Curable resin composition, cured film, laminate, method for producing cured film, and semiconductor device
By using a curable resin composition of polyimide, polybenzoxazole, polyamideimide resin and organic metal complex with a specific structure, the problem of insufficient pattern resolution is solved and high resolution and Chemically resistant photosensitive film suitable for semiconductor device manufacturing.
Patent Information
- Application Number
- CN202180016937.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-28
- Filing Date
- 2021-02-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-02-25
Smart Images

Figure GDA0003815522380000071 
Figure GDA0003815522380000081 
Figure GDA0003815522380000101
Abstract
Description
Technical Field
[0001] The present invention relates to a curable resin composition, a cured film, a laminate, a method for producing the cured film, and a semiconductor device. Background Art
[0002] Since resins such as polyimide, polybenzoxazole, and polyamide-imide have excellent heat resistance and insulation properties, they are suitable for various uses. The above uses are not particularly limited. For example, if a semiconductor device for packaging is used, the use as an insulating film or sealing material, or a protective film can be cited. In addition, it is also used as a base film or coverlay film of a flexible substrate.
[0003] For example, in the above-mentioned applications, resins such as polyimide, polybenzoxazole, and polyamideimide are used in the form of a curable resin composition containing at least one resin selected from a polyimide precursor, a polybenzoxazole precursor, and a polyamideimide precursor.
[0004] Such a curable resin composition is applied to a substrate by, for example, coating to form a photosensitive film, and then, if necessary, subjected to exposure, development, heating, etc., to form a cured product on the substrate.
[0005] The polyimide precursor, polybenzoxazole precursor, and polyamideimide precursor are cyclized, for example, by heating, and become polyimide, polybenzoxazole, and polyamideimide, respectively, in a cured product.
[0006] Since the curable resin composition can be applied by a known coating method, it can be said that the adaptability in manufacturing is excellent, for example, the curable resin composition has a high degree of freedom in designing the shape, size, and application position when applied. In addition to the high performance of polyimide, polybenzoxazole, polyamide-imide, etc., from the perspective of excellent adaptability in manufacturing, the application expansion of the above-mentioned curable resin composition in the industry is increasingly expected.
[0007] For example, Patent Document 1 describes a negative photosensitive resin composition comprising 100 parts by mass of a polyimide precursor of a specific structure, 1 to 20 parts by mass of a photopolymerization initiator, and 0.01 to 10 parts by mass of a monocarboxylic acid compound having 2 to 30 carbon atoms and having one or more functional groups selected from hydroxyl groups, ether groups, and ester groups.
[0008] Previous technical literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2011-191749 Summary of the invention
[0011] Technical issues to be solved by the invention
[0012] When forming a pattern composed of a curable resin composition, it is required to improve the resolution.
[0013] An object of the present invention is to provide a curable resin composition having excellent resolution during pattern formation, a cured film formed by curing the curable resin composition, a cured laminate including the cured film, a method for producing the cured film, and a semiconductor device including the cured film or the laminate.
[0014] Means for solving technical problems
[0015] Representative embodiments of the present invention are shown below.
[0016] A curable resin composition comprising:
[0017] at least one resin selected from a polyimide precursor including at least one of a cyclic imide structure and a cyclic isoimide structure, a polybenzoxazole precursor including a benzoxazole structure, and a polyamideimide precursor including at least one of a cyclic imide structure and a cyclic isoimide structure; and
[0018] Organometallic complexes,
[0019] The total molar content of the cyclic imide structure and the cyclic isoimide structure contained in 1 g of the polyimide precursor is 0.08 to 1.68 mmol / g.
[0020] The molar amount of the benzoxazole structure contained in 1 g of the polybenzoxazole precursor is 0.22 to 3.97 mmol / g.
[0021] The total molar content of the cyclic imide structure and the cyclic isoimide structure contained in 1 g of the polyimide precursor is 0.062 to 1.186 mmol / g.
[0022] <2> The curable resin composition according to <1>, further comprising a photopolymerization initiator.
[0023] <3> The curable resin composition according to <1> or <2>, wherein the photopolymerization initiator is an oxime compound.
[0024] <4> The curable resin composition according to any one of <1> to <3>, further comprising a crosslinking agent.
[0025] <5> The curable resin composition according to any one of <1> to <4>, wherein the organic metal complex is a metallocene compound.
[0026] <6> The curable resin composition according to any one of <1> to <5>, wherein the metal contained in the organic metal complex is at least one metal selected from titanium, zirconium, and hafnium.
[0027] <7> The curable resin composition according to any one of <1> to <6>, wherein the organic metal complex has a photoradical polymerization initiation capability.
[0028] <8> The curable resin composition according to any one of <1> to <7>, which is used for forming a photosensitive film for negative-type development.
[0029] <9> The curable resin composition according to any one of <1> to <8>, which is used for forming an interlayer insulating film for a redistribution layer.
[0030] <10> A cured film obtained by curing the curable resin composition according to any one of <1> to <9>.
[0031] <11> A laminate comprising two or more layers of the cured films according to <10>, wherein a metal layer is provided between any of the cured films.
[0032] <12> A method for producing a cured film, the method comprising: a film forming step of applying the curable resin composition according to any one of <1> to <9> to a substrate to form a film.
[0033] <13> The method for producing a cured film according to <12>, comprising: an exposure step of exposing the film to light; and a development step of developing the film.
[0034] <14> The method for producing a cured film according to <13>, wherein the exposure light used in the exposure includes light having a wavelength of 405 nm.
[0035] <15> The method for producing a cured film according to <13> or <14>, wherein the exposure is exposure by a laser direct imaging method.
[0036] <16> The method for producing a cured film according to any one of <12> to <15>, comprising a heating step of heating the film at 50 to 450°C.
[0037] <17> A semiconductor device comprising the cured film according to <10> or the laminated body according to <11>.
[0038] Effects of the Invention
[0039] According to the present invention, there are provided a curable resin composition having excellent resolution during pattern formation, a cured film formed by curing the curable resin composition, a laminate including the cured film, a method for producing the cured film, and a semiconductor device including the cured film or the laminate. DETAILED DESCRIPTION
[0040] Hereinafter, the main embodiments of the present invention will be described. However, the present invention is not limited to the embodiments described above.
[0041] In the present specification, a numerical range expressed using a symbol such as “to” means a range including the numerical values described before and after “to” as the lower limit and the upper limit, respectively.
[0042] In this specification, the term "process" includes not only independent processes but also processes that cannot be clearly distinguished from other processes as long as the intended effect of the process can be achieved.
[0043] In the marking of groups (atomic groups) in this specification, the marking not indicating substituted and unsubstituted includes groups (atomic groups) without substitution and also includes groups (atomic groups) with substitution. For example, "alkyl" includes not only alkyl groups without substitution (unsubstituted alkyl groups) but also alkyl groups with substitution (substituted alkyl groups).
[0044] In this specification, unless otherwise specified, "exposure" includes not only exposure using light but also exposure using particle beams such as electron beams and ion beams. In addition, examples of light used for exposure include active light or radiation such as the bright line spectrum of a mercury lamp, far ultraviolet rays represented by excimer lasers, extreme ultraviolet rays (EUV rays), X-rays, and electron beams.
[0045] In this specification, “(meth)acrylate” means both or either “acrylate” and “methacrylate”, “(meth)acrylic acid” means both or either “acrylic acid” and “methacrylic acid”, and “(meth)acryloyl” means both or either “acryloyl” and “methacryloyl”.
[0046] In the present specification, Me in the structural formula represents a methyl group, Et represents an ethyl group, Bu represents a butyl group, and Ph represents a phenyl group.
[0047] In this specification, the total solid content refers to the total mass of the components after removing the solvent from all the components of the composition. In addition, in this specification, the solid content concentration refers to the mass percentage of the other components excluding the solvent relative to the total mass of the composition.
[0048] In this specification, as long as there is no special description, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are defined as polystyrene conversion values according to gel permeation chromatography (GPC measurement). In this specification, the weight average molecular weight (Mw) and the number average molecular weight (Mn) can be obtained, for example, by using HLC-8220GPC (manufactured by TOSOH CORPORATION), and using protective columns HZ-L, TSKgel Super HZM-M, TSKgel Super HZ4000, TSKgel Super HZ3000, TSKgel Super HZ2000 (manufactured by TOSOH CORPORATION) as columns. As long as there is no special description, these molecular weights are measured using THF (tetrahydrofuran) as eluent. And, as long as there is no special description, the detection in the GPC measurement uses a wavelength 254nm detector of UV line (ultraviolet rays).
[0049] In this specification, when the positional relationship of each layer constituting the laminate is recorded as "up" or "down", it is sufficient to have other layers on the upper side or lower side of the layer that serves as the reference among the multiple layers of interest. That is, a third layer or element may be further inserted between the layer that serves as the reference and the above-mentioned other layers, and the layer that serves as the reference does not need to be in contact with the above-mentioned other layers. In addition, unless otherwise specified, the direction of stacking layers on the substrate is referred to as "up", or when a photosensitive film is present, the direction from the substrate toward the photosensitive film is referred to as "up", and the opposite direction is referred to as "down". In addition, the setting of the up and down directions is for convenience in this specification, and in actual practice, the "up" direction in this specification may also be different from the vertically upward direction.
[0050] In this specification, unless otherwise specified, in the composition, as each component contained in the composition, two or more compounds corresponding to the component may be included. Furthermore, unless otherwise specified, the content of each component in the composition refers to the total content of all compounds corresponding to the component.
[0051] In this specification, unless otherwise specified, the temperature is 23° C., the air pressure is 101,325 Pa (1 atmosphere), and the relative humidity is 50% RH.
[0052] In the present specification, a combination of preferred embodiments is a more preferred embodiment.
[0053] (Curable resin composition)
[0054] The curable resin composition of the present invention comprises: at least one resin selected from a polyimide precursor comprising at least one of a cyclic imide structure and a cyclic isoimide structure, a polybenzoxazole precursor comprising a benzoxazole structure, and a polyamide-imide precursor comprising at least one of a cyclic imide structure and a cyclic isoimide structure (hereinafter also referred to as a "specific resin"); and an organic metal complex, wherein the total molar amount of the cyclic imide structure and the cyclic isoimide structure contained in 1 g of the above-mentioned polyimide precursor is 0.08 to 1.68 mmol / g, the molar amount of the above-mentioned benzoxazole structure contained in 1 g of the above-mentioned polybenzoxazole precursor is 0.22 to 3.97 mmol / g, and the total molar amount of the above-mentioned cyclic imide structure and the above-mentioned cyclic isoimide structure contained in 1 g of the above-mentioned polyamide-imide precursor is 0.062 to 1.186 mmol / g.
[0055] The curable resin composition of the present invention is preferably used to form a photosensitive film to be exposed and developed, and is preferably used to form a film to be exposed and developed using a developer containing an organic solvent.
[0056] Furthermore, the curable resin composition of the present invention is preferably used to form a photosensitive film for negative-type development.
[0057] In the present invention, negative tone development refers to development in which non-exposed areas are removed by development during exposure and development, and positive tone development refers to development in which exposed areas are removed by development.
[0058] As the exposure method, the developer, and the development method, for example, the exposure method described in the exposure step in the description of the method for producing a cured film described later, and the developer and the development method described in the development step can be used.
[0059] The curable resin composition of the present invention is excellent in exposure sensitivity and chemical resistance of the obtained pattern.
[0060] The mechanism by which the above-mentioned effects can be obtained is not clear, but is presumed to be as follows.
[0061] For example, as described in Patent Document 1, an organic titanium compound or the like is added to a curable resin composition in order to improve chemical resistance.
[0062] However, when patterning is performed using a composition containing an organic metal complex, the organic metal complex aggregates in the film, and resolution may decrease.
[0063] In the present invention, as the resin in the resin composition, a resin containing a cyclic imide structure, a cyclic isoimide structure or a benzoxazole structure in a specific content is used. It is believed that these structures interact strongly with the organic metal complex, and the organic metal complex contained in the composition is dispersed in a nearly uniform state in the film. As a result, it is speculated that the resolution of the resin composition of the present invention is excellent.
[0064] Hereinafter, the components contained in the curable resin composition of the present invention will be described in detail.
[0065] <Specified resin>
[0066] The curable resin composition of the present invention comprises at least one resin (specific resin) selected from a polyimide precursor comprising at least one of a cyclic imide structure and a cyclic isoimide structure, a polybenzoxazole precursor comprising a benzoxazole structure, and a polyamideimide precursor comprising at least one of a cyclic imide structure and a cyclic isoimide structure.
[0067] The curable resin composition of the present invention preferably includes, as a specific resin, a polyimide precursor including at least one of a cyclic imide structure and a cyclic isoimide structure.
[0068] Furthermore, the specific resin preferably has a radical polymerizable group.
[0069] When the specific resin has a radical polymerizable group, the curable resin composition preferably contains a photoradical polymerization initiator as described below as a photosensitizer, more preferably contains a photoradical polymerization initiator as described below as a photosensitizer and a radical crosslinking agent as described below, and further preferably contains a photoradical polymerization initiator as described below as a photosensitizer, a radical crosslinking agent as described below, and a sensitizer as described below. For example, a negative photosensitive film is formed from such a curable resin composition.
[0070] Furthermore, the specific resin may have a polarity conversion group such as an acid-decomposable group.
[0071] When the specific resin has an acid-decomposable group, the curable resin composition preferably contains a photoacid generator as described below as a photosensitizer. Such a curable resin composition can form, for example, a chemically amplified positive photosensitive film or a negative photosensitive film.
[0072] When the resin composition contains a polyimide precursor as a specific resin, from the viewpoint of resolution, the total molar content of the cyclic imide structure and the cyclic isoimide structure in 1 g of the above-mentioned polyimide precursor is 0.08 to 1.68 mmol / g, preferably 0.10 to 1.00 mmol / g, more preferably 0.12 to 0.80 mmol / g, and further preferably 0.15 to 0.60 mmol / g.
[0073] Furthermore, the polyimide precursor preferably includes at least a cyclic imide structure.
[0074] The polyimide precursor may have at least one of a cyclic imide structure and a cyclic isoimide structure in a side chain, but preferably has it in a main chain.
[0075] In this specification, the main chain of a resin refers to the longest molecular chain in a molecule.
[0076] When the resin composition contains a polybenzoxazole precursor as a specific resin, the molar content of the benzoxazole structure in 1 g of the polybenzoxazole precursor is 0.22 to 3.97 mmol / g, preferably 0.25 to 3.00 mmol / g, more preferably 0.28 to 2.50 mmol / g, and further preferably 0.30 to 2.00 mmol / g from the viewpoint of resolution.
[0077] The polybenzoxazole precursor may have a benzoxazole structure in a side chain, but preferably has it in a main chain.
[0078] When the resin composition contains a polyamideimide precursor as a specific resin, from the viewpoint of resolution, the total molar content of the cyclic imide structure and the cyclic isoimide structure in 1 g of the above-mentioned polyamideimide precursor is 0.062 to 1.186 mmol / g, preferably 0.070 to 1.000 mmol / g, more preferably 0.080 to 0.800 mmol / g, and further preferably 0.090 to 0.700 mmol / g.
[0079] Furthermore, the polyamide-imide precursor preferably includes at least a cyclic imide structure.
[0080] The polyamide-imide precursor may have at least one of a cyclic imide structure and a cyclic isoimide structure in a side chain, but preferably has it in a main chain.
[0081] 〔Polyimide precursor〕
[0082] The polyimide precursor used in the present invention is not particularly limited in type or the like, but preferably contains a repeating unit represented by the following formula (2).
[0083] [Chemical formula 1]
[0084]
[0085] In formula (2), A 1 and A 2 Each independently represents an oxygen atom or NH, R 111 represents a divalent organic group, R 115represents a tetravalent organic group, R 113 and R 114 Each independently represents a hydrogen atom or a monovalent organic group.
[0086] A in formula (2) 1 and A 2 Each independently represents an oxygen atom or NH, preferably an oxygen atom.
[0087] R in formula (2) 111 Represents a divalent organic group. As a divalent organic group, a group comprising a straight-chain or branched aliphatic group, a cyclic aliphatic group and an aromatic group can be exemplified, preferably a group consisting of a straight-chain or branched aliphatic group having 2 to 20 carbon atoms, a cyclic aliphatic group having 6 to 20 carbon atoms, an aromatic group having 6 to 20 carbon atoms or a combination thereof, and more preferably a group consisting of an aromatic group having 6 to 20 carbon atoms. As a particularly preferred embodiment of the present invention, a group represented by -Ar-L-Ar- can be exemplified. Among them, Ar is independently an aromatic group, and L is a group consisting of an aliphatic hydrocarbon group having 1 to 10 carbon atoms that can be substituted with a fluorine atom, -O-, -CO-, -S-, -SO2- or -NHCO-, or a combination of two or more of the above. These preferred ranges are as described above.
[0088] R 111 It is preferably derived from a diamine. Examples of the diamine used in the production of the polyimide precursor include linear or branched aliphatic, cyclic aliphatic or aromatic diamines. The diamine may be used alone or in combination of two or more.
[0089] Specifically, diamines containing a group consisting of a linear or branched aliphatic group having 2 to 20 carbon atoms, a cyclic aliphatic group having 6 to 20 carbon atoms, an aromatic group having 6 to 20 carbon atoms, or a combination thereof are preferred, and diamines containing a group consisting of an aromatic group having 6 to 20 carbon atoms are more preferred. Examples of the aromatic group include the following.
[0090] [Chemical formula 2]
[0091]
[0092] In the formula, A is preferably a single bond or a group selected from an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted by a fluorine atom, -O-, -C(=O)-, -S-, -SO2-, -NHCO- or a combination thereof, more preferably a single bond or an alkylene group having 1 to 3 carbon atoms which may be substituted by a fluorine atom, further preferably a group selected from -O-, -C(=O)-, -S- or -SO2-, -CH2-, -O-, -S-, -SO2-, -C(CF3)2- or -C(CH3)2-.
[0093] In the formula, * indicates the bonding site with other structures.
[0094] The diamine may specifically include at least one selected from the group consisting of 1,2-diaminoethane, 1,2-diaminopropane, 1,3-diaminopropane, 1,4-diaminobutane and 1,6-diaminohexane; 1,2- or 1,3-diaminocyclopentane, 1,2-, 1,3- or 1,4-diaminocyclohexane, 1,2-, 1,3- or 1,4-bis(aminomethyl)cyclohexane, bis-(4-aminocyclohexyl)methane, bis-(3-aminocyclohexyl)methane, 4,4'-diamino-3,3'-dimethylcyclohexylmethane and isophorone diamine; m- or p-phenylenediamine, diaminotoluene, 4,4'- or 3,3'-diaminobiphenyl, 4,4'-diaminodiphenyl ether, 3,3-diaminodiphenyl ether , 4,4'- and 3,3'-diaminodiphenylmethane, 4,4'- and 3,3'-diaminodiphenyl sulfone, 4,4'- and 3,3'-diaminodiphenyl sulfide, 4,4'- or 3,3'-diaminobenzophenone, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis(3-hydroxy-4-aminophenyl)propane, 2,2-bis(3-hydroxy-4-aminophenyl)hexafluoropropane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4 -hydroxyphenyl) hexafluoropropane, bis(3-amino-4-hydroxyphenyl) sulfone, bis(4-amino-3-hydroxyphenyl) sulfone, 4,4'-diaminoterphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(2-aminophenoxy)phenyl]sulfone, 1,4-bis(4-aminophenoxy)benzene, 9,10-bis(4-aminophenyl)anthracene, 3,3'-dimethyl-4,4'-diaminodiphenylsulfone, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenyl)benzene, 3,3'-diethyl-4,4'-diaminodiphenylmethane alkane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 4,4'-diaminooctafluorobiphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 9,9-bis(4-aminophenyl)-10-hydroanthracene, 3,3',4,4'-tetraaminobiphenyl, 3,3',4,4'-tetraaminodiphenyl ether, 1,4-diaminoanthraquinone, 1,5-diaminoanthraquinone, 3,3-dihydroxy-4,4'-diaminobiphenyl, 9,9'-bis(4-aminophenyl)fluorene, 4,4'-dimethyl-3,3'-diaminodiphenyl sulfone, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, 2,4- and 2,5-Diaminoisopropylbenzene, 2,5-dimethyl-p-phenylenediamine, acetoguanamine, 2,3,5,6-tetramethyl-p-phenylenediamine, 2,4,6-trimethyl-m-phenylenediamine, bis(3-aminopropyl)tetramethyldisiloxane, 2,7-diaminofluorene, 2,5-diaminopyridine, 1,2-bis(4-aminophenyl)ethane, diaminobenzanilide, esters of diaminobenzoic acid, 1,5-diaminonaphthalene, diaminotrifluoromethane benzene, 1,3-bis(4-aminophenyl)hexafluoropropane, 1,4-bis(4-aminophenyl)octafluorobutane, 1,5-bis(4-aminophenyl)decafluoropentane, 1,7-bis(4-aminophenyl)tetradecafluoroheptane, 2,2-bis[4-(3-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis[4-(2-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)-3, 5-dimethylphenyl]hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)-3,5-bis(trifluoromethyl)phenyl]hexafluoropropane, p-bis(4-amino-2-trifluoromethylphenoxy)benzene, 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl, 4,4'-bis(4-amino-3-trifluoromethylphenoxy)biphenyl, 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl Sulfone, 4,4'-bis(3-amino-5-trifluoromethylphenoxy)diphenyl sulfone, 2,2-bis[4-(4-amino-3-trifluoromethylphenoxy)phenyl]hexafluoropropane, 3,3',5,5'-tetramethyl-4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 2,2',5,5',6,6'-hexafluorotoluidine and 4,4'-diaminotetraphenyl.
[0095] Furthermore, diamines (DA-1) to (DA-18) described in paragraphs 0030 to 0031 of International Publication No. 2017 / 038598 are also preferred.
[0096] Furthermore, diamines having two or more alkylene glycol units in the main chain described in paragraphs 0032 to 0034 of International Publication No. 2017 / 038598 can also be preferably used.
[0097] From the viewpoint of the flexibility of the obtained organic film, R 111 Preferably, it is represented by -Ar-L-Ar-. Ar is independently an aromatic group, and L is a group consisting of an aliphatic hydrocarbon group having 1 to 10 carbon atoms that may be substituted by a fluorine atom, -O-, -CO-, -S-, -SO2- or -NHCO-, or a combination of two or more of the above. Ar is preferably a phenylene group, and L is preferably an aliphatic hydrocarbon group having 1 or 2 carbon atoms that may be substituted by a fluorine atom, -O-, -CO-, -S- or -SO2-. The aliphatic hydrocarbon group here is preferably an alkylene group.
[0098] Furthermore, from the perspective of i-ray transmittance, R 111 Preferred are divalent organic groups represented by the following formula (51) or formula (61). In particular, from the viewpoint of i-ray transmittance and availability, divalent organic groups represented by formula (61) are more preferred.
[0099] Formula (51)
[0100] [Chemical formula 3]
[0101]
[0102] In formula (51), R 50 ~R 57 are independently a hydrogen atom, a fluorine atom or a monovalent organic group, R 50 ~R 57 At least one of them is a fluorine atom, a methyl group or a trifluoromethyl group.
[0103] As R 50 ~R 57 Examples of the monovalent organic group include an unsubstituted alkyl group having 1 to 10 carbon atoms (preferably 1 to 6 carbon atoms) and a fluorinated alkyl group having 1 to 10 carbon atoms (preferably 1 to 6 carbon atoms).
[0104] [Chemical formula 4]
[0105]
[0106] In formula (61), R 58 and R 59 are each independently a fluorine atom or a trifluoromethyl group.
[0107] Examples of the diamine compound that provides the structure of formula (51) or (61) include 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2'-bis(fluoro)-4,4'-diaminobiphenyl, and 4,4'-diaminooctafluorobiphenyl. These may be used alone or in combination of two or more.
[0108] In addition, the following diamines can also be preferably used.
[0109] [Chemical formula 5]
[0110]
[0111] R in formula (2) 115 The tetravalent organic group is preferably a tetravalent organic group containing an aromatic ring, and more preferably a group represented by the following formula (5) or (6).
[0112] In formula (5) or (6), * each independently represents a bonding site with another structure.
[0113] [Chemical formula 6]
[0114]
[0115] In formula (5), R 112 It is preferably a single bond or a group selected from aliphatic hydrocarbon groups having 1 to 10 carbon atoms which may be substituted by fluorine atoms, -O-, -CO-, -S-, -SO2- and -NHCO-, and combinations thereof; it is more preferably a single bond, a group selected from alkylene groups having 1 to 3 carbon atoms which may be substituted by fluorine atoms, -O-, -CO-, -S- and -SO2-; it is further preferably a divalent group selected from -CH2-, -C(CF3)2-, -C(CH3)2-, -O-, -CO-, -S- and -SO2-.
[0116] Specifically, R 115 Examples thereof include a tetracarboxylic acid residue remaining after an anhydride group is removed from tetracarboxylic dianhydride. The tetracarboxylic dianhydride may be used alone or in combination of two or more.
[0117] It is preferable that tetracarboxylic dianhydride is represented by the following formula (O).
[0118] [Chemical formula 7]
[0119]
[0120] In formula (O), R 115 represents a tetravalent organic group. 115 The preferred range of R in formula (2) 115 The meanings are the same and the preferred ranges are also the same.
[0121] Specific examples of tetracarboxylic dianhydrides include pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenyl sulfide tetracarboxylic dianhydride, 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-diphenylmethane tetracarboxylic dianhydride, 2,2',3,3'-diphenylmethane tetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-benzophenone tetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 1,4,5,7-naphthalene tetracarboxylic dianhydride, and 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride. , 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, 1,3-diphenylhexafluoropropane-3,3,4,4-tetracarboxylic dianhydride, 1,4,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-diphenyltetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 1,2,4,5-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,8,9,10-phenanthrenetetracarboxylic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2,3,4-benzenetetracarboxylic dianhydride, and alkyl derivatives having 1 to 6 carbon atoms and alkoxy derivatives having 1 to 6 carbon atoms thereof.
[0122] Furthermore, as preferred examples, tetracarboxylic dianhydrides (DAA-1) to (DAA-5) described in paragraph 0038 of International Publication No. 2017 / 038598 can also be mentioned.
[0123] R is also preferred 111 and R 115 More specifically, as R 111 , for example, residues of bisaminophenol derivatives can be mentioned.
[0124] R 113 and R 114 Each independently represents a hydrogen atom or a monovalent organic group, preferably R 113 and R 114 At least one of them contains a polymerizable group, and more preferably both contain a polymerizable group. As a polymerizable group, it is a group that can undergo a crosslinking reaction by the action of heat, free radicals, etc., preferably a free radical polymerizable group. As a specific example of a polymerizable group, a group with an ethylenically unsaturated bond, an alkoxymethyl group, a hydroxymethyl group, an acyloxymethyl group, an epoxy group, an oxetanyl group, a benzoxazolyl group, a blocked isocyanate group, a methylol group, and an amino group can be cited. As a free radical polymerizable group possessed by a polyimide precursor, a group with an ethylenically unsaturated bond is preferably present.
[0125] Examples of the group having an ethylenically unsaturated bond include a vinyl group, a (meth)allyl group, and a group represented by the following formula (III). Among them, a group represented by the following formula (III) is preferred.
[0126] [Chemical formula 8]
[0127]
[0128] In formula (III), R 200 represents a hydrogen atom or a methyl group, preferably a hydrogen atom.
[0129] In formula (III), * represents a bonding site with other structures.
[0130] In formula (III), R 201 It represents an alkylene group having 2 to 12 carbon atoms, -CH2CH(OH)CH2-, or a polyalkyleneoxy group.
[0131] Preferred R 201 Examples include ethylene, propylene, trimethylene, tetramethylene, 1,2-butanediyl, 1,3-butanediyl, pentamethylene, hexamethylene, octamethylene, dodecamethylene, -CH2CH(OH)CH2-, and polyalkyleneoxy groups, with ethylene, propylene, trimethylene, -CH2CH(OH)CH2-, and polyalkyleneoxy groups being more preferred, and polyalkyleneoxy groups being further preferred.
[0132] In the present invention, the polyalkyleneoxy group refers to a group in which two or more alkyleneoxy groups are directly bonded. The alkylene groups in the plurality of alkyleneoxy groups included in the polyalkyleneoxy group may be the same or different.
[0133] When the polyalkyleneoxy group includes a plurality of alkyleneoxy groups of different alkylene groups, the arrangement of the alkyleneoxy groups in the polyalkyleneoxy group may be a random arrangement, an arrangement having blocks, an arrangement having an alternating pattern, or the like.
[0134] The number of carbon atoms of the alkylene group (including the carbon atoms of the substituent when the alkylene group has a substituent) is preferably 2 or more, more preferably 2 to 10, more preferably 2 to 6, further preferably 2 to 5, further preferably 2 to 4, particularly preferably 2 or 3, and most preferably 2.
[0135] Furthermore, the above-mentioned alkylene group may have a substituent, and preferred substituents include an alkyl group, an aryl group, a halogen atom, and the like.
[0136] Furthermore, the number of alkyleneoxy groups contained in the polyalkyleneoxy group (the number of repetitions of the polyalkyleneoxy group) is preferably 2-20, more preferably 2-10, and even more preferably 2-6.
[0137] As the polyalkyleneoxy group, from the viewpoint of solvent solubility and solvent resistance, preferably, a group consisting of a plurality of ethyleneoxy groups and a plurality of propyleneoxy groups is used, more preferably a polyethyleneoxy group or a polypropyleneoxy group, and further preferably a polyethyleneoxy group. In the group consisting of a plurality of ethyleneoxy groups and a plurality of propyleneoxy groups, the ethyleneoxy groups and the propyleneoxy groups may be arranged randomly, may be arranged in blocks, or may be arranged in alternating patterns. The preferred form of the number of repetitions of the ethyleneoxy group and the like in these groups is as described above.
[0138] R 113 and R 114 Each independently represents a hydrogen atom or a monovalent organic group. As the monovalent organic group, an aromatic group and an aralkyl group having an acidic group bonded to one, two or three carbon atoms, preferably one carbon atom, constituting the aryl group can be cited. Specifically, an aromatic group having 6 to 20 carbon atoms and an aralkyl group having 7 to 25 carbon atoms can be cited. More specifically, a phenyl group having an acidic group and a benzyl group having an acidic group can be cited. The acidic group is preferably an OH group.
[0139] R 113 or R 114 Still more preferred are a hydrogen atom, a 2-hydroxybenzyl group, a 3-hydroxybenzyl group, and a 4-hydroxybenzyl group.
[0140] From the perspective of solubility in organic solvents, R 113 or R 114 The monovalent organic group is preferably a linear or branched alkyl group, a cyclic alkyl group, or an aromatic group, and more preferably an alkyl group substituted with an aromatic group.
[0141] The number of carbon atoms of the alkyl group is preferably 1 to 30. The alkyl group may be any of a straight chain, a branched chain, or a cyclic chain. Examples of the straight chain or branched chain alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a dodecyl group, a tetradecyl group, an octadecyl group, an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a 1-ethylpentyl group, a 2-ethylhexyl group, a 2-(2-(2-methoxyethoxy)ethoxy)ethoxy)ethoxy group, a 2-(2-(2-methoxyethoxy)ethoxy)ethoxy)ethoxy group, and a 2-(2-(2-(2-ethoxyethoxy)ethoxy)ethoxy)ethoxy)ethoxy group. The cyclic alkyl group may be a monocyclic cyclic alkyl group or a polycyclic cyclic alkyl group. As monocyclic cyclic alkyl, for example, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl and cyclooctyl can be mentioned. As polycyclic cyclic alkyl, for example, adamantyl, norbornyl, bornyl, camphenyl, decahydronaphthyl, tricyclodecyl, tetracyclodecyl, bornyl, dicyclohexyl and pyridyl can be mentioned. Among them, from the viewpoint of taking into account high sensitivity, cyclohexyl is most preferred. And, as the alkyl substituted with an aromatic group, a linear alkyl substituted with an aromatic group described later is preferred.
[0142] Specifically, the aromatic group includes a substituted or unsubstituted benzene ring, a naphthalene ring, a pentalene ring, an indene ring, an azulene ring, a heptalene ring, an indenyl ring, a perylene ring, a pentacene ring, an acenaphthene ring, a phenanthrene ring, an anthracene ring, a tetracene ring, Preferably, the ring is a benzofuran ring, a benzothiophene ring, an isobenzothiophene ring, a quinolizine ring, a quinoline ring, a phthalazine ring, a naphthyridine ring, a quinoxaline ring, an isoxazoline ring, an isoquinoline ring, a carbazole ring, a phenanthridine ring, an acridine ring, a phenanthroline ring, a thianthracene ring, a benzopyran ring, a xanthene ring, a phenoxathiol ring, a phenothiazine ring or a phenazine ring. The most preferred ring is a benzene ring.
[0143] In formula (2), R 113 In the case of a hydrogen atom or in the case of R 114 When it is a hydrogen atom, the polyimide precursor can form a counter salt with a tertiary amine compound having an ethylenically unsaturated bond. Examples of such tertiary amine compounds having an ethylenically unsaturated bond include N,N-dimethylaminopropyl methacrylate.
[0144] R 113 and R 114At least one of the groups may be a polarity conversion group such as an acid-decomposable group. The acid-decomposable group is not particularly limited as long as it is decomposed by an acid to generate an alkali-soluble group such as a phenolic hydroxyl group or a carboxyl group, but an acetal group, a ketal group, a silyl group, a silyl ether group, a tertiary alkyl ester group, etc. are preferred, and an acetal group is more preferred from the viewpoint of exposure sensitivity.
[0145] Specific examples of the acid-decomposable group include tert-butoxycarbonyl, isopropoxycarbonyl, tetrahydropyranyl, tetrahydrofuranyl, ethoxyethyl, methoxyethyl, ethoxymethyl, trimethylsilyl, tert-butoxycarbonylmethyl, trimethylsilyl ether, etc. From the viewpoint of exposure sensitivity, ethoxyethyl or tetrahydrofuranyl is preferred.
[0146] Furthermore, it is also preferred that the polyimide precursor has fluorine atoms in the structural unit. The fluorine atom content in the polyimide precursor is preferably 10% by mass or more and preferably 20% by mass or less.
[0147] Furthermore, the polyimide precursor may be copolymerized with an aliphatic group having a siloxane structure for the purpose of improving adhesion to the substrate. Specifically, as the diamine component, there can be mentioned an embodiment using bis(3-aminopropyl)tetramethyldisiloxane, bis(p-aminophenyl)octamethylpentasiloxane, and the like.
[0148] The repeating unit represented by formula (2) is preferably a repeating unit represented by formula (2-A). That is, at least one of the polyimide precursors used in the present invention is preferably a precursor having a repeating unit represented by formula (2-A). By setting such a structure, the width of the exposure latitude can be further expanded.
[0149] Formula (2-A)
[0150] [Chemical formula 9]
[0151]
[0152] In formula (2-A), A 1 and A 2 represents oxygen atom, R 111 and R 112 Each independently represents a divalent organic group, R 113 and R 114 Each independently represents a hydrogen atom or a monovalent organic group, R 113 and R 114 At least one of them is a group containing a polymerizable group, and preferably both of them are polymerizable groups.
[0153] A 1 , A 2 , R 111 , R 113 and R114 and A in formula (2) independently. 1 , A 2 , R 111 , R 113 and R 114 The meanings are the same and the preferred ranges are also the same.
[0154] R 112 With R in formula (5) 112 The meanings are the same and the preferred ranges are also the same.
[0155] The polyimide precursor may contain one or more repeating structural units represented by formula (2). Furthermore, the polyimide precursor may contain structural isomers of the repeating units represented by formula (2). Furthermore, in addition to the repeating units of formula (2), the polyimide precursor may also contain other types of repeating structural units.
[0156] As a repeating unit having at least one of a cyclic imide structure and a cyclic isoimide structure, the polyimide precursor preferably contains at least one repeating unit selected from the repeating units represented by any one of the following formulas (2-1) to (2-6), and more preferably contains at least one repeating unit selected from the repeating unit represented by the following formula (2-1), the repeating unit represented by the following formula (2-2) and the repeating unit represented by the following formula (2-3).
[0157] [Chemical formula 10]
[0158]
[0159] In formula (2-1) to formula (2-6), R 111 , R 113 , R 114 , R 115 , A 1 and A 2 Respectively with R in the above formula (2) 111 , R 113 , R 114 , R 115 , A 1 and A 2 The meanings are the same and the preferred aspects are also the same.
[0160] The total content of the repeating units represented by any one of Formula (2-1) to Formula (2-6) may be an amount such that the total content of the cyclic imide structure and the cyclic isomide structure in the polyimide precursor is within the above range.
[0161] As one embodiment of the polyimide precursor in the present invention, the total content of the repeating unit represented by the repeating unit represented by any one of the formulas (2-1) to (2-6) can be cited as 50 mol% or more of all repeating units. The above-mentioned total content is more preferably 70 mol% or more, further preferably 90 mol% or more, and particularly preferably more than 90 mol%. There is no particular limitation on the upper limit of the above-mentioned total content, except that all repeating units in the polyimide precursor at the end can be any one of the repeating units represented by the repeating unit represented by the formula (2) and any one of the repeating units represented by any one of the formulas (2-1) to (2-6).
[0162] The weight average molecular weight (Mw) of the polyimide precursor is preferably 18,000 to 30,000, more preferably 20,000 to 27,000, and further preferably 22,000 to 25,000. The number average molecular weight (Mn) is preferably 7,200 to 14,000, more preferably 8,000 to 12,000, and further preferably 9,200 to 11,200.
[0163] The molecular weight dispersion of the polyimide precursor is preferably 2.5 or more, more preferably 2.7 or more, and further preferably 2.8 or more. The upper limit of the molecular weight dispersion of the polyimide precursor is not particularly specified, for example, preferably 4.5 or less, more preferably 4.0 or less, further preferably 3.8 or less, further preferably 3.2 or less, further preferably 3.1 or less, further preferably 3.0 or less, and particularly preferably 2.95 or less.
[0164] In this specification, the molecular weight dispersion refers to a value calculated by weight average molecular weight / number average molecular weight.
[0165] 〔Polybenzoxazole precursor〕
[0166] The polybenzoxazole precursor used in the present invention has no particular restrictions on its structure, etc., but preferably contains a repeating unit represented by the following formula (3).
[0167] [Chemical formula 11]
[0168]
[0169] In formula (3), R 121 represents a divalent organic group, R 122 represents a tetravalent organic group, R 123 and R 124 Each independently represents a hydrogen atom or a monovalent organic group.
[0170] In formula (3), R 123 and R 124Respectively with R in formula (2) 113 The meanings are the same and the preferred ranges are also the same. That is, it is preferred that at least one is a polymerizable group.
[0171] In formula (3), R 121 represents a divalent organic group. As the divalent organic group, a group containing at least one of an aliphatic group and an aromatic group is preferred. As the aliphatic group, a straight-chain aliphatic group is preferred. 121 A dicarboxylic acid residue is preferred. Only one type of the dicarboxylic acid residue may be used, or two or more types may be used.
[0172] As the dicarboxylic acid residue, a dicarboxylic acid residue containing an aliphatic group and a dicarboxylic acid residue containing an aromatic group are preferred, and a dicarboxylic acid residue containing an aromatic group is more preferred.
[0173] As the dicarboxylic acid containing an aliphatic group, a dicarboxylic acid containing a linear or branched (preferably linear) aliphatic group is preferred, and a dicarboxylic acid composed of a linear or branched (preferably linear) aliphatic group and two -COOH groups is more preferred. The number of carbon atoms in the linear or branched (preferably linear) aliphatic group is preferably 2 to 30, more preferably 2 to 25, further preferably 3 to 20, further preferably 4 to 15, and particularly preferably 5 to 10. The linear aliphatic group is preferably an alkylene group.
[0174] Examples of the dicarboxylic acid containing a linear aliphatic group include malonic acid, dimethylmalonic acid, ethylmalonic acid, isopropylmalonic acid, di-n-butylmalonic acid, succinic acid, tetrafluorosuccinic acid, methylsuccinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, dimethylmethylsuccinic acid, glutaric acid, hexafluoroglutaric acid, 2-methylglutaric acid, 3-methylglutaric acid, 2,2-dimethylglutaric acid, 3,3-dimethylglutaric acid, 3-ethyl-3-methylglutaric acid, adipic acid, octafluoroadipic acid, 3-methyladipic acid, pimelic acid, 2,2,6,6-tetramethyl Pimelic acid, suberic acid, dodecanedioic acid, azelaic acid, sebacic acid, hexafluorosebacic acid, 1,9-azelaic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, eicosanedioic acid, eicosanedioic acid Monoacanedioic acid, behenedioic acid, tricosanedioic acid, tetracosanedioic acid, pentacosanedioic acid, hexacosanedioic acid, heptacosanedioic acid, octacanedioic acid, nonacosanedioic acid, triacontanedioic acid, triacontanedioic acid, triacontanedioic acid, diglycolic acid acid) and dicarboxylic acids represented by the following formula, etc.
[0175] [Chemical formula 12]
[0176]
[0177] (In the formula, Z is a hydrocarbon group having 1 to 6 carbon atoms, and n is an integer of 1 to 6.)
[0178] As the dicarboxylic acid containing an aromatic group, the following dicarboxylic acids having an aromatic group are preferred, and the following dicarboxylic acids consisting only of an aromatic group and two -COOH groups are more preferred.
[0179] [Chemical formula 13]
[0180]
[0181] In the formula, A represents a divalent group selected from -CH2-, -O-, -S-, -SO2-, -CO-, -NHCO-, -C(CF3)2- and -C(CH3)2-, and * independently represents a bonding site with other structures.
[0182] Specific examples of the dicarboxylic acid containing an aromatic group include 4,4′-carbonyldibenzoic acid, 4,4′-dicarboxydiphenyl ether, and terephthalic acid.
[0183] And, R 121 It may be a structure derived from a dicarboxylic acid or a dicarboxylic acid halide containing a benzoxazole structure. 121 With the above structure, a benzoxazole structure can be introduced into a benzoxazole precursor.
[0184] Examples of the above structure include the following structures. In the following structures, * each independently represents a bonding site with another structure.
[0185] [Chemical formula 14]
[0186]
[0187] In formula (3), R 122 represents a tetravalent organic group. As a tetravalent organic group, R in the above formula (2) 115 The meanings are the same and the preferred ranges are also the same.
[0188] R 122A group derived from a bisaminophenol derivative is also preferred. Examples of the group derived from a bisaminophenol derivative include 3,3'-diamino-4,4'-dihydroxybiphenyl, 4,4'-diamino-3,3'-dihydroxybiphenyl, 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone, 4,4'-diamino-3,3'-dihydroxydiphenyl sulfone, bis-(3-amino-4-hydroxyphenyl)methane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis-(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,2-bis-(4 2,2-bis-(4-amino-3-hydroxyphenyl)propane, 4,4'-diamino-3,3'-dihydroxybenzophenone, 3,3'-diamino-4,4'-dihydroxybenzophenone, 4,4'-diamino-3,3'-dihydroxydiphenyl ether, 3,3'-diamino-4,4'-dihydroxydiphenyl ether, 1,4-diamino-2,5-dihydroxybenzene, 1,3-diamino-2,4-dihydroxybenzene, 1,3-diamino-4,6-dihydroxybenzene, etc. These bisaminophenols can be used alone or in combination.
[0189] Among the bisaminophenol derivatives, the following bisaminophenol derivatives having an aromatic group are preferred.
[0190] [Chemical formula 15]
[0191]
[0192] In the formula, X1 represents -O-, -S-, -C(CF3)2-, -CH2-, -SO2-, -NHCO-, * and # represent the bonding sites with other structures respectively. R represents a hydrogen atom or a monovalent substituent, preferably a hydrogen atom or a hydrocarbon group, more preferably a hydrogen atom or an alkyl group. And, R 122 The structure represented by the above formula is also preferred. 122 In the case of the structure represented by the above formula, among the total of 4 * and #, it is preferred that any two of them are the same as R in formula (3). 122 The other two are the bonding sites of the nitrogen atom to which the R 122 The bonding site of the oxygen atom to which the bond is attached is preferably 2 * to R in formula (3). 122 The two # are the same as those of R in formula (3). 122 The bonding site of the nitrogen atom to which it is bonded, or the two * are R in formula (3) 122 The bonding site of the nitrogen atom to which it is bonded, and the two # are the same as R in formula (3) 122 The bonding site of the oxygen atom to which the bond is attached is preferably 2 * which is the same as R in formula (3). 122The two # are the same as those of R in formula (3). 122 The bonding site of the bonded nitrogen atom.
[0193] [Chemical formula 16]
[0194]
[0195] In formula (As), R1 is a hydrogen atom, an alkylene group, a substituted alkylene group, -O-, -S-, -SO2-, -CO-, -NHCO-, a single bond, or an organic group selected from the group of the following formula (A-sc). R2 is any one of a hydrogen atom, an alkyl group, an alkoxy group, an acyloxy group, and a cyclic alkyl group, which may be the same or different. R3 is any one of a hydrogen atom, a linear or branched alkyl group, an alkoxy group, an acyloxy group, and a cyclic alkyl group, which may be the same or different.
[0196] [Chemical formula 17]
[0197]
[0198] (In formula (A-sc), * represents an aromatic ring bonded to the aminophenol group of the bisaminophenol derivative represented by the above formula (As).)
[0199] In the above formula (As), it is particularly preferred to have a substituent at R3 ortho to the phenolic hydroxyl group because this brings the carbonyl carbon of the amide bond and the hydroxyl group closer together, thereby further improving the effect of a high cyclization rate during curing at low temperatures.
[0200] In the above formula (As), when R2 is an alkyl group and R3 is an alkyl group, it is preferable because high transparency to i-rays and a high cyclization rate can be maintained during curing at a low temperature.
[0201] Furthermore, in the above formula (As), it is further preferred that R1 is an alkylene group or a substituted alkylene group. Specific examples of the alkylene group and the substituted alkylene group of R1 include a linear or branched alkyl group having 1 to 8 carbon atoms, among which -CH2-, -CH(CH3)-, and -C(CH3)2- are more preferred from the viewpoint of obtaining a polybenzoxazole precursor having an excellent balance of maintaining high transparency to i-rays and high cyclization rate when cured at low temperature and having sufficient solubility in solvents.
[0202] As a method for producing the bisaminophenol derivative represented by the above formula (As), for example, reference can be made to paragraphs 0085 to 0094 and Example 1 (paragraphs 0189 to 0190) of JP-A-2013-256506, the contents of which are incorporated herein.
[0203] Specific examples of the structure of the bisaminophenol derivative represented by the formula (As) include structures described in paragraphs 0070 to 0080 of JP-A-2013-256506, and the contents thereof are incorporated herein, but are not limited thereto.
[0204] The polybenzoxazole precursor may contain other types of repeating structural units in addition to the repeating unit of the above formula (3).
[0205] As the repeating unit having a benzoxazole structure, the polybenzoxazole precursor preferably contains at least one repeating unit selected from the group consisting of a repeating unit represented by the following formula (3-1), a repeating unit represented by the following formula (3-2), and a repeating unit represented by the following formula (3-3).
[0206] [Chemical formula 18]
[0207]
[0208] In formula (3-1) to formula (3-3), R 121 , R 122 , R 123 and R 124 Respectively with R in formula (3) 121 , R 122 , R 123 and R 124 The same meaning applies, and the preferred aspects are also the same.
[0209] The content of the repeating unit represented by the formula (3-1), the repeating unit represented by the formula (3-2), and the repeating unit represented by the formula (3-3) may be such that the content of the benzoxazole structure in the polybenzoxazole precursor is within the above range.
[0210] Furthermore, from the viewpoint of being able to suppress warping associated with ring closure, the polybenzoxazole precursor preferably contains a diamine residue represented by the following formula (SL) as another type of repeating structural unit.
[0211] [Chemical formula 19]
[0212]
[0213] In formula (SL), Z has structure a and structure b, and R 1s is a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, R 2s is a hydrocarbon group having 1 to 10 carbon atoms, R 3s , R 4s , R 5s , R 6sAt least one of them is an aromatic group, and the rest are hydrogen atoms or organic groups having 1 to 30 carbon atoms, which may be the same or different. The polymerization of structure a and structure b may be block polymerization or random polymerization. Regarding the mole % of the Z part, structure a is 5 to 95 mole %, structure b is 95 to 5 mole %, and a+b is 100 mole %.
[0214] In formula (SL), preferred Z includes R in structure b. 5s and R 6s Z is a phenyl group. The molecular weight of the structure represented by formula (SL) is preferably 400 to 4,000, more preferably 500 to 3,000. By setting the molecular weight within the above range, the elastic modulus of the polybenzoxazole precursor after dehydration ring closure can be more effectively reduced, and both the effect of suppressing warpage and the effect of improving solvent solubility can be achieved.
[0215] When the diamine residue represented by the formula (SL) is included as another type of repeating structural unit, it is also preferred to further include a tetracarboxylic acid residue remaining after removing the anhydride group from tetracarboxylic dianhydride as a repeating structural unit. Examples of such a tetracarboxylic acid residue include R in the formula (2): 115 Example.
[0216] For example, when a polybenzoxazole precursor is used in the composition described below, the weight average molecular weight (Mw) of the polybenzoxazole precursor is preferably 18,000 to 30,000, more preferably 20,000 to 29,000, and further preferably 22,000 to 28,000. The number average molecular weight (Mn) is preferably 7,200 to 14,000, more preferably 8,000 to 12,000, and further preferably 9,200 to 11,200.
[0217] The molecular weight dispersion of the polybenzoxazole precursor is preferably 1.4 or more, more preferably 1.5 or more, and further preferably 1.6 or more. The upper limit of the molecular weight dispersion of the polybenzoxazole precursor is not particularly specified, for example, it is preferably 2.6 or less, more preferably 2.5 or less, further preferably 2.4 or less, further preferably 2.3 or less, and further preferably 2.2 or less.
[0218] 〔Polyamide-imide precursor〕
[0219] The polyamideimide precursor preferably includes a repeating unit represented by the following formula (PAI-2).
[0220] [Chemical formula 20]
[0221]
[0222] In the formula (PAI-2), R 117 represents a trivalent organic group, R 111 represents a divalent organic group, A 2 represents an oxygen atom or -NH-, R 113 It represents a hydrogen atom or a monovalent organic group.
[0223] In the formula (PAI-2), R 117 Examples include a linear or branched aliphatic group, a cyclic aliphatic group and an aromatic group, a heteroaromatic group, or a group in which two or more of these are linked via a single bond or a linking group. Preferably, it is a linear aliphatic group having 2 to 20 carbon atoms, a branched aliphatic group having 3 to 20 carbon atoms, a cyclic aliphatic group having 3 to 20 carbon atoms, an aromatic group having 6 to 20 carbon atoms, or a group in which two or more of these are combined via a single bond or a linking group. More preferably, it is an aromatic group having 6 to 20 carbon atoms, or a group in which two or more aromatic groups having 6 to 20 carbon atoms are combined via a single bond or a linking group.
[0224] As the above-mentioned connecting group, preferred are -O-, -S-, -C(=O)-, -S(=O)2-, alkylene, halogenated alkylene, arylene or a connecting group formed by bonding two or more of them, more preferred are -O-, -S-, alkylene, halogenated alkylene, arylene or a connecting group formed by bonding two or more of them.
[0225] The alkylene group is preferably an alkylene group having 1 to 20 carbon atoms, more preferably an alkylene group having 1 to 10 carbon atoms, and still more preferably an alkylene group having 1 to 4 carbon atoms.
[0226] As the above-mentioned haloalkylene group, a haloalkylene group having 1 to 20 carbon atoms is preferred, a haloalkylene group having 1 to 10 carbon atoms is more preferred, and a haloalkylene group having 1 to 4 carbon atoms is more preferred. Furthermore, as the halogen atom in the above-mentioned haloalkylene group, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc. can be mentioned, and a fluorine atom is preferred. The above-mentioned haloalkylene group may have a hydrogen atom, or all hydrogen atoms may be substituted by a halogen atom, but preferably all hydrogen atoms are substituted by a halogen atom. As examples of preferred haloalkylene groups, (ditrifluoromethyl)methylene and the like can be mentioned.
[0227] As the arylene group, a phenylene group or a naphthylene group is preferred, a phenylene group is more preferred, and a 1,3-phenylene group or a 1,4-phenylene group is further preferred.
[0228] And, R 117 It is preferably derived from a tricarboxylic acid compound in which at least one carboxyl group may be halogenated. As the halogenation, chlorination is preferred.
[0229] In the present invention, a compound having three carboxyl groups is referred to as a tricarboxylic acid compound.
[0230] Two of the three carboxyl groups of the above tricarboxylic acid compound may be converted to anhydride.
[0231] Examples of the tricarboxylic acid compound which may be halogenated and is used in the production of the polyamideimide precursor include branched aliphatic, cyclic aliphatic or aromatic tricarboxylic acid compounds.
[0232] These tricarboxylic acid compounds may be used alone or in combination of two or more.
[0233] Specifically, as the tricarboxylic acid compound, a tricarboxylic acid compound containing a linear aliphatic group having 2 to 20 carbon atoms, a branched aliphatic group having 3 to 20 carbon atoms, a cyclic aliphatic group having 3 to 20 carbon atoms, an aromatic group having 6 to 20 carbon atoms, or a group in which two or more of these are combined via a single bond or a linking group is preferred, and a tricarboxylic acid compound containing an aromatic group having 6 to 20 carbon atoms, or a group in which two or more aromatic groups having 6 to 20 carbon atoms are combined via a single bond or a linking group is more preferred.
[0234] In addition, specific examples of tricarboxylic acid compounds include 1,2,3-propanetricarboxylic acid, 1,3,5-pentanetricarboxylic acid, citric acid, trimellitic acid, 2,3,6-naphthalenetricarboxylic acid, phthalic acid (or phthalic anhydride) and benzoic acid compounds connected by a single bond, -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, -SO2- or phenylene.
[0235] These compounds may be compounds in which two carboxyl groups are anhydrified (for example, trimellitic anhydride), or compounds in which at least one carboxyl group is halogenated (for example, trimellitic anhydride chloride).
[0236] In the formula (PAI-2), R 111 , A 2 , R 113 The meanings of are respectively the same as those of R in the above formula (2) 111 , A 2 , R 113 The meanings are the same and the preferred aspects are also the same.
[0237] The polyamideimide precursor may also contain other repeating units.
[0238] Examples of other repeating units include the repeating unit represented by the above-mentioned formula (2), the repeating unit represented by any one of formulae (2-1) to (2-6), and the repeating unit represented by the following formula (PAI-1).
[0239] [Chemical formula 21]
[0240]
[0241] In the formula (PAI-1), R 116 represents a divalent organic group, R 111 It represents a divalent organic group.
[0242] In the formula (PAI-1), R 116 Examples include a linear or branched aliphatic group, a cyclic aliphatic group and an aromatic group, a heteroaromatic group, or a group in which two or more of these are linked via a single bond or a linking group. Preferably, it is a linear aliphatic group having 2 to 20 carbon atoms, a branched aliphatic group having 3 to 20 carbon atoms, a cyclic aliphatic group having 3 to 20 carbon atoms, an aromatic group having 6 to 20 carbon atoms, or a group in which two or more of these are combined via a single bond or a linking group. More preferably, it is an aromatic group having 6 to 20 carbon atoms, or a group in which two or more aromatic groups having 6 to 20 carbon atoms are combined via a single bond or a linking group.
[0243] As the above-mentioned connecting group, preferred are -O-, -S-, -C(=O)-, -S(=O)2-, alkylene, halogenated alkylene, arylene or a connecting group formed by bonding two or more of them, more preferred are -O-, -S-, alkylene, halogenated alkylene, arylene or a connecting group formed by bonding two or more of them.
[0244] The alkylene group is preferably an alkylene group having 1 to 20 carbon atoms, more preferably an alkylene group having 1 to 10 carbon atoms, and still more preferably an alkylene group having 1 to 4 carbon atoms.
[0245] As the above-mentioned haloalkylene group, a haloalkylene group having 1 to 20 carbon atoms is preferred, a haloalkylene group having 1 to 10 carbon atoms is more preferred, and a haloalkylene group having 1 to 4 carbon atoms is more preferred. Furthermore, as the halogen atom in the above-mentioned haloalkylene group, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc. can be mentioned, and a fluorine atom is preferred. The above-mentioned haloalkylene group may have a hydrogen atom, or all hydrogen atoms may be substituted by a halogen atom, but preferably all hydrogen atoms are substituted by a halogen atom. As examples of preferred haloalkylene groups, (ditrifluoromethyl)methylene and the like can be mentioned.
[0246] As the arylene group, a phenylene group or a naphthylene group is preferred, a phenylene group is more preferred, and a 1,3-phenylene group or a 1,4-phenylene group is further preferred.
[0247] And, R 116 Preferably, it is derived from a dicarboxylic acid compound or a dicarboxylic acid dihalide compound.
[0248] In the present invention, a compound having two carboxyl groups is referred to as a dicarboxylic acid compound, and a compound having two halogenated carboxyl groups is referred to as a dicarboxylic acid dihalide compound.
[0249] The carboxyl group in the dicarboxylic acid dihalide compound may be halogenated, but is preferably chlorinated, for example. That is, the dicarboxylic acid dihalide compound is preferably a dicarboxylic acid dichloride compound.
[0250] Examples of the dicarboxylic acid compound or dicarboxylic acid dihalide compound which may be halogenated and is used in the production of the polyamideimide precursor include linear or branched aliphatic, cyclic aliphatic or aromatic dicarboxylic acid compounds or dicarboxylic acid dihalide compounds.
[0251] These dicarboxylic acid compounds or dicarboxylic acid dihalide compounds may be used alone or in combination of two or more.
[0252] Specifically, as the dicarboxylic acid compound or dicarboxylic acid dihalide compound, a dicarboxylic acid compound or dicarboxylic acid dihalide compound containing a linear aliphatic group having 2 to 20 carbon atoms, a branched aliphatic group having 3 to 20 carbon atoms, a cyclic aliphatic group having 3 to 20 carbon atoms, an aromatic group having 6 to 20 carbon atoms, or a group formed by combining two or more of these groups via a single bond or a linking group is preferred, and a dicarboxylic acid compound or dicarboxylic acid dihalide compound containing an aromatic group having 6 to 20 carbon atoms, or a group formed by combining two or more aromatic groups having 6 to 20 carbon atoms via a single bond or a linking group is more preferred.
[0253] Specific examples of the dicarboxylic acid compound include malonic acid, dimethylmalonic acid, ethylmalonic acid, isopropylmalonic acid, di-n-butylmalonic acid, succinic acid, tetrafluorosuccinic acid, methylsuccinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, dimethylmethylsuccinic acid, glutaric acid, hexafluoroglutaric acid, 2-methylglutaric acid, 3-methylglutaric acid, 2,2-dimethylglutaric acid, 3,3-dimethylglutaric acid, 3-ethyl-3-methylglutaric acid, adipic acid, octafluoroadipic acid, 3-methyladipic acid, pimelic acid, 2,2,6,6-tetrafluorohexanedioic acid, 3-methylhexanedioic acid, 2,3-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, 2,3-dimethylmethylsuccinic acid, glutaric acid, hexafluoroglutaric acid, 2,2-dimethylglutaric acid, 3,3-dimethylglutaric acid, 3-ethyl-3-methylglutaric acid, adipic acid, octafluoroadipic acid, 3-methyladipic acid, pimelic acid, 2,2,6,6-tetrafluorohexanedioic acid, 2,3-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, 2,3-dimethylmethylsuccinic acid, 2,3-dimethyl Methyl pimelic acid, suberic acid, dodecanedioic acid, azelaic acid, sebacic acid, hexafluorosebacic acid, 1,9-azelaic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, eicosanedioic acid, eicosanedioic acid Monoacanedioic acid, behenedioic acid, tricosanedioic acid, tetracosanedioic acid, pentacosanedioic acid, hexacosanedioic acid, heptacosanedioic acid, octacanedioic acid, nonacosanedioic acid, triacontanedioic acid, triacontanedioic acid, triacontanedioic acid, diglycolic acid acid), phthalic acid, isophthalic acid, terephthalic acid, 4,4'-biphenylcarboxylic acid, 4,4'-biphenylcarboxylic acid, 4,4'-dicarboxydiphenyl ether, benzophenone-4,4'-dicarboxylic acid, etc.
[0254] Specific examples of the dicarboxylic acid dihalide compound include compounds having a structure in which two carboxyl groups among the specific examples of the above-mentioned dicarboxylic acid compounds are halogenated.
[0255] In the formula (PAI-1), R 111 The meaning of is the same as R in the above formula (2) 111 The meanings are the same and the preferred aspects are also the same.
[0256] As a repeating unit having at least one of a cyclic imide structure and a cyclic isoimide structure, the polyamideimide precursor preferably contains a repeating unit represented by any one of the following formulas (PAI-3) and (PAI-4), and more preferably contains a repeating unit represented by the following formula (PAI-3).
[0257] [Chemical formula 22]
[0258]
[0259] In formula (PAI-3) or formula (PAI-4), R 111 and R 117 Respectively with R in formula (PAI-2) 111 and R 117 The same meaning applies, and the preferred aspects are also the same.
[0260] The content of the repeating unit represented by either of the formulae (PAI-3) and (PAI-4) may be such that the total content of the cyclic imide structure and the cyclic isoimide structure in the polyamide-imide precursor falls within the above range.
[0261] Furthermore, the polyamide-imide also preferably has fluorine atoms in the structural unit. The fluorine atom content in the polyamide-imide precursor is preferably 10% by mass or more and preferably 20% by mass or less.
[0262] Furthermore, the polyamideimide precursor may be copolymerized with an aliphatic group having a siloxane structure for the purpose of improving adhesion to the substrate. Specifically, as the diamine component, there may be mentioned an embodiment using bis(3-aminopropyl)tetramethyldisiloxane, bis(p-aminophenyl)octamethylpentasiloxane, and the like.
[0263] As one embodiment of the polyamide-imide precursor in the present invention, the total content of the repeating unit represented by the formula (PAI-2), the repeating unit represented by the formula (PAI-1), the repeating unit represented by the formula (PAI-3), the repeating unit represented by the formula (PAI-4), the repeating unit represented by the formula (2), and the repeating unit represented by any one of the formulas (2-1) to (2-6) is 50 mol% or more of all the repeating units. The above total content is more preferably 70 mol% or more, further preferably 90 mol% or more, and particularly preferably more than 90 mol%. There is no particular limitation on the upper limit of the above-mentioned total content, except that all repeating units in the terminal polyamideimide precursor may be a repeating unit represented by formula (PAI-2), a repeating unit represented by formula (PAI-1), a repeating unit represented by any one of formulas (PAI-3) and (PAI-4), a repeating unit represented by formula (2), or a repeating unit represented by any one of formulas (2-1) to (2-6).
[0264] In addition, as another embodiment of the polyamide-imide precursor in the present invention, the total content of the repeating unit represented by the formula (PAI-2), the repeating unit represented by the formula (PAI-1), and the repeating unit represented by any one of the formulas (PAI-3) and (PAI-4) can be 50 mol% or more of all the repeating units. The above-mentioned total content is more preferably 70 mol% or more, further preferably 90 mol% or more, and particularly preferably more than 90 mol%. There is no particular limitation on the upper limit of the above-mentioned total content, except that all the repeating units in the polyamide-imide precursor at the end can be any one of the repeating units represented by the formula (PAI-2), the repeating unit represented by the formula (PAI-1), or the repeating unit represented by any one of the formulas (PAI-3) and (PAI-4).
[0265] The weight average molecular weight (Mw) of the polyamideimide precursor is preferably 2,000 to 500,000, more preferably 5,000 to 100,000, and further preferably 10,000 to 50,000. The number average molecular weight (Mn) is preferably 800 to 250,000, more preferably 2,000 to 50,000, and further preferably 4,000 to 25,000.
[0266] The molecular weight dispersion of the polyamideimide precursor is preferably 1.5 to 3.5, more preferably 2 to 3.
[0267] In this specification, the molecular weight dispersion refers to a value obtained by dividing the weight average molecular weight by the number average molecular weight (weight average molecular weight / number average molecular weight).
[0268] [Method for producing polyimide precursor, etc.]
[0269] The polyimide precursor and the like are obtained by reacting dicarboxylic acid or a dicarboxylic acid derivative with diamine, and are preferably obtained by halogenating dicarboxylic acid or a dicarboxylic acid derivative with a halogenating agent and then reacting with diamine.
[0270] In the method for producing a polyimide precursor, etc., it is preferred to use an organic solvent when performing the reaction. The organic solvent may be one kind or two or more kinds.
[0271] The organic solvent can be appropriately specified depending on the raw material, and examples thereof include pyridine, diethylene glycol dimethyl ether (diglyme), N-methylpyrrolidone, and N-ethylpyrrolidone.
[0272] Furthermore, it is also preferred that the above-mentioned halogenating agent is not used but a non-halogen catalyst is used for synthesis. As the above-mentioned non-halogen catalyst, a known amidation catalyst that does not contain a halogen atom can be used without particular limitation, for example, a boroxine trimer compound, an N-hydroxy compound, a tertiary amine, a phosphate ester, an amine salt, a urea compound, a carbodiimide compound, etc. can be cited. As the above-mentioned carbodiimide compound, N,N'-diisopropylcarbodiimide, N,N'-dicyclohexylcarbodiimide, etc. can be cited.
[0273] In the method for producing a polyimide precursor, etc., it is preferred to use an organic solvent when performing the reaction. The organic solvent may be one kind or two or more kinds.
[0274] The organic solvent can be appropriately specified depending on the raw material, and examples thereof include pyridine, diethylene glycol dimethyl ether (diglyme), N-methylpyrrolidone, and N-ethylpyrrolidone.
[0275] In the synthesis of polyimide, for example, by appropriately setting the reaction time, reaction temperature, and pH during the reaction of a dicarboxylic acid or a dicarboxylic acid derivative (which may be halogenated by a halogenating agent or may not be halogenated but a non-halogen catalyst is used) with a diamine, the total molar content of the cyclic imide structure and the cyclic isoimide structure, or the molar content of the benzoxazole structure can be adjusted.
[0276] -Capping agent-
[0277] When producing a polyimide precursor, in order to further improve storage stability, it is preferred to seal the ends of the polyimide precursor with an end-capping agent such as an acid anhydride, a monocarboxylic acid, a monoacyl chloride compound, or a monoactive ester compound. As the end-capping agent, a monoamine is more preferably used, and preferred monoamine compounds include aniline, 2-ethynylaniline, 3-ethynylaniline, 4-ethynylaniline, 5-amino-8-hydroxyquinoline, 1-hydroxy-7-aminonaphthalene, 1-hydroxy-6-aminonaphthalene, 1-hydroxy-5-aminonaphthalene, 1-hydroxy-4-aminonaphthalene, 2-hydroxy-7-aminonaphthalene, 2-hydroxy-6-aminonaphthalene, 2-hydroxy-5-aminonaphthalene, 1-carboxy-7-aminonaphthalene, 1-carboxy-6-aminonaphthalene, 1-carboxy- 5-aminonaphthalene, 2-carboxy-7-aminonaphthalene, 2-carboxy-6-aminonaphthalene, 2-carboxy-5-aminonaphthalene, 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, 2-aminobenzenesulfonic acid, 3-aminobenzenesulfonic acid, 4-aminobenzenesulfonic acid, 3-amino-4,6-dihydroxypyrimidine, 2-aminophenol, 3-aminophenol, 4-aminophenol, 2-aminothiophenol, 3-aminothiophenol, 4-aminothiophenol, etc. Two or more of these may be used, and a plurality of different terminal groups may be introduced by reacting a plurality of end-capping agents.
[0278] -Solid Precipitation-
[0279] When producing a polyimide precursor, etc., a step of precipitating a solid may be included. Specifically, a polyimide precursor, etc. in a reaction solution is precipitated in water, and then dissolved in a solvent such as tetrahydrofuran in which the polyimide precursor, etc. is soluble, so that a solid can be precipitated.
[0280] Then, the polyimide precursor etc. are dried to obtain a powdery polyimide precursor etc.
[0281] 〔content〕
[0282] The content of the specific resin in the composition of the present invention is preferably 20% by mass or more, more preferably 30% by mass or more, further preferably 40% by mass or more, further preferably 50% by mass or more, relative to the total solid content of the composition. Furthermore, the content of the resin in the composition of the present invention is preferably 99.5% by mass or less, more preferably 99% by mass or less, further preferably 98% by mass or less, further preferably 97% by mass or less, and further preferably 95% by mass or less, relative to the total solid content of the composition.
[0283] The composition of the present invention may contain only one specific resin or two or more specific resins. When containing two or more specific resins, the total amount is preferably within the above range.
[0284] Furthermore, the curable resin composition of the present invention preferably contains at least two kinds of resins.
[0285] Specifically, the curable resin composition of the present invention may contain two or more specific resins and other resins described below in total, or may contain two or more specific resins, but preferably contains two or more specific resins.
[0286] When the curable resin composition of the present invention contains two or more specific resins, for example, it is preferred to contain a polyimide precursor and a structure derived from a dianhydride (R 115 ) Two or more different polyimide precursors.
[0287] When the curable resin composition of the present invention contains two or more polyimide precursors, the total molar content of the cyclic imide structure and the cyclic isoimide structure contained in at least one polyimide precursor may be within the above-mentioned range. With respect to the case where the total amount of all polyimide precursors is set to 1g, the total molar content of the cyclic imide structure and the cyclic isoimide structure contained in all polyimide precursors is preferably within the above-mentioned range. The polyimide precursor contained in the curable resin composition more preferably contains the cyclic imide structure and the cyclic isoimide structure within the above-mentioned range, respectively.
[0288] When the curable resin composition of the present invention contains two or more polybenzoxazole precursors, the molar content of the benzoxazole structure contained in at least one polybenzoxazole precursor may be within the above range. The total molar content of the benzoxazole structure contained in all the polybenzoxazole precursors relative to the total amount of all the polybenzoxazole precursors is set to 1g is preferably within the above range. The polyimide precursor contained in the curable resin composition more preferably contains at least one of a cyclic imide structure and a cyclic isoimide structure within the above range.
[0289] When the curable resin composition of the present invention contains two or more polyamideimide precursors, the total molar content of the cyclic imide structure and the cyclic isoimide structure contained in at least one polyamideimide precursor may be within the above-mentioned range. With respect to the case where the total amount of all polyamideimide precursors is set to 1g, the total molar content of the cyclic imide structure and the cyclic isoimide structure contained in all polyamideimide precursors is preferably within the above-mentioned range. The polyamideimide precursor contained in the curable resin composition more preferably contains at least one of the cyclic imide structure and the cyclic isoimide structure within the above-mentioned range.
[0290] <Organometallic complex>
[0291] The curable resin composition of the present invention contains an organic metal complex.
[0292] The organometallic complex may be any organic complex compound containing a metal atom, and is preferably a complex compound containing a metal atom and an organic group, more preferably a compound in which an organic group is coordinated to a metal atom, and still more preferably a metallocene compound.
[0293] In the present invention, the metallocene compound refers to an organic metal complex having two cyclopentadienyl derivatives which may have substituents as η5-ligands.
[0294] The organic group is not particularly limited, but is preferably a group consisting of a hydrocarbon group or a combination of a hydrocarbon group and a hetero atom. The hetero atom is preferably an oxygen atom, a sulfur atom, or a nitrogen atom.
[0295] In the present invention, it is preferred that at least one of the organic groups is a cyclic group, and it is more preferred that at least two of the organic groups are cyclic groups.
[0296] The cyclic group is preferably selected from a 5-membered cyclic group and a 6-membered cyclic group, and more preferably a 5-membered cyclic group.
[0297] The cyclic group may be a hydrocarbon ring or a heterocyclic ring, but is preferably a hydrocarbon ring.
[0298] As the 5-membered cyclic group, a cyclopentadienyl group is preferred.
[0299] Furthermore, the organometallic complex used in the present invention preferably contains 2 to 4 cyclic groups in one molecule.
[0300] The metal contained in the organic metal complex is not particularly limited, but a metal corresponding to the Group 4 element is preferred, at least one metal selected from titanium, zirconium and hafnium is more preferred, at least one metal selected from titanium and zirconium is further preferred, and titanium is particularly preferred.
[0301] The organometallic complex may contain two or more metal atoms or one metal atom, but preferably contains one metal atom. When the organometallic complex contains two or more metal atoms, it may contain only one metal atom or two or more metal atoms.
[0302] The organometallic complex is preferably a ferrocene compound, a titanocene compound, a zirconocene compound or a hafnocene compound, more preferably a titanocene compound, a zirconocene compound or a hafnocene compound, further preferably a titanocene compound or a zirconocene compound, and particularly preferably a titanocene compound.
[0303] An embodiment in which the organometallic complex has a photoradical polymerization initiation capability is also one of the preferred embodiments of the present invention.
[0304] According to the present invention, it is considered that the organic metal complex is dispersed in a nearly uniform state in the film by using a specific resin.
[0305] Therefore, it is considered that when the organic metal complex has a photoradical polymerization initiation ability, aggregation of the local radical polymerization initiator caused by aggregation of the organic metal complex can be suppressed.
[0306] It is believed that by suppressing the aggregation of the radical polymerization initiator, the polymerization degree of the specific resin or the crosslinking agent is likely to be nearly uniform in the film, so that the generation of development residues and pattern disconnection are unlikely to occur, and the resolution is likely to be improved.
[0307] In the present invention, having the ability to initiate photo-radical polymerization means that free radicals capable of initiating free radical polymerization can be generated by irradiation with light. For example, when a composition comprising a free radical crosslinking agent and an organic metal complex is irradiated with light in a wavelength region in which the organic metal complex absorbs light and the free radical crosslinking agent does not absorb light, the presence or absence of the ability to initiate photo-radical polymerization can be confirmed by confirming the disappearance of the free radical crosslinking agent. When confirming the disappearance, an appropriate method can be selected according to the type of the free radical crosslinking agent, such as by IR measurement (infrared spectroscopy) or HPLC measurement (high performance liquid chromatography).
[0308] When the organometallic complex has the ability to initiate photoradical polymerization, the organometallic complex is preferably a metallocene compound, more preferably a titanocene compound, a zirconocene compound or a hafnocene compound, further preferably a titanocene compound or a zirconocene compound, and particularly preferably a titanocene compound.
[0309] In the case where the organic metal complex does not have the ability to initiate photoradical polymerization, the organic metal complex is preferably at least one compound selected from titanocene compounds, tetraalkoxytitanium compounds, acylated titanium compounds, chelated titanium compounds, zirconocene compounds and hafnocene compounds, more preferably at least one compound selected from titanocene compounds, zirconocene compounds and hafnocene compounds, further preferably at least one compound selected from titanocene compounds and zirconocene compounds, and particularly preferably a titanocene compound.
[0310] The molecular weight of the organic metal complex is preferably 50 to 2,000, more preferably 100 to 1,000.
[0311] Examples of the organic metal complex include compounds represented by the following formula (P).
[0312] [Chemical formula 23]
[0313]
[0314] In formula (P), M is a metal atom, and R is each independently a substituent.
[0315] It is preferred that the R's are each independently selected from an aromatic group, an alkyl group, a halogen atom, and an alkylsulfonyloxy group.
[0316] In formula (P), the metal atom represented by M is preferably an iron atom, a titanium atom, a zirconium atom or a hafnium atom, more preferably a titanium atom, a zirconium atom or a hafnium atom, further preferably a titanium atom or a zirconium atom, and particularly preferably a titanium atom.
[0317] Examples of the aromatic group in R in the formula (P) include aromatic groups having 6 to 20 carbon atoms, preferably aromatic hydrocarbon groups having 6 to 20 carbon atoms, such as phenyl, 1-naphthyl or 2-naphthyl.
[0318] The alkyl group in R in formula (P) is preferably an alkyl group having 1 to 20 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms, and examples thereof include methyl, ethyl, propyl, octyl, isopropyl, tert-butyl, isopentyl, 2-ethylhexyl, 2-methylhexyl, and cyclopentyl.
[0319] Examples of the halogen atom in the above R include F, Cl, Br and I.
[0320] The alkyl group constituting the alkylsulfonyloxy group in the above R is preferably an alkyl group having 1 to 20 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms, and examples thereof include methyl, ethyl, propyl, octyl, isopropyl, tert-butyl, isopentyl, 2-ethylhexyl, 2-methylhexyl, and cyclopentyl.
[0321] The above R may further have a substituent. Examples of the substituent include a halogen atom (F, Cl, Br, I), a hydroxyl group, a carboxyl group, an amino group, a cyano group, an aryl group, an alkoxy group, an aryloxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an acyloxy group, a monoalkylamino group, a dialkylamino group, a monoarylamino group, and a diarylamino group.
[0322] Specific examples of organic metal complexes are not particularly limited, and examples include tetraisopropoxytitanium, tetra(2-ethylhexyloxy)titanium, diisopropoxybis(ethyl acetoacetate)titanium, diisopropoxybis(acetylacetonate)titanium, bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, pentamethylcyclopentadienyltrimethoxide titanium, bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluorophenyl)titanium and the following compounds.
[0323] [Chemical formula 24]
[0324]
[0325] In addition, the compounds described in paragraphs 0078 to 0088 of International Publication No. 2018 / 025738 can also be used, but are not limited thereto.
[0326] The content of the organic metal complex is preferably 0.1 to 30% by mass relative to the total solid content of the curable resin composition of the present invention. The lower limit is more preferably 1.0% by mass or more, further preferably 1.5% by mass or more, and particularly preferably 3.0% by mass or more. The upper limit is more preferably 25% by mass or less.
[0327] The organic metal complex may be used alone or in combination of two or more. When two or more organic metal complexes are used, the total amount is preferably within the above range.
[0328] <Other resins>
[0329] The composition of the present invention may contain the above-mentioned specific resin and other resins different from the specific resin (hereinafter, also simply referred to as "other resins").
[0330] Examples of other resins include polyamideimide, polyamideimide precursors, phenolic resins, polyamides, epoxy resins, polysiloxanes, resins containing a siloxane structure, and acrylic resins.
[0331] For example, by further adding an acrylic resin, a composition having excellent coating properties can be obtained, and an organic film having excellent solvent resistance can be obtained.
[0332] For example, by adding a high-valent acrylic resin having a weight average molecular weight of 20,000 or less to the composition instead of or in addition to the crosslinking agent described below, the coating properties of the composition and the solvent resistance of the organic film can be improved.
[0333] When the composition of the present invention contains other resins, the content of the other resins is preferably 0.01 mass % or more, more preferably 0.05 mass % or more, further preferably 1 mass % or more, further preferably 2 mass % or more, further preferably 5 mass % or more, and further preferably 10 mass % or more, relative to the total solid content of the composition.
[0334] Furthermore, the content of other resins in the composition of the present invention is preferably 80% by mass or less, more preferably 75% by mass or less, further preferably 70% by mass or less, further preferably 60% by mass or less, and further preferably 50% by mass or less, relative to the total solid content of the composition.
[0335] Furthermore, as a preferred embodiment of the composition of the present invention, the content of the other resin can also be set to a low content. In the above embodiment, the content of the other resin is preferably 20% by mass or less, more preferably 15% by mass or less, further preferably 10% by mass or less, further preferably 5% by mass or less, and further preferably 1% by mass or less relative to the total solid content of the composition. The lower limit of the above content is not particularly limited, as long as it is 0% by mass or more.
[0336] The composition of the present invention may contain only one type of other resin or may contain two or more types. When containing two or more types, it is preferred that the total amount is within the above range.
[0337] <Solvent>
[0338] The curable resin composition of the present invention preferably contains a solvent. Any known solvent can be used as the solvent. The solvent is preferably an organic solvent. Examples of the organic solvent include compounds such as esters, ethers, ketones, cyclic hydrocarbons, sulfoxides, amides, ureas, and alcohols.
[0339] Preferred examples of the esters include ethyl acetate, n-butyl acetate, isobutyl acetate, hexyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, γ-butyrolactone, ε-caprolactone, δ-valerolactone, alkyl alkoxyacetates (e.g., methyl alkoxyacetate, ethyl alkoxyacetate, butyl alkoxyacetate (e.g., methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, etc.)), alkyl 3-alkoxypropionates (e.g., methyl 3-alkoxypropionate, ethyl 3-alkoxypropionate, etc. (e.g., methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, methyl 3-methoxypropionate, etc.), ethyl ethoxypropionate, etc.)), alkyl 2-alkoxypropionates (e.g., methyl 2-alkoxypropionate, ethyl 2-alkoxypropionate, propyl 2-alkoxypropionate, etc. (e.g., methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate, ethyl 2-ethoxypropionate)), methyl 2-alkoxy-2-methylpropionate and ethyl 2-alkoxy-2-methylpropionate (e.g., methyl 2-methoxy-2-methylpropionate, ethyl 2-ethoxy-2-methylpropionate, etc.), methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutyrate, ethyl 2-oxobutyrate, ethyl hexanoate, ethyl heptanoate, dimethyl malonate, diethyl malonate, etc.
[0340] As ethers, preferred ones include, for example, diethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl celulose acetate, ethyl celulose acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate, diethylene glycol ethyl methyl ether, propylene glycol monopropyl ether acetate, and the like.
[0341] Preferred examples of ketones include methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, 3-heptanone, 3-methylcyclohexanone, levoglucosan, and dihydrolevoglucosan.
[0342] Preferred examples of the cyclic hydrocarbons include aromatic hydrocarbons such as toluene, xylene, and anisole, and cyclic terpenes such as limonene.
[0343] As the sulfoxides, for example, dimethyl sulfoxide is preferred.
[0344] As amides, preferred ones include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, N,N-dimethylisobutyramide, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, N-formylmorpholine, N-acetylmorpholine and the like.
[0345] Preferred ureas include N,N,N',N'-tetramethylurea and 1,3-dimethyl-2-imidazolidinone.
[0346] Examples of the alcohols include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 1-pentanol, 1-hexanol, benzyl alcohol, ethylene glycol monomethyl ether, 1-methoxy-2-propanol, 2-ethoxyethanol, diethylene glycol monoethyl ether, diethylene glycol monohexyl ether, triethylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether, polyethylene glycol monomethyl ether, polypropylene glycol, tetraethylene glycol, ethylene glycol monobutyl ether, ethylene glycol monobenzyl ether, ethylene glycol monophenyl ether, methylbenzyl alcohol, n-pentanol, methylpentanol and diacetone alcohol.
[0347] From the viewpoint of improving the properties of the coating surface, etc., it is also preferred that the solvent is in the form of a mixture of two or more types.
[0348] In the present invention, it is preferred to select a solvent or a mixed solvent consisting of two or more of 3-ethoxypropionic acid methyl ester, 3-ethoxypropionic acid ethyl ester, ethyl celulose acetate, ethyl lactate, diethylene glycol dimethyl ether, butyl acetate, 3-methoxypropionic acid methyl ester, 2-heptanone, cyclohexanone, cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, ethyl carbitol acetate, butyl carbitol acetate, N-methyl-2-pyrrolidone, propylene glycol methyl ether and propylene glycol methyl ether acetate. It is particularly preferred to use dimethyl sulfoxide and γ-butyrolactone at the same time. In addition, it is also preferred to use a combination of N-methyl-2-pyrrolidone and ethyl lactate, a combination of N-methyl-2-pyrrolidone and ethyl lactate, a combination of diacetone alcohol and ethyl lactate, and a combination of cyclopentanone and γ-butyrolactone.
[0349] From the viewpoint of coating properties, the content of the solvent is preferably set to an amount in which the total solid content concentration of the curable resin composition of the present invention becomes 5 to 80% by mass, more preferably set to an amount in which the total solid content concentration of the curable resin composition of the present invention becomes 5 to 75% by mass, further preferably set to an amount in which the total solid content concentration of the curable resin composition of the present invention becomes 10 to 70% by mass, and further preferably set to an amount in which the total solid content concentration of the curable resin composition of the present invention becomes 40 to 70% by mass. The solvent content can be adjusted according to the desired thickness of the coating film and the coating method.
[0350] The solvent may be contained in one kind or in two or more kinds. When two or more kinds of solvents are contained, the total amount thereof is preferably within the above range.
[0351] <Photosensitive agent>
[0352] The composition of the present invention preferably comprises a photosensitizer.
[0353] The photosensitive agent does not contain the above-mentioned organic metal complex and is a compound having a photoradical polymerization initiation ability.
[0354] The composition of the present invention preferably contains a photopolymerization initiator.
[0355] 〔Photopolymerization initiator〕
[0356] The composition of the present invention preferably contains a photopolymerization initiator as a photosensitizer.
[0357] The photopolymerization initiator is preferably a photoradical polymerization initiator. There is no particular limitation on the photoradical polymerization initiator, and it can be appropriately selected from known photoradical polymerization initiators. For example, a photoradical polymerization initiator having photosensitivity to light in the ultraviolet region to the visible region is preferred. In addition, an activator that generates active free radicals by reacting with a photoexcited sensitizer may also be used.
[0358] In the present invention, the compound corresponding to the organic metal complex does not correspond to the photosensitizer and the photoradical polymerization initiator.
[0359] In the case where the organometallic complex has the ability to initiate photoradical polymerization, it is also preferred that the composition of the present invention does not actually contain a radical polymerization initiator other than the above-mentioned organometallic complex. Substantially not containing a radical polymerization initiator other than the above-mentioned organometallic complex means that in the composition of the present invention, the content of other radical polymerization initiators other than the above-mentioned organometallic complex is 5% by mass or less, preferably 3% by mass or less, more preferably 1% by mass or less, and further preferably 0.1% by mass, relative to the total mass of the above-mentioned organometallic complex.
[0360] Furthermore, when the composition of the present invention includes an organic metal complex having a radical polymerization initiation capability, the composition of the present invention also preferably includes the organic metal complex and a photoradical polymerization initiator. According to this embodiment, the generation of development residues, disconnection of patterns, etc. as described above can be suppressed, and the exposure sensitivity is also improved.
[0361] In the case where the composition of the present invention includes an organic metal complex that does not have the ability to initiate photo-radical polymerization, the composition of the present invention preferably includes a photo-radical polymerization initiator. It is believed that since the composition of the present invention includes a specific resin, the agglomeration of the organic metal complex can be suppressed. It is believed that by suppressing the agglomeration of the organic metal complex that does not have the ability to initiate photo-radical polymerization, the increase in the plasticity of the local film caused by agglomeration can be suppressed, and the increase in the local degree of polymerization in the agglomeration site can also be suppressed. As a result, it is believed that the generation of sensitivity deviation caused by the site of the film can be suppressed, and the resolution is improved.
[0362] When the composition of the present invention contains an organic metal complex and a photoradical polymerization initiator, the content of the organic metal complex is preferably 20 to 80% by mass, more preferably 30 to 70% by mass, based on the total content of the organic metal complex and the photoradical polymerization initiator.
[0363] Furthermore, as the photoradical polymerization initiator, an oxime compound described below is preferred.
[0364] The photo-radical polymerization initiator preferably contains at least one photopolymerization initiator having a wavelength of at least about 50 L·mol in the range of about 300 to 800 nm (preferably 330 to 500 nm). -1 cm -1 The molar absorption coefficient of the compound can be measured using a known method. For example, it is preferably measured by an ultraviolet visible spectrophotometer (Cary-5 spectrophotometer manufactured by Varian) using an ethyl acetate solvent at a concentration of 0.01 g / L.
[0365] As a photo-radical polymerization initiator, known compounds can be used arbitrarily. For example, halogenated hydrocarbon derivatives (for example, compounds with triazine skeletons, compounds with oxadiazole structures, compounds with trihalomethyl groups, etc.), acylphosphine compounds such as acylphosphine oxides, hexaarylbimidazoles, oxime compounds such as oxime derivatives, organic peroxides, sulfur compounds, ketone compounds, aromatic onium salts, ketoxime ethers, aminoacetophenone compounds, hydroxyacetophenones, azo compounds, azides, organic boron compounds, etc. can be cited. For these details, reference can be made to paragraphs 0165 to 0182 of Japanese Patent Publication No. 2016-027357 and paragraphs 0138 to 0151 of International Publication No. 2015 / 199219, and their contents are incorporated into this specification.
[0366] Examples of the ketone compound include compounds described in paragraph 0087 of JP-A-2015-087611, the contents of which are incorporated herein. Among commercially available products, KAYACURE DETX (manufactured by Nippon Kayaku Co., Ltd.) can also be preferably used.
[0367] In one embodiment of the present invention, as the photoradical polymerization initiator, hydroxyacetophenone compounds, aminoacetophenone compounds and acylphosphine compounds can be preferably used. More specifically, for example, aminoacetophenone-based initiators described in Japanese Patent Publication No. 10-291969 and acylphosphine oxide-based initiators described in Japanese Patent No. 4225898 can be used.
[0368] As the hydroxyacetophenone-based initiator, IRGACURE 184 (IRGACURE is a registered trademark), DAROCUR 1173, IRGACURE 500, IRGACURE 2959, and IRGACURE 127 (trade names: all manufactured by BASF Corporation) can be used.
[0369] As the aminoacetophenone-based initiator, commercially available products such as IRGACURE 907, IRGACURE 369, and IRGACURE 379 (trade names: all manufactured by BASF Corporation) can be used.
[0370] As the aminoacetophenone-based initiator, a compound described in Japanese Patent Application Laid-Open No. 2009-191179, which has an absorption maximum wavelength that matches a light source having a wavelength of 365 nm or 405 nm, can also be used.
[0371] Examples of the acylphosphine initiator include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, etc. Commercially available products such as IRGACURE 819 and IRGACURE TPO (trade names: both manufactured by BASF Corporation) can be used.
[0372] As the photoradical polymerization initiator, an oxime compound can be more preferably used. By using an oxime compound, the exposure latitude can be more effectively improved. Oxime compounds are particularly preferred because they have a wide exposure latitude (exposure margin) and also function as a photocuring accelerator.
[0373] Specific examples of the oxime compound include compounds described in JP-A-2001-233842, compounds described in JP-A-2000-080068, and compounds described in JP-A-2006-342166.
[0374] Preferred oxime compounds include, for example, compounds of the following structures or 3-benzoyloxyiminobutane-2-one, 3-acetoxyiminobutane-2-one, 3-propionyloxyiminobutane-2-one, 2-acetoxyiminopentane-3-one, 2-acetoxyimino-1-phenylpropane-1-one, 2-benzoyloxyimino-1-phenylpropane-1-one, 3-(4-toluenesulfonyloxy)iminobutane-2-one, and 2-ethoxycarbonyloxyimino-1-phenylpropane-1-one. In the composition of the present invention, it is particularly preferred to use an oxime compound (oxime-based photopolymerization initiator) as a photoradical polymerization initiator. The oxime-based photopolymerization initiator has a linking group of >C=NOC(=O)- in the molecule.
[0375] [Chemical formula 25]
[0376]
[0377] Among the commercial products, IRGACURE OXE 01, IRGACURE OXE 02, IRGACURE OXE 03, IRGACURE OXE 04 (all manufactured by BASF), Adeka Optomer N-1919 (manufactured by ADEKA CORPORATION, photoradical polymerization initiator 2 described in Japanese Patent Publication No. 2012-014052) can also be preferably used. In addition, TR-PBG-304 (manufactured by Changzhou Tronly New Electronic Materials CO., LTD.), ADEKA ARKLS NCI-831 and ADEKA ARKLS NCI-930 (manufactured by ADEKA CORPORATION) can also be used. In addition, DFI-091 (manufactured by Daito Chemix Corporation) can be used. In addition, oxime compounds of the following structures can also be used.
[0378] [Chemical formula 26]
[0379]
[0380] As the photopolymerization initiator, an oxime compound having a fluorene ring can also be used. Specific examples of the oxime compound having a fluorene ring include compounds described in JP-A-2014-137466 and compounds described in Japanese Patent No. 6636081.
[0381] As the photopolymerization initiator, an oxime compound having a carbazole ring and a skeleton in which at least one benzene ring is a naphthalene ring can also be used. Specific examples of such oxime compounds include compounds described in International Publication No. 2013 / 083505.
[0382] In addition, oxime compounds having fluorine atoms can also be used. Specific examples of such oxime compounds include compounds described in JP-A-2010-262028, compounds 24, 36 to 40 described in paragraph 0345 of JP-A-2014-500852, and compound (C-3) described in paragraph 0101 of JP-A-2013-164471.
[0383] As the most preferred oxime compound, there can be mentioned an oxime compound having a specific substituent as disclosed in JP-A-2007-269779 or an oxime compound having a thioaryl group as disclosed in JP-A-2009-191061.
[0384] From the viewpoint of exposure sensitivity, the photoradical polymerization initiator is preferably selected from trihalomethyltriazine compounds, benzyl dimethyl ketal compounds, α-hydroxyketone compounds, α-aminoketone compounds, acylphosphine compounds, phosphine oxide compounds, metallocene compounds, oxime compounds, triarylimidazole dimers, onium salt compounds, benzothiazole compounds, benzophenone compounds, acetophenone compounds and derivatives thereof, cyclopentadiene-ben-iron complexes and salts thereof, halomethyloxadiazole compounds, and 3-aryl substituted coumarin compounds.
[0385] Further preferred photoradical polymerization initiators are trihalomethyl triazine compounds, α-amino ketone compounds, acyl phosphine compounds, phosphine oxide compounds, metallocene compounds, oxime compounds, triaryl imidazole dimers, onium salt compounds, benzophenone compounds, and acetophenone compounds. Further preferred are at least one compound selected from trihalomethyl triazine compounds, α-amino ketone compounds, oxime compounds, triaryl imidazole dimers, and benzophenone compounds. Further preferred are metallocene compounds or oxime compounds, and further preferred are oxime compounds.
[0386] In addition, the photoradical polymerization initiator may also include benzophenone, N,N'-tetraalkyl-4,4'-diaminobenzophenone (Michelle's ketone) and the like, aromatic ketones such as 2-benzyl-2-dimethylamino-1-(4-morpholinylphenyl)-butanone-1,2-methyl-1-[4-(methylthio)phenyl]-2-morpholinyl-propanone-1, quinones condensed with aromatic rings such as alkyl anthraquinone, benzoin ether compounds such as benzoin alkyl ether, benzoin, benzoin compounds such as alkyl benzoin, benzyl derivatives such as benzyl dimethyl ketal, etc. In addition, compounds represented by the following formula (I) may also be used.
[0387] [Chemical formula 27]
[0388]
[0389] In formula (I), R I00 is an alkyl group having 1 to 20 carbon atoms, an alkyl group having 2 to 20 carbon atoms interrupted by one or more oxygen atoms, an alkoxy group having 1 to 12 carbon atoms, a phenyl group, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, a halogen atom, a cyclopentyl group, a cyclohexyl group, an alkenyl group having 2 to 12 carbon atoms, an alkyl group having 2 to 18 carbon atoms interrupted by one or more oxygen atoms, and a phenyl or biphenyl group substituted by at least one of the following: R I01 is a group represented by formula (II) or is I00 The same group, R I0 2~R I04 Each is independently an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or a halogen atom.
[0390] [Chemical formula 28]
[0391]
[0392] In the formula, R I05 ~R I07 R of the above formula (I) I0 2~R I04 same.
[0393] Furthermore, as the photoradical polymerization initiator, the compounds described in paragraphs 0048 to 0055 of International Publication No. 2015 / 125469 can also be used.
[0394] When a photopolymerization initiator is included, its content is preferably 0.1 to 30% by mass, more preferably 0.1 to 20% by mass, further preferably 0.5 to 15% by mass, and further preferably 1.0 to 10% by mass relative to the total solid content of the composition of the present invention. The photopolymerization initiator may contain only one or more than one. When containing two or more photopolymerization initiators, the total amount thereof is preferably within the above range.
[0395] 〔Photoacid generator〕
[0396] Furthermore, the composition of the present invention preferably contains a photoacid generator as a photosensitizer.
[0397] By including a photoacid generator, for example, an acid is generated in the exposed portion of the photosensitive film, so that the solubility of the exposed portion in a developer (eg, an alkaline aqueous solution) increases, and a positive pattern in which the exposed portion is removed by the developer can be obtained.
[0398] Furthermore, the composition may contain a crosslinking agent other than a photoacid generator and a free radical crosslinking agent described later, and the crosslinking reaction of the crosslinking agent may be promoted by using an acid generated in the exposed portion, so that the exposed portion is less likely to be removed by a developer than the non-exposed portion. In this manner, a negative pattern may be obtained.
[0399] The photoacid generator is not particularly limited as long as it generates an acid by exposure, and examples thereof include quinonediazide compounds, onium salt compounds such as diazonium salts, phosphonium salts, sulfonium salts, and iodonium salts, and sulfonate compounds such as imide sulfonates, oxime sulfonates, diazodisulfones, disulfones, and o-nitrobenzylsulfonate.
[0400] Examples of the quinonediazide compound include sulfonic acid compounds in which quinonediazide is bonded to a polyhydroxy compound via an ester bond, sulfonic acid compounds in which quinonediazide is bonded to a polyamino compound via a sulfonamide bond, and sulfonic acid compounds in which quinonediazide is bonded to a polyhydroxypolyamino compound via at least one of an ester bond and a sulfonamide bond. In the present invention, for example, it is preferred that 50 mol% or more of the total functional groups of these polyhydroxy compounds or polyamino compounds are substituted with quinonediazide groups.
[0401] In the present invention, the quinone diazide can preferably use any one of 5-naphthoquinone diazide sulfonyl and 4-naphthoquinone diazide sulfonyl. The 4-naphthoquinone diazide sulfonyl ester compound has absorption in the i-ray region of the mercury lamp and is suitable for i-ray exposure. The absorption of the 5-naphthoquinone diazide sulfonyl ester compound extends to the g-ray region of the mercury lamp and is suitable for g-ray exposure. In the present invention, it is preferred to select 4-naphthoquinone diazide sulfonyl ester compounds and 5-naphthoquinone diazide sulfonyl ester compounds according to the exposure wavelength. In addition, the naphthoquinone diazide sulfonyl ester compound having 4-naphthoquinone diazide sulfonyl and 5-naphthoquinone diazide sulfonyl in the same molecule may be contained, and the 4-naphthoquinone diazide sulfonyl ester compound and the 5-naphthoquinone diazide sulfonyl ester compound may also be contained.
[0402] The naphthoquinonediazide compounds can be synthesized by an esterification reaction of a compound having a phenolic hydroxyl group with a quinonediazide sulfonic acid compound, and can be synthesized by a known method. By using these naphthoquinonediazide compounds, the resolution, sensitivity, and residual film rate are further improved.
[0403] Examples of the naphthoquinonediazide compound include 1,2-naphthoquinone-2-diazide-5-sulfonic acid, 1,2-naphthoquinone-2-diazide-4-sulfonic acid, and salts or ester compounds thereof.
[0404] Examples of the onium salt compound or the sulfonate compound include compounds described in paragraphs 0064 to 0122 of JP-A-2008-013646.
[0405] The photoacid generator is also preferably a compound containing an oxime sulfonate group (hereinafter, also simply referred to as an "oxime sulfonate compound").
[0406] The oxime sulfonate compound is not particularly limited as long as it has an oxime sulfonate group, but is preferably an oxime sulfonate compound represented by the following formula (OS-1), formula (OS-103), formula (OS-104), or formula (OS-105) described later.
[0407] [Chemical formula 29]
[0408]
[0409] In formula (OS-1), X 3 represents an alkyl group, an alkoxy group or a halogen atom. 3 In the case of , they may be the same or different. 3 The alkyl group and alkoxy group in the above-mentioned X may have a substituent. 3 The alkyl group in is preferably a linear or branched alkyl group having 1 to 4 carbon atoms. 3The alkoxy group in the above-mentioned X is preferably a linear or branched alkoxy group having 1 to 4 carbon atoms. 3 The halogen atom in the formula (I) is preferably a chlorine atom or a fluorine atom.
[0410] In formula (OS-1), m3 represents an integer of 0 to 3, preferably 0 or 1. When m3 is 2 or 3, a plurality of X 3 Can be the same or different.
[0411] In formula (OS-1), R 34 W represents an alkyl group or an aryl group, and is preferably an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a haloalkyl group having 1 to 5 carbon atoms, a haloalkoxy group having 1 to 5 carbon atoms, a phenyl group which may be substituted with W, a naphthyl group which may be substituted with W, or an anthracenyl group which may be substituted with W. W represents a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a haloalkyl group having 1 to 5 carbon atoms, or a haloalkoxy group having 1 to 5 carbon atoms, an aryl group having 6 to 20 carbon atoms, or a haloaryl group having 6 to 20 carbon atoms.
[0412] In formula (OS-1), m3 is 3, X 3 Methyl, X 3 The substitution position is ortho, R 34 Particularly preferred are compounds of a linear alkyl group having 1 to 10 carbon atoms, 7,7-dimethyl-2-oxonorkanylmethyl or p-tolyl.
[0413] Specific examples of the oxime sulfonate compound represented by formula (OS-1) include the following compounds described in paragraphs 0064 to 0068 of JP-A-2011-209692 and paragraphs 0158 to 0167 of JP-A-2015-194674, and the contents thereof are incorporated herein.
[0414] [Chemical formula 30]
[0415]
[0416] In formula (OS-103) to formula (OS-105), R s1 represents an alkyl group, an aryl group or a heteroaryl group, and sometimes there are multiple R s2 Each independently represents a hydrogen atom, an alkyl group, an aryl group or a halogen atom, and a plurality of R may exist. s6 Each independently represents a halogen atom, an alkyl group, an alkoxy group, a sulfonic acid group, an aminosulfonyl group or an alkoxysulfonyl group, Xs represents O or S, ns represents 1 or 2, and ms represents an integer of 0-6.
[0417] In formula (OS-103) to formula (OS-105), R s1The alkyl group (preferably having 1 to 30 carbon atoms), aryl group (preferably having 6 to 30 carbon atoms) or heteroaryl group (preferably having 4 to 30 carbon atoms) represented by may have a substituent T.
[0418] In formula (OS-103) to formula (OS-105), R s2 Preferably, it is a hydrogen atom, an alkyl group (preferably having 1 to 12 carbon atoms) or an aryl group (preferably having 6 to 30 carbon atoms), and more preferably a hydrogen atom or an alkyl group. s2 Among them, preferably one or two are alkyl groups, aryl groups or halogen atoms, more preferably one is an alkyl group, aryl groups or halogen atoms, and particularly preferably one is an alkyl group and the rest are hydrogen atoms. s2 The alkyl group or aryl group represented may have a substituent T.
[0419] In formula (OS-103), formula (OS-104) or formula (OS-105), Xs represents O or S, preferably O. In the above formulas (OS-103) to (OS-105), the ring containing Xs as a ring member is a 5-membered ring or a 6-membered ring.
[0420] In formula (OS-103) to formula (OS-105), ns represents 1 or 2. When Xs is O, ns is preferably 1, and when Xs is S, ns is preferably 2.
[0421] In formula (OS-103) to formula (OS-105), R s6 The alkyl group (preferably having 1 to 30 carbon atoms) and alkoxy group (preferably having 1 to 30 carbon atoms) represented by the above-mentioned group may have a substituent.
[0422] In formula (OS-103) to formula (OS-105), ms represents an integer of 0 to 6, preferably an integer of 0 to 2, more preferably 0 or 1, and particularly preferably 0.
[0423] Furthermore, the compound represented by the above formula (OS-103) is particularly preferably a compound represented by the following formula (OS-106), formula (OS-110) or formula (OS-111), and is particularly preferably a compound represented by the above formula (OS-104) or a compound represented by the following formula (OS-107), and is particularly preferably a compound represented by the above formula (OS-105) or a compound represented by the following formula (OS-108) or formula (OS-109).
[0424] [Chemical formula 31]
[0425]
[0426] In formula (OS-106) to formula (OS-111), R t1 represents an alkyl group, an aryl group or a heteroaryl group, Rt7 represents a hydrogen atom or a bromine atom, R t8 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a halogen atom, a chloromethyl group, a bromomethyl group, a bromoethyl group, a methoxymethyl group, a phenyl group or a chlorophenyl group, and R t9 represents a hydrogen atom, a halogen atom, a methyl group or a methoxy group, R t2 represents a hydrogen atom or a methyl group.
[0427] In formula (OS-106) to formula (OS-111), R t7 represents a hydrogen atom or a bromine atom, and is preferably a hydrogen atom.
[0428] In formula (OS-106) to formula (OS-111), R t8 It represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a halogen atom, a chloromethyl group, a bromomethyl group, a bromoethyl group, a methoxymethyl group, a phenyl group or a chlorophenyl group, and is preferably an alkyl group having 1 to 8 carbon atoms, a halogen atom or a phenyl group, more preferably an alkyl group having 1 to 8 carbon atoms, further preferably an alkyl group having 1 to 6 carbon atoms, and particularly preferably a methyl group.
[0429] In formula (OS-106) to formula (OS-111), R t9 represents a hydrogen atom, a halogen atom, a methyl group or a methoxy group, and is preferably a hydrogen atom.
[0430] R t2 It represents a hydrogen atom or a methyl group, and is preferably a hydrogen atom.
[0431] Furthermore, in the above-mentioned oxime sulfonate compounds, the stereostructure (E, Z) of the oxime may be any one or a mixture.
[0432] Specific examples of the oxime sulfonate compounds represented by the formula (OS-103) to (OS-105) include compounds described in paragraphs 0088 to 0095 of JP-A-2011-209692 and paragraphs 0168 to 0194 of JP-A-2015-194674, and these contents are incorporated into the present specification.
[0433] As another preferred embodiment of the oxime sulfonate compound containing at least one oxime sulfonate group, compounds represented by the following formula (OS-101) and formula (OS-102) can be mentioned.
[0434] [Chemical formula 32]
[0435]
[0436] In formula (OS-101) or formula (OS-102), R u9represents a hydrogen atom, an alkyl group, an alkenyl group, an alkoxy group, an alkoxycarbonyl group, an acyl group, a carbamoyl group, a sulfamoyl group, a sulfo group, a cyano group, an aryl group or a heteroaryl group. u9 In the embodiment where R is cyano or aryl, it is further preferred that u9 The phenyl group is cyano, phenyl or naphthyl.
[0437] In formula (OS-101) or formula (OS-102), R u2a represents an alkyl group or an aryl group.
[0438] In formula (OS-101) or formula (OS-102), Xu represents -O-, -S-, -NH-, or -NR u5 -、-CH2-、-CR u6 H- or CR u6 R u7 -, R u5 ~R u7 Each independently represents an alkyl group or an aryl group.
[0439] In formula (OS-101) or formula (OS-102), R u1 ~R u4 R each independently represents a hydrogen atom, a halogen atom, an alkyl group, an alkenyl group, an alkoxy group, an amino group, an alkoxycarbonyl group, an alkylcarbonyl group, an arylcarbonyl group, an acylamino group, a sulfo group, a cyano group or an aryl group. u1 ~R u4 In this case, the ring can be condensed to form a condensed ring together with the benzene ring. u1 ~R u4 , preferably a hydrogen atom, a halogen atom or an alkyl group, and also preferably R u1 ~R u4 At least two of them are bonded to each other to form an aromatic group. Among them, R u1 ~R u4 All of the above substituents may further have a substituent.
[0440] The compound represented by the above formula (OS-101) is more preferably a compound represented by formula (OS-102).
[0441] Furthermore, in the above-mentioned oxime sulfonate compounds, the stereostructure (E, Z, etc.) of the oxime or benzothiazole ring may be any one or a mixture.
[0442] Specific examples of the compound represented by formula (OS-101) include compounds described in paragraphs 0102 to 0106 of JP-A-2011-209692 and paragraphs 0195 to 0207 of JP-A-2015-194674, and the contents thereof are incorporated into the present specification.
[0443] Among the above compounds, the following b-9, b-16, b-31 and b-33 are also preferred.
[0444] [Chemical formula 33]
[0445]
[0446] In addition, commercial products can also be used as photoacid generators. Examples of commercial products include WPAG-145, WPAG-149, WPAG-170, WPAG-199, WPAG-336, WPAG-367, WPAG-370, WPAG-443, WPAG-469, WPAG-638, and WPAG-699 (all manufactured by FUJIFILM Wako Pure Chemical Corporation), Omnicat 250 and Omnicat 270 (all manufactured by IGM Resins BV), Irgacure 250, Irgacure 270, and Irgacure 290 (all manufactured by BASF), and MBZ-101 (manufactured by Midori Kagaku Co., Ltd.).
[0447] Furthermore, as preferred examples, there can be mentioned compounds represented by the following structural formulas.
[0448] [Chemical formula 34]
[0449]
[0450] As the photoacid generator, an organic halide can also be used. As the organic halide, specifically, Wakabayashi et al. "Bull Chem. Soc Japan" 42, 2924 (1969), U.S. Patent No. 3,905,815, Japanese Patent Publication No. 46-4605, Japanese Patent Publication No. 48-36281, Japanese Patent Publication No. 55-32070, Japanese Patent Publication No. 60-239736, Japanese Patent Publication No. 61-169835, Japanese Patent Publication No. 61-169837, Japanese Patent Publication No. 62-58241, Japanese Patent Publication No. 62-212401, Japanese Patent Publication No. 63-70243, Japanese Patent Publication No. 63-298339, MP Hutt "Jurnal of Heterocyclic The compounds described in "Chemistry" 1 (No. 3), (1970) and the like, in particular, include oxazole compounds substituted with a trihalomethyl group: S-triazine compounds.
[0451] More preferably, there can be mentioned s-triazine derivatives in which at least one mono-, di- or tri-halogen-substituted methyl group is bonded to the s-triazine ring, and specifically, for example, there can be mentioned 2,4,6-tris(monochloromethyl)-s-triazine, 2,4,6-tris(dichloromethyl)-s-triazine, 2,4,6-tris(trichloromethyl)-s-triazine, 2-methyl-4,6-bis(trichloromethyl)-s-triazine, 2-n-propyl-4,6-bis(trichloromethyl)-s-triazine, triazine, 2-(α,α,β-trichloroethyl)-4,6-bis(trichloromethyl)-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(3,4-epoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-chlorophenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-[1-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine phenyl)-2,4-butadienyl〕-4,6-bis(trichloromethyl)-s-triazine, 2-phenylvinyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-isopropoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-naphthyl)- s-triazine, 2-methyl-4,6-bis(tribromomethyl)-s-triazine, 2-methoxy-4,6-bis(tribromomethyl)-s-triazine, and the like.
[0452] As the photoacid generator, an organic borate compound can also be used. As the organic borate compound, specific examples thereof include Japanese Patent Publication No. 62-143044, Japanese Patent Publication No. 62-150242, Japanese Patent Publication No. 9-188685, Japanese Patent Publication No. 9-188686, Japanese Patent Publication No. 9-188710, Japanese Patent Publication No. 2000-131837, Japanese Patent Publication No. 2002-107916, Japanese Patent No. 2764769, Japanese Patent Application No. 2000-310808, and Kunz, Martin "Rad Tech '98. Proceedings" Organic borates described in "Chicago" etc., organic borate salts described in Japanese Patent Laid-Open No. 6-157623, Japanese Patent Laid-Open No. 6-175564, organic boron sulfonium complexes or organic boron oxysulfonium complexes described in Japanese Patent Laid-Open No. 6-175561, organic boron oxysulfonium complexes described in Japanese Patent Laid-Open No. 6-175554, and Japanese Patent Laid-Open No. 6-175553 The organic boron iodonium complex described in , the organic boron phosphonium complex described in JP-A-9-188710, the organic boron transition metal coordination complexes such as JP-A-6-348011, JP-A-7-128785, JP-A-7-140589, JP-A-7-306527, and JP-A-7-292014.
[0453] As the photoacid generator, a disulfone compound can also be used. Examples of the disulfone compound include compounds described in Japanese Patent Application Laid-Open No. 61-166544, Japanese Patent Application No. 2001-132318, and diazodisulfone compounds.
[0454] Examples of the onium salt compound include diazonium salts described in S. Schlesinger, Photogr. Sci. Eng., 18, 387 (1974), and T. S. Bal et al., Polymer, 21, 423 (1980), ammonium salts described in U.S. Pat. No. 4,069,055, Japanese Patent Application Laid-Open No. 4-365049, etc., phosphonium salts described in U.S. Pat. No. 4,069,055, and U.S. Pat. No. 4,069,056, European Patent No. 104,143, U.S. Pat. No. 339,049, and U.S. Pat. No. 410,201, Japanese Patent Application Laid-Open No. 2-150848, and Japanese Patent Application Laid-Open No. 2-296514, European Patent No. 370,693, European Patent No. 39 Sulfonium salts described in the specifications of Patent No. 0,214, European Patent No. 233,567, European Patent No. 297,443, European Patent No. 297,442, U.S. Patent No. 4,933,377, U.S. Patent No. 161,811, U.S. Patent No. 410,201, U.S. Patent No. 339,049, U.S. Patent No. 4,760,013, U.S. Patent No. 4,734,444, U.S. Patent No. 2,833,827, German Patent No. 2,904,626, German Patent No. 3,604,580, German Patent No. 3,604,581, JV Crivello et al, Macromolecules, 10(6), 1307 (1977), selenium salts described in JV Crivello et al, J. Polymer Sci., Polymer Chem. Ed., 17, 1047 (1979), arsenic salts and onium salts such as pyridinium salts described in CS Wen et al, Teh, Proc. Conf. Rad. Curing ASIA, p478 Tokyo, Oct (1988), and the like.
[0455] Examples of the onium salt include onium salts represented by the following general formulae (RI-I) to (RI-III).
[0456] [Chemical formula 35]
[0457]
[0458] In formula (RI-I), Ar 11Z represents an aryl group having 20 or less carbon atoms which may have 1 to 6 substituents, and preferred substituents include an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 1 to 12 carbon atoms, an alkynyl group having 1 to 12 carbon atoms, an aryl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryloxy group having 1 to 12 carbon atoms, a halogen atom, an alkylamino group having 1 to 12 carbon atoms, a dialkylamino group having 1 to 12 carbon atoms, an alkylamido group or an arylamido group having 1 to 12 carbon atoms, a carbonyl group, a carboxyl group, a cyano group, a sulfonyl group, a thioalkyl group having 1 to 12 carbon atoms, and a thioaryl group having 1 to 12 carbon atoms. 11 - represents a monovalent anion, which is a halide ion, a perchlorate ion, a hexafluorophosphate ion, a tetrafluoroborate ion, a sulfonate ion, a sulfinic acid ion, a thiosulfinic acid ion, or a sulfate ion. From the perspective of stability, perchlorate ion, hexafluorophosphate ion, tetrafluoroborate ion, sulfonate ion, or a sulfinic acid ion is preferred. 21 ,Ar 22 Each independently represents an aryl group having 20 or less carbon atoms which may have 1 to 6 substituents, and preferred substituents include alkyl groups having 1 to 12 carbon atoms, alkenyl groups having 1 to 12 carbon atoms, alkynyl groups having 1 to 12 carbon atoms, aryl groups having 1 to 12 carbon atoms, alkoxy groups having 1 to 12 carbon atoms, aryloxy groups having 1 to 12 carbon atoms, halogen atoms, alkylamino groups having 1 to 12 carbon atoms, dialkylamino groups having 1 to 12 carbon atoms, alkylamido groups or arylamido groups having 1 to 12 carbon atoms, carbonyl groups, carboxyl groups, cyano groups, sulfonyl groups, thioalkyl groups having 1 to 12 carbon atoms, and thioaryl groups having 1 to 12 carbon atoms. 21 - represents a monovalent anion, which is a halide ion, a perchlorate ion, a hexafluorophosphate ion, a tetrafluoroborate ion, a sulfonate ion, a sulfinic acid ion, a thiosulfonate ion, or a sulfate ion. In terms of stability and reactivity, perchlorate ion, hexafluorophosphate ion, tetrafluoroborate ion, sulfonate ion, sulfinic acid ion, or a carboxylate ion is preferred. In formula (RI-III), R 31 , R 32 , R 33Each independently represents an aryl group or an alkyl group, an alkenyl group, or an alkynyl group having 20 or less carbon atoms which may have 1 to 6 substituents, and is preferably an aryl group in terms of reactivity and stability. Preferred substituents include an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 1 to 12 carbon atoms, an alkynyl group having 1 to 12 carbon atoms, an aryl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryloxy group having 1 to 12 carbon atoms, a halogen atom, an alkylamino group having 1 to 12 carbon atoms, a dialkylamino group having 1 to 12 carbon atoms, an alkylamido group or an arylamido group having 1 to 12 carbon atoms, a carbonyl group, a carboxyl group, a cyano group, a sulfonyl group, a thioalkyl group having 1 to 12 carbon atoms, and a thioaryl group having 1 to 12 carbon atoms. Z 31 - represents a monovalent anion, which is a halide ion, a perchlorate ion, a hexafluorophosphate ion, a tetrafluoroborate ion, a sulfonate ion, a sulfinic acid ion, a thiosulfinic acid ion, or a sulfate ion. In terms of stability and reactivity, perchlorate ion, hexafluorophosphate ion, tetrafluoroborate ion, sulfonate ion, sulfinic acid ion, or a carboxylate ion is preferred.
[0459] As specific examples, the following can be cited.
[0460] [Chemical formula 36]
[0461]
[0462] [Chemical formula 37]
[0463]
[0464] [Chemical formula 38]
[0465]
[0466] [Chemical formula 39]
[0467]
[0468] When a photoacid generator is included, its content is preferably 0.1 to 30% by mass, more preferably 0.1 to 20% by mass, and further preferably 2 to 15% by mass relative to the total solid content of the composition of the present invention. The photoacid generator may contain only one type or two or more types. When two or more photoacid generators are contained, the total amount thereof is preferably within the above range.
[0469] 〔Photobase generator〕
[0470] The curable resin composition of the present invention may contain a photobase generator as a photosensitizer.
[0471] When the curable resin composition contains a photobase generator and a crosslinking agent described later, for example, the base generated in the exposed portion promotes the cyclization of the specific resin and the crosslinking reaction of the crosslinking agent, so that the exposed portion is less likely to be removed by a developer than the non-exposed portion. According to this method, a negative pattern can be obtained.
[0472] The photobase generator is not particularly limited as long as it generates a base by exposure, and a known photobase generator can be used.
[0473] For example, M. Shirai and M. Tsunooka, Prog. Polym. Sci., 21, 1 (1996); Masahiro Kadoka, Polymer Processing, 46, 2 (1997); C. Kutal, Coord. Chem. Rev., 211, 353 (2001); Y. Kaneko, A. Sarker, and D. Neckers, Chem. Mater., 11, 170 (1999); H. Tachi, M. Shirai, and M. Tsunooka, J. Photopolym. Sci. Technol., 13, 153 (2000); M. Winkle, and K. Graziano, J. Photopolym. Sci. Technol., 3, 419 (1990); M. Tsunooka, H. Tachi, and S. Yoshitaka, J. Photopolym. Sci. Technol., 9, 13 (1996); K. Suyama, H. Araki, M. Shirai, J. Photopolym. Sci. Technol., 19, 81 (2006) state that examples thereof include transition metal compound complexes, substances having structures such as ammonium salts, substances whose amidine moieties are latentized by forming salts with carboxylic acids, ionic compounds whose base components are neutralized by forming salts, and non-ionic compounds whose base components are latentized by carbamate bonds or oxime bonds, such as carbamate derivatives, oxime ester derivatives, and acyl compounds.
[0474] In the present invention, more preferred examples of the photobase generator include carbamate derivatives, amide derivatives, imide derivatives, α-cobalt complexes, imidazole derivatives, cinnamamide derivatives, and oxime derivatives.
[0475] The basic substance generated from the photobase generator is not particularly limited, and examples thereof include compounds having an amino group, particularly polyamines such as monoamines and diamines, and amidines.
[0476] From the viewpoint of imidization rate, the alkaline substance preferably has a large pKa in DMSO (dimethyl sulfoxide) of the conjugate acid. The pKa is preferably 1 or more, more preferably 3 or more. The upper limit of the pKa is not particularly limited, but is preferably 20 or less.
[0477] Here, the pKa represents the logarithm of the reciprocal of the first dissociation constant of the acid, and can refer to the values described in Determination of Organic Structures by Physical Methods (author: Brown, HC, McDaniel, DH, Hafliger, O., Nachod, FC; editor: Braude, EA, Nachod, FC; Academic Press, New York, 1955) or Data for Biochemical Research (author: Dawson, RMC et al; Oxford, Clarendon Press, 1959). For compounds not described in these documents, the value calculated from the structural formula was used as pKa using ACD / pKa (manufactured by ACD / Labs) software.
[0478] From the viewpoint of storage stability of the curable resin composition, as the photobase generator, it is preferred that the photobase generator does not contain salt in the structure, and it is preferred that there is no charge on the nitrogen atom of the base part generated in the photobase generator. As the photobase generator, it is preferred that the base generated is latent by covalent bond, and it is preferred that the mechanism of base generation is a mechanism in which the covalent bond between the nitrogen atom of the base part generated and the adjacent atom is cut to generate the base. If it is a photobase generator that does not contain salt in the structure, the photobase generator can be made neutral, so the solvent solubility is better and the service life is extended. Considering these reasons, the amine generated from the photobase generator used in the present invention is preferably a primary amine or a secondary amine.
[0479] Furthermore, from the viewpoint of chemical resistance of the pattern, the photobase generator is preferably one containing a salt in its structure.
[0480] Furthermore, from the above reasons, as the photobase generator, the generated base is preferably latent via a covalent bond as described above, and the generated base is preferably latent via an amide bond, a carbamate bond, or an oxime bond.
[0481] As the photobase generator involved in the present invention, for example, there can be mentioned a photobase generator having a cinnamamide structure as disclosed in Japanese Patent Publication No. 2009-080452 and International Publication No. 2009 / 123122, a photobase generator having a carbamate structure as disclosed in Japanese Patent Publication No. 2006-189591 and Japanese Patent Publication No. 2008-247747, and a photobase generator having an oxime structure or a carbamoyl oxime structure as disclosed in Japanese Patent Publication No. 2007-249013 and Japanese Patent Publication No. 2008-003581, but the present invention is not limited to these, and other than these, the structure of a known photobase generator can be used.
[0482] In addition, examples of the photobase generator include compounds described in paragraphs 0185 to 0188, 0199 to 0200, and 0202 of JP-A-2012-093746, compounds described in paragraphs 0022 to 0069 of JP-A-2013-194205, compounds described in paragraphs 0026 to 0074 of JP-A-2013-204019, and compounds described in paragraph 0052 of International Publication No. 2010 / 064631.
[0483] In addition, as the photobase generator, a commercially available product can be used. As commercially available products, WPBG-266, WPBG-300, WPGB-345, WPGB-140, WPBG-165, WPBG-027, WPBG-018, WPGB-015, WPBG-041, WPGB-172, WPGB-174, WPBG-166, WPGB-158, WPGB-025, WPGB-168, WPGB-167, WPBG-082 (all manufactured by FUJIFILM Wako Pure Chemical Corporation), A2502, B5085, N0528, N1052, O0396, O0447, O0448 (manufactured by Tokyo Chemical Industry Co., Ltd.), etc. can be cited.
[0484] When a photobase generator is included, its content is preferably 0.1 to 30% by mass, more preferably 0.1 to 20% by mass, and further preferably 2 to 15% by mass relative to the total solid content of the curable resin composition of the present invention. The photobase generator may contain only one or more than one. When two or more photobase generators are contained, it is preferred that the total amount is within the above range.
[0485] <Thermal polymerization initiator>
[0486] The composition of the present invention may contain a thermal polymerization initiator, and in particular, may contain a thermal free radical polymerization initiator. A thermal free radical polymerization initiator is a compound that generates free radicals by thermal energy to initiate or promote the polymerization reaction of a polymerizable compound. By adding a thermal free radical polymerization initiator, the polymerization reaction of the resin and the crosslinking agent is also carried out in the heating step described later, so that the solvent resistance can be further improved.
[0487] Specific examples of the thermal radical polymerization initiator include compounds described in paragraphs 0074 to 0118 of JP-A-2008-063554.
[0488] When a thermal polymerization initiator is contained, its content is preferably 0.1 to 30% by mass, more preferably 0.1 to 20% by mass, and further preferably 0.5 to 15% by mass relative to the total solid content of the composition of the present invention. The thermal polymerization initiator may contain only one or more than one. When containing two or more thermal polymerization initiators, the total amount thereof is preferably within the above range.
[0489] <Thermal Acid Generator>
[0490] The compositions of the present invention may contain a thermal acid generator.
[0491] The thermal acid generator has an effect of promoting a crosslinking reaction of at least one compound selected from the group consisting of compounds having a hydroxymethyl group, an alkoxymethyl group or an acyloxymethyl group, an epoxy compound, an oxetane compound and a benzoxazine compound by generating an acid upon heating.
[0492] The thermal decomposition starting temperature of the thermal acid generator is preferably 50° C. to 270° C., more preferably 50° C. to 250° C. Furthermore, if a thermal acid generator is selected as the thermal acid generator, which does not generate acid during drying (prebaking: about 70 to 140° C.) after the composition is applied to the substrate, but generates acid during final heating (curing: about 100 to 400° C.) after patterning during subsequent exposure and development, it is preferred because a decrease in sensitivity during development can be suppressed.
[0493] The thermal decomposition starting temperature is determined as the peak temperature of the lowest exothermic peak when the thermal acid generator is heated to 500° C. at 5° C. / min in a pressure-resistant capsule.
[0494] As an instrument used when measuring the thermal decomposition starting temperature, Q2000 (produced by TA Instruments) and the like can be mentioned.
[0495] The acid generated from the thermal acid generator is preferably a strong acid, preferably an arylsulfonic acid such as p-toluenesulfonic acid and benzenesulfonic acid, an alkylsulfonic acid such as methanesulfonic acid, ethanesulfonic acid, butanesulfonic acid, or a halogenated alkylsulfonic acid such as trifluoromethanesulfonic acid, etc. Examples of such thermal acid generators include the thermal acid generators described in paragraph 0055 of Japanese Patent Application Laid-Open No. 2013-072935.
[0496] Among them, from the viewpoint of less residue in the organic film and less likely to deteriorate the physical properties of the organic film, a substance that generates an alkylsulfonic acid having 1 to 4 carbon atoms or a halogenated alkylsulfonic acid having 1 to 4 carbon atoms is more preferred, and as the thermal acid generator, (4-hydroxyphenyl)dimethylsulfonium methanesulfonate, (4-((methoxycarbonyl)oxy)phenyl)dimethylsulfonium methanesulfonate, benzyl(4-hydroxyphenyl)methylsulfonium methanesulfonate, benzyl(4-((methoxycarbonyl)oxy)phenyl)methylsulfonium methanesulfonate, (4-hydroxyphenyl)methyl((2-methylphenyl)methyl)sulfonium methanesulfonate, trifluoromethanesulfonate are preferred. (4-Hydroxyphenyl)dimethylsulfonium, (4-((methoxycarbonyl)oxy)phenyl)dimethylsulfonium trifluoromethanesulfonate, benzyl(4-hydroxyphenyl)methylsulfonium trifluoromethanesulfonate, benzyl(4-((methoxycarbonyl)oxy)phenyl)methylsulfonium trifluoromethanesulfonate, (4-hydroxyphenyl)methyl((2-methylphenyl)methyl)sulfonium trifluoromethanesulfonate, 3-(5-(((propylsulfonyl)oxy)imino)thiophen-2(5H)-ylidene)-2-(o-tolyl)propionitrile, 2,2-bis(3-(methanesulfonylamino)-4-hydroxyphenyl)hexafluoropropane.
[0497] Furthermore, the compounds described in paragraph 0059 of JP-A-2013-167742 are also preferred as the thermal acid generator.
[0498] The content of the thermal acid generator is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the specific resin. By containing 0.01 parts by mass or more, the cross-linking reaction is promoted, so the mechanical properties and solvent resistance of the organic film can be further improved. In addition, from the viewpoint of the electrical insulation of the organic film, it is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and further preferably 10 parts by mass or less.
[0499] <Onium salt>
[0500] The curable resin composition of the present invention may further contain an onium salt.
[0501] In particular, when the curable resin composition of the present invention contains a polyimide precursor or a polybenzoxazole precursor as a specific resin, it is preferred to contain an onium salt.
[0502] The type of the onium salt is not particularly limited, but preferred examples include ammonium salts, iminium salts, sulfonium salts, iodonium salts, and phosphonium salts.
[0503] Among these, ammonium salts or iminium salts are preferred from the viewpoint of high thermal stability, and sulfonium salts, iodonium salts or phosphonium salts are preferred from the viewpoint of compatibility with the polymer.
[0504] Furthermore, the onium salt is a salt of a cation having an onium structure and an anion, and the cation and the anion may or may not be bonded via a covalent bond.
[0505] That is, the onium salt may be an intramolecular salt having a cation part and an anion part in the same molecular structure, or an intermolecular salt formed by ionic bonding of cation molecules and anion molecules of different molecules, but is preferably an intermolecular salt. Furthermore, in the curable resin composition of the present invention, the cation part or cation molecule and the anion part or anion molecule may be bonded by ionic bonding or may be dissociated.
[0506] The cation in the onium salt is preferably an ammonium cation, a pyridinium cation, a sulfonium cation, an iodonium cation or a phosphonium cation, and more preferably at least one cation selected from the group consisting of a tetraalkylammonium cation, a sulfonium cation and an iodonium cation.
[0507] The onium salt used in the present invention may be a thermal base generator described later.
[0508] The thermal base generator is a compound that generates a base when heated, and examples thereof include compounds that generate a base when heated to 40° C. or higher.
[0509] As an onium salt, for example, the onium salt described in paragraphs 0122 to 0138 of International Publication No. 2018 / 043262 can be mentioned. In addition, an onium salt used in the field of polyimide precursors can be used without particular limitation.
[0510] When the curable resin composition of the present invention includes an onium salt, the content of the onium salt is preferably 0.1 to 50% by mass relative to the total solid content of the curable resin composition of the present invention. The lower limit is more preferably 0.5% by mass or more, more preferably 0.85% by mass or more, and more preferably 1% by mass or more. The upper limit is more preferably 30% by mass or less, more preferably 20% by mass or less, more preferably 10% by mass or less, and may be 5% by mass or less, or 4% by mass or less.
[0511] The onium salt can be used alone or in combination of two or more. When two or more are used, the total amount is preferably within the above range.
[0512] <Thermal alkali generator>
[0513] The curable resin composition of the present invention may further contain a thermal base generator.
[0514] In particular, when the curable resin composition of the present invention contains a polyimide precursor or a polybenzoxazole precursor as a specific resin, it is preferred to contain a thermal base generator.
[0515] The other thermal base generator may be a compound corresponding to the above-mentioned onium salt, or may be a thermal base generator other than the above-mentioned onium salt.
[0516] Examples of the thermal base generator other than the above-mentioned onium salt include nonionic thermal base generators.
[0517] Examples of the nonionic thermal base generator include compounds represented by formula (B1) or formula (B2).
[0518] [Chemical formula 40]
[0519]
[0520] In formula (B1) and formula (B2), Rb 1 , Rb 2 and Rb 3 are independently an organic group without a tertiary amine structure, a halogen atom or a hydrogen atom. 1 and Rb 2 will not become a hydrogen atom at the same time. 1 , Rb 2 and Rb 3 In addition, in this specification, the tertiary amine structure refers to a structure in which the three bonds of the trivalent nitrogen atom are covalently bonded to the carbon atoms of the hydrocarbon system. Therefore, when the bonded carbon atom is a carbon atom constituting a carbonyl group, that is, when an acylamino group is formed together with a nitrogen atom, it is not limited to this.
[0521] In formula (B1) and (B2), regarding Rb 1 , Rb 2 and Rb 3 , preferably at least one of these contains a cyclic structure, more preferably at least two contain a cyclic structure. As the cyclic structure, it can be any one of a monocyclic ring and a condensed ring, preferably a monocyclic ring or a condensed ring formed by condensing two monocyclic rings. The monocyclic ring is preferably a 5-membered ring or a 6-membered ring, more preferably a 6-membered ring. The monocyclic ring is preferably a cyclohexane ring and a benzene ring, more preferably a cyclohexane ring.
[0522] More specifically, Rb 1 and Rb 2Preferably, it is a hydrogen atom, an alkyl group (preferably having 1 to 24 carbon atoms, more preferably 2 to 18, and further preferably 3 to 12), an alkenyl group (preferably having 2 to 24 carbon atoms, more preferably 2 to 18, and further preferably 3 to 12), an aryl group (preferably having 6 to 22 carbon atoms, more preferably 6 to 18, and further preferably 6 to 10 carbon atoms), or an arylalkyl group (preferably having 7 to 25 carbon atoms, more preferably 7 to 19, and further preferably 7 to 12 carbon atoms). These groups may have a substituent within the range in which the effects of the present invention are exerted. Rb 1 and Rb 2 They may be bonded to each other to form a ring. The ring formed is preferably a 4- to 7-membered nitrogen-containing heterocyclic ring. 1 and Rb 2 Particularly preferred is a linear, branched or cyclic alkyl group which may have a substituent (preferably having 1 to 24 carbon atoms, more preferably 2 to 18, and even more preferably 3 to 12 carbon atoms), more preferably a cycloalkyl group which may have a substituent (preferably having 3 to 24 carbon atoms, more preferably 3 to 18, and even more preferably 3 to 12 carbon atoms), and even more preferably a cyclohexyl group which may have a substituent.
[0523] As Rb 3 , examples thereof include alkyl groups (preferably having 1 to 24 carbon atoms, more preferably 2 to 18, and further preferably 3 to 12), aryl groups (preferably having 6 to 22 carbon atoms, more preferably 6 to 18, and further preferably 6 to 10), alkenyl groups (preferably having 2 to 24 carbon atoms, more preferably 2 to 12, and further preferably 2 to 6), arylalkyl groups (preferably having 7 to 23 carbon atoms, more preferably 7 to 19, and further preferably 7 to 12), arylalkenyl groups (preferably having 8 to 24 carbon atoms, more preferably 8 to 20, and further preferably 8 to 16), alkoxy groups (preferably having 1 to 24 carbon atoms, more preferably 2 to 18, and further preferably 3 to 12), aryloxy groups (preferably having 6 to 22 carbon atoms, more preferably 6 to 18, and further preferably 6 to 12), and arylalkoxy groups (preferably having 7 to 23 carbon atoms, more preferably 7 to 19, and further preferably 7 to 12). Among them, cycloalkyl (preferably having 3 to 24 carbon atoms, more preferably 3 to 18 carbon atoms, and even more preferably 3 to 12 carbon atoms), arylalkenyl, and arylalkoxy groups are preferred. 3 The compound may further have a substituent within a range where the effects of the present invention are exhibited.
[0524] The compound represented by formula (B1) is preferably a compound represented by the following formula (B1-1) or the following formula (B1-2).
[0525] [Chemical formula 41]
[0526]
[0527] In the formula, Rb 11 and Rb 12 and Rb 31 and Rb 32 Respectively with Rb in formula (B1) 1 and Rb 2 same.
[0528] R 13 It is an alkyl group (preferably having 1 to 24 carbon atoms, more preferably 2 to 18, and further preferably 3 to 12), an alkenyl group (preferably having 2 to 24 carbon atoms, more preferably 2 to 18, and further preferably 3 to 12), an aryl group (preferably having 6 to 22 carbon atoms, more preferably 6 to 18, and further preferably 6 to 12), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably 7 to 19, and further preferably 7 to 12), and may have a substituent within the range in which the effects of the present invention are exerted. Among them, Rb 13 Preferred is an arylalkyl group.
[0529] R 33 and Rb 34 Each of them is independently a hydrogen atom, an alkyl group (preferably having 1 to 12 carbon atoms, more preferably 1 to 8, and further preferably 1 to 3), an alkenyl group (preferably having 2 to 12 carbon atoms, more preferably 2 to 8, and further preferably 2 to 3), an aryl group (preferably having 6 to 22 carbon atoms, more preferably 6 to 18, and further preferably 6 to 10), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably 7 to 19, and further preferably 7 to 11), and is preferably a hydrogen atom.
[0530] R 35 It is an alkyl group (preferably having 1 to 24 carbon atoms, more preferably 1 to 12, and further preferably 3 to 8), an alkenyl group (preferably having 2 to 12 carbon atoms, more preferably 2 to 10, and further preferably 3 to 8), an aryl group (preferably having 6 to 22 carbon atoms, more preferably 6 to 18, and further preferably 6 to 12), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably 7 to 19, and further preferably 7 to 12), and is preferably an aryl group.
[0531] The compound represented by formula (B1-1) is preferably a compound represented by formula (B1-1a).
[0532] [Chemical formula 42]
[0533]
[0534] R 11 and Rb 12 With Rb in formula (B1-1) 11 and Rb 12 Synonymous.
[0535] R 15 and Rb 16 It is a hydrogen atom, an alkyl group (preferably having 1 to 12 carbon atoms, more preferably 1 to 6, and further preferably 1 to 3), an alkenyl group (preferably having 2 to 12 carbon atoms, more preferably 2 to 6, and further preferably 2 to 3), an aryl group (preferably having 6 to 22 carbon atoms, more preferably 6 to 18, and further preferably 6 to 10), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably 7 to 19, and further preferably 7 to 11), and is preferably a hydrogen atom or a methyl group.
[0536] R 17 It is an alkyl group (preferably having 1 to 24 carbon atoms, more preferably 1 to 12, and further preferably 3 to 8), an alkenyl group (preferably having 2 to 12 carbon atoms, more preferably 2 to 10, and further preferably 3 to 8), an aryl group (preferably having 6 to 22 carbon atoms, more preferably 6 to 18, and further preferably 6 to 12), and an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably 7 to 19, and further preferably 7 to 12), among which an aryl group is preferred.
[0537] The molecular weight of the nonionic thermal base generator is preferably 800 or less, more preferably 600 or less, and further preferably 500 or less. The lower limit is preferably 100 or more, more preferably 200 or more, and further preferably 300 or more.
[0538] As specific examples of the compound as the thermal base generator among the above-mentioned onium salts or specific examples of the thermal base generator other than the above-mentioned onium salts, the following compounds can be mentioned.
[0539] [Chemical formula 43]
[0540]
[0541] [Chemical formula 44]
[0542]
[0543] [Chemical formula 45]
[0544]
[0545] The content of other hot alkali generators is preferably 0.1 to 50% by mass relative to the total solid content of the curable resin composition of the present invention. The lower limit is more preferably 0.5% by mass or more, and more preferably 1% by mass or more. The upper limit is more preferably 30% by mass or less, and more preferably 20% by mass or less. The hot alkali generator can be used in one or more than two kinds. When using two or more kinds, the total amount is preferably within the above range.
[0546] <Cross-linking agent>
[0547] The curable resin composition of the present invention preferably contains a cross-linking agent.
[0548] Examples of the crosslinking agent include radical crosslinking agents and other crosslinking agents.
[0549] <Free Radical Crosslinking Agent>
[0550] The curable resin composition of the present invention preferably further contains a radical crosslinking agent.
[0551] The free radical crosslinking agent is a compound having a free radical polymerizable group. As the free radical polymerizable group, a group containing an ethylenically unsaturated bond is preferred. As the above-mentioned group containing an ethylenically unsaturated bond, groups having an ethylenically unsaturated bond such as vinyl, allyl, vinylphenyl, (meth)acryloyl, etc. can be cited.
[0552] Among these, as the group containing an ethylenically unsaturated bond, a (meth)acryloyl group is preferred, and from the viewpoint of reactivity, a (meth)acryloyl group is more preferred.
[0553] The radical crosslinking agent may be a compound having one or more ethylenically unsaturated bonds, and more preferably a compound having two or more ethylenically unsaturated bonds.
[0554] The compound having two ethylenically unsaturated bonds is preferably a compound having two of the above-mentioned groups containing an ethylenically unsaturated bond.
[0555] Furthermore, from the viewpoint of film strength of the obtained pattern, the curable resin composition of the present invention preferably contains a compound having 3 or more ethylenically unsaturated bonds as a free radical crosslinking agent. As the compound having 3 or more ethylenically unsaturated bonds, a compound having 3 to 15 ethylenically unsaturated bonds is preferred, a compound having 3 to 10 ethylenically unsaturated bonds is more preferred, and a compound having 3 to 6 ethylenically unsaturated bonds is further preferred.
[0556] Furthermore, the compound having 3 or more ethylenically unsaturated bonds is preferably a compound having 3 or more of the above-mentioned groups containing ethylenically unsaturated bonds, more preferably a compound having 3 to 15, further preferably a compound having 3 to 10, and particularly preferably a compound having 3 to 6.
[0557] Furthermore, from the viewpoint of the film strength of the obtained pattern, the curable resin composition of the present invention preferably contains a compound having two ethylenically unsaturated bonds and a compound having three or more of the above ethylenically unsaturated bonds.
[0558] The molecular weight of the radical crosslinking agent is preferably 2,000 or less, more preferably 1,500 or less, and further preferably 900 or less. The lower limit of the molecular weight of the radical crosslinking agent is preferably 100 or more.
[0559] Specific examples of free radical crosslinking agents include unsaturated carboxylic acids (e.g., acrylic acid, methacrylic acid, itaconic acid, crotonic acid, isocrotonic acid, maleic acid, etc.) or their esters and amides, preferably esters of unsaturated carboxylic acids and polyol compounds and amides of unsaturated carboxylic acids and polyamine compounds. In addition, unsaturated carboxylic acid esters or amides having nucleophilic substituents such as hydroxyl groups, amino groups, sulfhydryl groups, and addition reaction products with monofunctional or polyfunctional isocyanates or epoxies, or dehydration condensation reaction products with monofunctional or polyfunctional carboxylic acids can also be preferably used. In addition, it is also possible to preferably use unsaturated carboxylic acid esters or amides with electron-withdrawing substituents such as isocyanate groups or epoxy groups and addition reactants of monofunctional or polyfunctional alcohols, amines, and thiols, and unsaturated carboxylic acid esters or amides with disengagement substituents such as halogeno groups or tosyloxy groups and substitution reactants of monofunctional or polyfunctional alcohols, amines, and thiols. In addition, as another example, it is also possible to use a compound group replaced with vinylbenzene derivatives such as unsaturated phosphonic acid, styrene, vinyl ether, allyl ether, etc. to replace the above-mentioned unsaturated carboxylic acid. As a specific example, it is possible to refer to the records of paragraphs 0113 to 0122 of Japanese Patent Publication No. 2016-027357, and these contents are incorporated into this specification.
[0560] Furthermore, the radical crosslinking agent is preferably a compound having a boiling point of 100° C. or higher under normal pressure. Examples thereof include compounds obtained by adding ethylene oxide or propylene oxide to a polyfunctional alcohol such as polyethylene glycol di(meth)acrylate, trimethylolethane tri(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, hexanediol (meth)acrylate, trimethylolpropane tri(acryloxypropyl) ether, tri(acryloxyethyl) isocyanurate, glycerol or trimethylolethane, and then (meth)acrylating the resulting mixture. Esterified compounds, such as urethane (meth) acrylates described in Japanese Patent Publication No. 48-041708, Japanese Patent Publication No. 50-006034, Japanese Patent Publication No. 51-037193, polyester acrylates described in Japanese Patent Publication No. 48-064183, Japanese Patent Publication No. 49-043191, Japanese Patent Publication No. 52-030490, epoxy acrylates as reaction products of epoxy resin and (meth) acrylic acid, and polyfunctional acrylates or methacrylates and mixtures thereof. In addition, compounds described in paragraphs 0254 to 0257 of Japanese Patent Publication No. 2008-292970 are also preferred. In addition, polyfunctional (meth) acrylates obtained by reacting compounds having a cyclic ether group and an ethylenically unsaturated bond such as (meth) acrylate glycidyl ester with a polyfunctional carboxylic acid can also be cited.
[0561] Furthermore, as preferred radical crosslinking agents other than those described above, compounds having a fluorene ring and having two or more groups containing ethylenically unsaturated bonds, or cardo resins described in JP-A-2010-160418, JP-A-2010-129825, and JP-4364216 may be used.
[0562] In addition, as other examples, specific unsaturated compounds described in Japanese Patent Publication No. 46-043946, Japanese Patent Publication No. 01-040337, Japanese Patent Publication No. 01-040336, or vinylphosphonic acid compounds described in Japanese Patent Publication No. 02-025493 can also be cited. In addition, compounds containing perfluoroalkyl groups described in Japanese Patent Publication No. 61-022048 can also be used. In addition, substances introduced as photopolymerizable monomers and oligomers in the Journal of the Japanese Adhesion Society, vol. 20, No. 7, pages 300 to 308 (1984) can also be used.
[0563] In addition to the above, compounds described in paragraphs 0048 to 0051 of JP-A-2015-034964 and compounds described in paragraphs 0087 to 0131 of WO-2015 / 199219 can also be preferably used, and the contents thereof are incorporated into the present specification.
[0564] Furthermore, compounds described in Japanese Patent Application Laid-Open No. 10-062986 as formula (1) and formula (2) together with specific examples thereof, which are obtained by adding ethylene oxide or propylene oxide to a polyfunctional alcohol and then (meth)acrylating the added ethylene oxide or propylene oxide, can also be used as radical crosslinking agents.
[0565] In addition, the compounds described in paragraphs 0104 to 0131 of JP-A-2015-187211 can also be used as a radical crosslinking agent, and these contents are incorporated into the present specification.
[0566] As the radical crosslinking agent, dipentaerythritol triacrylate (commercially available as KAYARAD D-330; manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol tetraacrylate (commercially available as KAYARAD D-320; manufactured by Nippon Kayaku Co., Ltd., A-TMMT: manufactured by Shin-Nakamura Chemical Co., Ltd.), dipentaerythritol penta(meth)acrylate (commercially available as KAYARAD D-310; manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol hexa(meth)acrylate (commercially available as KAYARAD DPHA; manufactured by Nippon Kayaku Co., Ltd., A-DPH; manufactured by Shin-Nakamura Chemical Co., Ltd.), and structures in which (meth)acryloyl groups thereof are bonded via ethylene glycol residues or propylene glycol residues are preferred. These oligomer types can also be used.
[0567] Commercially available products of the radical crosslinking agent include, for example, SR-494 manufactured by Sartomer Company, Inc., which is a tetrafunctional acrylate having four ethyleneoxy chains; SR-209, 231, and 239 manufactured by Sartomer Company, Inc., which are bifunctional methacrylates having four ethyleneoxy chains; DPCA-60 manufactured by Nippon Kayaku Co., Ltd., which is a hexafunctional acrylate having six pentyloxy chains; TPA-330 manufactured by Nippon Kayaku Co., Ltd., which is a trifunctional acrylate having three isobutyleneoxy chains; urethane oligomers UAS-10 and UAB-140 (manufactured by Nippon Paper Industries Co., Ltd.); NK Ester M-40G, NK Ester 4G, NK Ester M-9300, NK Ester A-9300, and UA-7200 (manufactured by Shin-Nakamura Chemical Co., Ltd.); Co., Ltd.), DPHA-40H (manufactured by Nippon Kayaku Co., Ltd.), UA-306H, UA-306T, UA-306I, AH-600, T-600, AI-600 (manufactured by Kyoeisha Chemical Co., Ltd.), BLEMMER PME400 (manufactured by NOF CORPORATION), etc.
[0568] As the radical crosslinking agent, urethane acrylates described in Japanese Patent Publication No. 48-041708, Japanese Patent Publication No. 51-037193, Japanese Patent Publication No. 02-032293, Japanese Patent Publication No. 02-016765, and urethane compounds having an ethylene oxide skeleton described in Japanese Patent Publication No. 58-049860, Japanese Patent Publication No. 56-017654, Japanese Patent Publication No. 62-039417, and Japanese Patent Publication No. 62-039418 are also preferred. In addition, as the radical crosslinking agent, compounds having an amino structure or a sulfide structure in the molecule described in Japanese Patent Publication No. 63-277653, Japanese Patent Publication No. 63-260909, and Japanese Patent Publication No. 01-105238 can also be used.
[0569] The free radical crosslinking agent may also be a free radical crosslinking agent having an acid group such as a carboxyl group or a phosphoric acid group. The free radical crosslinking agent having an acid group is preferably an ester of an aliphatic polyhydroxy compound and an unsaturated carboxylic acid, and more preferably a free radical crosslinking agent having an acid group by reacting a non-aromatic carboxylic acid anhydride with an unreacted hydroxyl group of an aliphatic polyhydroxy compound. It is particularly preferred that the aliphatic polyhydroxy compound is a compound of pentaerythritol or dipentaerythritol among the free radical crosslinking agents having an acid group by reacting a non-aromatic carboxylic acid anhydride with an unreacted hydroxyl group of an aliphatic polyhydroxy compound. As commercially available products, for example, polyacid-modified acrylic oligomers manufactured by TOAGOSEI CO., LTD. include M-510, M-520, etc.
[0570] The preferred acid value of the free radical crosslinking agent having an acid group is particularly preferably 0.1 to 40 mgKOH / g, 5 to 30 mgKOH / g. If the acid value of the free radical crosslinking agent is within the above range, the workability in production is excellent, and further, the developability is excellent. In addition, the polymerizability is good. On the other hand, from the perspective of the developing speed during alkali development, the preferred acid value of the free radical crosslinking agent having an acid group is 0.1 to 300 mgKOH / g, and particularly preferably 1 to 100 mgKOH / g. The above acid value is measured according to the description of JIS K0070:1992.
[0571] From the viewpoint of pattern resolution and film stretchability, the curable resin composition of the present invention preferably uses a bifunctional methacrylate or acrylate. As specific compounds, triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, tetraethylene glycol diacrylate, PEG200 diacrylate, PEG200 dimethacrylate, PEG600 diacrylate, PEG600 dimethacrylate, polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, 3-methyl-1,5-pentanediol diacrylate, 1,6-hex ... Dimethacrylate, dimethylol-tricyclodecane diacrylate, dimethylol-tricyclodecane dimethacrylate, the EO adduct diacrylate of bisphenol A, the EO adduct dimethacrylate of bisphenol A, the PO adduct diacrylate of bisphenol A, the PO adduct dimethacrylate of bisphenol A, 2-hydroxy-3-acryloxypropyl methacrylate, isocyanuric acid EO modified diacrylate, isocyanuric acid modified dimethacrylate, and 2 functional acrylates with carbamate bonds, 2 functional methacrylates with carbamate bonds. These can be mixed and used in two or more according to needs. In addition, for example, PEG200 diacrylate refers to polyethylene glycol diacrylate and the formula weight of polyethylene glycol chain is about 200.
[0572] In addition, from the viewpoint of suppressing the warping accompanying the elastic modulus control of the pattern, as a free radical crosslinking agent, a monofunctional free radical crosslinking agent can be preferably used. As a monofunctional free radical crosslinking agent, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, carbitol (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, N-hydroxymethyl (meth)acrylamide, glycidyl (meth)acrylate, polyethylene glycol mono (meth)acrylate, polypropylene glycol mono (meth)acrylate and other (meth)acrylic acid derivatives, N-vinyl pyrrolidone, N-vinyl caprolactam and other N-vinyl compounds, allyl glycidyl ether, diallyl phthalate, trimellitic acid triallyl ester and the like can be preferably used. As the monofunctional radical crosslinking agent, a compound having a boiling point of 100° C. or higher under normal pressure is also preferred in order to suppress volatilization before exposure.
[0573] When a free radical crosslinking agent is contained, its content is preferably more than 0% by mass and less than 60% by mass relative to the total solid content of the curable resin composition of the present invention. The lower limit is more preferably 5% by mass or more. The upper limit is more preferably 50% by mass or less, and further preferably 30% by mass or less.
[0574] The radical crosslinking agent may be used alone or in combination of two or more. When two or more radical crosslinking agents are used simultaneously, the total amount thereof is preferably within the above range.
[0575] <Other cross-linking agents>
[0576] The curable resin composition of the present invention preferably contains another crosslinking agent different from the above-mentioned radical crosslinking agent.
[0577] In the present invention, other crosslinking agents refer to crosslinking agents other than the above-mentioned free radical crosslinking agents, preferably compounds having multiple groups in the molecule that promote the reaction of forming covalent bonds with other compounds in the composition or their reaction products through the photosensitization of the above-mentioned photosensitizer, and preferably compounds having multiple groups in the molecule that promote the reaction of forming covalent bonds with other compounds in the composition or their reaction products through the action of acids or bases.
[0578] The acid or base is preferably an acid or base generated from a photoacid generator or a photobase generator as a photosensitizer in an exposure step.
[0579] As other crosslinking agents, compounds having at least one group selected from methylol groups and alkoxymethyl groups are preferred, and compounds having a structure in which at least one group selected from methylol groups and alkoxymethyl groups is directly bonded to a nitrogen atom are more preferred.
[0580] As other crosslinking agents, for example, compounds having a structure in which a hydrogen atom of the amino group is substituted with a hydroxymethyl group or an alkoxymethyl group by reacting formaldehyde or formaldehyde and an alcohol with a compound containing an amino group such as melamine, acetylene carbamide, urea, alkylene urea, benzoguanamine, etc. The production method of these compounds is not particularly limited, as long as the compounds have the same structure as the compounds produced by the above method. In addition, oligomers formed by self-condensation of the hydroxymethyl groups of these compounds may be used.
[0581] A cross-linking agent using melamine as the amino group-containing compound is referred to as a melamine-based cross-linking agent, a cross-linking agent using acetylene urea, urea or alkylene urea is referred to as a urea-based cross-linking agent, a cross-linking agent using alkylene urea is referred to as an alkylene urea-based cross-linking agent, and a cross-linking agent using benzoguanamine is referred to as a benzoguanamine-based cross-linking agent.
[0582] Among these, the curable resin composition of the present invention preferably contains at least one compound selected from urea-based crosslinking agents and melamine-based crosslinking agents, and more preferably contains at least one compound selected from glycoluril-based crosslinking agents and melamine-based crosslinking agents described below.
[0583] Specific examples of the melamine-based crosslinking agent include hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, and hexabutoxybutylmelamine.
[0584] Specific examples of the urea-based crosslinking agent include monohydroxymethylated glycoluril, dihydroxymethylated glycoluril, trihydroxymethylated glycoluril, tetrahydroxymethylated glycoluril, monomethoxymethylated glycoluril, dimethoxymethylated glycoluril, trimethoxymethylated glycoluril, tetramethoxymethylated glycoluril, monomethoxymethylated glycoluril, dimethoxymethylated glycoluril, trimethoxymethylated glycoluril, tetraethoxymethylated glycoluril, monopropoxymethylated glycoluril, dipropoxymethylated glycoluril, tripropoxymethylated glycoluril, tetrapropoxymethylated glycoluril, monobutoxymethylated glycoluril, dibutoxymethylated glycoluril, tributoxymethylated glycoluril, or tetrabutoxymethylated glycoluril.
[0585] Urea crosslinking agents such as bismethoxymethyl urea, bisethoxymethyl urea, bispropoxymethyl urea, and bisbutoxymethyl urea;
[0586] Ethylene urea crosslinking agents such as monohydroxymethylated ethylene urea or dihydroxymethylated ethylene urea, monomethoxymethylated ethylene urea, dimethoxymethylated ethylene urea, monoethoxymethylated ethylene urea, diethoxymethylated ethylene urea, monopropoxymethylated ethylene urea, dipropoxymethylated ethylene urea, monobutoxymethylated ethylene urea or dibutoxymethylated ethylene urea;
[0587] Propylene urea crosslinking agents such as monohydroxymethylated propylene urea, dihydroxymethylated propylene urea, monomethoxymethylated propylene urea, dimethoxymethylated propylene urea, monoethoxymethylated propylene urea, diethoxymethylated propylene urea, monopropoxymethylated propylene urea, dipropoxymethylated propylene urea, monobutoxymethylated propylene urea or dibutoxymethylated propylene urea;
[0588] 1,3-bis(methoxymethyl)4,5-dihydroxy-2-imidazolidinone, 1,3-bis(methoxymethyl)-4,5-dimethoxy-2-imidazolidinone, etc. Imidazolidinone
[0589] Specific examples of the benzoguanamine-based crosslinking agent include monohydroxymethylated benzoguanamine, dihydroxymethylated benzoguanamine, trihydroxymethylated benzoguanamine, tetrahydroxymethylated benzoguanamine, monomethoxymethylated benzoguanamine, dimethoxymethylated benzoguanamine, trimethoxymethylated benzoguanamine, tetramethoxymethylated benzoguanamine, monomethoxymethylated benzoguanamine, dimethoxymethylated benzoguanamine, trimethoxymethylated benzoguanamine, tetraethoxymethylated benzoguanamine, monopropoxymethylated benzoguanamine, dipropoxymethylated benzoguanamine, tripropoxymethylated benzoguanamine, tetrapropoxymethylated benzoguanamine, monobutoxymethylated benzoguanamine, dibutoxymethylated benzoguanamine, tributoxymethylated benzoguanamine, and tetrabutoxymethylated benzoguanamine.
[0590] Furthermore, as the compound having at least one group selected from a hydroxymethyl group and an alkoxymethyl group, a compound in which at least one group selected from a hydroxymethyl group and an alkoxymethyl group is directly bonded to an aromatic ring (preferably a benzene ring) can also be preferably used.
[0591] Specific examples of such compounds include benzyl alcohol, bis(hydroxymethyl)cresol, bis(hydroxymethyl)dimethoxybenzene, bis(hydroxymethyl)diphenyl ether, bis(hydroxymethyl)benzophenone, hydroxymethylphenyl hydroxymethylbenzoate, bis(hydroxymethyl)biphenyl, dimethylbis(hydroxymethyl)biphenyl, bis(methoxymethyl)benzene, bis(methoxymethyl)cresol, bis(methoxymethyl)dimethoxybenzene, bis(methoxymethyl)diphenyl ether, bis(methoxymethyl) 1,3-benzenedimethanol], 3,3',5,5'-tetrakis(methoxymethyl)-1,1'-biphenyl-4,4'-diol, and the like.
[0592] As other crosslinking agents, commercially available products may be used. Preferred commercially available products include 46DMOC, 46DMOEP (all manufactured by ASAHI YUKIZAI CORPORATION), DML-PC, DML-PEP, DML-OC, DML-OEP, DML-34X, DML-PTBP, DML-PCHP, DML-OCHP, DML-PFP, DML-PSBP, DML-POP, DML-MBOC, DML-MBPC, DML-MTrisPC, DML-BisOC-Z, DML-BisOCHP-Z, DML-BPC, DMLBisOC-P, DMOM-PC, and DMOM -PTBP, DMOM-MBPC, TriML-P, TriML-35XL, TML-HQ, TML-BP, TML-pp-BPF, TML-BPE, TML-BPA, TML-BPAF, TML-BPAP, TMOM-BP, TMOM-BPE, TMOM-BPA, TMOM-BPAF, TMOM-BPAP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, HMOM-TPHAP (all manufactured by Honshu Chemical Industry Co., Ltd.), NIKARAC (registered trademark, hereinafter the same) MX-290, NIKARAC MX-280, NIKARAC MX-270, NIKARACMX-279, NIKARAC MW-100LM, NIKARAC MX-750LM (all manufactured by Sanwa Chemical Co., Ltd.), etc.
[0593] Furthermore, the curable resin composition of the present invention also preferably contains at least one compound selected from epoxy compounds, oxetane compounds, and benzoxazine compounds as another crosslinking agent.
[0594] [Epoxy compounds (compounds having an epoxy group)]
[0595] As the epoxy compound, a compound having two or more epoxy groups in one molecule is preferred. The epoxy group undergoes a crosslinking reaction below 200°C and does not produce a dehydration reaction derived from the crosslinking, so it is not easy to cause film shrinkage. Therefore, containing an epoxy compound is effective for low-temperature curing of the curable resin composition and suppression of warping.
[0596] The epoxy compound preferably contains a polyethylene oxide group. This further reduces the elastic modulus and can suppress warping. The polyethylene oxide group means that the number of repeating units of ethylene oxide is 2 or more, and preferably the number of repeating units is 2 to 15.
[0597] Examples of epoxy compounds include bisphenol A epoxy resins; bisphenol F epoxy resins; alkylene glycol type epoxy resins or polyol hydrocarbon type epoxy resins such as propylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, butanediol diglycidyl ether, hexamethylene glycol diglycidyl ether, and trimethylolpropane triglycidyl ether; polyalkylene glycol type epoxy resins such as polypropylene glycol diglycidyl ether; epoxy group-containing silicones such as polymethyl (glycidyloxypropyl) siloxane, etc., but are not limited to these. Specific examples include EPICLON (registered trademark) 850-S, EPICLON (registered trademark) HP-4032, EPICLON (registered trademark) HP-7200, EPICLON (registered trademark) HP-820, EPICLON (registered trademark) HP-4700, EPICLON (registered trademark) EXA-4710, EPICLON (registered trademark) HP-4770, EPICLON (registered trademark) EXA-859CRP, EPICLON (registered trademark) EXA-1514, EPICLON (registered trademark) EXA-4880, EPICLON (registered trademark) HP ... ON (registered trademark) EXA-4850-150, EPICLON (registered trademark) EXA-4850-1000, EPICLON (registered trademark) EXA-4816, EPICLON (registered trademark) EXA-4822, EPICLON (registered trademark) EXA-830LVP, EPICLON (registered trademark) EXA-8183, EPICLON (registered trademark) EXA-8169, EPICLON (registered trademark) N-660, EPICLON (registered trademark) N-665-EXP-S, EPICLON (registered trademark) N-740, Rika Rika Resin (registered trademark) BEO-20E (the above are trade names, manufactured by DIC Corporation), Rika Resin (registered trademark) BEO-60E, Rika Resin (registered trademark) HBE-100, Rika Resin (registered trademark) DME-100, Rika Resin (registered trademark) L-200 (trade name, New Japan Chemical Co., Ltd.), EP-4003S, EP-4000S, EP-4088S, EP-3950S (these are trade names, manufactured by ADEKA CORPORATION), CELLOXIDE (registered trademark) 2021P, 2081, 2000, 3000, EHPE3150, EPOLEAD (registered trademark) GT400, CELVENUS (registered trademark) B0134, B0177 (these are trade names, manufactured by Daicel Corporation), NC-3000, NC-3000-L, NC-3000-H, NC-3000-FH-75M, NC-3100, CER-3000-L, NC-2000-L, XD-1000, NC-7000L, NC-7300L, EPPN-501H, EPPN-501HY, EPPN-502H, EOCN-1020, EOCN-102S, EOCN-103S, EOCN-104S, CER-1020, EPPN-201, BREN-S, BREN-10S (the above are trade names, manufactured by Nippon Kayaku Co., Ltd.), etc. .
[0598] [Oxetane compounds (compounds having an oxetane group)]
[0599] Examples of the oxetane compound include compounds having two or more oxetane rings in one molecule, 3-ethyl-3-hydroxymethyloxetane, 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, 3-ethyl-3-(2-ethylhexylmethyl)oxetane, 1,4-benzenedicarboxylic acid-bis[(3-ethyl-3-oxetanyl)methyl]ester, etc. As a specific example, ARON OXETANE series (e.g., OXT-121, OXT-221, OXT-191, OXT-223) manufactured by TOAGOSEI CO., LTD. can be preferably used, and these can be used alone or in combination of two or more.
[0600] [Benzoxazine compounds (compounds having a benzoxazolyl group)]
[0601] Benzoxazine compounds are preferred because they do not generate outgassing during curing due to a crosslinking reaction caused by a ring-opening addition reaction and further reduce thermal shrinkage to suppress the generation of warpage.
[0602] Preferred examples of the benzoxazine compound include Ba-type benzoxazine, Bm-type benzoxazine, Pd-type benzoxazine, Fa-type benzoxazine (these are trade names, manufactured by SHIKOKU CHEMICALS CORPORATION), benzoxazine adducts of polyhydroxystyrene resins, and phenol novolac-type dihydrobenzoxazine compounds. These may be used alone or in combination of two or more.
[0603] The content of other crosslinking agents is preferably 0.1 to 30% by mass, more preferably 0.1 to 20% by mass, further preferably 0.5 to 15% by mass, and particularly preferably 1.0 to 10% by mass relative to the total solid content of the curable resin composition of the present invention. Other crosslinking agents may contain only one or more. In the case of containing two or more other crosslinking agents, it is preferred that the total is within the above range.
[0604] <Compounds having a sulfonamide structure, compounds having a thiourea structure>
[0605] From the viewpoint of improving the adhesion to the substrate of the obtained pattern, the curable resin composition of the present invention preferably further contains at least one compound selected from the group consisting of compounds having a sulfonamide structure and compounds having a thiourea structure.
[0606] [Compounds having a sulfonamide structure]
[0607] The sulfonamide structure is a structure represented by the following formula (S-1).
[0608] [Chemical formula 46]
[0609]
[0610] In formula (S-1), R represents a hydrogen atom or an organic group, and R may be bonded to other structures to form a ring structure, and * each independently represents a bonding site to other structures.
[0611] The above R is preferably the same as R in the following formula (S-2): 2 Same group.
[0612] The compound having a sulfonamide structure may be a compound having two or more sulfonamide structures, and is preferably a compound having one or more sulfonamide structures.
[0613] The compound having a sulfonamide structure is preferably a compound represented by the following formula (S-2).
[0614] [Chemical formula 47]
[0615]
[0616] In formula (S-2), R 1 , R 2 and R 3 Each independently represents a hydrogen atom or a monovalent organic group, R 1 , R 2 and R 3 Two or more of them may be bonded to each other to form a ring structure.
[0617] Preferred R 1 , R 2 and R 3 Each independently is a monovalent organic group.
[0618] As R 1 , R 2 and R 3 Examples of the group include a hydrogen atom, an alkyl group, a cycloalkyl group, an alkoxy group, an alkyl ether group, an alkylsilyl group, an alkoxysilyl group, an aryl group, an aryl ether group, a carboxyl group, a carbonyl group, an allyl group, a vinyl group, a heterocyclic group, or a combination of two or more of these groups.
[0619] The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 6 carbon atoms. Examples of the alkyl group include methyl, ethyl, propyl, butyl, pentyl, hexyl, isopropyl, and 2-ethylhexyl.
[0620] The cycloalkyl group is preferably a cycloalkyl group having 5 to 10 carbon atoms, and more preferably a cycloalkyl group having 6 to 10 carbon atoms. Examples of the cycloalkyl group include cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl.
[0621] The alkoxy group is preferably an alkoxy group having 1 to 10 carbon atoms, and more preferably an alkoxy group having 1 to 5 carbon atoms. Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, and a pentyloxy group.
[0622] The alkoxysilyl group is preferably an alkoxysilyl group having 1 to 10 carbon atoms, and more preferably an alkoxysilyl group having 1 to 4 carbon atoms. Examples of the alkoxysilyl group include a methoxysilyl group, an ethoxysilyl group, a propoxysilyl group, and a butoxysilyl group.
[0623] The aryl group is preferably an aryl group having 6 to 20 carbon atoms, and more preferably an aryl group having 6 to 12 carbon atoms. The aryl group may have a substituent such as an alkyl group. Examples of the aryl group include phenyl, tolyl, xylyl, and naphthyl.
[0624] Examples of the heterocyclic group include a group obtained by removing one hydrogen atom from a heterocyclic structure such as a triazole ring, a pyrrole ring, a furan ring, a thiophene ring, an imidazole ring, an oxazole ring, a thiazole ring, a pyrazole ring, an isoxazole ring, an isothiazole ring, a tetrazole ring, a pyridine ring, a pyridazine ring, a pyrimidine ring, a pyrazine ring, a piperidine ring, a piperazine ring, a morpholine ring, a dihydropyran ring, a tetrahydropyranyl ring, and a triazine ring.
[0625] Among these, R 1 is aryl and preferably R 2 and R 3 A compound wherein each of them is independently a hydrogen atom or an alkyl group.
[0626] Examples of compounds having a sulfonamide structure include benzenesulfonamide, dimethylbenzenesulfonamide, N-butylbenzenesulfonamide, sulfonamide, o-toluenesulfonamide, p-toluenesulfonamide, hydroxynaphthylsulfonamide, naphthyl-1-sulfonamide, naphthyl-2-sulfonamide, m-nitrobenzenesulfonamide, p-chlorobenzenesulfonamide, methanesulfonamide, N,N-dimethylmethanesulfonamide, N,N-dimethylethanesulfonamide, N,N-diethylmethanesulfonamide, N-methoxymethanesulfonamide, N-dodecylmethanesulfonamide, N-cyclohexyl-1-butanesulfonamide, and 2-aminoethanesulfonamide.
[0627] 〔Compounds with thiourea structure〕
[0628] The thiourea structure is a structure represented by the following formula (T-1).
[0629] [Chemical formula 48]
[0630]
[0631] In formula (T-1), R 4 and R 5 Each independently represents a hydrogen atom or a monovalent organic group, R 4 and R 5 Can bond to form a ring, R 4 It can bond with other structures bonded by * to form a ring structure, R 5 It may bond with other structures bonded with * to form a ring structure, and * each independently represents a bonding site with other structures.
[0632] Preferred R 4 and R 5 are each independently a hydrogen atom.
[0633] As R 4 and R 5Examples of the group include a hydrogen atom, an alkyl group, a cycloalkyl group, an alkoxy group, an alkyl ether group, an alkylsilyl group, an alkoxysilyl group, an aryl group, an aryl ether group, a carboxyl group, a carbonyl group, an allyl group, a vinyl group, a heterocyclic group, or a combination of two or more of these groups.
[0634] The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 6 carbon atoms. Examples of the alkyl group include methyl, ethyl, propyl, butyl, pentyl, hexyl, isopropyl, and 2-ethylhexyl.
[0635] The cycloalkyl group is preferably a cycloalkyl group having 5 to 10 carbon atoms, and more preferably a cycloalkyl group having 6 to 10 carbon atoms. Examples of the cycloalkyl group include cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl.
[0636] The alkoxy group is preferably an alkoxy group having 1 to 10 carbon atoms, and more preferably an alkoxy group having 1 to 5 carbon atoms. Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, and a pentyloxy group.
[0637] The alkoxysilyl group is preferably an alkoxysilyl group having 1 to 10 carbon atoms, and more preferably an alkoxysilyl group having 1 to 4 carbon atoms. Examples of the alkoxysilyl group include a methoxysilyl group, an ethoxysilyl group, a propoxysilyl group, and a butoxysilyl group.
[0638] The aryl group is preferably an aryl group having 6 to 20 carbon atoms, and more preferably an aryl group having 6 to 12 carbon atoms. The aryl group may have a substituent such as an alkyl group. Examples of the aryl group include phenyl, tolyl, xylyl, and naphthyl.
[0639] Examples of the heterocyclic group include a group obtained by removing one hydrogen atom from a heterocyclic structure such as a triazole ring, a pyrrole ring, a furan ring, a thiophene ring, an imidazole ring, an oxazole ring, a thiazole ring, a pyrazole ring, an isoxazole ring, an isothiazole ring, a tetrazole ring, a pyridine ring, a pyridazine ring, a pyrimidine ring, a pyrazine ring, a piperidine ring, a piperazine ring, a morpholine ring, a dihydropyran ring, a tetrahydropyranyl ring, and a triazine ring.
[0640] The compound having a thiourea structure may be a compound having two or more thiourea structures, but is preferably a compound having one thiourea structure.
[0641] The compound having a thiourea structure is preferably a compound represented by the following formula (T-2).
[0642] [Chemical formula 49]
[0643]
[0644] In formula (T-2), R4 ~R 7 Each independently represents a hydrogen atom or a monovalent organic group, R 4 ~R 7 At least two of them may be bonded to each other to form a ring structure.
[0645] In formula (T-2), R 4 and R 5 With R in formula (T-1) 4 and R 5 The meanings are the same and the preferred aspects are also the same.
[0646] In formula (T-2), preferably R 6 and R 7 Each independently is a monovalent organic group.
[0647] In formula (T-2), R 6 and R 7 The preferred embodiment of the monovalent organic group in formula (T-1) is the same as R 4 and R 5 The preferred embodiment of the monovalent organic group in is the same as that in the above examples.
[0648] Examples of the compound having a thiourea structure include N-acetylthiourea, N-allylthiourea, N-allyl-N'-(2-hydroxyethyl)thiourea, 1-adamantylthiourea, N-benzoylthiourea, N,N'-diphenylthiourea, 1-benzyl-phenylthiourea, 1,3-dibutylthiourea, 1,3-diisopropylthiourea, 1,3-dicyclohexylthiourea, 1-(3-(trimethoxysilyl)propyl)-3-methylthiourea, trimethylthiourea, tetramethylthiourea, N,N-diphenylthiourea, ethylenethiourea (2-imidazolinethione), carbimazole, and 1,3-dimethyl-2-thiohydantoin.
[0649] 〔content〕
[0650] The total content of the compound having a sulfonamide structure and the compound having a thiourea structure is preferably 0.05 to 10% by mass, more preferably 0.1 to 5% by mass, and further preferably 0.2 to 3% by mass based on the total mass of the curable resin composition of the present invention.
[0651] The curable resin composition of the present invention may contain only one compound selected from the group consisting of compounds having a sulfonamide structure and compounds having a thiourea structure, or may contain two or more compounds. When only one compound is contained, the content of the compound is within the above range, and when two or more compounds are contained, the total amount thereof is preferably within the above range.
[0652] <Migration inhibitor>
[0653] The curable resin composition of the present invention preferably further contains a migration inhibitor. By containing the migration inhibitor, it is possible to effectively suppress the migration of metal ions originating from the metal layer (metal wiring) into the photosensitive film.
[0654] The migration inhibitor is not particularly limited, and examples thereof include compounds having a heterocyclic ring (pyrrole ring, furan ring, thiophene ring, imidazole ring, triazole ring, oxazole ring, thiazole ring, pyrazole ring, isoxazole ring, isothiazole ring, tetrazole ring, pyridine ring, pyridazine ring, pyrimidine ring, pyrazine ring, piperidine ring, piperazine ring, morpholine ring, 2H-pyran ring, 6H-pyran ring, triazine ring), thioureas, compounds having a sulfhydryl group, hindered phenol compounds, salicylic acid derivative compounds, and hydrazide derivative compounds. In particular, triazole compounds such as 1,2,4-triazole and benzotriazole, and tetrazole compounds such as 1H-tetrazole and 5-phenyltetrazole can be preferably used.
[0655] Alternatively, an ion capture agent that captures anions such as halogen ions may also be used.
[0656] As other migration inhibitors, the rust inhibitor described in paragraph 0094 of Japanese Patent Application Publication No. 2013-015701, the compounds described in paragraphs 0073 to 0076 of Japanese Patent Application Publication No. 2009-283711, the compound described in paragraph 0052 of Japanese Patent Application Publication No. 2011-059656, the compounds described in paragraphs 0114, 0116 and 0118 of Japanese Patent Application Publication No. 2012-194520, the compound described in paragraph 0166 of International Publication No. 2015 / 199219, etc. can be used.
[0657] Specific examples of the migration inhibitor include the following compounds.
[0658] [Chemical formula 50]
[0659]
[0660] When the curable resin composition contains a migration inhibitor, the content of the migration inhibitor is preferably 0.01 to 5.0 mass %, more preferably 0.05 to 2.0 mass %, and even more preferably 0.1 to 1.0 mass % based on the total solid content of the curable resin composition.
[0661] The migration inhibitor may be one kind or two or more kinds. When there are two or more kinds of migration inhibitors, the total amount thereof is preferably within the above range.
[0662] <Polymerization inhibitor>
[0663] The curable resin composition of the present invention preferably contains a polymerization inhibitor.
[0664] As the polymerization inhibitor, for example, hydroquinone, o-methoxyphenol, methoxyhydroquinone, p-methoxyphenol, di-tert-butyl-p-cresol, gallol, p-tert-butylcatechol (tert-butylcatechol), 1,4-benzoquinone, diphenyl-p-benzoquinone, 4,4'-thiobis(3-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), N-nitroso-N-phenylhydroxylamine aluminum salt, phenothiazine, N-nitrosodiphenylamine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-4-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl)-1-naphthol, -N-sulfopropylamino)phenol, N-nitrosophenylhydroxylamine cerium salt, N-nitroso-N-(1-naphthyl)hydroxylamine ammonium salt, bis(4-hydroxy-3,5-tert-butyl)phenylmethane, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 4-hydroxy-2,2,6,6-tetramethylpiperidinium 1-oxyl free radical, phenothiazine, 1,1-diphenyl-2-pyrrolohydrazine, dibutyldithiocarbamate copper(II), nitrobenzene, N-nitroso-N-phenylhydroxylamine aluminum salt, N-nitroso-N-phenylhydroxylamine ammonium salt, N,N'-diphenyl-p-phenylenediamine, 2,4-di-tert-butylphenol, di-tert-butylhydroxytoluene, 1,4-naphthoquinone, etc. Furthermore, the polymerization inhibitor described in paragraph 0060 of JP-A-2015-127817 and the compounds described in paragraphs 0031 to 0046 of WO 2015 / 125469 can also be used.
[0665] Furthermore, the following compounds can be used.
[0666] [Chemical formula 51]
[0667]
[0668] When the curable resin composition of the present invention contains a polymerization inhibitor, the content of the polymerization inhibitor is 0.01 to 20.0% by mass, preferably 0.01 to 5% by mass, more preferably 0.02 to 3% by mass, and further preferably 0.05 to 2.5% by mass, relative to the total solid content of the curable resin composition of the present invention.
[0669] The polymerization inhibitor may be one kind or two or more kinds. When there are two or more kinds of polymerization inhibitors, the total amount thereof is preferably within the above range.
[0670] <Metal Adhesion Improver>
[0671] The curable resin composition of the present invention preferably contains a metal adhesion improver for improving adhesion to metal materials used in electrodes or wiring, etc. Examples of the metal adhesion improver include silane coupling agents, aluminum-based adhesion aids, titanium-based adhesion aids, compounds having a sulfonamide structure and compounds having a thiourea structure, phosphoric acid derivative compounds, β-ketoester compounds, amino compounds, and the like.
[0672] Examples of silane coupling agents include compounds described in paragraph 0167 of International Publication No. 2015 / 199219, compounds described in paragraphs 0062 to 0073 of Japanese Patent Application Laid-Open No. 2014-191002, compounds described in paragraphs 0063 to 0071 of International Publication No. 2011 / 080992, compounds described in paragraphs 0060 to 0061 of Japanese Patent Application Laid-Open No. 2014-191252, compounds described in paragraphs 0045 to 0052 of Japanese Patent Application Laid-Open No. 2014-041264, and compounds described in paragraph 0055 of International Publication No. 2014 / 097594. In addition, as described in paragraphs 0050 to 0058 of Japanese Patent Application Laid-Open No. 2011-128358, it is also preferred to use two or more different silane coupling agents. Furthermore, the following compounds are also preferably used as the silane coupling agent. In the following formula, Et represents an ethyl group.
[0673] [Chemical formula 52]
[0674]
[0675] Examples of other silane coupling agents include vinyl trimethoxysilane, vinyl triethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, 3-glycidyloxypropyl methyl dimethoxysilane, 3-glycidyloxypropyl trimethoxysilane, 3-glycidyloxypropyl methyl diethoxysilane, 3-glycidyloxypropyl triethoxysilane, p-phenylenediyl trimethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl methyl diethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-acryloxypropyl Acyloxypropyl trimethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxysilane, N-2-(aminoethyl)-3-aminopropyl trimethoxysilane, 3-aminopropyl trimethoxysilane, 3-aminopropyl triethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylene) propylamine, N-phenyl-3-aminopropyl trimethoxysilane, tris-(trimethoxysilylpropyl) isocyanurate, 3-ureidopropyl trialkoxysilane, 3-butylene propyl methyl dimethoxysilane, 3-butylene propyl trimethoxysilane, 3-isocyanate propyl triethoxysilane, 3-trimethoxysilylpropyl succinic anhydride. These can be used alone or in combination of two or more.
[0676] 〔Aluminum-based adhesive additive〕
[0677] Examples of the aluminum-based adhesion promoter include tris(ethylacetoacetate)aluminum, tris(acetylacetonate)aluminum, and ethylacetoacetate aluminum diisopropyl.
[0678] As the metal adhesion improver, the compounds described in paragraphs 0046 to 0049 of JP-A-2014-186186 and the sulfide compounds described in paragraphs 0032 to 0043 of JP-A-2013-072935 can also be used.
[0679] The content of the metal adhesion improver is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, and further preferably 0.5 to 5 parts by mass relative to 100 parts by mass of the specific resin. By setting it to above the above lower limit, the adhesion between the pattern and the metal layer becomes good, and by setting it to below the above upper limit, the heat resistance and mechanical properties of the pattern become good. The metal adhesion improver may be only one or more than two. When using two or more, it is preferred that the total is within the above range.
[0680] <Metal Adhesion Improver>
[0681] The curable resin composition of the present invention preferably contains a metal adhesion improver for improving adhesion to metal materials used in electrodes or wiring, etc. As the metal adhesion improver, compounds described in paragraphs 0046 to 0049 of Japanese Unexamined Patent Publication No. 2014-186186 and sulfide compounds described in paragraphs 0032 to 0043 of Japanese Unexamined Patent Publication No. 2013-072935 can also be used.
[0682] The content of the metal adhesion improver is preferably 0.1 to 30 parts by mass, more preferably in the range of 0.5 to 15 parts by mass, and further preferably in the range of 0.5 to 5 parts by mass, relative to 100 parts by mass of the polymer precursor containing the heterocycle. By setting it to above the above lower limit, the adhesion between the pattern and the metal layer after the heating process becomes good, and by setting it to below the above upper limit, the heat resistance and mechanical properties of the cured product after the heating process become good. The metal adhesion improver may be only one or more than two. When using two or more, it is preferred that the total is within the above range.
[0683] <Other additives>
[0684] The curable resin composition of the present invention can be formulated with various additives as needed within the range in which the effects of the present invention can be obtained, such as sensitizers, chain transfer agents, surfactants, higher fatty acid derivatives, inorganic particles, curing agents, curing catalysts, fillers, antioxidants, ultraviolet absorbers, anti-agglomeration agents, etc. When these additives are formulated, the total amount thereof is preferably set to 3% by mass or less of the solid content of the curable resin composition.
[0685] 〔Sensitizer〕
[0686] The curable resin composition of the present invention may contain a sensitizer. The sensitizer absorbs specific active radiation and becomes an electronically excited state. The sensitizer in the electronically excited state contacts with a thermal curing accelerator, a thermal free radical polymerization initiator, a photo-free radical polymerization initiator, etc. to generate electron transfer, energy transfer, heat generation, etc. As a result, the thermal curing accelerator, the thermal free radical polymerization initiator, and the photo-free radical polymerization initiator undergo chemical changes and decompose, thereby generating free radicals, acids, or bases.
[0687] Examples of the sensitizer include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzylidene)cyclopentane, 2,6-bis(4'-diethylaminobenzylidene)cyclohexanone, 2,6-bis(4'-diethylaminobenzylidene)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, p-dimethylaminophenylallylidene dihydroindanone, p-Dimethylaminobenzylidene dihydroindanone, 2-(p-dimethylaminophenyl biphenylene)-benzothiazole, 2-(p-dimethylaminophenyl vinylene)benzothiazole, 2-(p-dimethylaminophenyl vinylene)isonaphthylthiazole, 1,3-bis(4'-dimethylaminobenzylidene)acetone, 1,3-bis(4'-diethylaminobenzylidene)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-acetyl-7-dimethyl 3-Methoxycarbonyl-7-dimethylaminocoumarin, 3-Benzyloxycarbonyl-7-dimethylaminocoumarin, 3-Methoxycarbonyl-7-diethylaminocoumarin, 3-Ethoxycarbonyl-7-diethylaminocoumarin, N-Phenyl-N'-ethylethanolamine, N-Phenyldiethanolamine, N-p-Tolyldiethanolamine, N-Phenylethanolamine, 4-Morpholinobenzophenone, Isoamyl Dimethylaminobenzoate, Diethylaminobenzyl isopentyl ester, 2-benzimidazole, 1-phenyl-5-benzyltetrazolyl, 2-benzthiazole, 2-(p-dimethylaminostyrene)benzoxazole, 2-(p-dimethylaminostyrene)benzothiazole, 2-(p-dimethylaminostyrene)naphtho(1,2-d)thiazole, 2-(p-dimethylaminobenzoyl)styrene, diphenylacetamide, benzanilide, N-methylacetanilide, 3',4'-dimethylacetanilide, etc.
[0688] As the sensitizer, a sensitizing dye may also be used.
[0689] For details of the sensitizing dye, reference can be made to paragraphs 0161 to 0163 of Japanese Patent Application Laid-Open No. 2016-027357, the contents of which are incorporated herein.
[0690] When the curable resin composition of the present invention contains a sensitizer, the content of the sensitizer is preferably 0.01 to 20% by mass, more preferably 0.1 to 15% by mass, and further preferably 0.5 to 10% by mass relative to the total solid content of the curable resin composition of the present invention. The sensitizer may be used alone or in combination of two or more.
[0691] 〔Chain transfer agent〕
[0692] The curable resin composition of the present invention may contain a chain transfer agent. Chain transfer agents are defined, for example, in the third edition of the Polymer Dictionary (edited by the Polymer Society, 2005) on pages 683-684. As chain transfer agents, for example, a compound group having SH, PH, SiH and GeH in the molecule can be used. These can supply hydrogen to low-activity free radicals to generate free radicals, or generate free radicals by deprotonation after oxidation. In particular, thiol compounds can be preferably used.
[0693] Furthermore, as the chain transfer agent, the compounds described in paragraphs 0152 to 0153 of International Publication No. 2015 / 199219 can also be used.
[0694] When the curable resin composition of the present invention has a chain transfer agent, the content of the chain transfer agent is preferably 0.01 to 20 parts by mass, more preferably 1 to 10 parts by mass, and further preferably 1 to 5 parts by mass relative to 100 parts by mass of the total solid content of the curable resin composition of the present invention. The chain transfer agent may be only one or more than two. When there are two or more chain transfer agents, it is preferred that the total is within the above range.
[0695] 〔Surfactant〕
[0696] From the viewpoint of further improving the coating property, a surfactant can be added to the curable resin composition of the present invention. As the surfactant, various surfactants such as fluorine-based surfactants, nonionic surfactants, cationic surfactants, anionic surfactants, silicone surfactants can be used. In addition, the following surfactants are also preferred. In the following formula, the brackets representing the repeating units of the main chain represent the content (mol %) of each repeating unit, and the brackets representing the repeating units of the side chains represent the number of repetitions of each repeating unit.
[0697] [Chemical formula 53]
[0698]
[0699] Furthermore, as the surfactant, the compounds described in paragraphs 0159 to 0165 of International Publication No. 2015 / 199219 can also be used.
[0700] Regarding the fluorine-based surfactant, a fluorine-containing polymer having an ethylenically unsaturated group in a side chain can also be used as the fluorine-based surfactant. As specific examples, compounds described in paragraphs 0050 to 0090 and paragraphs 0289 to 0295 of Japanese Patent Application Publication No. 2010-164965, such as MEGAFACE RS-101, RS-102, and RS-718K manufactured by DIC Corporation can be cited.
[0701] The fluorine content in the fluorine-based surfactant is preferably 3 to 40% by mass, more preferably 5 to 30% by mass, and particularly preferably 7 to 25% by mass. From the perspective of uniformity of the thickness of the coating film or liquid saving, a fluorine-based surfactant having a fluorine content within this range is effective and has good solubility in the composition.
[0702] Examples of the silicone surfactant include Toray Silicone DC3PA, Toray Silicone SH7PA, Toray Silicone DC11PA, Toray Silicone SH21PA, Toray Silicone SH28PA, Toray Silicone SH29PA, Toray Silicone SH30PA, and Toray Silicone SH8400 (all manufactured by Dow Corning Toray Co., Ltd.), TSF-4440, TSF-4300, TSF-4445, TSF-4460, and TSF-4452 (all manufactured by Momentive Performance Materials Inc.), KP341, KF6001, and KF6002 (all manufactured by Shin-Etsu Chemical Co., Ltd.), BYK307, BYK323, and BYK330 (all manufactured by BYK Chemie GmbH).
[0703] Examples of the hydrocarbon-based surfactant include PIONIN A-76, New Kalgen FS-3PG, PIONIN B-709, PIONIN B-811-N, PIONIN D-1004, PIONIN D-3104, PIONIN D-3605, PIONIN D-6112, PIONIN D-2104-D, PIONIN D-212, PIONIN D-931, PIONIN D-941, PIONIN D-951, PIONIN E-5310, PIONIN P-1050-B, PIONIN P-1028-P, and PIONIN P-4050-T (all manufactured by Takemoto Oil & Fat Co., Ltd.).
[0704] Examples of the nonionic surfactant include glycerin, trimethylolpropane, trimethylolethane, and ethoxylates and propoxylates thereof (e.g., glycerin propoxylate, glycerin ethoxylate, etc.), polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyethylene glycol dilaurate, polyethylene glycol distearate, sorbitan fatty acid esters, Pluronic (registered trademark) L10, L31, L61, L62, 10R5, 17R2, 25R2 (manufactured by BASF), Tetronic 304, 701, 704, 901, 904, 150R1 (manufactured by BASF), Solsperse 20000 (manufactured by Lubrizol Japan Limited.), NCW-101, NCW-1001, NCW-1002 (manufactured by Wako Pure Chemical Industries, Ltd.), PIONIN D-6112, D-6112-W, D-6315 (manufactured by Takemoto Oil & Fat Co., Ltd.), Olfine E1010, Surfynol 104, 400, 440 (manufactured by Nissin Chemical Co., Ltd.), etc.
[0705] Specific examples of the cationic surfactant include organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.), (meth)acrylic (co)polymer Polyflow No. 75, No. 77, No. 90, No. 95 (manufactured by Kyoeisha Chemical Co., Ltd.), and W001 (manufactured by Yusho Co., Ltd.).
[0706] Specific examples of the anionic surfactant include W004, W005, and W017 (manufactured by Yusho Co., Ltd.), and SANDET BL (manufactured by Sanyo Kasei Co., Ltd.).
[0707] When the curable resin composition of the present invention has a surfactant, the content of the surfactant is preferably 0.001 to 2.0 mass %, more preferably 0.005 to 1.0 mass % relative to the total solid content of the curable resin composition of the present invention. The surfactant may be only one or more than two. When there are two or more surfactants, it is preferred that the total is within the above range.
[0708] 〔Higher fatty acid derivatives〕
[0709] In order to prevent polymerization inhibition caused by oxygen, a higher fatty acid derivative such as behenic acid or behenic acid amide may be added to the curable resin composition of the present invention so as to be unevenly distributed on the surface of the curable resin composition during the drying process after coating.
[0710] Furthermore, as the higher fatty acid derivatives, compounds described in paragraph 0155 of International Publication No. 2015 / 199219 can also be used.
[0711] When the curable resin composition of the present invention has a higher fatty acid derivative, the content of the higher fatty acid derivative is preferably 0.1 to 10% by mass relative to the total solid content of the curable resin composition of the present invention. The higher fatty acid derivative may be only one or more than two. When there are two or more higher fatty acid derivatives, it is preferred that the total is within the above range.
[0712] 〔Inorganic particles〕
[0713] The resin composition of the present invention may contain inorganic particles. Specifically, the inorganic particles may include calcium carbonate, calcium phosphate, silicon dioxide, kaolin, talc, titanium dioxide, aluminum oxide, barium sulfate, calcium fluoride, lithium fluoride, zeolite, molybdenum sulfide, glass, and the like.
[0714] The average particle size of the inorganic particles is preferably 0.01 to 2.0 μm, more preferably 0.02 to 1.5 μm, further preferably 0.03 to 1.0 μm, and particularly preferably 0.04 to 0.5 μm.
[0715] When the average particle diameter of the inorganic particles is large, the mechanical properties of the cured film may be deteriorated. Also, when the average particle diameter of the inorganic particles exceeds 2.0 μm, the resolution may be reduced due to scattering of exposure light.
[0716] 〔Ultraviolet light absorber〕
[0717] The composition of the present invention may contain an ultraviolet absorber. As the ultraviolet absorber, a salicylate-based, benzophenone-based, benzotriazole-based, substituted acrylonitrile-based, triazine-based, or other ultraviolet absorber may be used.
[0718] Examples of salicylate-based ultraviolet absorbers include phenyl salicylate, p-octylphenyl salicylate, and p-tert-butylphenyl salicylate. Examples of benzophenone-based ultraviolet absorbers include 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2,4-dihydroxybenzophenone, and 2-hydroxy-4-octyloxybenzophenone. Examples of the benzotriazole ultraviolet absorber include 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-amyl-5'-isobutylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-isobutyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-isobutyl-5'-propylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 2-[2'-hydroxy-5'-(1,1,3,3-tetramethyl)phenyl]benzotriazole.
[0719] Examples of the substituted acrylonitrile-based ultraviolet absorber include ethyl 2-cyano-3,3-diphenylacrylate and 2-ethylhexyl 2-cyano-3,3-diphenylacrylate. Examples of triazine-based ultraviolet absorbers include mono(hydroxyphenyl)triazine compounds such as 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2-(2,4-dihydroxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine; 2,4-bis(2-hydroxy-4-propoxyphenyl)-6-(2,4-dimethylphenyl)-1,3,5-triazine; Bis(hydroxyphenyl)triazine compounds such as 2,4-bis(2-hydroxy-3-methyl-4-propoxyphenyl)-6-(4-methylphenyl)-1,3,5-triazine and 2,4-bis(2-hydroxy-3-methyl-4-hexyloxyphenyl)-6-(2,4-dimethylphenyl)-1,3,5-triazine; tris(hydroxyphenyl)triazine compounds such as 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-octyloxyphenyl)-1,3,5-triazine and 2,4,6-tris[2-hydroxy-4-(3-butoxy-2-hydroxypropoxy)phenyl]-1,3,5-triazine, etc.
[0720] In the present invention, the above-mentioned various ultraviolet absorbers may be used alone or in combination of two or more.
[0721] The composition of the present invention may or may not contain a UV absorber, but when containing a UV absorber, the content of the UV absorber is preferably 0.001% by mass to 1% by mass, more preferably 0.01% by mass to 0.1% by mass, relative to the total solid content of the composition of the present invention.
[0722] 〔Organotitanium compounds〕
[0723] The resin composition of the present embodiment may contain an organic titanium compound. When the resin composition contains an organic titanium compound, a resin layer having excellent chemical resistance can be formed even when the resin composition is cured at a low temperature.
[0724] Examples of the organic titanium compound that can be used include compounds in which an organic group is bonded to a titanium atom via a covalent bond or an ionic bond.
[0725] Specific examples of the organic titanium compound are shown in the following I) to VII):
[0726] I) Titanium chelate compound: Among them, from the viewpoint of good storage stability of the negative photosensitive resin composition and the ability to obtain a good cured pattern, a titanium chelate compound having two or more alkoxy groups is more preferred. Specific examples include bis(triethanolamine)titanium diisopropoxide, bis(2,4-glutarate)di(n-butoxy)titanium, diisopropoxytitanium bis(2,4-glutarate), diisopropoxytitanium bis(tetramethylpimelate), diisopropoxytitanium bis(ethyl acetate), and the like.
[0727] II) Tetraalkoxytitanium compounds: for example, tetra(n-butoxy)titanium, tetraethoxytitanium, tetra(2-ethylhexyloxy)titanium, tetraisobutoxytitanium, tetraisopropoxytitanium, tetramethoxytitanium, tetramethoxypropoxytitanium, tetramethylphenoxytitanium, tetra(n-nonoxy)titanium, tetra(n-propoxy)titanium, tetrastearyltitanium, tetrakis[bis{2,2-(allyloxymethyl)butoxy}]titanium, etc.
[0728] III) Titanocene compounds: for example, pentamethylcyclopentadienyl titanium trimethoxide, bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluorophenyl)titanium, bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, etc.
[0729] IV) Monoalkoxy titanium compound: for example, tris(dioctyl phosphate)isopropoxytitanium, tris(dodecylbenzene sulfonate)isopropoxytitanium, and the like.
[0730] V) Titanium oxide compound: for example, bis(glutarate)titanium oxide, bis(tetramethylpimelate)titanium oxide, titanium phthalocyanine oxide, and the like.
[0731] VI) Titanium tetraacetylacetonate compound: for example, titanium tetraacetylacetonate.
[0732] VII) Titanate coupling agent: for example, isopropyl tridodecylbenzenesulfonyl titanate.
[0733] Among them, as an organic titanium compound, from the viewpoint of exerting better chemical resistance, at least one compound selected from the above-mentioned I) titanium chelate compound, II) tetraalkoxy titanium compound and III) titanocene compound is preferred. In particular, bis(ethyl acetoacetate)diisopropoxytitanium, tetra(n-butoxy)titanium and bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium are preferred.
[0734] When an organic titanium compound is added, the amount thereof is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 2 parts by mass, relative to 100 parts by mass of the precursor of the cyclized resin. When the amount is 0.05 parts by mass or more, good heat resistance and chemical resistance are exhibited in the obtained cured pattern, while when the amount is 10 parts by mass or less, the storage stability of the composition is excellent.
[0735] 〔Antioxidant〕
[0736] The composition of the present invention may contain an antioxidant. By containing an antioxidant as an additive, the ductility characteristics of the cured film or the adhesion to the metal material can be improved. As the antioxidant, phenol compounds, phosphite compounds, thioether compounds, etc. can be mentioned. As the phenol compound, any phenol compound known as a phenolic antioxidant can be used. As a preferred phenol compound, a hindered phenol compound can be mentioned. Preferably, a compound has a substituent at the position adjacent to the phenolic hydroxyl group (ortho position). As the substituent, a substituted or unsubstituted alkyl group having 1 to 22 carbon atoms is preferred. In addition, a compound having a phenol group and a phosphite group in the same molecule is also preferred. In addition, the antioxidant can also preferably use a phosphorus antioxidant. Examples of the phosphorus-based antioxidant include tris[2-[[2,4,8,10-tetrakis(1,1-dimethylethyl)dibenzo[d,f][1,3,2]dioxaphosphepin-6-yl]oxy]ethyl]amine, tris[2-[(4,6,9,11-tetrakis-tert-butyldibenzo[d,f][1,3,2]dioxaphosphepin-2-yl)oxy]ethyl]amine, and bis(2,4-di-tert-butyl-6-methylphenol)ethyl phosphite. As commercially available antioxidants, for example, ADKSTAB AO-20, ADKSTAB AO-30, ADKSTAB AO-40, ADKSTAB AO-50, ADKSTAB AO-50F, ADKSTAB AO-60, ADKSTAB AO-60G, ADKSTAB AO-80, ADKSTAB AO-330 (all manufactured by ADEKA CORPORATION) and the like can be cited. In addition, the antioxidant can also use the compounds described in paragraphs 0023 to 0048 of Japanese Patent Gazette No. 6268967. In addition, the composition of the present invention may contain a potential antioxidant as required. As a potential antioxidant, a compound in which the site that acts as an antioxidant is protected by a protecting group and the protecting group is detached by heating at 100 to 250° C. or heating at 80 to 200° C. in the presence of an acid / base catalyst, thereby acting as an antioxidant. As potential antioxidants, compounds described in International Publication No. 2014 / 021023, International Publication No. 2017 / 030005, and Japanese Patent Publication No. 2017-008219 can be cited. Commercially available products of potential antioxidants include ADEKAARKLS GPA-5001 (manufactured by ADEKA CORPORATION) and the like. Examples of preferred antioxidants include 2,2-thiobis(4-methyl-6-tert-butylphenol), 2,6-di-tert-butylphenol, and compounds represented by the general formula (3).
[0737] [Chemical formula 54]
[0738]
[0739] In the general formula (3), R 5 represents a hydrogen atom or an alkyl group having 2 or more carbon atoms, R 6 represents an alkylene group having 2 or more carbon atoms. 7 represents an alkylene group having 2 or more carbon atoms, or a monovalent to tetravalent organic group containing at least one of an O atom and an N atom. k represents an integer of 1 to 4.
[0740] The compound represented by the general formula (3) suppresses oxidative degradation of aliphatic groups or phenolic hydroxyl groups of resins and can suppress metal oxidation by its rust-proofing effect on metal materials.
[0741] Since it can act on both the resin and the metal material, k is more preferably an integer of 2 to 4. 7 , alkyl, cycloalkyl, alkoxy, alkyl ether, alkyl silyl, alkoxy silyl, aryl, aryl ether, carboxyl, carbonyl, allyl, vinyl, heterocyclic, -O-, -NH-, -NHNH-, combinations thereof, etc. may be mentioned, and may further have a substituent. Among them, alkyl ether and -NH- are preferred from the viewpoint of solubility in a developer or metal adhesion, and -NH- is more preferred from the viewpoint of interaction with a resin and metal adhesion based on metal complex formation.
[0742] Examples of the compound represented by the following general formula (3) include the following compounds, but are not limited to the following structures.
[0743] [Chemical formula 55]
[0744]
[0745] [Chemical formula 56]
[0746]
[0747] [Chemical formula 57]
[0748]
[0749] [Chemical formula 58]
[0750]
[0751] The amount of the antioxidant added is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, relative to the resin. When the amount added is less than 0.1 parts by mass, it is difficult to obtain the effect of improving the ductility characteristics after reliability or the adhesion to the metal material, and when the amount added is more than 10 parts by mass, the sensitivity of the resin composition may decrease due to the interaction with the photosensitive agent. Only one antioxidant may be used, or two or more antioxidants may be used. When two or more antioxidants are used, the total amount is preferably within the above range.
[0752] <Regulation on other substances contained>
[0753] From the viewpoint of the coating surface properties, the water content of the curable resin composition of the present invention is preferably less than 5% by mass, more preferably less than 1% by mass, and further preferably less than 0.6% by mass. As a method for maintaining the water content, the humidity under the storage conditions, the porosity of the storage container, etc. can be cited.
[0754] From the viewpoint of insulation, the metal content of the curable resin composition of the present invention is preferably less than 5 mass ppm (parts per million), more preferably less than 1 mass ppm, and further preferably less than 0.5 mass ppm. Examples of the metal include sodium, potassium, magnesium, calcium, iron, chromium, nickel, etc. When multiple metals are included, the total amount of these metals is preferably within the above range.
[0755] In addition, as a method for reducing metal impurities unintentionally contained in the curable resin composition of the present invention, the following methods can be cited: selecting a raw material with a low metal content as a raw material constituting the curable resin composition of the present invention; filtering the raw material constituting the curable resin composition of the present invention; lining the inside of the apparatus with polytetrafluoroethylene or the like to perform distillation under conditions that minimize contamination.
[0756] In the curable resin composition of the present invention, if the use as a semiconductor material is considered, the content of halogen atoms is preferably less than 500 mass ppm, more preferably less than 300 mass ppm, and further preferably less than 200 mass ppm from the viewpoint of wiring corrosion. Among them, the content in the form of halogen ions is preferably less than 5 mass ppm, more preferably less than 1 mass ppm, and further preferably less than 0.5 mass ppm. As halogen atoms, chlorine atoms and bromine atoms can be cited. Preferably, the total of chlorine atoms and bromine atoms, or chlorine ions and bromide ions, is within the above range.
[0757] As a method for adjusting the content of halogen atoms, ion exchange treatment or the like is preferably mentioned.
[0758] As a storage container for the curable resin composition of the present invention, a conventionally known storage container can be used. In addition, as a storage container, in order to suppress the mixing of impurities into the raw materials or the curable composition, it is also preferred to use a multilayer bottle whose inner wall is composed of 6 kinds of 6 layers of resin or a bottle having a 7-layer structure made of 6 kinds of resin. As such a container, for example, the container described in Japanese Patent Publication No. 2015-123351 can be cited.
[0759] <Application of curable resin composition>
[0760] The curable resin composition of the present invention is preferably used for forming an interlayer insulating film for a redistribution layer.
[0761] Furthermore, in addition to these, the present invention can also be used for forming an insulating film of a semiconductor device, forming a stress buffer film, and the like.
[0762] <Preparation of curable resin composition>
[0763] The curable resin composition of the present invention can be prepared by mixing the above-mentioned components. The mixing method is not particularly limited, and can be carried out by a conventionally known method.
[0764] Furthermore, for the purpose of removing foreign matter such as dust or particles in the curable resin composition, it is preferred to filter using a filter. The filter pore size is preferably less than 1 μm, more preferably less than 0.5 μm, and further preferably less than 0.1 μm. On the other hand, from the perspective of productivity, it is preferably less than 5 μm, more preferably less than 3 μm, and further preferably less than 1 μm. The material of the filter is preferably polytetrafluoroethylene, polyethylene or nylon. The filter can use a filter that has been pre-cleaned with an organic solvent. In the filter filtering process, a variety of filters can be connected in series or in parallel. When using a variety of filters, filters with different pore sizes or materials can be used in combination. Furthermore, various materials can be filtered multiple times. When filtering multiple times, it can be a circulation filter. Furthermore, filtering can be performed by pressurization. When filtering by pressurization, the pressurization pressure is preferably 0.05 MPa or more and 0.3 MPa or less. On the other hand, from the viewpoint of productivity, it is preferably 0.01 MPa to 1.0 MPa, more preferably 0.03 MPa to 0.9 MPa, and even more preferably 0.05 MPa to 0.7 MPa.
[0765] In addition to filtering using a filter, impurity removal using an adsorbent may also be performed. Filter filtering and impurity removal using an adsorbent may also be combined. As the adsorbent, a known adsorbent may be used. For example, inorganic adsorbents such as silica gel and zeolite, and organic adsorbents such as activated carbon may be cited.
[0766] (Cured film, laminated body, semiconductor device and method for manufacturing the same)
[0767] Next, a cured film, a laminated body, a semiconductor device, and a method for producing the same will be described.
[0768] The cured film of the present invention is a cured film formed by curing the resin composition of the present invention. The cured film is preferably a patterned cured film. The film thickness of the cured film of the present invention can be, for example, 0.5 μm or more, or 1 μm or more. And, as an upper limit, it can be 100 μm or less, or 30 μm or less.
[0769] The cured film of the present invention can be stacked in 2 or more layers, and further 3 to 7 layers to form a laminate. The laminate of the present invention preferably includes a mode in which two or more cured films are included and a metal layer is included between any of the above-mentioned cured films. For example, as a preferred laminate, there can be cited a laminate having a layer structure including at least three layers of a first cured film, a metal layer, and a second cured film stacked in sequence. The above-mentioned first cured film and the above-mentioned second cured film are both the cured films of the present invention. As a preferred mode, for example, there can be cited a mode in which the above-mentioned first cured film and the above-mentioned second cured film are both films formed by curing the resin composition of the present invention. The resin composition of the present invention used to form the above-mentioned first cured film and the resin composition of the present invention used to form the above-mentioned second cured film may be a composition of the same composition or a composition of different composition. The metal layer in the laminate of the present invention can be preferably used as a metal wiring of a redistribution layer or the like.
[0770] As the fields to which the cured film of the present invention can be applied, there can be cited insulating films of semiconductor devices, interlayer insulating films for redistribution layers, pressure buffer films, etc. In addition, there can be cited the formation of patterns on sealing films, substrate materials (base films or cover films of flexible printed substrates, interlayer insulating films), or insulating films for packaging purposes as described above by etching. For these uses, for example, reference can be made to SCIENCE AND TECHNOLOGY CO., LTD. "High Functionalization and Application Technology of Polyimide" April 2008, supervised by Masaaki Kakimoto, CMC Technical library "Basics and Development of Polyimide Materials" November 2011, Japan Polyimide and Aromatic Polymer Research Association / Editor "Latest Polyimide Basics and Applications" NTS Inc., August 2010, etc.
[0771] Furthermore, the cured film of the present invention can also be used in the production of printing plates such as offset printing plates and screen printing plates, in the etching of molded components, and in the production of protective varnishes and dielectric layers in electronics, especially microelectronics.
[0772] The method for producing a cured film of the present invention (hereinafter, also simply referred to as “the production method of the present invention”) preferably includes a film forming step of applying the resin composition of the present invention to a substrate to form a film (resin film).
[0773] The method for producing a cured film of the present invention preferably includes the film forming step, an exposure step of exposing the film, and a development step of developing the film. The exposure step and the development step can obtain a pattern of the cured film.
[0774] Furthermore, the method for producing a cured film of the present invention more preferably includes the film forming step and, if necessary, the developing step, and also includes a heating step of heating the film at 50 to 450°C.
[0775] Specifically, it is also preferable to include the following steps (a) to (d).
[0776] (a) Film forming step of applying the resin composition to a substrate to form a film (resin composition layer)
[0777] (b) After the film forming step, an exposure step of exposing the film to light
[0778] (c) A developing step of developing the exposed film
[0779] (d) a heating step of heating the developed film at 50 to 450° C.
[0780] By heating in the heating step, the resin layer cured by exposure can be further cured. In the heating step, for example, the thermal base generator is decomposed to obtain sufficient curability.
[0781] The method for manufacturing a laminated body according to a preferred embodiment of the present invention includes a method for manufacturing a cured film of the present invention. After forming a cured film according to the method for manufacturing a laminated body of the present embodiment, the process (a) or the processes (a) to (c) or the processes (a) to (d) are further performed again. In particular, it is preferred that the above-mentioned processes are performed in sequence multiple times, for example 2 to 5 times (i.e., 3 to 6 times in total). By stacking the cured films in this way, a laminated body can be made. In the present invention, a metal layer is preferably provided on a portion where a cured film is provided or between the cured films, or on a portion where a cured film is provided and between the cured films. In addition, when manufacturing a laminated body, it is not necessary to repeatedly perform all the processes (a) to (d). As described above, a laminated body of a cured film can be obtained by performing at least multiple times (a), preferably multiple times (a) to (c) or (a) to (d).
[0782] <Film forming step (layer forming step)>
[0783] The production method according to a preferred embodiment of the present invention includes a film forming step (layer forming step) of applying the resin composition to a substrate to form a film (layer).
[0784] The type of substrate can be appropriately specified according to the purpose, and can be a semiconductor manufacturing substrate such as silicon, silicon nitride, polycrystalline silicon, silicon oxide, amorphous silicon, quartz, glass, optical film, ceramic material, vapor-deposited film, magnetic film, reflective film, Ni, Cu, Cr, Fe and other metal substrates, paper, SOG (Spin On Glass: spin-coated glass), TFT (thin film transistor) array substrate, plasma display panel (PDP) electrode plate, etc., without any particular restrictions. In addition, these substrates can be provided with a layer such as a close contact layer or an oxide layer on the surface. In the present invention, semiconductor manufacturing substrates are particularly preferred, and silicon substrates, Cu substrates and molded substrates are more preferred.
[0785] Furthermore, these substrates may be provided with a layer such as an adhesion layer or an oxide layer formed of hexamethyldisilazane (HMDS) or the like on the surface.
[0786] Furthermore, as the base material, for example, a plate-shaped base material (substrate) can be used.
[0787] The shape of the substrate is not particularly limited and may be circular or rectangular, but is preferably rectangular.
[0788] The size of the substrate is, for example, 100 to 450 mm in diameter, preferably 200 to 450 mm in diameter, in the case of a circular shape, and for example, 100 to 1000 mm in length, preferably 200 to 700 mm in length of the short side in the case of a rectangular shape.
[0789] Furthermore, when the resin composition layer is formed on the surface of the resin layer or the surface of the metal layer, the resin layer or the metal layer serves as a substrate.
[0790] As a method of applying the resin composition to a substrate, coating is preferred.
[0791] Specifically, as the applicable method, dip coating, air knife coating, curtain coating, wire rod coating, gravure coating, extrusion coating, spray coating, spin coating, slit coating and inkjet can be exemplified. From the viewpoint of the uniformity of the thickness of the resin composition layer, spin coating, slit coating, spray coating, and inkjet are more preferred. By adjusting the appropriate solid content concentration or coating conditions according to the method, a resin layer of the desired thickness can be obtained. In addition, the coating method can also be appropriately selected according to the shape of the substrate. If it is a circular substrate such as a wafer, spin coating, spray coating, inkjet, etc. are preferred. If it is a rectangular substrate, slit coating, spray coating, inkjet, etc. are preferred. In the case of spin coating, for example, it can be applied at a rotation speed of 500 to 2,000 rpm for about 10 seconds to 1 minute.
[0792] Furthermore, it is also preferred to apply the photosensitive resin composition at a rotation speed of 300 to 3,500 rpm for 10 to 180 seconds depending on the viscosity of the photosensitive resin composition or the film thickness to be set. In order to obtain uniform film thickness, it is also possible to apply the composition at a combination of multiple rotation speeds.
[0793] Furthermore, a method of transferring a coating film formed on a temporary support body by the above-mentioned imparting method in advance to a substrate can also be applied.
[0794] Regarding the transfer method, the production method described in paragraphs 0023 and 0036 to 0051 of Japanese Patent Application Laid-Open No. 2006-023696 or paragraphs 0096 to 0108 of Japanese Patent Application Laid-Open No. 2006-047592 can also be preferably used in the present invention.
[0795] In addition, a process of removing excess film may be performed at the end of the substrate. Examples of such a process include edge bead residue rinsing (EBR), air knife, back rinse, and the like.
[0796] Furthermore, a pre-wetting step may be adopted in which various solvents are applied to the substrate before the resin composition is applied to the substrate to improve the wettability of the substrate, and then the resin composition is applied.
[0797] <Drying process>
[0798] The manufacturing method of the present invention may include a drying step for removing the solvent after the film forming step (layer forming step). The preferred drying temperature is 50 to 150° C., more preferably 70 to 130° C., and further preferably 90 to 110° C. The drying time may be 30 seconds to 20 minutes, preferably 1 to 10 minutes, and more preferably 3 to 7 minutes.
[0799] <Exposure process>
[0800] The manufacturing method of the present invention may include an exposure step of exposing the film (resin composition layer) to light. The exposure amount is not particularly limited as long as the resin composition can be cured. For example, it is preferably irradiated with 100 to 10,000 mJ / cm2 in terms of exposure energy at a wavelength of 365 nm. 2 , more preferably irradiation 200 to 8,000 mJ / cm 2 .
[0801] The exposure wavelength can be appropriately set within the range of 190 to 1,000 nm, and is preferably 240 to 550 nm.
[0802] Furthermore, the exposure light preferably includes light having a wavelength of 365 nm or a wavelength of 405 nm, and more preferably includes light having a wavelength of 405 nm.
[0803] When the exposure wavelength is explained in relation to the light source, examples include (1) semiconductor lasers (wavelengths of 830 nm, 532 nm, 488 nm, 405 nm, etc.), (2) metal halide lamps, (3) high-pressure mercury lamps, g-rays (wavelength 436 nm), h-rays (wavelength 405 nm), i-rays (wavelength 365 nm), broadband (three wavelengths of g, h, and i-rays), (4) excimer lasers, KrF excimer lasers (wavelength 248 nm), ArF excimer lasers (wavelength 193 nm), F2 excimer lasers (wavelength 157 nm), (5) extreme ultraviolet rays; EUV (wavelength 13.6 nm), (6) electron beams, (7) second harmonics of YAG lasers at 532 nm and tertiary harmonics at 355 nm, etc. For the resin composition of the present invention, exposure by a high-pressure mercury lamp is particularly preferred, and exposure by i-rays is particularly preferred. In this way, particularly high exposure sensitivity can be obtained.
[0804] Furthermore, from the viewpoint of handling and productivity, a high-pressure mercury lamp with a broad wavelength (three wavelengths of g, h, and i rays) or a semiconductor laser of 405 nm is also preferred.
[0805] The exposure method is not particularly limited as long as at least a portion of the film (photosensitive film) composed of the curable resin composition is exposed, and examples thereof include exposure using a photomask and exposure by laser direct imaging.
[0806] In the present invention, one of the preferred embodiments is that the exposure in the exposure step is performed by a laser direct imaging method.
[0807] <Development process>
[0808] The manufacturing method of the present invention may include a developing step of developing the exposed film (resin composition layer) (developing the above-mentioned film). The unexposed portion (non-exposed portion) is removed by developing. The developing method is not particularly limited as long as the desired pattern can be formed. For example, the developer can be sprayed from a nozzle, sprayed, immersed in the developer of the substrate, etc., and preferably, the developer can be sprayed from a nozzle. In the developing step, a step of continuously supplying the developer to the substrate, a step of keeping the developer on the substrate in a substantially stationary state, a step of vibrating the developer with ultrasound, etc., and a step of combining these can be adopted.
[0809] The development is performed using a developer. The developer can be used without particular limitation as long as it can remove the unexposed portion (non-exposed portion).
[0810] As the developer, a developer containing an organic solvent or an alkaline aqueous solution can be used.
[0811] In the present invention, the developer preferably contains an organic solvent having a ClogP value of -1 to 5, and more preferably contains an organic solvent having a ClogP value of 0 to 3. The ClogP value can be obtained as a calculated value by inputting the structural formula into ChemBioDraw.
[0812] When the developer is a developer containing an organic solvent, the organic solvent may be preferably esters such as ethyl acetate, n-butyl acetate, amyl formate, isoamyl acetate, isobutyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, γ-butyrolactone, ε-caprolactone, δ-valerolactone, alkyl alkoxyacetates (e.g., methyl alkoxyacetate, ethyl alkoxyacetate, butyl alkoxyacetate (e.g., methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate), , ethyl ethoxylate, etc.)), 3-alkoxy alkyl propionates (e.g., methyl 3-alkoxypropionate, ethyl 3-alkoxypropionate, etc. (e.g., methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, etc.)), 2-alkoxy alkyl propionates (e.g., methyl 2-alkoxypropionate, ethyl 2-alkoxypropionate, propyl 2-alkoxypropionate, etc. (e.g., methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate, ethyl 2-ethoxypropionate, etc.) ethyl ester)), methyl 2-alkoxy-2-methylpropionate and ethyl 2-alkoxy-2-methylpropionate (for example, methyl 2-methoxy-2-methylpropionate, ethyl 2-ethoxy-2-methylpropionate, etc.), methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutyrate, ethyl 2-oxobutyrate, and the like, and, as ethers, for example, diethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl celulose acetate, ethyl celulose acetate, diethylene glycol mono Methyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, etc., and, as ketones, for example, methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, 3-heptanone, N-methyl-2-pyrrolidone, etc. can be preferably mentioned, and, as cyclic hydrocarbons, for example, toluene, xylene, anisole, limonene, etc. can be preferably mentioned, as sulfoxides, for example, dimethyl sulfoxide can be preferably mentioned, and mixtures of these organic solvents can also be preferably mentioned.
[0813] When the developer contains an organic solvent, cyclopentanone and γ-butyrolactone are particularly preferred in the present invention, and cyclopentanone is more preferred. When the developer contains an organic solvent, the organic solvent may be used alone or in combination of two or more.
[0814] When the developer contains an organic solvent, the developer preferably contains 50% by mass or more of the organic solvent, more preferably 70% by mass or more of the organic solvent, and further preferably 90% by mass or more of the organic solvent. Furthermore, the developer may contain 100% by mass of the organic solvent.
[0815] The developer may further contain other components.
[0816] As other components, a well-known surfactant, a well-known defoaming agent, etc. are mentioned, for example.
[0817] When the developer is an alkaline aqueous solution, examples of alkaline compounds that can be contained in the alkaline aqueous solution include TMAH (tetramethylammonium hydroxide), KOH (potassium hydroxide), sodium carbonate, etc., preferably TMAH. For example, when TMAH is used, the content of the alkaline compound in the developer is preferably 0.01 to 10% by mass, more preferably 0.1 to 5% by mass, and further preferably 0.3 to 3% by mass in the total mass of the developer.
[0818] [Developer supply method]
[0819] The method of supplying the developer is not particularly limited as long as the desired pattern can be formed, and there are methods of immersing the substrate in the developer, immersion development using a nozzle to supply the developer to the substrate, or continuous supply of the developer. The type of nozzle is not particularly limited, and examples thereof include a straight nozzle, a shower nozzle, a spray nozzle, and the like.
[0820] From the viewpoints of the permeability of the developer, the removability of the non-image area, and the manufacturing efficiency, the method of supplying the developer using a straight nozzle or the method of continuously supplying the developer using a spray nozzle is preferred. From the viewpoint of the permeability of the developer to the image area, the method of supplying the developer using a spray nozzle is more preferred.
[0821] Furthermore, a process can be adopted in which the developer is continuously supplied through a straight nozzle, the developer is removed from the substrate by rotating the substrate, and after spin drying, the developer is continuously supplied again through a straight nozzle, and the developer is removed from the substrate by rotating the substrate, and this process can be repeated multiple times.
[0822] In addition, as a method for supplying the developer in the development process, a process of continuously supplying the developer to the substrate, a process of maintaining the developer in a substantially static state on the substrate, a process of vibrating the developer on the substrate using ultrasound, etc., and a combination of these processes can be adopted.
[0823] The development time is preferably 5 seconds to 10 minutes, more preferably 10 seconds to 5 minutes. The temperature of the developer during development is not particularly limited, but can be generally 10 to 45°C, preferably 20 to 40°C.
[0824] After the treatment with the developer, further rinsing may be performed. In addition, a method such as supplying a rinsing solution while the developer in contact with the pattern is not completely dried may be adopted. Preferably, rinsing is performed in a solvent different from the developer. For example, rinsing can be performed using a solvent contained in the resin composition.
[0825] When the developer contains an organic solvent, the rinse liquid includes PGMEA (propylene glycol monoethyl ether acetate) and IPA (isopropyl alcohol), and PGMEA is preferred. Water is preferred as a rinse liquid for development with a developer containing an alkaline aqueous solution.
[0826] The rinsing time is preferably 10 seconds to 10 minutes, more preferably 20 seconds to 5 minutes, and even more preferably 5 seconds to 1 minute.
[0827] The temperature of the rinsing liquid during rinsing is not particularly limited, but the rinsing can be performed preferably at 10 to 45°C, more preferably 18 to 30°C.
[0828] When the rinsing liquid contains an organic solvent, the organic solvent may be preferably esters such as ethyl acetate, n-butyl acetate, amyl formate, isoamyl acetate, isobutyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, γ-butyrolactone, ε-caprolactone, δ-valerolactone, alkyl alkoxyacetates (e.g., methyl alkoxyacetate, ethyl alkoxyacetate, butyl alkoxyacetate (e.g., methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, etc.)), alkyl 3-alkoxypropionates (e.g., 3-alkoxypropionic acid methyl ester, 3-alkoxypropionic acid ethyl ester, etc. (for example, 3-methoxypropionic acid methyl ester, 3-methoxypropionic acid ethyl ester, 3-ethoxypropionic acid methyl ester, 3-ethoxypropionic acid ethyl ester, etc.)), 2-alkoxy propionic acid alkyl esters (for example: 2-alkoxypropionic acid methyl ester, 2-alkoxypropionic acid ethyl ester, 2-alkoxypropionic acid propyl ester, etc. (for example, 2-methoxypropionic acid methyl ester, 2-methoxypropionic acid ethyl ester, 2-methoxypropionic acid propyl ester, 2-ethoxypropionic acid methyl ester, 2-ethoxypropionic acid ethyl ester)), 2-alkoxy-2-methylpropionic acid methyl ester and 2-alkoxy-2-methylpropionic acid ethyl ester (for example, 2-methoxy-2- The ethers include, for example, diethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl celulose acetate, ethyl celulose acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether (PGME), propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate Esters, etc., and, as ketones, for example, methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, 3-heptanone, N-methyl-2-pyrrolidone, etc., and, as aromatic hydrocarbons, for example, toluene, xylene, anisole, limonene, etc., can be preferably mentioned, as sulfoxides, for example, dimethyl sulfoxide can be preferably mentioned, and, as alcohols, for example, methanol, ethanol, propanol, isopropanol, butanol, pentanol, octanol, diethylene glycol, propylene glycol, methyl isobutyl carbitol, triethylene glycol, etc. can be mentioned, and as amides, N-methylpyrrolidone, N-ethylpyrrolidone, dimethylformamide, etc. can be mentioned.
[0829] When the rinse liquid contains an organic solvent, the organic solvent can be used alone or in combination of two or more. In the present invention, cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, N-methylpyrrolidone, cyclohexanone, PGMEA, and PGME are particularly preferred, cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, PGMEA, and PGME are more preferred, and cyclohexanone and PGMEA are further preferred.
[0830] When the rinse liquid contains an organic solvent, the organic solvent preferably accounts for 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. The organic solvent may also account for 100% by mass of the rinse liquid.
[0831] The rinsing solution may further comprise other ingredients.
[0832] As other components, a well-known surfactant, a well-known defoaming agent, etc. are mentioned, for example.
[0833] [Method of supplying flushing fluid]
[0834] There is no particular limitation on the method of supplying the rinsing liquid as long as the desired pattern can be formed. There are methods of immersing the substrate in the rinsing liquid, supplying the rinsing liquid on the substrate by covering the substrate, supplying the rinsing liquid to the substrate by a shower, and continuously supplying the rinsing liquid to the substrate by a mechanism such as a straight nozzle.
[0835] From the viewpoint of the permeability of the rinse liquid, the removal of the non-image part, and the efficiency in manufacturing, it is preferred to use a method of supplying the rinse liquid using a shower nozzle, a straight nozzle, a spray nozzle, etc., and a method of continuously supplying using a spray nozzle. From the viewpoint of the permeability of the rinse liquid to the image part, it is more preferred to use a spray nozzle to supply. The type of nozzle is not particularly limited, and examples thereof include a straight nozzle, a shower nozzle, a spray nozzle, etc.
[0836] That is, the rinsing step is preferably a step of supplying or continuously supplying the rinsing liquid to the exposed film using a straight nozzle, and more preferably a step of supplying the rinsing liquid using a spray nozzle.
[0837] Furthermore, as a method for supplying the developer in the rinsing step, a process of continuously supplying the rinsing liquid to the substrate, a process of maintaining the rinsing liquid in a substantially static state on the substrate, a process of vibrating the rinsing liquid on the substrate using ultrasound or the like, and a combination of these processes can be adopted.
[0838] <Heating process>
[0839] The production method of the present invention preferably includes a step of heating the developed film at 50 to 450° C. (heating step).
[0840] It is preferred that a heating step be included after the film forming step (layer forming step), the drying step, and the developing step. In the heating step, for example, a cyclization reaction of the precursor of the specific resin is carried out by generating a base by decomposing the above-mentioned thermal base generator. In addition, the resin composition of the present invention may contain a free radical polymerizable compound other than the precursor of the specific resin, and the curing of the unreacted free radical polymerizable compound other than the precursor of the specific resin can also be carried out in this step. The heating temperature (maximum heating temperature) of the layer in the heating step is preferably 50°C or more, more preferably 80°C or more, more preferably 140°C or more, more preferably 150°C or more, more preferably 160°C or more, and even more preferably 170°C or more. As an upper limit, it is preferably 500°C or less, more preferably 450°C or less, more preferably 350°C or less, more preferably 250°C or less, and even more preferably 220°C or less.
[0841] The heating is preferably carried out at a heating rate of 1 to 12°C / min from the temperature at the start of heating to the maximum heating temperature, more preferably 2 to 10°C / min, and further preferably 3 to 10°C / min. By setting the heating rate to be 1°C / min or more, productivity can be ensured while preventing excessive volatilization of amines, and by setting the heating rate to be 12°C / min or less, the residual stress of the cured film can be reduced. Moreover, in the case of an oven capable of rapid heating, the heating rate is preferably carried out at a heating rate of 1 to 8°C / sec from the temperature at the start of heating to the maximum heating temperature, more preferably 2 to 7°C / sec, and further preferably 3 to 6°C / sec.
[0842] The temperature at the start of heating is preferably 20°C to 150°C, more preferably 20°C to 130°C, and further preferably 25°C to 120°C. The temperature at the start of heating refers to the temperature at the start of the process of heating to the maximum heating temperature. For example, in the case where the resin composition is applied to a substrate and then dried, it refers to the temperature of the dried film (layer), and it is preferably gradually heated from a temperature 30 to 200°C lower than the boiling point of the solvent contained in the resin composition.
[0843] The heating time (heating time at the maximum heating temperature) is preferably 10 to 360 minutes, more preferably 20 to 300 minutes, and even more preferably 30 to 240 minutes.
[0844] In particular, when a multilayer laminate is formed, from the viewpoint of the adhesion between the layers of the cured film, the heating temperature is preferably 180° C. to 320° C., and more preferably 180° C. to 260° C. The reason for this is not clear, but it is believed that the acetylene groups of the specific resin between the layers undergo a cross-linking reaction by setting the temperature to this level.
[0845] Heating can be performed in stages. As an example, the following pretreatment process can be performed: heating from 25°C to 180°C at 3°C / min, maintaining at 180°C for 60 minutes, heating from 180°C to 200°C at 2°C / min, and maintaining at 200°C for 120 minutes. The heating temperature of the pretreatment process is preferably 100-200°C, more preferably 110-190°C, and further preferably 120-185°C. In this pretreatment process, it is also preferred to treat while irradiating ultraviolet rays as described in the specification of U.S. Patent No. 9159547. By this pretreatment process, the properties of the film can be improved. The pretreatment process can be performed in a short time of about 10 seconds to 2 hours, more preferably 15 seconds to 30 minutes. The pretreatment can also be set as a step of more than two stages, for example, pretreatment process 1 can be performed in the range of 100-150°C, and then pretreatment process 2 can be performed in the range of 150-200°C.
[0846] The heating may be followed by cooling, and the cooling rate at this time is preferably 1 to 5° C. / min.
[0847] From the viewpoint of preventing decomposition of the specific resin, the heating step is preferably performed in an atmosphere of low oxygen concentration by flowing an inert gas such as nitrogen, helium, or argon. The oxygen concentration is preferably 50 ppm (volume ratio) or less, more preferably 20 ppm (volume ratio) or less.
[0848] The heating means is not particularly limited, and examples thereof include a hot plate, an infrared oven, an electric heating oven, and a hot air oven.
[0849] <Metal layer forming step>
[0850] The production method of the present invention preferably includes a metal layer forming step of forming a metal layer on the surface of the developed film (resin composition layer).
[0851] The metal layer is not particularly limited, and any conventional metal can be used. Examples thereof include copper, aluminum, nickel, vanadium, titanium, chromium, cobalt, gold, and tungsten. Copper, aluminum, and alloys containing these metals are more preferred, and copper is further preferred.
[0852] The formation method of the metal layer is not particularly limited, and existing methods can be used. For example, the method described in Japanese Patent Publication No. 2007-157879, Japanese Patent Table No. 2001-521288, Japanese Patent Publication No. 2004-214501, and Japanese Patent Publication No. 2004-101850 can be used. For example, photolithography, peeling (lift off), electrolytic plating, electroless plating, etching, printing and the method of combining these can be considered. More specifically, a patterning method combining sputtering, photolithography and etching, and a patterning method combining photolithography and electrolytic plating can be cited.
[0853] The thickness of the metal layer is preferably 0.01 to 100 μm, more preferably 0.1 to 50 μm, and even more preferably 1 to 10 μm at the thickest portion.
[0854] <Lamination process>
[0855] The production method of the present invention preferably further includes a lamination step.
[0856] The lamination process refers to a series of processes including performing (a) film formation process (layer formation process), (b) exposure process, (c) development process, and (d) heating process in sequence again on the surface of the cured film (resin layer) or the metal layer. However, it is also possible to repeat only the film formation process (a). In addition, it is also possible to perform the (d) heating process at the end or in the middle of the lamination. That is, it is possible to perform the processes (a) to (c) repeatedly for a specified number of times, and then perform (d) heating, thereby curing the laminated resin composition layer in a lump. In addition, the (e) metal layer formation process may be included after the (c) development process, and in this case, the heating (d) may be performed each time, or the heating (d) may be performed in a lump after the specified number of laminations. Of course, the above-mentioned drying process or heating process may be further appropriately included in the lamination process.
[0857] When the lamination step is further performed after the lamination step, a surface activation treatment step may be further performed after the heating step, after the exposure step, or after the metal layer forming step. As the surface activation treatment, plasma treatment can be exemplified.
[0858] The lamination step is preferably performed 2 to 20 times, more preferably 2 to 5 times, and more preferably 3 to 5 times.
[0859] Furthermore, each layer in the lamination step may be the same in composition, shape, film thickness, etc., or may be different in composition, shape, film thickness, etc.
[0860] For example, a structure in which the resin layers have more than 2 layers and less than 20 layers, such as resin layer / metal layer / resin layer / metal layer / resin layer / metal layer, is preferred, a structure in which the resin layers have more than 3 layers and less than 7 layers is more preferred, and a structure in which the resin layers have more than 3 layers and less than 5 layers is further preferred.
[0861] In the present invention, it is particularly preferred that after the metal layer is provided, a cured film (resin layer) of the above-mentioned resin composition is further formed in a manner covering the above-mentioned metal layer. Specifically, a method of repeatedly performing the order of (a) film forming step, (b) exposure step, (c) developing step, (e) metal layer forming step, and (d) heating step can be cited, or a method of repeatedly performing the order of (a) film forming step, (b) exposure step, (c) developing step, and (e) metal layer forming step and arranging (d) heating step at the end or in the middle can be cited. By alternately performing the lamination step and the metal layer forming step of the laminated resin composition layer (resin layer), the resin composition layer (resin layer) and the metal layer can be alternately laminated.
[0862] (Surface activation treatment process)
[0863] The method for producing a laminate of the present invention may include a surface activation treatment step of performing surface activation treatment on at least a portion of the metal layer and the photosensitive resin composition layer.
[0864] The surface activation treatment step is usually performed after the metal layer forming step. However, the metal layer forming step may be performed after the above-mentioned exposure and development steps and then after the photosensitive resin composition layer is subjected to the surface activation treatment step.
[0865] The surface activation treatment may be performed only on at least a portion of the metal layer, or only on at least a portion of the photosensitive resin composition layer after exposure, or may be performed on at least a portion of both the metal layer and the photosensitive resin composition layer after exposure. Preferably, at least a portion of the metal layer is subjected to the surface activation treatment, and preferably, a portion or all of the region of the metal layer where the photosensitive resin composition layer is formed on the surface is subjected to the surface activation treatment. In this way, by performing the surface activation treatment on the surface of the metal layer, the adhesion with the resin layer provided on the surface can be improved.
[0866] Furthermore, it is preferred that a part or all of the exposed photosensitive resin composition layer (resin layer) is also subjected to a surface activation treatment. Thus, by subjecting the surface of the photosensitive resin composition layer to a surface activation treatment, adhesion to a metal layer or a resin layer disposed on the surface subjected to the surface activation treatment can be improved.
[0867] As the surface activation treatment, specifically, plasma treatment selected from various raw material gases (oxygen, hydrogen, argon, nitrogen, nitrogen / hydrogen mixed gas, argon / oxygen mixed gas, etc.), corona discharge treatment, etching treatment based on CF4 / O2, NF3 / O2, SF6, NF3, NF3 / O2, surface treatment based on ultraviolet (UV) ozone method, immersion in hydrochloric acid aqueous solution to remove oxide film and then immersion in an organic surface treatment agent containing a compound having at least one of an amino group and a thiol group, mechanical roughening treatment using a brush, preferably plasma treatment, especially preferably oxygen plasma treatment using oxygen in the raw material gas. In the case of corona discharge treatment, the energy is preferably 500 to 200,000 J / m 2 , more preferably 1000 to 100,000 J / m 2 , most preferably 10,000 to 50,000 J / m 2 .
[0868] The present invention also discloses a semiconductor device including the cured film or laminate of the present invention. As a specific example of a semiconductor device in which the resin composition of the present invention is used to form an interlayer insulating film for a redistribution layer, reference can be made to the description of paragraphs 0213 to 0218 of Japanese Patent Publication No. 2016-027357 and the description of FIG. 1, which are incorporated into this specification.
[0869] Example
[0870] Below, give examples to further specifically describe the present invention. The materials, usage, ratio, processing content, processing sequence, etc. shown in the following examples can be appropriately changed without departing from the purpose of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. As long as there is no special description, "part", "%" is a mass reference.
[0871] <Synthesis Example 1: Synthesis of polymer A-1>
[0872] 23.48 g of 4,4'-oxydiphthalic anhydride (ODPA) and 22.27 g of 4,4'-biphenyltetracarboxylic anhydride (BPDA) were placed in a separable flask, and 39.69 g of 2-hydroxyethyl methacrylate (HEMA) and 136.83 g of γ-butyrolactone were added, and stirred at room temperature, and 24.66 g of pyridine was added while stirring to obtain a reaction mixture. After the heat generated by the reaction ended, the mixture was naturally cooled to room temperature and left at room temperature for 16 hours.
[0873] Next, a solution of 62.46 g of dicyclohexylcarbodiimide (DCC) dissolved in 61.57 g of γ-butyrolactone was added to the reaction mixture over 40 minutes while stirring under ice cooling, and then a mixture of 27.42 g of 4,4'-diaminodiphenyl ether (DADPE) suspended in 119.73 g of γ-butyrolactone was added over 60 minutes while stirring. In addition, after stirring at room temperature for a certain period of time, 7.17 g of ethanol was added and stirred for 1 hour, and then 136.83 g of γ-butyrolactone was added. The precipitate generated in the reaction mixture was removed by filtration to obtain a reaction solution.
[0874] By extending the above-mentioned certain time, the total molar content of the cyclic imide structure and the cyclic isoimide structure in the polyimide precursor can be increased, and by shortening the above-mentioned certain time, the above-mentioned total molar content can be reduced. For example, by setting the above-mentioned time to 30 minutes, a resin having a total molar content of 0.083 mmol / g of the above-mentioned cyclic imide structure and the above-mentioned cyclic isoimide structure contained in 1 g of the above-mentioned polyimide precursor is obtained.
[0875] In the present embodiment and comparative example, the above-mentioned certain time was appropriately adjusted, and the polyimide precursor with a changed total molar content of the cyclic imide structure and the cyclic isoimide structure in the polyimide precursor was used for the experiment. In each embodiment and comparative example, the total molar content of the cyclic imide structure and the cyclic isoimide structure is recorded in the column of "Specific structure mmol / g" in the table.
[0876] The obtained reaction solution was added to 716.21 g of ethanol to generate a precipitate consisting of a crude polymer. The generated crude polymer was filtered out and dissolved in 403.49 g of tetrahydrofuran to obtain a crude polymer solution. The obtained crude polymer solution was added dropwise to 8470.26 g of water to precipitate the polymer, and the obtained precipitate was filtered out and then vacuum dried to obtain a powdered polymer (polyimide precursor) A-1. The molecular weight of polymer A-1 was measured by gel permeation chromatography (standard polystyrene conversion), and the result was that the weight average molecular weight (Mw) was 20,000.
[0877] <Synthesis Example 2: Synthesis of polymer A-2>
[0878] Polymer A-2 was synthesized by the same method as in Synthesis Example 1 except that ODPA 23.48 g and BPDA 22.27 g were changed to ODPA 46.96 g. In the Examples, the column "Specific structure mmol / g" in the table describes the total molar content of the cyclic imide structure and the cyclic isoimide structure.
[0879] <Synthesis Example 3: Synthesis of polymer A-3>
[0880] Polymer A-3 was synthesized by the same method as in Synthesis Example 1 except that ODPA 23.48 g and BPDA 22.27 g were changed to ODPA 46.96 g, and HEMA 39.69 g were changed to HEMA 19.85 g and diethylene glycol monomethyl ether 18.32 g. In the Examples, the column "Specific structure mmol / g" in the table describes the total molar content of the cyclic imide structure and the cyclic isoimide structure.
[0881] <Synthesis Example 4: Synthesis of polymer A-4>
[0882] In a dry reactor equipped with a stirrer, a condenser, and a flat-bottomed joint equipped with an internal thermometer, 10.65 g (50 mmol) of 4,6-dihydroxy-1,3-phenylenediamine dihydrochloride was dissolved in 85.8 g of N-methylpyrrolidone (NMP) while removing water. Then, 9.74 g (48 mmol) of terephthalic acid chloride was dissolved in 55.0 g of NMP, dropped over 1 hour, and stirred at 25° C. for a certain period of time.
[0883] By extending the above-mentioned certain time, the molar content of the benzoxazole structure in the polybenzoxazole precursor can be increased, and by shortening the above-mentioned certain time, the molar content of the benzoxazole structure in the polybenzoxazole precursor can be reduced. For example, by setting the time to 15 minutes, the molar content of the benzoxazole structure can be set to 0.373 mmol / g.
[0884] After stirring, the mixture was precipitated in 2 liters of water / methanol = 75 / 25 (volume ratio) and stirred at 2,000 rpm for 30 minutes. The precipitated polybenzoxazole precursor resin was filtered and removed, and rinsed in 1.5 liters of water. The obtained resin was dried at 40° C. under reduced pressure for 1 day to obtain A-4.
[0885] <Synthesis Example 5: Synthesis of Polymer A-5>
[0886] 29.08 g of trimellitic anhydride was added to a separable flask, 19.85 g of 2-hydroxyethyl methacrylate (HEMA) and 136.83 g of γ-butyrolactone were added, and stirred at room temperature, and 24.66 g of pyridine was added while stirring to obtain a reaction mixture. After the heat generated by the reaction ended, the mixture was naturally cooled to room temperature and left at room temperature for 16 hours.
[0887] Next, a solution of 62.46 g of dicyclohexylcarbodiimide (DCC) dissolved in 61.57 g of γ-butyrolactone was added to the reaction mixture over 40 minutes while stirring under ice cooling, and then a mixture of 27.42 g of 4,4'-diaminodiphenyl ether (DADPE) suspended in 119.73 g of γ-butyrolactone was added over 60 minutes while stirring. In addition, after stirring at room temperature for a certain period of time, 7.17 g of ethanol was added and stirred for 1 hour, and then 136.83 g of γ-butyrolactone was added. The precipitate generated in the reaction mixture was removed by filtration to obtain a reaction solution.
[0888] By extending the above-mentioned certain time, the total molar content of the cyclic imide structure and the cyclic isoimide structure in the polyamide-imide precursor can be increased, and by shortening the above-mentioned certain time, the above-mentioned total molar content can be reduced. For example, by setting it to 15 minutes, the molar content of the benzoxazole structure can be set to 0.104 mmol / g.
[0889] The obtained reaction solution was added to 716.21 g of ethanol to generate a precipitate consisting of a crude polymer. The generated crude polymer was filtered out and dissolved in 403.49 g of tetrahydrofuran to obtain a crude polymer solution. The obtained crude polymer solution was added dropwise to 8470.26 g of water to precipitate the polymer, and the obtained precipitate was filtered out and vacuum dried to obtain a powdered polymer (polyamide-imide precursor) A-5.
[0890] <Synthesis Example 6: Synthesis of Polymer A-6>
[0891] Polymer A-6 was synthesized by the same method as in Synthesis Example 1 except that 23.48 g of ODPA and 22.27 g of BPDA were changed to 44.54 g of BPDA. In the Examples, the column "Specific structure mmol / g" in the table indicates the total molar content of the cyclic imide structure and the cyclic isoimide structure.
[0892] <Synthesis Example 7: Synthesis of Polymer A-7>
[0893] Polymer A-7 was synthesized by the same method as in Synthesis Example 1, except that 23.48 g of ODPA and 22.27 g of BPDA were changed to 46.96 g of ODPA, and 39.69 g of HEMA was changed to 52.52 g of the compound represented by the following formula (7-1). In the examples, the column "Specific structure mmol / g" in the table records the total molar content of the cyclic imide structure and the above-mentioned cyclic isoimide structure.
[0894] [Chemical formula 59]
[0895]
[0896] <Examples and Comparative Examples>
[0897] In each example, the components described in the following table were mixed to obtain each curable resin composition. In addition, in each comparative example, the components described in the following table were mixed to obtain each comparative composition.
[0898] Specifically, the content of each component described in Tables 1 to 5 is the amount (parts by mass) described in the parentheses in each column of Tables 1 to 5.
[0899] The obtained curable resin composition and comparative composition were filtered under pressure using a polytetrafluoroethylene filter having a pore width of 0.8 μm.
[0900] In Tables 1 to 5, "-" indicates that the composition does not contain the component.
[0901] [Table 1]
[0902]
[0903] [Table 2]
[0904]
[0905] [Table 3]
[0906]
[0907] [Table 4]
[0908]
[0909] [Table 5]
[0910]
[0911] The details of each component described in Tables 1 to 5 are as follows.
[0912] 〔Resin〕
[0913] ·A-1 to A-7: Polymers A-1 to A-7 obtained in the above-mentioned synthesis examples
[0914] [Photosensitive agent (photoradical polymerization initiator)]
[0915] ·B-1 to B-3: Compounds of the following structures
[0916] [Chemical formula 60]
[0917]
[0918] 〔Organometallic complex〕
[0919] ·X-1: Bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium
[0920] ·X-2: Pentamethylcyclopentadienyl titanium trimethoxide
[0921] ·X-3: Bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluorophenyl)titanium
[0922] ·X-4: Tetraisopropoxytitanium (manufactured by Matsumoto Fine Chemical Co. Ltd.)
[0923] ·X-5: Diisopropoxybis(acetylacetonate)titanium (manufactured by Matsumoto Fine Chemical Co. Ltd.)
[0924] X-6 to X-8: compounds having the following structures.
[0925] [Chemical formula 61]
[0926]
[0927] The above-mentioned X-1 and X-3 are compounds having the ability to initiate photoradical polymerization.
[0928] 〔Crosslinking agent (free radical crosslinking agent)〕
[0929] ·C-1~C-2: Compounds of the following structures
[0930] [Chemical formula 62]
[0931]
[0932] 〔Polymerization inhibitors, migration inhibitors〕
[0933] ·D-1 to D-7: Compounds of the following structures
[0934] [Chemical formula 63]
[0935]
[0936] 〔additive〕
[0937] ·E-1 to E-6: Compounds of the following structures
[0938] [Chemical formula 64]
[0939]
[0940] <Metal Adhesion Improver>
[0941] ·F-1 to F-6: Compounds of the following structures
[0942] [Chemical formula 65]
[0943]
[0944] In the above structural formula, Me represents a methyl group, and Et represents an ethyl group.
[0945] 〔Solvent (solvent)〕
[0946] ·NMP: N-methyl-2-pyrrolidone
[0947] EL: Ethyl lactate
[0948] DMSO: dimethyl sulfoxide
[0949] <Evaluation>
[0950] [Determination of molar content of ring structure]
[0951] For the resin used in each example, the total molar content of the cyclic imide structure and the cyclic isoimide structure contained in 1 g of the polyimide precursor, the molar content of the benzoxazole structure contained in 1 g of the polybenzoxazole precursor, and the total molar content of the cyclic imide structure and the cyclic isoimide structure contained in 1 g of the polyamide-imide precursor were measured. The measurement results are recorded in the column "Specific structure mmol / g" in the table.
[0952] Specifically, NMR was used to measure the polymer by dissolving 0.1 g in 0.9 g of heavy DMSO. The cyclic imide structure content of the polyimide precursor or polyamideimide precursor was determined from the ratio of the peak area around 7.15 ppm to the peak area of the aromatic ring.
[0953] Likewise, the amounts of the cyclic isoimide structure in the polyimide precursor or the polyamideimide precursor and the benzoxazole structure in the polybenzoxazole precursor were determined.
[0954] 〔Resolution evaluation〕
[0955] In each example or comparative example, the prepared curable resin composition or comparative composition was applied on a silicon wafer by spin coating, and the silicon wafer was dried on a hot plate at 100° C. for 5 minutes to form a curable resin composition layer with a uniform thickness of 20 μm on the silicon wafer.
[0956] In the example described as "M" in the exposure conditions, the curable resin composition layer on the silicon wafer was exposed using a stepper. The exposure was performed using light of the wavelength described in "Exposure wavelength nm" in the table, and using a mask of a fuse box with a scale of 1 μm from 5 μm to 25 μm. The exposure amount was set to the exposure amount that minimizes the minimum line width described later.
[0957] In the example described as "D" in the exposure condition, exposure was performed using a direct exposure device (AdTech DE-6UH III). Regarding exposure, laser direct imaging exposure was performed at a wavelength of 405 nm so that the exposed portion became a line portion in a line and space pattern with a scale of 1 μm from 5 μm to 25 μm. The exposure amount was set to the exposure amount that minimized the minimum line width described later.
[0958] The exposed curable resin composition layer was developed with cyclopentanone for 60 seconds, and then rinsed with PGMEA (propylene glycol monomethyl ether acetate).
[0959] In the pattern obtained after development, the line width with the smallest line width among the line patterns that exposed the silicon wafer between the line patterns was taken as the "minimum line width" and evaluated according to the following evaluation criteria. It can be said that the smaller the line width, the better the resolution. For example, it means that the width of the metal wiring formed in the subsequent plating process can be miniaturized, so it is a preferred result. The measurement limit is 5μm. The evaluation results are recorded in the "resolution" column in the table.
[0960] -Evaluation Criteria-
[0961] A: The minimum line width is 5 μm or more and less than 8 μm.
[0962] B: The minimum line width is 8 μm or more and less than 10 μm.
[0963] C: The minimum line width is 10 μm or more and less than 12 μm.
[0964] D: The minimum line width is 12 μm or more.
[0965] [Exposure sensitivity evaluation]
[0966] By the same method as the above-mentioned resolution evaluation, a curable resin composition layer having a uniform thickness of 20 μm was formed on the silicon wafer.
[0967] In the example where the exposure conditions are recorded as "M", the curable resin composition layer on the silicon wafer was exposed by a stepper using a mask having a mask portion (an example where the developing conditions in the table are recorded as "negative") or a non-mask portion (an example where the developing conditions in the table are recorded as "positive") with a diameter of 15.0 μm. The exposure wavelength is recorded as "exposure wavelength nm" in the table. The exposure amount is 50 to 500 mJ / cm2 In the range of 50mJ / cm 2 Scale changes.
[0968] In the example described as "D" in the exposure condition, laser direct imaging exposure was performed using a direct exposure device (AdTech DE-6UH III). The exposure wavelength was set to 405 nm, and the exposure was performed in such a way that a non-exposed portion with a diameter of 15.0 μm was formed. The exposure amount was 50 to 500 mJ / cm 2 In the range of 50mJ / cm 2 Scale changes.
[0969] The sensitivity was evaluated according to the following evaluation criteria based on the minimum exposure amount for forming a hole pattern with a bottom diameter of 15.0 μm. The smaller the minimum exposure amount (the higher the sensitivity), the more preferred it is, and it can be said that the exposure sensitivity is excellent. The evaluation results are recorded in the "Sensitivity" column in the table.
[0970] -Evaluation Criteria-
[0971] A: The above minimum exposure is less than 100mJ / cm 2 .
[0972] B: The minimum exposure is 100mJ / cm 2 Above and less than 150mJ / cm 2 .
[0973] C: The minimum exposure is 150mJ / cm 2 above.
[0974] From the above results, it is understood that the curable resin composition of the present invention is excellent in resolution.
[0975] Regarding the polyimide precursors contained in the comparative compositions of Comparative Examples 1 to 4, the total molar content of the cyclic imide structure and the cyclic isoimide structure contained in 1 g of the polyimide precursor was less than 0.08 mmol / g.
[0976] Regarding the polyimide precursor contained in the comparative composition of Comparative Example 5, the total molar content of the cyclic imide structure and the cyclic isoimide structure contained in 1 g of the polyimide precursor exceeded 1.68 mmol / g.
[0977] Regarding the polybenzoxazole precursor included in the comparative composition of Comparative Example 6, the molar amount of the benzoxazole structure included in 1 g of the polybenzoxazole precursor was less than 0.22 mmol / g.
[0978] Regarding the polybenzoxazole precursor included in the comparative composition of Comparative Example 7, the molar amount of the benzoxazole structure included in 1 g of the polybenzoxazole precursor exceeded 3.97 mmol / g.
[0979] Regarding the polyamide-imide precursor contained in the comparative composition of Comparative Example 8, the total molar content of the cyclic imide structure and the cyclic isoimide structure contained in 1 g of the polyimide precursor exceeded 1.186 mmol / g.
[0980] Regarding the polyamide-imide precursor contained in the comparative composition of Comparative Example 9, the total molar content of the cyclic imide structure and the cyclic isoimide structure contained in 1 g of the polyamide-imide precursor was less than 0.062 mmol / g.
[0981] When these comparative compositions were used, the resolution was poor.
[0982] <Example 101>
[0983] By spin coating, the curable resin composition used in Example 1 was applied in layers to the surface of the copper thin layer of the resin substrate having a copper thin layer formed on the surface, and after drying at 100°C for 4 minutes to form a photosensitive film with a film thickness of 20 μm, it was exposed using a stepper (Nikon Co., Ltd., NSR1505 i6). Exposure was performed at a wavelength of 365nm via a mask (a binary mask with a pattern of 1:1 line and space and a line width of 10 μm). After exposure, it was heated at 100°C for 4 minutes. After the above heating, it was developed with cyclohexanone for 2 minutes and rinsed with PGMEA for 30 seconds to obtain a pattern of the layer.
[0984] Next, the temperature was raised at a rate of 10° C. / min in a nitrogen atmosphere to 230° C. and then maintained at 230° C. for 120 minutes to form a redistribution layer interlayer insulating film having excellent insulation properties.
[0985] Furthermore, semiconductor devices were manufactured using these interlayer insulating films for redistribution layers, and it was confirmed that they could operate normally.
Claims
1. A curable resin composition comprising: at least one resin selected from a polyimide precursor including at least one of a cyclic imide structure and a cyclic isoimide structure, a polybenzoxazole precursor including a benzoxazole structure, and a polyamideimide precursor including at least one of a cyclic imide structure and a cyclic isoimide structure; and Organometallic complexes, The total molar content of the cyclic imide structure and the cyclic isoimide structure contained in 1 g of the polyimide precursor is 0.285 mmol / g to 1.00 mmol / g, The molar amount of the benzoxazole structure contained in 1 g of the polybenzoxazole precursor is 0.22 mmol / g to 3.97 mmol / g, The total molar content of the cyclic imide structure and the cyclic isoimide structure contained in 1 g of the polyamide-imide precursor is 0.062 mmol / g to 1.186 mmol / g, The determination method of the molar amount is as follows: Using NMR, 0.1 g of the polyimide precursor, the polybenzoxazole precursor or the polyamide-imide precursor is dissolved in 0.9 g of heavy DMSO, and the molar content of the cyclic imide structure in the polyimide precursor, the molar content of the cyclic isoimide structure, the molar content of the benzoxazole structure in the polybenzoxazole precursor, the molar content of the cyclic imide structure in the polyamide-imide precursor, and the molar content of the cyclic isoimide structure are determined based on the ratio of the peak area near 7.15 ppm and the peak area of the aromatic ring. 2 . The curable resin composition according to claim 1 , further comprising a photopolymerization initiator.
3. The curable resin composition according to claim 2, wherein The photopolymerization initiator is an oxime compound. The curable resin composition according to claim 1 or 2, further comprising a crosslinking agent.
5. The curable resin composition according to claim 1 or 2, wherein The organic metal complex is a metallocene compound.
6. The curable resin composition according to claim 1 or 2, wherein The metal contained in the organic metal complex is at least one metal selected from titanium, zirconium and hafnium.
7. The curable resin composition according to claim 1 or 2, wherein The organic metal complex has the ability to initiate photo-radical polymerization.
8. The curable resin composition according to claim 1 or 2, which is used for forming a photosensitive film for negative tone development. 9 . The curable resin composition according to claim 1 , which is used for forming an interlayer insulating film for a redistribution layer. 10 . The curable resin composition according to claim 1 , wherein a total molar content of the cyclic imide structure and the cyclic isoimide structure contained in 1 g of the polyimide precursor is 0.285 mmol / g to 0.593 mmol / g. 11 . A cured film obtained by curing the curable resin composition according to claim 1 . 12 . A laminate comprising two or more layers of the cured film according to claim 11 , comprising a metal layer between any of the cured films.
13. A method for producing a cured film, comprising: The film forming step is to apply the curable resin composition according to any one of claims 1 to 10 to a substrate to form a film.
14. The method for producing a cured film according to claim 13, comprising: An exposure step of exposing the film to light; as well as In the developing step, the film is developed.
15. The method for producing a cured film according to claim 14, wherein: The exposure light used in the exposure includes light with a wavelength of 405 nm.
16. The method for producing a cured film according to claim 14, wherein: The exposure is exposure based on a laser direct imaging method.
17. The method for producing a cured film according to claim 13, comprising: In the heating step, the film is heated at 50°C to 450°C. 18 . A semiconductor device comprising the cured film according to claim 11 .