretching ratio of 3 times, and then, it is passed through the heat fixing zone Z3 to produce an obliquely stretched PC film 1 with a film thickness of 50μm, a width of 1500mm, and an orientation angle θ=45° (value at the center of the width). The produced obliquely stretched PC film 1 is wound to form a film roll. It should be noted that the temperature T1 (preheating temperature) of the preheating zone Z1 of the stretching section is (Tg+15)°C, the temperature T2 (stretching temperature) of the stretching zone Z2 is (Tg+11)°C, and the temperature T3 of the heat fixing zone Z3 is (Tg+9)°C. The obtained phase difference film is referred to as phase difference film 1.

[0455] (Phase difference film 2)

[0456] The retardation film 2 is a film having a structure in which the above-mentioned TAC-1 is laminated on the above-mentioned retardation film 1. The pressure-sensitive adhesive layer (A1) used in the following [5] Preparation of an organic EL display device was used to bond the retardation film 1 and TAC-1.

[0457] [4] Production of polarizing film

[0458] The layers obtained in [1] to [3] above were stacked in the combinations shown in Tables VI-1 to 3 to produce polarizers 1 to 10. It should be noted that the phase difference film and the polarizer, and the protective film and the polarizer were bonded using a completely saponified polyvinyl alcohol aqueous solution (water paste). In addition, the phase difference film 2 was stacked with the TAC-1 side facing the polarizer side. In addition, in Tables VI-1 to 3, multiple identical polarizer numbers are marked. When the polarizer numbers are the same, they are polarizers of exactly the same structure.

[0459] As a polarizing plate 11 (with a pressure-sensitive adhesive layer) of a comparative example, a polarizing film with a pressure-sensitive adhesive layer obtained by the method of Example 1 described in paragraphs 0168 to 0171 of JP-A-2017-168430 was produced. The obtained polarizing film with a pressure-sensitive adhesive layer has the following structure: pressure-sensitive adhesive layer (containing an ultraviolet absorber; Tinosorb S (trade name, manufactured by BASF Japan Co., Ltd., maximum absorption wavelength: 346 nm)) / cycloolefin polymer film / polarizer / acrylic film / pressure-sensitive adhesive layer (containing a compound equivalent to the pigment compound (D); BONASORB UA3911 (trade name, manufactured by Orient Chemical Industries, Ltd., maximum absorption wavelength: 398 nm)) / phase difference film / pressure-sensitive adhesive layer (containing a compound equivalent to the pigment compound (D); BONASORB UA3912 (trade name, manufactured by Orient Chemical Industries, Ltd., maximum absorption wavelength: 386 nm)).

[0460] [5] Fabrication of organic EL display devices

[0461] Polarizers 1 to 10 shown in Tables VI-1 to 3 were stacked with organic EL elements via the following pressure-sensitive adhesive layer (A1) to produce an organic EL display device and evaluate it. Specifically, GALAXY S10 (trade name) manufactured by SAMSUNG equipped with an organic EL panel was decomposed, the circular polarizer was peeled off from the organic EL element, and the polarizers 1 to 10 shown in Tables VI-1 to 3 were respectively laminated on the peeled surface via the pressure-sensitive adhesive layer (A1) with the hard coating side as the visible side and the phase difference film side as the organic EL element side to produce an organic EL display device.

[0462] On the other hand, the polarizing plate 11 is laminated with the pressure-sensitive adhesive layer (containing a compound corresponding to the pigment compound (D); BONASORB UA3912 (trade name, manufactured by Orient Chemical Industries, Ltd., maximum absorption wavelength: 386 nm) as the organic EL element side to produce an organic EL display device.

[0463] (Production of Pressure-Sensitive Adhesive Composition (A1))

[0464] To a monomer mixture consisting of 78 parts by mass of 2-ethylhexyl acrylate (2EHA), 18 parts by mass of N-vinyl-2-pyrrolidone (NVP), and 15 parts by mass of 2-hydroxyethyl acrylate (HEA) were added 0.035 parts by mass of 1-hydroxycyclohexyl phenyl ketone (trade name: Ilgacur 184, manufactured by BASF Japan Co., Ltd.) as a photopolymerization initiator and 0.035 parts by mass of 2,2-dimethoxy-1,2-diphenylethane-1-one (trade name: Ilgacur 651, manufactured by BASF Japan Co., Ltd.), and then irradiated with ultraviolet rays until the viscosity (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30° C.) reached about 20 Pa·s, thereby obtaining a prepolymer composition (polymerization ratio: 8%) in which part of the above monomer components were polymerized. Next, 0.15 parts by mass of hexanediol diacrylate (HDDA) and 0.3 parts by mass of a silane coupling agent (trade name: KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) were added to the prepolymer composition and mixed to obtain an acrylic pressure-sensitive adhesive composition (a).

[0465] To the obtained acrylic pressure-sensitive adhesive composition (a), 0.2 parts by mass of bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (trade name: Ilgacur 819, manufactured by BASF Japan Co., Ltd.) were added (the monomer components forming the acrylic polymer were set to 100 parts by mass), and the mixture was stirred to obtain a pressure-sensitive adhesive composition (A1).

[0466] (Production of Pressure-Sensitive Adhesive Layer (A1))

[0467] The pressure-sensitive adhesive composition (A1) was applied onto the release film so that the thickness of the pressure-sensitive adhesive layer formed was 150 μm, and then the release film was attached to the surface of the pressure-sensitive adhesive composition layer. 2 , Light intensity: 1500mJ / cm 2 , and irradiated with ultraviolet light at a peak wavelength of 350 nm to photocure the adhesive composition layer to form a pressure-sensitive adhesive layer (A1).

[0468] [evaluate]

[0469] The obtained organic EL display device was subjected to the following durability tests (1) to (3). The results are shown in Tables VI-1 to 3, respectively.

[0470] (1) High radiation durability test

[0471] The obtained organic EL display device was subjected to a 1000 W / m 2 The light of an artificial solar lighting lamp (XC-100A, manufactured by Serik Co., Ltd.) was continuously irradiated for 10 minutes, and the visibility after irradiation was evaluated. White display, black display, and image display were performed on the display device, and the reflected light when the fluorescent light was reflected from the front and at an angle of 60° was observed. The display quality at the front and at an angle of 60° was evaluated based on the following criteria.

[0472] (Evaluation Criteria)

[0473] A: No visual recognition of coloring at all

[0474] B: Although the color difference is visually recognizable, it is very small

[0475] C: The color tone is different, but the reflected light is small, so there is no problem in use.

[0476] D: The visual color tone is poor and there is a lot of reflected light, which is unacceptable

[0477] (2) Low-radiation durability test

[0478] The obtained organic EL display device was subjected to a 100 W / m 2 The light of an artificial solar lighting lamp (XC-100A, manufactured by Serik Co., Ltd.) was continuously irradiated for 24 hours, and the visibility after irradiation was evaluated. A grid image with a spacing of 1 mm was displayed on a display device, and the shape of the grid was observed from the front direction (normal direction relative to the display surface). The evaluation was performed based on the following evaluation criteria.

[0479] (Evaluation Criteria)

[0480] A: The grid is clearly visually identifiable

[0481] B: The color difference of the grid is very slightly visually recognized

[0482] C: The four corners of the grid are blurred and can be recognized visually, but there is no problem in use

[0483] D: Blurred vision to the four sides of the grid, unacceptable

[0484] (3) Weathering test

[0485] The obtained organic EL display device was continuously irradiated with a xenon lamp (60 W / m 2 The protective film of the display device and the interface of the polarizer after irradiation were peeled off, and the absorbance of the protective film formed with the hard coating layer before irradiation (0 hour) and after irradiation was measured by a spectrophotometer, and the pigment residual rate was measured according to the following formula (3).

[0486] Pigment residual rate (%) = {(A1) / (A0)}×100 Formula (3)

[0487] [Where A0 is the absorbance before xenon lamp irradiation, and A1 is the absorbance after xenon lamp irradiation.]

[0488] In addition, "absorbance" indicates the absorbance at the maximum absorption wavelength of each compound, and the higher the residual rate of the pigment, the more difficult the compound is to be decomposed by light, indicating higher weather resistance. Weather resistance was evaluated according to the following criteria.

[0489] (Evaluation Criteria)

[0490] A: Pigment residual rate is more than 65%

[0491] B: Pigment residual rate is 40% or more and less than 65%

[0492] C: Pigment residual rate is 10% or more and less than 40%

[0493] D: Pigment residual rate is less than 10%

[0494] In Tables VI-1 to 3, the composition of the polarizer and the composition number of Table I that the composition conforms to are shown together with the evaluation results. In Tables VI-1 to 3, in the columns of hard coat, protective film, and phase difference film, when the number and the pigment compound (D) or the ultraviolet absorber are contained, the type thereof is recorded. In the case of not containing the pigment compound (D) or the ultraviolet absorber, it is recorded as "-". Furthermore, with respect to the protective film, the type of resin is recorded. In Tables VI-1 to 3, "UA3912" means BONASORBUA3912. "TN928" means チヌビン 928. "COP", "CE" and "Ac" respectively represent cycloolefin resin, cellulose ester resin and acrylic resin.

[0495]

[0496]

[0497]

[0498] As shown in Tables VI-1 to 3, when the layer containing the pigment compound (D) is arranged closer to the visible side than the layer containing the ultraviolet absorber, it is confirmed that the visibility of the display device after irradiation with artificial sunlight is improved regardless of the type of the pigment compound (D), the ultraviolet absorber, and the resin of the protective film. It is speculated that this is because, by arranging in a specific order, the heat generated from the pigment compound (D) will not be hindered by the heat generation of the layer containing the ultraviolet absorber and will be released from the surface of the display device to the outside, which can suppress the change of the in-plane phase difference of the phase difference film.

[0499] When the hard coat layer contains the pigment compound (D) and the protective film contains the ultraviolet absorber, that is, in the case of configuration 1 and configuration 4, it was confirmed that the visibility after irradiation with artificial sunlight was further improved. It is speculated that the reason is that by arranging in a specific order, the heat generated from the pigment compound (D) is not prevented from being emitted to the outside from the surface of the display device by the heat generation of the layer containing the ultraviolet absorber, and the shrinkage of the polarizer can be suppressed, and by arranging the layer containing the ultraviolet absorber at a position closer to the visible side than the polarizer, the degradation of the polarizer caused by external light can be suppressed.

[0500] When a dicyanomethene compound (compound (1)-1 or compound (1)-2) is used as the dye compound (D), it is confirmed that weather resistance is improved. This is presumably because the dicyano group lowers its energy level and increases its oxidation potential, making it less likely to be oxidized.

[0501] Industrial Applicability

[0502] In the present invention, a polarizing plate can be provided, which, when used in a display device, particularly an organic EL display device, can protect a display element from the influence of external light and can suppress the degradation of a phase difference film and a polarizer caused by heat. In addition, by using the polarizing plate, an organic EL display device can be provided in which the quality degradation during long-term use is suppressed.

[0503] Description of Reference Numerals

[0504] 10A, 10B Polarizer

[0505] 1 Hard coating

[0506] 2. Protective film

[0507] 3 Polarizer

[0508] 4 Retardation Film

[0509] 5. Pressure-sensitive adhesive layer

[0510] 20 Organic EL display device

[0511] 11 Organic EL components

[0512] 80 Manufacturing device for oblique stretched film

[0513] 81 Film release unit

[0514] 82, 86 Conveying direction change unit

[0515] 83, 85 guide roller

[0516] 84 Stretching Department

[0517] 87 Film winding unit

Claims

1. A polarizing plate, which is a polarizing plate having a hard coating layer, a protective film, a polarizer and a phase difference film in order from the visible side, wherein: The hard coating layer contains a pigment compound having a maximum absorption wavelength in a range of more than 380 nm and less than 430 nm in an absorption spectrum in a wavelength range of 300 to 460 nm, The protective film contains an ultraviolet absorber, The layer containing the pigment compound is located on the visible side relative to the layer containing the ultraviolet absorber.

2. The polarizing plate according to claim 1, wherein The pigment compound includes a compound having a structure represented by the following general formula (1): General formula (1) In the general formula (1), Z represents a heteroaryl group containing at least one nitrogen atom as a heteroatom, and Z may have a substituent.

3. The polarizing plate according to claim 1 or 2, wherein: The retardation film is provided with a pressure-sensitive adhesive layer on the side opposite to the visible side.

4. An organic electroluminescent display device, comprising the polarizing plate according to any one of claims 1 to 3 on a visible side.

Citation Information

Patent Citations

  • Production of mixed fatty acid ester of cellulose

    JP1998045804A

  • Ultraviolet-ray absorbing fine particles and their use

    JP1999116240A

  • Polarizing plate and its production

    JP2000338329A

  • Polycarbonate optical retardation film and method for manufacturing the same

    JP2003167121A

  • Optical film and polarizing plate

    JP2005121813A