A non-uniformly loaded metal / K + Doped carbon nitride nanorods and preparation method and application thereof
By non-uniformly loading metal/K+ doped C3N4 nanorod photocatalysts, the problem of low carrier separation efficiency of g-C3N4 photocatalyst is solved, and efficient oxidation of organic pollutants and hydrogenation-reduction dehalogenation of halogenated organic compounds are achieved, demonstrating Excellent photocatalytic performance.
Patent Information
- Application Number
- CN202210787902.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-04
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-07-04
AI Technical Summary
The existing graphite phase carbon nitride (g-C3N4) photocatalyst has small specific surface area, weak light absorption and poor carrier separation efficiency, resulting in poor photocatalytic performance and unable to meet the needs of practical applications.
A non-uniformly loaded metal/K+ doped C3N4 nanorod photocatalyst is used. Through K+ doping and non-uniformly distributed metal nanoparticle deposition, an efficient separation structure of photogenerated electrons and holes is formed to improve the photocatalytic performance.
The carrier separation efficiency and photocatalytic performance of the photocatalyst are significantly improved, and it can efficiently oxidize and degrade organic pollutants and hydrogenate, reduce, and dehalogenate halogenated organic pollutants, showing good application prospects.
Smart Images

Figure CN115155638B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of environmental chemistry and catalytic chemistry, and specifically relates to a non-uniformly loaded metal / K + Preparation of doped C3N4 nanorod photocatalysts and their applications in photocatalytic oxidation degradation of organic pollutants and photocatalytic hydrogenation reduction dehalogenation degradation of halogenated organic pollutants. Background Art
[0002] The photocatalytic process can generate oxidative holes and reductive electrons. The photogenerated holes can react with water to produce hydroxyl radicals. Therefore, the photocatalytic method can be applied to both oxidation reactions and reduction reactions, and has shown good application prospects in environmental purification, energy and chemical conversion and synthesis.
[0003] Graphitic carbon nitride (g-C3N4) has the advantages of good stability, simple preparation method and suitable band gap (2.7eV), and has attracted great attention as a photocatalyst. However, g-C3N4 prepared by conventional methods often has poor photocatalytic performance due to its small specific surface area, weak light absorption or poor carrier separation efficiency, and cannot meet the needs of practical applications. Therefore, modifying it to significantly enhance its photocatalytic performance has always been a research hotspot.
[0004] Common modification methods include increasing specific surface area, controlling morphology, constructing heterojunction structures with other photocatalysts, incorporating heteroatoms and loading metals, etc. Among them, alkali metal doping and noble metal deposition are very effective strategies. Zhang et al. prepared KCl by heat treating amorphous C3N4 materials with KCl as a structural inducing agent. + Gradient doped C3N4. + A built-in electric field is formed in the doped C3N4, which promotes the rapid separation of the generated carriers, making its photocatalytic hydrogen production rate 34 times higher than that of amorphous C3N4 (ACS Catalysis 2021, 11 (12), 6995-7005). Common precious metals such as gold (Au), silver (Ag), palladium (Pd), platinum (Pt), etc., when their nanoparticles are deposited on g-C3N4, will form a Schottky junction with g-C3N4. The difference in the Fermi energy levels of the two and the plasma resonance effect of the precious metals jointly promote the rapid separation of photogenerated carriers. At the same time, the precious metal particles can also trigger reactions as reaction active centers, greatly accelerating the photocatalytic reaction. For example, Xiong et al. deposited single-atom Pt on g-C3N4. The hydrogen production rate of this material is 1340 times that of g-C3N4 without Pt deposition. In the single-atom Pt deposited g-C3N4, Pt combines with the surrounding nitrogen atoms to form Pt 2+ -N bond. When the catalyst is excited by light, the generated electrons are injected, resulting in Pt 2+ Reduction to form Pt0 , and accompanied by Pt 2+ -N bond breaking and -C=N bond formation, resulting in the directional migration of electrons and holes to Pt and g-C3N4, respectively, to achieve efficient separation of photogenerated electrons and holes (Angewandte Chemie, 2020, 132(15), 6283-6288). Lei et al. prepared Pd-loaded g-C3N4 (Pd / g-C3N4) by chemical reduction, and applied it to the reduction degradation of BDE47 under visible light (wavelength greater than 400nm). It was found that the reaction of 120min can lead to complete debromination of BDE47 (Applied Catalysis B: Environmental, 2020, 261, 118236). However, it should be pointed out that in the currently reported metal-modified C3N4 materials, the metal loading or deposition is usually evenly distributed on C3N4. Summary of the invention
[0005] Aiming at the shortcomings of poor carrier separation efficiency and poor photocatalytic performance of g-C3N4 photocatalyst, the present invention provides a non-uniformly loaded metal / K + Doped C3N4 nanorod photocatalyst. This non-uniform loading of metal / K + Doped C3N4 nanorod photocatalyst has the following characteristics: (1) K + Doped C3N4 into nanorods; (2) Nanometal particles in a single K + The distribution of doped C3N4 nanorods on the surface is extremely uneven and clusters; (3) The metal nanoparticles at different K + The distribution on the doped C3N4 nanorods is also extremely uneven.
[0006] The purpose of the present invention is not only to provide the above-mentioned non-uniform loading metal / K + The invention discloses a preparation method of a doped C3N4 nanorod photocatalyst and also provides the application of the catalyst in the oxidation degradation of organic pollutants and the catalytic hydrogenation reduction dehalogenation reaction of halogenated organic pollutants.
[0007] The non-uniformly loaded metal / K + Doped C3N4 nanorods were prepared in three steps:
[0008] (1) Accurately weigh a certain amount of carbon-nitrogen precursor, place it in a crucible with a lid, heat it to 500° C. in a muffle furnace connected to air, maintain it for 4 h, and then cool it naturally to room temperature to obtain an intermediate product A.
[0009] (2) Weigh a certain amount of intermediate product A and KCl / LiCl composite salt (referring to a mixture of KCl and LiCl), grind and mix them in a mortar, transfer them to a covered porcelain boat, put them in a tube furnace, introduce Ar gas to exhaust the air in the tube furnace, heat them to 550°C at 10°C / min after 30-60 minutes, keep them for 4 hours, and then cool them naturally to room temperature; disperse the product in deionized water, separate them by filtration through a filter membrane, wash them with water several times, collect the product, and dry it in a vacuum drying oven at 60°C for 8-12 hours to obtain K + Doped C3N4 nanorods.
[0010] (3) Accurately weigh a certain amount of K + Doped C3N4 nanorods were dispersed in 50 mL of deionized water. After 5 min of ultrasonic dispersion, the prepared aqueous solution of metal ions was added and stirred at a constant temperature of 25 ° C (speed 100-150 rpm) for 30 min. Then, under the condition of vigorous stirring (speed 400-600 rpm), NaBH4 aqueous solution was added dropwise. After the addition, vigorous stirring was continued for 30 min, and the suspension was filtered through a filter membrane for separation. After the solid and liquid were completely separated, 5 mL of sulfuric acid aqueous solution (0.1 mol·L -1 ) and 50 mL of deionized water to wash the obtained solid product; finally, the solid product was transferred to a vacuum drying oven at 60° C. and dried for 8-12 h to obtain a non-uniformly loaded metal / K + Doped C3N4 nanorods.
[0011] Preferably, the carbon-nitrogen precursor in step (1) is one or more of melamine, dicyandiamide and urea.
[0012] Preferably, in step (2), the mass ratio of the intermediate product A to the KCl / LiCl composite salt is 1:5 to 1:25.
[0013] Preferably, the mass percentage of KCl in the KCl / LiCl composite salt in step (2) is 30% to 60%.
[0014] Preferably, the flow rate of Ar in step (2) is 40 to 80 cc / min.
[0015] Preferably, the metal ion described in step (3) is Pd 2+ , Pt 4+ , Pt 2+ , Ag + , Au 3+ , Rh 3+ , Ru 3+ , Cu 2+ , Ni 2+ One of the following; the mass of the metal ion is K +The doped C3N4 nanorods account for 0.1% to 2% of their mass.
[0016] Preferably, the molar amount of NaBH4 added in step (3) is 1 to 10 times the molar amount of the metal ion.
[0017] The non-uniformly loaded metal / K + The method for photocatalytic oxidation of organic pollutants in water by doping C3N4 nanorods is carried out as follows: adding non-uniformly loaded metal / K + Doped C3N4 nanorods are used as catalysts to oxidatively degrade organic pollutants in water at room temperature under the conditions of light irradiation and the introduction of air or oxygen.
[0018] The non-uniformly loaded metal / K + The method for photocatalytic hydrogenation reduction degradation of halogenated organic pollutants in water by doping C3N4 nanorods is carried out as follows: adding non-uniformly loaded metal / K + C3N4 nanorods are doped as catalysts and a certain amount of organic alcohol is added (the volume ratio of organic alcohol to water is 5:95 to 95:5, and the two are miscible). Under the conditions of light, deoxygenation and room temperature, the halogenated organic pollutants in the aqueous solution are reduced, degraded and dehalogenated.
[0019] The non-uniformly loaded metal / K + The light used by the doped C3N4 nanorod photocatalyst in the oxidative degradation of organic pollutants and the catalytic hydrogenation reduction dehalogenation reaction of halogenated organic pollutants can be ultraviolet light, visible light or sunlight.
[0020] Compared with the existing photocatalysts, the non-uniformly loaded metal / K + Doped C3N4 nanorods have the following advantages:
[0021] (1) Metals are concentrated in one K + A region where photogenerated electrons are concentrated can be formed on a certain area of the doped C3N4 nanorods, which is beneficial to the separation of photogenerated carriers;
[0022] (2) Metal is concentrated in the K + Doping C3N4 nanorods will result in this part of K + The doped C3N4 nanorods become the concentrated distribution area of photogenerated electrons, which is different from the K + The doped C3N4 nanorods form a heterojunction structure, which further facilitates the separation of photogenerated carriers;
[0023] (3) The spatial separation of photogenerated carriers can not only improve the separation efficiency of photogenerated carriers, thereby increasing the yield of photogenerated holes and electrons, but also provide different reaction areas for subsequent oxidation-reduction reactions, which is more conducive to the oxidation and reduction reactions.
[0024] The non-uniformly loaded metal / K + Doped C3N4 nanorod photocatalysts show good photocatalytic performance under ultraviolet light, visible light and even sunlight, and have good application prospects in the field of pollution control. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 :(a) Pd / g-C3N4 and (b) Pd / K + Transmission electron microscopy image of doped C3N4 nanorods.
[0026] Figure 2 :K + Doped C3N4 nanorods, Pd / K + X-ray diffraction spectra of doped C3N4 nanorods, g-C3N4 and Pd / g-C3N4.
[0027] Figure 3 :K + Doped C3N4 nanorods, Pd / K + X-ray photoelectron spectra of doped C3N4 nanorods, g-C3N4 and Pd / g-C3N4: (a) C1s, (b) N1s, (c) K2p and (d) Pd3d.
[0028] Figure 4 : Reduction degradation curves of p-bromophenol in different photocatalytic systems.
[0029] Figure 5 : p-Bromophenol in Pd / K + Reduction debromination curve in the doped C3N4 nanorod photocatalytic system.
[0030] Figure 6 :BDE47 in Pd / K + Reductive degradation debromination curve in the doped C3N4 nanorod photocatalytic system. DETAILED DESCRIPTION
[0031] The applicant will further describe the present invention in detail below with reference to the examples and drawings, but the protection scope of the present invention is not limited to these examples. The experimental methods used in the following examples are conventional methods unless otherwise specified; the materials, reagents, etc. used are all commercially available unless otherwise specified.
[0032] Example 1: Non-uniform loading Pd / K +Preparation of doped C3N4 nanorods. The specific preparation process is as follows:
[0033] (1) Using a 50 mL crucible, accurately weigh 5 g of melamine and place it in a covered crucible, heat it to 500° C. in a muffle furnace connected to air, maintain it for 4 hours, and then naturally cool it to room temperature to obtain an intermediate product A.
[0034] (2) Weigh 0.6 g of the intermediate product A prepared in step (1), 3.3 g of KCl and 2.7 g of LiCl, grind and mix them in a mortar, transfer them to a covered porcelain boat, put them in a tube furnace, introduce 60 cc / min of Ar gas to exhaust the air in the tube furnace, and after 30 min, heat to 550° C. at 10° C. / min, maintain for 4 h, and then cool naturally to room temperature; disperse the product in deionized water, separate it by filtration through a filter membrane, wash it with water three times (10 mL each time), collect the product, and dry it in a vacuum drying oven at 60° C. for 12 h to obtain K + Doped C3N4 nanorods.
[0035] (3) Accurately weigh 0.1 g of K prepared in step (2) + Doped C3N4 nanorods were dispersed in 50 mL of water. After 5 min of ultrasonic dispersion, 2 mL of Pd 2+ Concentration 1g·L -1 The PdCl2 aqueous solution was stirred at 25°C (120 rpm) for 30 min, and then 2 mL of 2 g·L -1 After adding the NaBH4 aqueous solution, continue to stir vigorously for 30 minutes, and then filter the mixture through a 0.45μm filter membrane. After the solid and liquid are completely separated, add 5mL of sulfuric acid aqueous solution (0.1mol·L -1 ) and 50 mL of deionized water to wash the obtained solid product. Finally, the solid product was transferred to a vacuum drying oven at 60 ° C for 8 h to obtain a non-uniformly loaded Pd / K + C3N4 nanorods were doped. In addition, AgNO3 and H2PtCl6·6H2O were used as Ag + and Pt 4+ Source, following the same steps and parameters (including volume, metal ion concentration, etc.) as above, Ag / K + Doped C3N4 nanorods and Pt / K + Doped C3N4 nanorods.
[0036] Comparative Example 1: Pd-loaded g-C3N4 (Pd / g-C3N4) was prepared according to the following steps:
[0037] (1) Using a 50 mL crucible, accurately weigh 5 g of melamine and place it in a covered crucible, heat it to 500° C. in a muffle furnace connected to air, maintain it for 4 hours, and then naturally cool it to room temperature to obtain an intermediate product A.
[0038] (2) Weigh 1 g of the intermediate product A prepared in step (1), transfer it to a covered porcelain boat, put it into a tube furnace, introduce 60 cc / min Ar gas to exhaust the air in the tube furnace, and after 30 minutes, heat it to 550°C at 10°C / min, maintain it for 4 hours, and then cool it naturally to room temperature. The obtained product is washed with water for multiple times, filtered and separated, and then dried in a vacuum drying oven at 60°C for 12 hours. The final product is g-C3N4.
[0039] (3) Accurately weigh 0.1 g of g-C3N4 prepared in step (2) and disperse it in 50 mL of water. After 5 min of ultrasonic dispersion, add 2 mL of Pd 2+ Concentration 1g·L -1 PdCl2 aqueous solution was stirred at 25℃ (speed 120 rpm) for 30 min. Under vigorous stirring (speed 500 rpm), 2 mL 2 g·L -1 After adding the NaBH4 aqueous solution, continue to stir vigorously for 30 minutes, and then filter the mixture through a 0.45μm filter membrane. After the solid and liquid are completely separated, add 5mL of sulfuric acid aqueous solution (0.1mol·L -1 ) and 50 mL of deionized water to wash the obtained solid product. Finally, the solid product was transferred to a vacuum drying oven at 60° C. and dried for 8 h to obtain Pd / g-C3N4.
[0040] The non-uniformly loaded Pd / K prepared in Example 1 was examined by transmission electron microscopy (TEM). + The Pd / g-C3N4 prepared in the doped C3N4 nanorods and comparative example 1 were characterized. Figure 1 . Figure 1 (a) shows that the Pd / g-C3N4 sample presents a typical nano-layered stacking structure, and the nano-Pd particles are evenly distributed on the g-C3N4. Figure 1 The sample of Example 1 shown in (b) is obviously different in morphology. Its main features are as follows: K + The doped C3N4 appears as nanorods with diameters of 30-70nm and varying lengths; the distribution and deposition of Pd particles on the nanorods are uneven, and the deposited Pd particles have different morphologies, showing three different forms of Pd clusters marked in the figure: small-sized Pd species in region ①; large-sized clusters that grow further in region ②, and large-scale clusters in region ③. Figure 1 The results in FIG. 1 show that the non-uniform load Pd / K provided by the present invention+ Doped C3N4 nanorods have novel morphology and structure.
[0041] The non-uniformly loaded Pd / K prepared in Example 1 was analyzed by X-ray diffractometer. + The Pd / g-C3N4 prepared in the doped C3N4 nanorods and comparative example 1 were characterized. Figure 2 .from Figure 2 It can be seen that K + Doped C3N4 nanorods (prepared in step (2) of Example 1), Pd / K + The four samples of doped C3N4 nanorods, g-C3N4 (prepared in step (2) of comparative example 1) and Pd / g-C3N4 all showed two narrow diffraction peaks, corresponding to the (100) and (002) crystal planes of C3N4, respectively. + The X-ray diffraction peaks of doped C3N4 nanorods and g-C3N4 did not change significantly, indicating that the loaded Pd was mainly deposited on the K + On the surface of doped C3N4 nanorods and g-C3N4, K did not enter the C3N4 crystal structure. However, compared with g-C3N4 and Pd / g-C3N4, + Doped C3N4 nanorods and Pd / K + The diffraction peak of the doped C3N4 nanorods corresponding to the (002) plane in the C3N4 heterocyclic plane shifted from 27.5° to 28.2°, and the diffraction peak attributable to the (100) plane shifted from 13.1° to 8.1°, indicating that K + Doping changes the crystal structure of g-C3N4, reducing its interlayer spacing from 0.323nm to 0.316nm, which is more conducive to the transfer and separation of carriers between layers.
[0042] The non-uniformly loaded Pd / K prepared in Example 1 was analyzed by X-ray photoelectron spectroscopy. + The Pd / g-C3N4 prepared in the doped C3N4 nanorods and comparative example 1 were characterized. Figure 3 .from Figure 3 It can be seen that K + Doped C3N4 nanorods (prepared in step (2) of Example 1), Pd / K + C1s and N1s were detected in all four samples of doped C3N4 nanorods, g-C3N4 (prepared in step (2) of Comparative Example 1) and Pd / g-C3N4. Figure 3 In (a), K + Doped C3N4 nanorods and Pd / K + The peak at 286.7 eV of the C3N4 nanorod-doped sample is attributed to K +Doping leads to the introduction of -C≡N groups, but this peak is not detected in the g-C3N4 and Pd / g-C3N4 samples. Figure 3 (c) shows that in K + Doped C3N4 nanorods and Pd / K + An obvious K2p signal was detected in the C3N4 nanorod-doped sample, but this peak was not detected in the g-C3N4 and Pd / g-C3N4 samples. Figure 2 ), these results show that in K + Doped C3N4 nanorods and Pd / K + In the C3N4 nanorod-doped samples, K was successfully introduced into the crystal structure of C3N4. Figure 3 As shown in (d), the peaks at 334-345 eV are attributed to Pd 3d orbital electrons. The peak at 335.6 eV is attributed to Pd 0 , the peak at 337.9 eV is caused by Pd n+ Compared with Pd / g-C3N4 sample, Pd / K + The Pd-doped C3N4 nanorods 0 The peak of Pd / K + The electron cloud density of Pd species deposited on the doped C3N4 nanorod sample is higher. Further analysis shows that the Pd in the Pd / g-C3N4 sample 0 and Pd n+ The ratio of Pd / K is 51.62%:48.38%, while + In the C3N4 nanorods doped samples, their ratio is 48.35%:51.65%. n+ Pd generated by load 0 Oxidized by air during storage. Combined with the results of TEM ( Figure 1 ), this result shows that Pd / K + The Pd clusters loaded on the doped C3N4 nanorod samples have higher chemical reactivity and are more easily oxidized by air during storage, thus producing a higher proportion of high-valent Pd species. The above characterization results fully demonstrate that the sample prepared in Example 1 is a non-uniformly loaded Pd / K + Doped C3N4 nanorods.
[0043] Example 2: Taking phenol as the representative organic pollutant, the Pd / K + Doped C3N4 nanorods, Pt / K + Doped C3N4 nanorods, Ag / K +Pd / g-C3N4 prepared by doping C3N4 nanorods and comparative example 1 was used as a photocatalyst to photocatalytically oxidize and degrade organic pollutants in water. -1 25 mg of each of the four catalysts was added to the aqueous solution of phenol. At this time, the dosage of the photocatalyst was 0.5 g·L -1 The initial pH value of the reaction solution was 11. The reaction temperature was controlled at 25°C using a water bath. The xenon lamp was turned on to oxidize and degrade the phenol in the aqueous solution. The results are shown in Table 1. + Doped C3N4 nanorods, Pt / K + Doped C3N4 nanorods, Ag / K + When C3N4 nanorods were doped as photocatalysts, the oxidation degradation rates of phenol reached 100%, 88% and 85% after 45 minutes of reaction. In contrast, when Pd / g-C3N4 was used as photocatalyst under the same reaction conditions, the oxidation degradation rate of phenol was only 10% after 45 minutes of reaction. The comparison results show that the non-uniformly loaded metal / K + Doped C3N4 nanorods have better performance in photocatalytic oxidation degradation of organic pollutants.
[0044] Table 1: Non-uniform loading of metal / K + Effect of doped C3N4 nanorods on photocatalytic oxidation of phenol
[0045]
[0046] Example 3: Taking p-bromophenol as the representative of halogenated organic pollutants, the Pd / K + Doped C3N4 nanorods were used as photocatalysts to photocatalytically reduce and degrade halogenated organic pollutants in water. 10 mg Pd / K + C3N4 nanorods were doped as catalysts, and methanol was added to a total volume of 50 mL. At this time, the initial concentration of p-bromophenol was 25 μmol·L -1 , Pd / K + The dosage of doped C3N4 nanorods was 0.2 g·L -1 , the volume ratio of methanol to water is about 3:7. The reaction temperature is controlled at 25°C using a water bath. High-purity N2 gas is introduced into the above-mentioned mixed solution to remove dissolved oxygen in the water. After N2 gas is introduced for 30 minutes, the xenon lamp light source is turned on, and the light below 420nm is filtered out with a 420nm filter. Under visible light irradiation, the p-bromophenol in the solution is reduced, degraded and debrominated.
[0047] Figure 4 K prepared in Example 1 and Comparative Example 1 +Doped C3N4 nanorods, Pd / g-C3N4 and non-uniformly loaded Pd / K + The doped C3N4 nanorods were used as photocatalysts to reduce and degrade 4-bromophenol. Figure 4 As shown, using K + Doped C3N4 nanorods and Pd / g-C3N4 as photocatalysts, under deoxygenation and light conditions, the degradation of bromophenol was not significant (degradation rate was less than 5%) after 20 min of reaction. However, when the photocatalyst was replaced by non-uniformly loaded Pd / K + When doped with C3N4 nanorods, p-bromophenol can be completely degraded within 10 min. The comparison results show that the non-uniform loading of Pd / K + Doped C3N4 nanorods have better photocatalytic performance, and it also shows that K + Doped C3N4 nanorods and deposited Pd species are non-uniformly loaded with Pd / K + Two essential conditions for the high photocatalytic performance of doped C3N4 nanorods.
[0048] Figure 5 The non-uniformly loaded Pd / K prepared in Example 1 + The debromination effect of doped C3N4 nanorods as photocatalysts in the photocatalytic reduction degradation of bromophenol. The results show that the non-uniform loading of Pd / K + Doped C3N4 nanorods as photocatalysts, under visible light, the concentration of bromide ions increased rapidly with the degradation of p-bromophenol. After 10 min of reaction, p-bromophenol was completely degraded, and the bromide ion concentration reached 24.3 μmol·L -1 When the reaction time was extended to 20 min, the bromide ion concentration reached 25 μmol·L -1 , achieving complete debromination degradation of p-bromophenol.
[0049] Table 2 shows the non-uniform loading of Pd / K prepared in Example 1 + Doped C3N4 nanorods as photocatalysts, according to Example 3, the degradation and debromination effects of different brominated phenols were investigated by photocatalytic reduction. As shown in Table 2, the non-uniformly loaded Pd / K + Under visible light illumination, the degradation rate and debromination rate of the brominated phenol investigated by the doped C3N4 nanorod photocatalyst were both 100% in a relatively short period of time, indicating that the photocatalyst provided by the present invention has good application prospects in the efficient degradation and dehalogenation of halogenated organic matter.
[0050] Table 2: Halogenated organic compounds at Pd / K + Degradation and dehalogenation in visible light photocatalytic system of doped C3N4 nanorods
[0051]
[0052] Example 4: Taking BDE47 (tetrabromodiphenyl ether), which is more difficult to degrade, as a representative of halogenated organic pollutants, the Pd / K prepared in Example 1 was used to + Doped C3N4 nanorods were used as photocatalysts to photocatalytically reduce and degrade halogenated organic pollutants in water. 10 mg Pd / K + Doped C3N4 nanorods as photocatalysts. At this time, the initial concentration of BDE47 was 20 mg·L -1 , Pd / K + The dosage of doped C3N4 nanorods was 0.2 g·L -1 , the volume ratio of methanol to water is 7:3. The reaction temperature is controlled at 25°C using a water bath. High-purity Ar gas is introduced into the above-mentioned mixed solution to remove dissolved oxygen in the water. After passing Ar gas for 30 minutes, the xenon lamp light source is turned on, and the light below 420nm is filtered out with a 420nm filter. Under visible light irradiation, BDE47 in the solution is reduced, degraded and debrominated. The results are as follows Figure 6 As shown. Within 30 minutes, the degradation rate of BDE47 reached more than 98%, and the debromination rate reached more than 98%. According to the analysis of liquid chromatography-mass spectrometry, after 30 minutes of reaction, the debromination products were mainly diphenyl ether and benzofuran.
[0053] Based on the above brominated pollutant degradation and debromination experimental results, the novel structure of the non-uniformly loaded Pd / K + Doped C3N4 nanorod photocatalyst has the advantages of short reaction time, fast degradation rate and high dehalogenation efficiency in the application of photocatalytic reduction dehalogenation, and shows great application prospects in the treatment of halogenated organic matter.
[0054] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A non-uniformly loaded metal Pd / K for photocatalytic reduction and degradation of halogenated organic pollutants in water + Doped C 3 N 4 A method for preparing a nanorod photocatalyst, the method comprising the following three steps composition: (1) Weigh a certain amount of carbon-nitrogen precursor, place it in a covered crucible, heat it to 500 °C in a muffle furnace connected to air, maintain it for 4 h, and then cool it naturally to room temperature to obtain an intermediate product A; (2) Weigh a certain amount of the intermediate product A prepared in step (1) and KCl / LiCl composite salt, wherein the KCl / LiCl composite salt is a mixture of KCl and LiCl, grind and mix them, transfer them to a porcelain boat with a lid, put them into a tube furnace, introduce Ar gas to exhaust the air in the tube furnace, heat them to 550°C at 10°C / min, maintain for 4 h, and then naturally cool them to room temperature. Disperse the product in deionized water, separate it by filtration through a filter membrane, wash it with water several times, collect the product, and dry it in a vacuum drying oven at 60°C for 8-12 h to obtain K + Doped C 3 N 4 Nanorods; (3) Weigh a certain amount of K prepared in step (2) + Doped C 3 N 4 Nanorods were dispersed in deionized water and then ultrasonically dispersed. 2+ The aqueous solution of ions was stirred at 100-150 rpm for 30 min at a constant temperature of 25°C, and then NaBH was added dropwise under vigorous stirring at 400-600 rpm. 4 After adding the aqueous solution, continue to stir vigorously for 30 minutes, and then filter the suspension through a filter membrane to separate it; after the solid and liquid are completely separated, add 0.1 mol·L -1 The solid product was washed with sulfuric acid aqueous solution and deionized water; finally, the solid product was transferred to a vacuum drying oven and dried at 60 °C for 8-12 h to obtain a non-uniformly loaded metal Pd / K + Doped C 3 N 4 Nanorods; In step (3), Pd 2+ The mass of the ion is K + Doped C 3 N 4 0.1% ~ 2% of the mass of the nanorods.
2. The preparation method according to claim 1, Features: The carbon-nitrogen precursor in step (1) is one or more of melamine, dicyandiamide and urea.
3. The preparation method according to claim 1, Features: In step (2), the mass ratio of the intermediate product A to the KCl / LiCl composite salt is 1:5 to 1:
25.
4. The preparation method according to claim 1, Features: The mass percentage of KCl in the KCl / LiCl composite salt in step (2) is 30% to 60%.
5. The preparation method according to claim 1, Features: In step (2), the flow rate of Ar gas is 40 to 80 cc / min; the time of passing Ar gas is 30 to 60 min.
6. The preparation method according to claim 1, Features: In step (3), NaBH 4 The molar amount of Pd added is 2+ 1 to 10 times the molar amount of the ion.
7. The non-uniformly loaded metal Pd / K prepared by the preparation method according to any one of claims 1 to 6 + Doped C 3 N 4 Method for photocatalytic reduction and degradation of halogenated organic pollutants in water by nanorod photocatalysts, It is characterized in that Adding the heterogeneously loaded metal Pd / K + Doped C 3 N 4 Nanorods are used as photocatalysts, and a certain amount of organic alcohol is added so that the volume ratio of organic alcohol to water is 5:95 ~ 95:
5. Under the conditions of light, deoxygenation and room temperature, halogenated organic pollutants in the aqueous solution are reduced, degraded and dehalogenated.
8. The method according to claim 7, Features: The light source of the illumination is ultraviolet light, visible light or sunlight.