Semiconductor-on-insulator substrate and method for manufacturing the same

By using a carrier sheet and trench to fill the semiconductor layer in the insulator semiconductor structure, the problems of high cost of insulator buried layer process and introduction of impurities are solved, and efficient manufacturing of semiconductor substrates on insulators are achieved, and device performance is improved.

CN115188704BActive Publication Date: 2024-11-12WUHAN XINXIN SEMICON MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210818307.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-12
Publication Date
2024-11-12
Estimated Expiration
2042-07-12

AI Technical Summary

Technical Problem

The insulating buried layer in the existing semiconductor structure on insulators has high cost and complex processes, and is easy to introduce oxygen and hydrogen impurities, resulting in reduced device performance.

Method used

The carrier is used to form an insulating dielectric layer, the trench fills the semiconductor layer, and the insulating dielectric layer and the semiconductor layer are bonded to the insulating buried layer, removing the carrier, avoiding oxygen injection oxidation and intelligent peeling technology, reducing process difficulty and cost , while avoiding the existence of oxygen impurities and hydrogen impurities.

Benefits of technology

While realizing the shallow trench isolation structure and active region of the semiconductor substrate on the insulator, it reduces process costs and difficulty, improves device performance, and avoids the existence of oxygen impurities and hydrogen impurities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115188704B_ABST
    Figure CN115188704B_ABST
Patent Text Reader

Abstract

The present invention provides a semiconductor-on-insulator substrate and a manufacturing method thereof, comprising: providing a carrier sheet, on which an insulating dielectric layer is formed; forming a groove in the insulating dielectric layer, wherein the groove exposes the surface of the carrier sheet; forming a semiconductor layer to fill the groove; providing a lower substrate and an insulating buried layer, wherein the insulating buried layer is formed on the lower substrate; bonding the insulating dielectric layer and the semiconductor layer to the insulating buried layer on a side away from the carrier sheet; and removing the carrier sheet. The technical solution of the present invention reduces the process difficulty and cost, and can avoid the presence of oxygen impurities and hydrogen impurities in the semiconductor-on-insulator substrate, thereby improving the device performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor integrated circuit manufacturing, and in particular to a semiconductor-on-insulator substrate and a manufacturing method thereof. Background Art

[0002] The semiconductor on insulator (SOI) process refers to the introduction of an insulating buried layer between the upper semiconductor layer and the lower substrate, with the aim of completely eliminating the parasitic latch effect in the bulk silicon process. Since the parasitic capacitance of the semiconductor on insulator structure to the substrate is greatly reduced, it has great prospects in radio frequency applications.

[0003] At present, the buried insulating layer in the semiconductor-on-insulator structure is completed based on the oxygen injection oxidation process or the smart stripping technology, which is costly and complex, and also introduces oxygen and hydrogen impurities into the upper semiconductor layer, resulting in reduced device performance.

[0004] Therefore, how to improve the manufacturing method of semiconductor-on-insulator structures is an urgent problem that needs to be solved. Summary of the invention

[0005] The object of the present invention is to provide a semiconductor-on-insulator substrate and a method for manufacturing the same, so as to reduce the process difficulty and cost, and to avoid the presence of oxygen impurities and hydrogen impurities in the semiconductor-on-insulator substrate, thereby improving device performance.

[0006] To achieve the above object, the present invention provides a method for manufacturing a semiconductor-on-insulator substrate, comprising:

[0007] Providing a carrier sheet, on which an insulating dielectric layer is formed;

[0008] forming a groove in the insulating dielectric layer, wherein the groove exposes the surface of the carrier sheet;

[0009] forming a semiconductor layer to fill the trench;

[0010] Providing a lower substrate and an insulating buried layer, wherein the insulating buried layer is formed on the lower substrate;

[0011] Bonding the insulating dielectric layer and the semiconductor layer on a side away from the carrier sheet to the insulating buried layer;

[0012] The carrier sheet is removed.

[0013] Optionally, the step of forming the trench in the insulating dielectric layer includes:

[0014] forming a hard mask layer covering the insulating dielectric layer;

[0015] forming a patterned photoresist layer on the hard mask layer;

[0016] Using the patterned photoresist layer as a mask, etching the hard mask layer and the insulating dielectric layer to form a groove exposing the surface of the carrier sheet;

[0017] The patterned photoresist layer and the hard mask layer are removed.

[0018] Optionally, the width of the groove gradually decreases from top to bottom.

[0019] Optionally, the step of removing the carrier sheet includes:

[0020] Performing a plasma bombardment thinning process or a first chemical mechanical polishing process to remove a portion of the thickness of the carrier sheet;

[0021] Performing a wet etching process to planarize the remaining surface of the carrier sheet;

[0022] A second chemical mechanical polishing process is performed to remove the remaining thickness of the carrier sheet.

[0023] Optionally, the insulating dielectric layer is a two-layer stacked structure, and the insulating dielectric layer includes a silicon nitride layer and a silicon oxide layer sequentially formed on the carrier sheet.

[0024] Optionally, after removing the carrier sheet, the method for manufacturing the semiconductor-on-insulator substrate further includes:

[0025] The silicon nitride layer and the semiconductor layer surrounded by the silicon nitride layer are removed.

[0026] Optionally, a polishing speed of the first chemical mechanical polishing process is greater than a polishing speed of the second chemical mechanical polishing process, and a polishing accuracy of the second chemical mechanical polishing process is greater than a polishing accuracy of the first chemical mechanical polishing process.

[0027] Optionally, the semiconductor layer is formed in the trench by an epitaxial process.

[0028] Optionally, a defect-trapping polysilicon layer is formed between the lower substrate and the insulating buried layer.

[0029] The invention also provides a semiconductor-on-insulator substrate, which is manufactured by adopting the manufacturing method of the semiconductor-on-insulator substrate.

[0030] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0031] 1. The manufacturing method of the semiconductor-on-insulator substrate of the present invention provides a carrier sheet formed with an insulating dielectric layer, forms a semiconductor layer to fill the groove in the insulating dielectric layer, and bonds the insulating dielectric layer and the semiconductor layer to the insulating buried layer on one side away from the carrier sheet, so that after removing the carrier sheet, the insulating dielectric layer serves as a shallow trench isolation structure in the upper semiconductor layer, and the semiconductor layer serves as an active area in the upper semiconductor layer, thereby completing the manufacturing of the semiconductor-on-insulator substrate while also completing the manufacturing of the shallow trench isolation structure and the active area in the upper semiconductor layer of the semiconductor-on-insulator substrate. The manufacturing method of the semiconductor-on-insulator substrate of the present invention is free from oxygen injection oxidation process and intelligent stripping technology, thereby reducing process difficulty and cost, and can avoid the presence of oxygen impurities and hydrogen impurities in the semiconductor-on-insulator substrate, thereby improving device performance.

[0032] 2. The semiconductor-on-insulator substrate of the present invention is manufactured by the manufacturing method of the semiconductor-on-insulator substrate, so that oxygen impurities and hydrogen impurities do not exist in the upper semiconductor layer of the semiconductor-on-insulator substrate, thereby improving the device performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1a to Figure 1b The invention is a schematic diagram of a device in a method for manufacturing a semiconductor-on-insulator substrate;

[0034] Figure 2a to Figure 2d is a schematic diagram of a device in another method for manufacturing a semiconductor-on-insulator substrate;

[0035] Figure 3 is a flow chart of a method for manufacturing a semiconductor-on-insulator substrate according to an embodiment of the present invention;

[0036] Figure 4a to Figure 4h yes Figure 3 A schematic diagram of a device in a method for manufacturing a semiconductor-on-insulator substrate is shown.

[0037] Among them, Figure 1a to Figure 4h The reference numerals are described as follows:

[0038] 11-substrate; 111-free oxygen layer; 12-insulating buried layer; 21-first substrate; 211-free hydrogen layer; 22-insulating buried layer; 23-second substrate; 31-carrier; 32-insulating dielectric layer; 321-silicon nitride layer; 322-silicon oxide layer; 33-groove; 331-hard mask layer; 332-patterned photoresist layer; 333-opening; 34-semiconductor layer; 35-lower substrate; 36-insulating buried layer. DETAILED DESCRIPTION

[0039] See also Figure 1a to Figure 1bThe steps of manufacturing a semiconductor-on-insulator substrate based on an oxygen implantation oxidation process include: first, Figure 1a As shown, oxygen atoms are implanted into the interior of the substrate 11 to form a free oxygen layer 111 in the substrate 11; then, as shown in Figure 1b As shown, high temperature annealing oxidation is performed to convert the free oxygen layer 111 into an insulating buried layer 12, and the substrate 11 on the top and bottom surfaces of the insulating buried layer 12 serves as an upper semiconductor layer and a lower substrate, respectively. Since oxygen atoms diffuse when performing high temperature annealing oxidation, the thickness of the formed insulating buried layer 12 is difficult to control, and the thickness precision of the insulating buried layer 12 is low; and oxygen impurities exist in the upper semiconductor layer and the lower substrate, which reduces the performance of the device.

[0040] See also Figure 2a to Figure 2d , the steps of manufacturing a semiconductor-on-insulator substrate based on the smart lift-off technology include: first, Figure 2a As shown, hydrogen ions are implanted into the interior of the first substrate 21 to form a free hydrogen layer 211 in the first substrate 11; then, as shown in Figure 2b As shown, an insulating buried layer 22 is formed on the first substrate 21; then, as shown in Figure 2c As shown, the side of the insulating buried layer 22 away from the first substrate 21 is bonded to the second substrate 23 (i.e., the lower substrate); then, as shown in Figure 2d As shown, high temperature treatment is performed to form bubbles at the free hydrogen layer 211, thereby breaking the chemical bonds (such as silicon bonds) of the first substrate 21 at the free hydrogen layer 211, so that the first substrate 21 is peeled off from the free hydrogen layer 211. After peeling, the first substrate 21 located on the insulating buried layer 22 serves as the upper semiconductor layer. This method has high process difficulty and high cost, and hydrogen impurities will exist in the remaining upper semiconductor layer after peeling, resulting in reduced device performance.

[0041] Therefore, the present invention proposes a semiconductor-on-insulator substrate and a method for manufacturing the same, which can reduce process difficulty and avoid the presence of oxygen impurities and hydrogen impurities in the substrate, thereby improving device performance.

[0042] In order to make the purpose, advantages and features of the present invention more clear, the semiconductor-on-insulator substrate and the manufacturing method thereof proposed by the present invention are further described in detail below in conjunction with the accompanying drawings. It should be noted that the accompanying drawings are all in a very simplified form and are not in precise proportions, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0043] An embodiment of the present invention provides a method for manufacturing a semiconductor-on-insulator substrate. Figure 3 , Figure 3 1 is a flow chart of a method for manufacturing a semiconductor-on-insulator substrate according to an embodiment of the present invention, wherein the method for manufacturing a semiconductor-on-insulator substrate comprises:

[0044] Step S1, providing a carrier sheet, on which an insulating dielectric layer is formed;

[0045] Step S2, forming a groove in the insulating dielectric layer, wherein the groove exposes the surface of the carrier sheet;

[0046] Step S3, forming a semiconductor layer to fill the trench;

[0047] Step S4, providing a lower substrate and an insulating buried layer, wherein the insulating buried layer is formed on the lower substrate;

[0048] Step S5, bonding the insulating dielectric layer and the semiconductor layer on a side away from the carrier sheet to the insulating buried layer;

[0049] Step S6: removing the carrier sheet.

[0050] See below Figure 4a to Figure 4h The method for manufacturing the semiconductor-on-insulator substrate provided by this embodiment is described in more detail. Figure 4a to Figure 4h It is a schematic diagram of a longitudinal cross-section of a semiconductor substrate on an insulator.

[0051] Follow step S1, refer to Figure 4a , providing a carrier sheet 31 , on which an insulating dielectric layer 32 is formed.

[0052] The material of the carrier sheet 31 can be any suitable substrate material known to those skilled in the art, such as silicon, germanium, etc.

[0053] The insulating dielectric layer 32 is a single-layer structure or a stacked structure of at least two layers.

[0054] The insulating dielectric layer 32 may be made of at least one insulating material such as silicon oxide, silicon nitride, or silicon oxynitride.

[0055] like Figure 4a As shown, when the insulating dielectric layer 32 is a two-layer stacked structure, the insulating dielectric layer 32 may include a silicon nitride layer 321 and a silicon oxide layer 322 sequentially formed on the carrier sheet 31 .

[0056] In other embodiments, the insulating dielectric layer 32 may be a single-layer silicon oxide layer.

[0057] According to step S2, refer to Figure 4a to Figure 4b , a groove 33 is formed in the insulating dielectric layer 32 , and the groove 33 exposes the surface of the carrier sheet 31 .

[0058] The steps of forming the groove 33 in the insulating dielectric layer 32 include: first, Figure 4aAs shown, a hard mask layer 331 is formed to cover the insulating dielectric layer 32; then, as shown Figure 4a As shown, a patterned photoresist layer 332 is formed on the hard mask layer 331, and the patterned photoresist layer 332 has an opening 333 that exposes a portion of the surface of the hard mask layer 331; then, as shown Figure 4b As shown, the hard mask layer 331 and the insulating dielectric layer 32 are etched by a dry etching process using the patterned photoresist layer 332 as a mask to form a groove 33 exposing the surface of the carrier film 31; then, the patterned photoresist layer 332 and the hard mask layer 331 are removed.

[0059] The hard mask layer 331 may be a single-layer structure or a stacked structure of at least two layers. Preferably, the hard mask layer 331 includes an amorphous carbon layer and a silicon oxynitride layer sequentially formed on the insulating dielectric layer 32 .

[0060] Furthermore, the hard mask layer 331 and the patterned photoresist layer 332 may further form a bottom anti-reflection layer (not shown), and the material of the bottom anti-reflection layer may be organic.

[0061] The width of the groove 33 may gradually decrease from the top to the bottom, and the longitudinal cross-section of the groove 33 may be a trapezoid.

[0062] According to step S3, refer to Figure 4c to Figure 4d , forming a semiconductor layer 34 filling the trench 33 .

[0063] The steps include: first, Figure 4c As shown, an epitaxial growth process is used to form a doped semiconductor layer 34, the semiconductor layer 34 is filled in the groove 33 and covers the insulating dielectric layer 32, and a single crystal semiconductor layer 34 is formed in the groove 33 by an epitaxial process, so that the active area in the upper semiconductor layer of the finally formed semiconductor-on-insulator substrate is single crystal; then, as shown in Figure 4d As shown, the semiconductor layer 34 is ground by a chemical mechanical grinding process until the semiconductor layer 34 on the insulating dielectric layer 32 is removed, and preferably a partial thickness of the insulating dielectric layer 32 is ground to ensure that the semiconductor layer 34 on the insulating dielectric layer 32 is completely removed, so that the semiconductor layer 34 after grinding is only located in the groove 33, and the top surface of the semiconductor layer 34 in the groove 33 after grinding is flush with the top surface of the insulating dielectric layer 32.

[0064] exist Figure 4c to Figure 4d In the illustrated embodiment, a portion of the thickness of the silicon oxide layer 322 is removed by grinding.

[0065] According to step S4, refer to Figure 4e, providing a lower substrate 35 and an insulating buried layer 36, wherein the insulating buried layer 36 is formed on the lower substrate 35.

[0066] Preferably, a defect-trapping polysilicon layer (not shown) is formed between the lower substrate 35 and the buried insulating layer 36 .

[0067] The defect capture polysilicon layer is polysilicon with more defects. The defect capture polysilicon layer is used to absorb free charges on the surface of each layer structure (such as the insulating buried layer 36 and the semiconductor layer 34) during the production process, and fix the absorbed free charges to prevent the free charges from affecting device performance.

[0068] According to step S5, refer to Figure 4e , bonding the insulating dielectric layer 32 and the semiconductor layer 34 on a side away from the carrier sheet 31 to the insulating buried layer 36 .

[0069] like Figure 4e As shown, the silicon oxide layer 322 and the semiconductor layer 34 are bonded to the insulating buried layer 36 on a side away from the carrier film 31 .

[0070] According to step S6, refer to Figure 4f to Figure 4g , remove the carrier sheet 31.

[0071] The steps of removing the carrier sheet 31 include: first, Figure 4f As shown, a plasma bombardment thinning process or a first chemical mechanical polishing process is performed to thin and remove part of the thickness of the carrier film 31; then, a wet etching process is performed to flatten the surface of the remaining carrier film; then, a second chemical mechanical polishing process is performed to remove the remaining carrier film 31.

[0072] The polishing speed of the first chemical mechanical polishing process is greater than the polishing speed of the second chemical mechanical polishing process, and the polishing accuracy of the second chemical mechanical polishing process is greater than the polishing accuracy of the first chemical mechanical polishing process. Therefore, compared with the first chemical mechanical polishing process, the second chemical mechanical polishing process is easier to control the thickness of the carrier sheet 31 removed by grinding, and the uniformity of the structure surface after grinding is better.

[0073] Among them, since the plasma bombardment thinning process and the first chemical mechanical polishing process have very fast thinning speeds, it is difficult to control the thickness of the thinned and removed structure and the surface of the thinned structure is very rough. In addition, the plasma bombardment thinning process uses physical bombardment, which is easy to damage the structure below the required thinned structure. Therefore, in order to accurately control the thinned thickness and the uniformity of the surface of the structure after thinning, only the plasma bombardment thinning process or the first chemical mechanical polishing process is used to quickly thin and remove most of the thickness of the carrier film 31, and then the wet etching process is used to flatten the surface of the remaining carrier film 31, and then the second chemical mechanical polishing process that is easier to control the thickness and surface uniformity of the removed structure is used to remove the remaining thickness of the carrier film 31, and then the surface treatment after thinning is performed.

[0074] If the insulating dielectric layer 32 includes the silicon nitride layer 321 and the silicon oxide layer 322, then Figure 4g As shown, after removing the carrier sheet 31 , the method for manufacturing the semiconductor substrate on an insulator may further include: removing the silicon nitride layer 321 and the semiconductor layer 34 surrounded by the silicon nitride layer 321 , such as by using a second chemical mechanical polishing process.

[0075] Among them, since the ratio of the grinding rate of the silicon nitride layer 321 and the silicon oxide layer 322 in the second chemical mechanical polishing process is 10, the silicon nitride layer 321 is formed between the carrier plate 31 and the silicon oxide layer 322, so that after the silicon nitride layer 321 is ground by the second chemical mechanical polishing process, the surface of the silicon oxide layer 322 can have good uniformity; and when the plasma bombardment thinning process is performed, the silicon nitride layer 321 can also protect the silicon oxide layer 322 from damage.

[0076] Preferably, the method for manufacturing the semiconductor substrate on an insulator also includes: performing a second chemical mechanical polishing process to remove a partial thickness of the silicon oxide layer 322 and a partial thickness of the semiconductor layer 34 surrounded by the silicon oxide layer 322, so as to ensure that the silicon nitride layer 321 is completely removed and the top surface of the remaining silicon oxide layer 322 is flush with the top surface of the semiconductor layer 34.

[0077] In addition, according to device requirements, the method for manufacturing the semiconductor-on-insulator substrate may further include: first, Figure 4hAs shown, a wet etching process is used to etch and remove a portion of the thickness of the semiconductor layer 34, so that the top surface of the silicon oxide layer 322 is higher than the top surface of the semiconductor layer 34, so as to facilitate subsequent production processes (such as ion implantation to form a well region in the semiconductor layer 34, forming a gate structure on the semiconductor layer 34, etc.), and can remove the grinding damage caused by the second chemical mechanical polishing process; then, the surface of the semiconductor layer 34 is oxidized to form an oxide layer to remove the broken bonds caused by the wet etching process, thereby improving the surface performance of the device. It should be noted that the oxide layer can be removed before the gate structure is subsequently formed on the semiconductor layer 34.

[0078] Furthermore, if the width of the groove 33 gradually decreases from the top to the bottom, Figure 4g and Figure 4h As shown, the width of the semiconductor layer 34 gradually increases from the side facing away from the insulating buried layer 36 to the side facing the insulating buried layer 36, and the longitudinal cross-section of the semiconductor layer 34 may be an inverted trapezoid.

[0079] From the above content, it can be known that after removing the carrier film 31, the lower substrate 35, the insulating buried layer 36, the semiconductor layer 34 and the insulating dielectric layer 32 together constitute a semiconductor-on-insulator substrate, and the insulating dielectric layer 32 serves as a shallow trench isolation structure in the upper semiconductor layer, and the semiconductor layer 34 serves as an active area in the upper semiconductor layer, so that when the semiconductor-on-insulator substrate is manufactured, the shallow trench isolation structure and the active area in the upper semiconductor layer of the semiconductor-on-insulator substrate are also manufactured, thereby simplifying the production process; and, the manufacturing method of the semiconductor-on-insulator substrate of the present invention is separated from the oxygen injection oxidation process and the intelligent stripping technology, thereby reducing the process difficulty and cost, and can avoid the presence of oxygen impurities and hydrogen impurities in the semiconductor-on-insulator substrate, thereby improving the device performance.

[0080] Furthermore, if the insulating dielectric layer 32 includes the silicon nitride layer 321 and the silicon oxide layer 322, after removing a portion of the thickness of the silicon oxide layer 322 and a portion of the thickness of the semiconductor layer 34 surrounded by the silicon oxide layer 322, the lower substrate 35, the insulating buried layer 36, the remaining thickness of the silicon oxide layer 322 and the semiconductor layer 34 surrounded by the remaining thickness of the silicon oxide layer 322 together constitute a semiconductor substrate on an insulator, and the remaining thickness of the silicon oxide layer 322 serves as a shallow trench isolation structure in the upper semiconductor layer, and the remaining thickness of the silicon oxide layer 322 serves as an active region in the upper semiconductor layer.

[0081] In summary, the manufacturing method of the semiconductor-on-insulator substrate provided by the present invention provides a carrier sheet formed with an insulating dielectric layer, forms a semiconductor layer to fill the groove in the insulating dielectric layer, and bonds the insulating dielectric layer and the semiconductor layer to the insulating buried layer on one side away from the carrier sheet, so that after removing the carrier sheet, the insulating dielectric layer serves as a shallow trench isolation structure in the upper semiconductor layer, and the semiconductor layer serves as an active area in the upper semiconductor layer, thereby completing the manufacturing of the semiconductor-on-insulator substrate while also completing the manufacturing of the shallow trench isolation structure and the active area in the upper semiconductor layer of the semiconductor-on-insulator substrate. The manufacturing method of the semiconductor-on-insulator substrate of the present invention is free from the oxygen injection oxidation process and the intelligent stripping technology, thereby reducing the process difficulty and cost, and can avoid the presence of oxygen impurities and hydrogen impurities in the semiconductor-on-insulator substrate, thereby improving the device performance.

[0082] An embodiment of the present invention provides a semiconductor-on-insulator substrate. Figure 4h The semiconductor-on-insulator substrate is manufactured using the semiconductor-on-insulator substrate manufacturing method.

[0083] The method for manufacturing the semiconductor-on-insulator substrate can be found in the above description and will not be described in detail here.

[0084] Compared with the presence of oxygen impurities in the upper semiconductor layer formed by the oxygen injection oxidation process and the presence of hydrogen impurities in the upper semiconductor layer formed by the smart stripping technology, since the semiconductor substrate on insulator of the present invention is manufactured using the manufacturing method of the semiconductor substrate on insulator, the upper semiconductor layer in the semiconductor substrate on insulator is formed by an epitaxial process, there are no oxygen impurities and hydrogen impurities in the upper semiconductor layer of the present invention, thereby improving the device performance.

[0085] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.

Claims

1. A method for manufacturing a semiconductor-on-insulator substrate, characterized in that: include: Providing a carrier sheet, on which an insulating dielectric layer is formed; forming a groove in the insulating dielectric layer, wherein the groove exposes the surface of the carrier sheet; Forming a semiconductor layer to fill the trench, the insulating dielectric layer serving as a shallow trench isolation structure in the upper semiconductor layer, and the semiconductor layer serving as an active region in the upper semiconductor layer; Providing a lower substrate and an insulating buried layer, wherein the insulating buried layer is formed on the lower substrate; Bonding the insulating dielectric layer and the semiconductor layer on a side away from the carrier sheet to the insulating buried layer; The carrier sheet is removed.

2. The method for manufacturing a semiconductor-on-insulator substrate according to claim 1, wherein: The step of forming the trench in the insulating dielectric layer comprises: forming a hard mask layer covering the insulating dielectric layer; forming a patterned photoresist layer on the hard mask layer; Using the patterned photoresist layer as a mask, etching the hard mask layer and the insulating dielectric layer to form a groove exposing the surface of the carrier sheet; The patterned photoresist layer and the hard mask layer are removed.

3. The method for manufacturing a semiconductor-on-insulator substrate according to claim 1, wherein: The width of the groove gradually decreases from top to bottom.

4. The method for manufacturing a semiconductor-on-insulator substrate according to claim 1, wherein: The step of removing the carrier sheet comprises: Performing a plasma bombardment thinning process or a first chemical mechanical polishing process to remove a portion of the thickness of the carrier sheet; Performing a wet etching process to planarize the remaining surface of the carrier sheet; A second chemical mechanical polishing process is performed to remove the remaining thickness of the carrier sheet.

5. The method for manufacturing a semiconductor-on-insulator substrate according to claim 1, wherein: The insulating dielectric layer is a two-layer stacked structure, and the insulating dielectric layer includes a silicon nitride layer and a silicon oxide layer which are sequentially formed on the carrier.

6. The method for manufacturing a semiconductor-on-insulator substrate according to claim 5, wherein: After removing the carrier sheet, the method for manufacturing the semiconductor-on-insulator substrate further includes: The silicon nitride layer and the semiconductor layer surrounded by the silicon nitride layer are removed.

7. The method for manufacturing a semiconductor-on-insulator substrate according to claim 4, wherein: The polishing speed of the first chemical mechanical polishing process is greater than the polishing speed of the second chemical mechanical polishing process, and the polishing accuracy of the second chemical mechanical polishing process is greater than the polishing accuracy of the first chemical mechanical polishing process.

8. The method for manufacturing a semiconductor-on-insulator substrate according to claim 1, wherein: The semiconductor layer is formed in the trench by using an epitaxial process.

9. The method for manufacturing a semiconductor-on-insulator substrate according to any one of claims 1 to 8, characterized in that: A defect-trapping polysilicon layer is formed between the lower substrate and the insulating buried layer.

10. A semiconductor-on-insulator substrate, characterized in that: The method for manufacturing a semiconductor-on-insulator substrate is used as described in any one of claims 1 to 9.