A catalyst composition for alpha-olefin polymerization and its preparation and application
By using boron trifluoride and proton-type cocatalyst compositions in the catalytic system, the acidity of the catalytic system is adjusted, and the problem of uncontrollable isomerization of the base oil of low-viscosity PAO synthetic oil is solved, and the viscosity index and low-temperature performance of the product are improved. Highly selective oligomer preparation is achieved.
Patent Information
- Application Number
- CN202110405183.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-04-15
AI Technical Summary
When preparing low-viscosity PAO synthetic oil base oil, the degree of isomerization is uncontrollable, the product performance stability is poor, and the target product selectivity is low.
Boron trifluoride and proton-type cocatalyst compositions are used as catalysts to adjust the acidity of the catalytic system through heteroatom-induced effects, control the degree of product isomerization, and improve the selectivity of the target product.
The narrow molecular weight oligomerization of low viscosity PAO products is achieved, the viscosity index and low temperature performance are improved, and the selectivity and stability of the target product are improved.
Smart Images

Figure CN115212922B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of poly-alpha-olefin synthetic oil base oil, and in particular to a catalyst composition for alpha-olefin polymerization and the preparation and application thereof. Background Art
[0002] Poly-alpha-olefin (PAO) synthetic oil is the best performing synthetic lubricant base oil currently available, with high viscosity index, low volatility, low fluidity, good shear performance and excellent resistance to high-temperature oxidation. Compared with traditional mineral lubricant base oils (Group I, II and III base oils), PAO has the characteristics of low evaporation loss, good stability, wide operating temperature range, good compatibility with common materials and non-toxicity. It is not only widely used in civil industries such as automobiles and industry, but is also the main source of high-end lubricant base oils used in aviation, aerospace, military and other industries.
[0003] PAO is generally composed of C6-C 20 A type of branched saturated oligomer synthesized by the catalytic polymerization of α-olefins. The catalytic polymerization of α-olefins is a known technology for preparing PAO synthetic lubricants. Generally speaking, the catalyst systems commonly used for preparing PAO include BF3 system, Cr system, Al compound system, Ziegler-Natta, metallocene and ionic liquids. The selection of different types of catalysts has a significant impact on the yield of the polymer, the control of the degree of polymerization and the performance of the product. The PAO synthetic oil prepared by Lewis acid catalysts has a high yield and a narrow molecular weight distribution. Therefore, the selection of BF3 and initiator as the catalytic system for preparing low-viscosity polyα-olefin synthetic oil base oil has a better effect.
[0004] When low-viscosity PAO is produced using a BF3 catalytic system, the products are mainly trimers, tetramers, and pentamers, with a narrow product distribution, and are ideal components with a viscosity range of 4 to 6 cSt. At the same time, according to the results of PAO structure and performance research, straight-chain alkanes have a high viscosity index, but poor low-temperature performance. Only alkanes with a certain degree of isomerization, that is, reasonable isomerization, are ideal components of lubricating oils. Therefore, by selecting a suitable cationic catalytic system, a certain degree of isomerization occurs in the presence of catalytic active centers, and PAO base oils with excellent comprehensive performance can be obtained.
[0005] US3763244 discloses the use of BF3 / water system to catalyze C6~C 16A method for preparing lubricating oil base oil from α-olefins, under the condition of reaction temperature of 10-60℃, using water as initiator, wherein the molar ratio of water to trifluoroboron is excessive, and the product under the action of the catalyst system has a low pour point and a high viscosity index. US5191140A uses boron trifluoride as the main catalyst, water or alcohols and acetic anhydride as co-catalysts, and obtains a product with a kinematic viscosity of 3.58cSt at 100℃ and a viscosity index of 125 through the polymerization reaction of olefins, and the olefin conversion rate is 76.8%. This method can increase the yield of low-viscosity olefin oligomers and improve production efficiency by shortening the reaction time. US3742082A discloses a method for catalyzing α-olefins using BF3 as the main catalyst and phosphoric acid or water as co-catalysts, the molar ratio of catalyst to olefin is 0.005:1~0.1:1, the reaction temperature is 100~150℃, and the obtained base oil product has a lower pour point. The above patent uses water as a co-catalyst, and the product performance and catalytic efficiency are both good, and the production cost is reduced. However, it is particularly prone to corrosion problems, which requires improving the corrosion resistance level of the material, which will greatly increase the investment cost of the equipment. Therefore, this type of method is not suitable for large-scale production.
[0006] In the subsequent development of catalyst technology, there are also some reports based on BF3 as the main catalyst and alcohols, ethers, esters and ketones as co-catalysts, but most of the literature uses alcohols as co-catalysts. CN1274725C provides a polyalphaolefin base oil with a kinematic viscosity of 4 to 6 cSt at 100°C, a Noack weight loss of 4 to 9%, a viscosity index of 130 to 145, and a pour point of -60°C to -50°C. The yield of the target product component is only 70% after composition analysis. CN101883838A uses C8 to C 12 α-olefins are used as raw materials, and are polymerized with boron trifluoride-butanol catalyst. Unreacted raw materials and dimers are then separated, and the vacuum fraction is hydrogenated and refined as base oil. The product has a kinematic viscosity of 5mm at 100°C. 2 / s, the pour point is lower than -50℃, and the viscosity at -40℃ is lower than 3000cSt. CN105925340A uses BF3 as a catalyst, alcohols or alkyl esters as co-catalysts, decene-1 and dodecene-1 as raw materials, the ratio of decene-1 to dodecene-1 is 7:3, the reaction is carried out at 18℃, 0.2MPa, the co-initiator is ethanol: ethyl acetate in a ratio of 12:1, and the kinematic viscosity of the polymerization product at 100℃ is 4mm 2 / s, the pour point is less than -60°C, but the product yield is less than 80%. CN101054332A uses boron trifluoride as a catalyst and alcohol as an initiator, wherein the alcohol is methanol, ethanol, propanol, butanol or amyl alcohol, wherein the weight ratio of the initiator to the raw material olefin is 0.01-1.0%, and the weight ratio of BF3 to the raw material olefin is 1-5%.
[0007] The traditional catalytic system used to produce low-viscosity PAO has relatively good viscosity-temperature performance and low-temperature performance. However, after the Lewis acid catalyst and the co-catalysts such as alcohol, ester, and ether act in the polymerization reaction, the isomerization degree of the oligomer product is uncontrollable, the performance of the product is greatly affected by the process conditions, the product stability is poor, and the selectivity of the ideal component in the viscosity range of 4 to 6 cSt is low. Therefore, in order to solve the above problems, it is necessary to develop new co-catalysts in the hope of improving the selectivity of the target products (trimers and tetramers). Summary of the invention
[0008] Aiming at the deficiencies in the existing catalytic system, the present invention proposes a novel proton-type co-catalyst for the boron trifluoride catalytic system, develops a catalyst composition for α-olefin polymerization, realizes directional polymerization of α-olefin, and has high selectivity for the target product.
[0009] The first object of the present invention is to provide a catalyst composition for the polymerization of α-olefins.
[0010] The second object of the present invention is to provide a method for preparing the catalyst composition for α-olefin polymerization.
[0011] The third object of the present invention is to provide an application of the catalyst composition for α-olefin polymerization.
[0012] In order to achieve the above purpose, the present invention adopts the following technical solutions:
[0013] The first aspect of the present invention provides a catalyst composition for the polymerization of α-olefins, the catalyst composition comprising boron trifluoride and at least one proton-type co-catalyst;
[0014] The general structural formula of the proton type co-catalyst is:
[0015] X-(CH2) n -OH
[0016] Wherein, n is selected from an integer of 1-10;
[0017] X is selected from nitro (-NO2), halogen, cyano (-CN), sulfonic acid (-SO3H), aldehyde (-CHO), acyl (-COR, R is alkyl), carboxyl (-COOH) and amino (-NH2).
[0018] The present invention uses a variety of different co-catalysts in the design and selection process. It is surprisingly found in the test process that the introduction of a variety of different functional groups into the same molecule can control the isomerization degree of the base oil and improve the selectivity of the target product (trimer and tetramer).
[0019] The cationic polymerization of long-chain α-olefins undergoes five steps: catalyst complexation, initiation, chain growth, chain transfer, and chain termination. Among them, the ability of carbon cations to resolve affects the acidity of the active center and the yield of the reaction product; the stability of the carbon cation intermediate affects the regularity of the polymerization.
[0020] The catalyst composition provided by the present invention is used to prepare low-viscosity PAO synthetic oil base oil. Compared with the traditional catalytic system, a proton-type co-catalyst is introduced to form a composite catalytic system with the main catalyst, and the heteroatom induction effect in the proton-type co-catalyst affects the dissociation ability of the carbon cation (i.e., the release of H + The ability of the catalyst to regulate the acidity of the catalyst system, improve the stability of the active center, control the degree of product isomerization, solve the problem of regular polymerization of long-chain α-olefin molecules at the active site, achieve narrow molecular weight oligomerization of α-olefins, improve the selectivity of the target product, and prepare low-viscosity PAO products with excellent viscosity-temperature performance and low-temperature performance.
[0021] Specifically, the structure of the proton-type co-catalyst finally selected by the present invention includes a hydroxyl group and another functional group X, wherein the X group can be a nitro group, a halogen group, a cyano group, a sulfonic acid group, an aldehyde group, an acyl group, a carboxyl group and an amino group, and the acidity of the catalytic system is adjusted by the heteroatom induction effect, thereby affecting the carbon cation, H + Dissociation ability.
[0022] According to the catalyst composition of the present invention, preferably, the acyl group is -COR, wherein R is an alkyl group, preferably a methyl group.
[0023] According to the catalyst composition of the present invention, preferably, the halogen includes fluorine (—F), chlorine (—Cl), bromine (—Br) and iodine (—I).
[0024] According to the catalyst composition of the present invention, preferably, the molar ratio of the boron trifluoride to the proton-type promoter is 0.1 to 3.0, preferably 0.5 to 2.0, and more preferably 0.8 to 1.5.
[0025] According to the catalyst composition of the present invention, preferably, the proton type promoter is selected from 2-nitroethanol, 3-nitropropanol, 2-chloroethanol, 3-chloro-1-propanol, 4-chloro-1-butanol, 5-chloro-1-pentanol, 6-chloro-1-hexanol, 7-chloro-1-heptanol, 8-chloro-1-octanol, 9-chloro-1-nonanol, 10-chloro-1-decanol, 2-fluoroethanol, 3-fluoro-1-propanol, 4-fluoro-1-butanol, 5-fluoro ...chloro-1-pentanol, 6-chloro-1-hexanol, 7-chloro-1-heptanol, 8-chloro-1-octanol, 9-chloro-1-nonanol, 1 -1-pentanol, 6-fluoro-1-hexanol, 7-fluoro-1-heptanol, 8-fluoro-1-octanol, 9-fluoro-1-nonanol, 10-fluoro-1-decanol, 2-bromoethanol, 3-bromo-1-propanol, 4-bromo-1-butanol, 5-bromo-1-pentanol, 6-bromo-1-hexanol, 7-bromo-1-heptanol, 8-bromo-1-octanol, 9-bromo-1-nonanol, 10-bromo-1-decanol, 2-iodoethanol, 3-iodo-1-propanol, 4- Iodo-1-butanol, 5-iodo-1-pentanol, 6-iodo-1-hexanol, 7-iodo-1-heptanol, 8-iodo-1-octanol, 9-iodo-1-nonanol, 10-iodo-1-decanol, 3-hydroxypropionitrile, 4-hydroxybutyronitrile, 2-hydroxyethylsulfonic acid, 3-hydroxypropanesulfonic acid, 4-hydroxybutanesulfonic acid, glycolaldehyde, 3-hydroxypropanal, 4-hydroxybutyraldehyde, 5-hydroxyvaleraldehyde, 6-hydroxyhexanal, 8-hydroxyoctanal, 6-hydroxy-2-hexanone , 5-hydroxy-2-hexanone, glycolic acid, 3-hydroxypropionic acid, 4-hydroxybutyric acid, 6-hydroxyhexanoic acid, 7-hydroxyheptanoic acid, 8-hydroxyoctanoic acid, 9-hydroxynonanoic acid, 10-hydroxydecanoic acid, 3-amino-1-propanol, 4-amino-1-butanol, 5-amino-1-pentanol, 6-amino-1-hexanol, 7-amino-1-heptanol, 8-amino-1-octanol and 10-amino-1-decanol, or a combination of two or more thereof.
[0026] According to the catalyst composition of the present invention, preferably, the proton-type co-catalyst is selected from one or a combination of two or more of 4-fluoro-1-butanol, 3-chloro-1-propanol, 3-iodo-1-propanol, 4-bromo-1-butanol, 6-hydroxyhexanoic acid, 3-nitropropanol, 2-hydroxyethanesulfonic acid, 4-hydroxybutanesulfonic acid, 6-hydroxy-2-hexanone, 5-hydroxyvaleraldehyde, 8-hydroxyoctanoic acid and 10-hydroxydecanoic acid.
[0027] According to the catalyst composition of the present invention, preferably, X in the proton-type co-catalyst is selected from halogen and carboxyl.
[0028] According to the catalyst composition of the present invention, preferably, the proton type co-catalyst is selected from one or a combination of two or more of 4-fluoro-1-butanol, 4-bromo-1-butanol and 8-hydroxyoctanoic acid, and the molar ratio of boron trifluoride to the proton type co-catalyst is 1 to 1.2.
[0029] The second aspect of the present invention provides a method for preparing the above catalyst composition, which comprises: mixing the proton-type co-catalyst and the main catalyst boron trifluoride, and reacting at a predetermined temperature for a predetermined time to obtain the catalyst composition.
[0030] According to the preparation method of the present invention, preferably, the process of mixing the proton type co-catalyst and boron trifluoride comprises: firstly, using nitrogen to heat purge the catalyst preparation reactor, after nitrogen purge, adding the proton type co-catalyst, while starting stirring, raising the temperature to a predetermined temperature, and adding boron trifluoride in proportion. The catalyst preparation reactor is a closed container, which is heat purged with nitrogen to remove water and oxygen.
[0031] According to the preparation method of the present invention, preferably, the predetermined temperature is -30°C to 50°C, preferably -10°C to 30°C.
[0032] According to the preparation method of the present invention, preferably, the predetermined time is 0.5h to 4.0h, preferably 0.5h to 3.0h.
[0033] According to the preparation method of the present invention, preferably, the proton type co-catalyst is subjected to a refining treatment.
[0034] According to the preparation method of the present invention, preferably, the refining treatment includes but is not limited to distillation, adsorbent removal method, etc., and the water content of the proton-type co-catalyst after the refining treatment is less than 100 ppm.
[0035] The preparation method comprises: firstly, using nitrogen to heat purge a catalyst preparation reactor for 5 to 10 minutes, adding a refined proton type co-catalyst after nitrogen purge, and simultaneously starting stirring, and controlling the temperature to be -30°C to 50°C; adding boron trifluoride in proportion, reacting for 0.5 to 4.0 hours, and obtaining the catalyst composition.
[0036] The third aspect of the present invention provides an application of the above catalyst composition in synthesizing poly-α-olefin synthetic oil base oil, that is, a method for preparing poly-α-olefin synthetic oil base oil using the above catalyst composition.
[0037] According to the application of the present invention, preferably, the application comprises the following steps:
[0038] The raw material α-olefin is added into a kettle polymerization reactor, and the catalyst composition is continuously added into the kettle polymerization reactor, and the reaction temperature is controlled at 20° C. to 50° C. (preferably 25° C.) and the residence time is 20 min to 100 min (preferably 60 min). After the reaction is completed, the catalyst is separated and hydrogenated to obtain the polyα-olefin synthetic oil base oil.
[0039] According to the application of the present invention, preferably, the catalyst composition is added in an amount of 0.1% to 2.0% of the mass of the raw α-olefin.
[0040] The catalyst composition of the present invention can be used to produce poly-alpha-olefin synthetic oil base oil, and is particularly suitable for preparing low-viscosity poly-alpha-olefin synthetic oil base oil. The obtained polymerization products mainly include dimers, trimers, tetramers and pentamers. Among them, by adjusting the ratio of Lewis acid and proton type co-catalyst, unexpected test results are obtained. The chromatographic analysis of trimers and tetramers can reach more than 90%. In addition, the viscosity of the poly-alpha-olefin synthetic oil base oil is 4.02 mm 2 / s, viscosity index is 132, pour point is <-60℃.
[0041] Compared with the prior art, the present invention aims at the deficiencies existing in the existing catalytic system and provides a catalyst composition that can be used to prepare a low-viscosity poly-α-olefin synthetic oil base oil, and its advantages are mainly reflected in:
[0042] (1) The catalyst composition of the present invention introduces a proton-type co-catalyst to form a composite catalytic system with the main catalyst, and the heteroatom induction effect of the proton-type co-catalyst affects the carbon cations, H + The dissociation ability can regulate the acidity of the catalytic system, improve the stability of the active center, control the degree of product isomerization, solve the problem of the difficulty of regular polymerization of long-chain α-olefin molecules at the active site, realize the narrow molecular weight oligomerization of α-olefins, and improve the selectivity of the target product.
[0043] (2) The poly-α-olefin synthetic oil base oil obtained by using the catalyst composition of the present invention has a higher viscosity index, good quality, and a higher yield of the target product. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 This is the NMR carbon spectrum of the boron trifluoride-4-fluoro-1-butanol complex prepared in Example 1.
[0045] Figure 2 This is the NMR carbon spectrum of the boron trifluoride-3-chloro-1-propanol complex prepared in Example 2.
[0046] Figure 3 This is the H NMR spectrum of the boron trifluoride-3-chloro-1-propanol complex prepared in Example 2.
[0047] Figure 4 This is the NMR carbon spectrum of the boron trifluoride-hydroxyacetic acid complex prepared in Example 6.
[0048] Figure 5 This is the gas chromatogram of the product obtained from the catalyst composition of Example 1.
[0049] Figure 6 This is the gas chromatogram of the product obtained from the catalyst composition of Comparative Example 3. DETAILED DESCRIPTION
[0050] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0051] All numerical specifications herein (e.g., temperature, time, concentration, and weight, etc., including ranges for each thereof) are generally approximate values that may be appropriately varied (+) or (-) in increments of 0.1 or 1.0. All numerical specifications may be understood as being preceded by the term "about."
[0052] The promoters in the following examples were all purchased from commercial sources and were refined to remove impurities and water as much as possible. The specific refining treatment includes, but is not limited to, conventional process methods such as distillation or physical adsorption. The water content of the proton-type promoter after the refining treatment is less than 100 ppm.
[0053] Example 1
[0054] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0055] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 4-fluoro-1-butanol (1 mol) was added. At the same time, stirring was started, the temperature was raised to 50°C, and the main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.1:1. After reacting for 0.5 hours, the prepared polymerization catalyst (boron trifluoride-4-fluoro-1-butanol complex) was obtained and stored for later use.
[0056] Tetramethylsilane (TMS) was used as the internal standard and D2O as the external standard lock solvent. The NOVA 400MHz NMR instrument was set to adjust the relevant instrument parameters and the obtained boron trifluoride-4-fluoro-1-butanol complex was subjected to 13 C NMR characterization, the nuclear magnetic carbon spectrum is obtained as Figure 1 shown.
[0057] Depend on Figure 1It is known that the δ values of α-C, β-C, ω-C, γ-C atoms of boron trifluoride-4-fluoro-1-butanol complex are respectively located at 61.6ppm, 44.3ppm, 28.4ppm, 26.6ppm. In addition, the catalyst composition nuclear magnetic carbon spectrum in embodiment 3, embodiment 5, embodiment 10 is similar to the spectrogram, except that α-C, β-C have certain displacement. As the electron-withdrawing ability of the introduced group is enhanced, the α-C atom moves to the direction of low-field high δ value, and the variation trend of β-C atom is opposite. In addition, the main catalyst BF3 molecule itself has a strong electron-withdrawing inductive effect, and when forming BO coordination bond, BF3 in order to attract electrons as much as possible, to adjacent atoms (C atoms and H atoms on α-C) also produce an electron-withdrawing inductive effect, causing the corresponding atomic deshielding effect to be enhanced, and the electron cloud density decreases, and its δ value shows as moving to the direction of low-field high displacement.
[0058] Example 2
[0059] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0060] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 3-chloro-1-propanol (1 mol) was added. At the same time, stirring was started, the temperature was raised to 40°C, and the Lewis acid main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.5. After reacting for 0.8 hours, the prepared polymerization catalyst (boron trifluoride-3-chloro-1-propanol complex) was obtained and stored for later use.
[0061] Using tetramethylsilane (TMS) as the internal standard and D2O as the external standard lock solvent, the NOVA 400MHz NMR instrument was set to adjust the relevant instrument parameters and the boron trifluoride-3-chloro-1-propanol complex was measured. 1 H NMR and 13 C NMR characterization, such as Figure 2 and Figure 3 shown.
[0062] Depend on Figure 2 It can be seen that the δ values of α-C, β-C, and ω-C atoms of the boron trifluoride-3-chloro-1-propanol complex are located at 59.1ppm, 41.3ppm, and 35.4ppm, respectively. In addition, the nuclear magnetic carbon spectra of the catalyst compositions in Examples 4 and 8 are similar to the spectra, except that α-C and β-C have certain displacements. The electron-withdrawing ability of the terminal group is enhanced, and the α-C atom moves toward the low-field high δ value direction, while the change trend of the β-C atom is opposite to that of the α-C atom.
[0063] Depend on Figure 3It can be seen that the δ of hydrogen protons in the α-CH2-, β-CH2-, and ω-CH2- groups of the boron trifluoride-3-chloro-1-propanol complex are at 3.83ppm~3.85ppm, 2.05ppm~2.08ppm, and 3.62ppm~3.66ppm, respectively. Boron trifluoride produces an electron-withdrawing inductive effect on the hydrogen protons on the 3-chloro-1-propanol ligand (2.19ppm, alcohol hydroxyl hydrogen proton peak), which enhances the deshielding effect of each hydrogen atom, reduces the electron cloud density, and moves the corresponding hydrogen atoms to the low-field high δ value direction.
[0064] Example 3
[0065] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0066] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 4-chloro-1-butanol (1 mol) was added. At the same time, stirring was started, the temperature was raised to 30°C, and the main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.8. After reacting for 1.0 h, the prepared polymerization catalyst was obtained and stored for later use.
[0067] Example 4
[0068] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0069] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 3-iodine-1-propanol (1 mol) was added. At the same time, stirring was started, the temperature was raised to 20°C, and the main catalyst aluminum chloride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 1.0. After reacting for 1.5 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0070] Example 5
[0071] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0072] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 4-bromo-1-butanol (1 mol) was added. At the same time, stirring was started, the temperature was raised to 10°C, and the main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 1.5. After reacting for 2.0 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0073] Example 6
[0074] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0075] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst hydroxyacetic acid (1 mol) was added, and stirring was started at the same time. The circulating cooler was turned on, and the temperature was controlled to 0°C. The main catalyst sulfur trioxide was added in proportion, and the molar ratio of the main catalyst to the co-catalyst was 2.0. After reacting for 2.5 hours, the prepared polymerization catalyst (boron trifluoride-hydroxyacetic acid complex) was obtained and stored for later use.
[0076] Tetramethylsilane (TMS) was used as the internal standard and D2O as the external standard lock solvent. The NOVA 400MHz NMR instrument was set to adjust the relevant instrument parameters and the boron trifluoride-hydroxyacetic acid complex was measured. 13 C NMR characterization, the spectrum is as follows Figure 4 shown.
[0077] Depend on Figure 4 It can be seen that the carbon atom at the carboxyl position of the boron trifluoride-hydroxyacetic acid complex and the δ value of α-C are located at 177.1ppm and 60.5ppm respectively. In addition, the nuclear magnetic carbon spectra of the catalyst compositions in Examples 7, 9, 10, 13 and 14 are similar to the spectrum, and all have obvious peaks generated by carbon on the carboxyl group, but the difference is that the carbon numbers are different and there are multiple peaks generated by secondary carbon.
[0078] Example 7
[0079] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0080] The catalyst preparation reactor was purged with gas heat for 10 minutes. After purging with nitrogen, the refined co-catalyst 6-hydroxyhexanoic acid (1 mol) was added. At the same time, stirring was started, the circulating cooler was turned on, the temperature was controlled at -10°C, and the main catalyst ferric bromide was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 2.5. After reacting for 3.0 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0081] Example 8
[0082] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0083] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 3-nitropropanol (1 mol) was added, and stirring was started at the same time. The circulating cooler was turned on, and the temperature was controlled at -10°C. The main catalyst boron trifluoride was added in proportion, and the molar ratio of the main catalyst to the co-catalyst was 3.0. After reacting for 4.0 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0084] Example 9
[0085] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0086] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 2-hydroxyethanesulfonic acid (1 mol) was added, and stirring was started at the same time. The circulating cooler was turned on, and the temperature was controlled to -20°C. The main catalyst boron trifluoride was added in proportion, and the molar ratio of the main catalyst to the co-catalyst was 2.0. After reacting for 1.0 h, the prepared polymerization catalyst was obtained and stored for later use.
[0087] Example 10
[0088] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0089] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 4-hydroxybutanesulfonic acid (1 mol) was added, and stirring was started at the same time. The circulating cooler was turned on, and the temperature was controlled at -30°C. The main catalyst boron trifluoride was added in proportion, and the molar ratio of the main catalyst to the co-catalyst was 0.5. After reacting for 2.0 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0090] Embodiment 11
[0091] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0092] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 6-hydroxy-2-hexanone (1 mol) was added, and stirring was started at the same time. The circulating cooler was turned on, and the temperature was controlled at -10°C. The main catalyst boron trifluoride was added in proportion, and the molar ratio of the main catalyst to the co-catalyst was 1.5. After reacting for 0.7 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0093] Example 12
[0094] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0095] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 5-hydroxypentanal (1 mol) was added, and stirring was started at the same time. The circulating cooler was turned on, and the temperature was controlled at -30°C. The main catalyst boron trifluoride was added in proportion, and the molar ratio of the main catalyst to the co-catalyst was 0.6. After reacting for 1.0 h, the prepared polymerization catalyst was obtained and stored for later use.
[0096] Embodiment 13
[0097] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0098] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 8-hydroxyoctanoic acid (1 mol) was added, and stirring was started at the same time. The circulating cooler was turned on, and the temperature was controlled to -20°C. The main catalyst boron trifluoride was added in proportion, and the molar ratio of the main catalyst to the co-catalyst was 1.2. After reacting for 2.0 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0099] Embodiment 14
[0100] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0101] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 10-hydroxydecanoic acid (1 mol) was added, and stirring was started at the same time. The temperature was controlled at 10°C, and the main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.5. After reacting for 4.0 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0102] Embodiment 15
[0103] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0104] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After nitrogen purging, the refined co-catalysts 4-fluoro-1-butanol (0.5 mol) and 6-hydroxy-hexanoic acid (0.5 mol) (the molar ratio of 4-fluoro-1-butanol to 6-hydroxy-hexanoic acid was 1:1) were added. At the same time, stirring was started, the temperature was controlled at 10°C, and the main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.6. After reacting for 3.0 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0105] Example 16
[0106] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0107] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After nitrogen purging, the refined co-catalysts 3-nitropropanol (1 mol) and 4-hydroxybutanesulfonic acid (0.5 mol) (the molar ratio of 3-nitropropanol to 4-hydroxybutanesulfonic acid was 2:1) were added. At the same time, stirring was started, the temperature was controlled at 10°C, and the main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 1.0. After reacting for 2.0 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0108] Embodiment 17
[0109] This embodiment prepares a catalyst composition, which specifically includes the following steps:
[0110] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalysts 5-hydroxypentanal (1 mol), 10-hydroxydecanoic acid (1 mol) and 4-chloro-1-butanol (1 mol) (the molar ratio of 5-hydroxypentanal, 10-hydroxydecanoic acid and 4-chloro-1-butanol was 1:1:1) were added. At the same time, stirring was started, the temperature was controlled at 20°C, and the main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.8. After reacting for 4.0 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0111] Comparative Example 1
[0112] This comparative example prepares a catalyst composition, which specifically includes the following steps:
[0113] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 4-fluoro-1-butanol (1 mol) was added. Stirring was started at the same time. The temperature was controlled at 50°C. The main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 4.0. After reacting for 0.5 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0114] Comparative Example 2
[0115] This comparative example prepares a catalyst composition, which specifically includes the following steps:
[0116] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst 4-fluoro-1-butanol (1 mol) was added. Stirring was started at the same time. The temperature was controlled at 50°C. The main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.05. After reacting for 0.5 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0117] Comparative Example 3
[0118] This comparative example prepares a catalyst composition, which specifically includes the following steps:
[0119] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst butanol (1 mol) was added. Stirring was started at the same time. The temperature was controlled at 50°C. The main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.1. After reacting for 0.5 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0120] Comparative Example 4
[0121] This comparative example prepares a catalyst composition, which specifically includes the following steps:
[0122] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst isopropanol (1 mol) was added. Stirring was started at the same time. The temperature was controlled at 50°C. The main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.1. After reacting for 0.5 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0123] Comparative Example 5
[0124] This comparative example prepares a catalyst composition, which specifically includes the following steps:
[0125] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst acetic acid (1 mol) was added. Stirring was started at the same time. The temperature was controlled at 50°C. The main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.1. After reacting for 0.5 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0126] Comparative Example 6
[0127] This comparative example prepares a catalyst composition, which specifically includes the following steps:
[0128] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, refined co-catalyst deionized water (1 mol) was added. Stirring was started at the same time. The temperature was controlled at 50°C. The main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.1. After reacting for 0.5 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0129] Comparative Example 7
[0130] This comparative example prepares a catalyst composition, which specifically includes the following steps:
[0131] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst ethyl acetate (1 mol) was added, and stirring was started at the same time. The temperature was controlled at 50°C, and the main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.1. After reacting for 0.5 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0132] Comparative Example 8
[0133] This comparative example prepares a catalyst composition, which specifically includes the following steps:
[0134] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst phosphoric acid (1 mol) was added. Stirring was started at the same time. The temperature was controlled at 50°C. The main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.1. After reacting for 0.5 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0135] Comparative Example 9
[0136] This comparative example prepares a catalyst composition, which specifically includes the following steps:
[0137] The catalyst preparation reactor was purged with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst dimethyl ether (1 mol) was added. Stirring was started at the same time. The temperature was controlled at 50°C. The main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.1. After reacting for 0.5 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0138] Comparative Example 10
[0139] This comparative example prepares a catalyst composition, which specifically includes the following steps:
[0140] The catalyst preparation reactor was prepared by hot-purging with nitrogen for 10 minutes. After purging with nitrogen, the refined co-catalyst acetone (1 mol) was added, and stirring was started at the same time. The temperature was controlled at 50°C, and the main catalyst boron trifluoride was added in proportion. The molar ratio of the main catalyst to the co-catalyst was 0.1. After reacting for 0.5 hours, the prepared polymerization catalyst was obtained and stored for later use.
[0141] Catalyst performance evaluation test:
[0142] Using 1-decene as a raw material, the raw material is first pumped into a kettle polymerization reactor, and the catalyst compositions prepared in Examples 1-17 and Comparative Examples 1-4 are respectively continuously added to the polymerization reactor, wherein the amount of the catalyst composition is 1.0wt.‰ (accounting for the mass fraction of the 1-decene raw material), the reaction temperature is controlled at 25°C, and the residence time is 60min. After the reaction is completed, the catalyst is separated, and the product is obtained after hydrogenation. The product is collected for chromatographic analysis and performance testing, and the results are shown in Tables 1 and 2.
[0143] Table 1 Preparation conditions of the catalyst composition in each embodiment and comparative example and corresponding product performance parameters
[0144]
[0145]
[0146] Table 2 Composition distribution of products obtained by preparing the catalyst composition of each embodiment and comparative example
[0147]
[0148]
[0149] It can be seen from the product performance parameters and composition distribution of the above embodiments that the Lewis acid is used as the main catalyst, 4-fluoro-1-butanol, 3-chloro-1-propanol, 4-chloro-1-butanol, 3-iodo-1-propanol, 4-bromo-1-butanol, glycolic acid, 6-hydroxy-hexanoic acid, 3-nitropropanol, 4-amino-1-butanol, 4-hydroxybutanesulfonic acid, 6-hydroxy-2-hexanone, 5-hydroxyvaleraldehyde, 8-hydroxyoctanoic acid and 10-hydroxydecanoic acid are used as co-catalysts, and the obtained base oil has a kinematic viscosity of 4-10 mm at 100°C. 2 / s, viscosity index greater than 130, target product (C 30 +C 40 ) is much higher than that of Comparative Examples 3-10 (using conventional butanol, isopropanol, acetic acid, deionized water, ethyl acetate, phosphoric acid or dimethyl ether acetone as co-catalyst).
[0150] The products obtained under the catalyst composition in Example 1 and Comparative Example 3 were analyzed by gas chromatography. The results are as follows: Figure 5 and Figure 6 As shown, the product composition obtained by using the initiator of the present invention is mainly C 30 and C 40 ( Figure 5 The retention times were 15-17min and 20-23min respectively), while the product composition distribution obtained with butanol as the initiator was relatively wide, such as Figure 6 As shown. The chromatographic analysis used a hydrogen flame ionization detector, the carrier gas was nitrogen, the column front pressure was 0.07MPa, the hydrogen flow rate was 30mL / min, and the air flow rate was 250mL / min. The injection port temperature was 250℃, the detector temperature was 400℃, the vaporization chamber temperature was 450℃, the split ratio was 100:1, and the program temperature was used: the initial temperature was 50℃, maintained for 10min; then the temperature was increased at a heating rate of 9℃ / min to the end temperature of 380℃, maintained for 10min.
[0151] By comparing Example 1 with Comparative Examples 1 and 2, it can be seen that within the molar ratio range of the main catalyst to the co-catalyst provided by the present invention, a target product with good product performance and high selectivity can be obtained.
[0152] In addition, the catalyst composition prepared in Example 1 was used to perform performance tests with other α-olefins as raw materials. The specific process is as follows: 1-octene, 1-dodecene, and coal-based α-olefins were used as raw materials, respectively. The raw materials were first pumped into a kettle polymerization reactor, and the catalyst composition prepared in Example 1 was continuously added to the polymerization reactor, wherein the amount of the catalyst composition was 1.0wt.‰ (accounting for the mass fraction of the α-olefin raw material), the reaction temperature was controlled at 25°C, and the residence time was 60min. After the reaction was completed, the catalyst was separated, and the product was obtained after hydrogenation. The product was collected for chromatographic analysis and performance testing, and the results are shown in Table 3.
[0153] As can be seen from Table 3, the catalyst composition of the present invention is applicable to the polymerization reaction of various α-olefins (1-octene, 1-dodecene, coal-based α-olefins), and the viscosity-temperature performance and low-temperature performance of the obtained polymerization products are relatively good.
[0154] Table 3 Product performance parameters corresponding to different α-olefin raw materials
[0155] Serial number α-Olefin Raw Materials <![CDATA[KV100℃ / mm 2 / s]]> Viscosity Index Pour point / ℃ 1 1-Octene 3.03 125 -60℃ 2 1-Dodecene 5.07 132 -60℃ 3 Coal-to-α-olefins (C6-C14 components) 4.15 134 -60℃
[0156] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A catalyst composition for the polymerization of α-olefins, wherein: The catalyst composition includes boron trifluoride and at least one proton-type promoter; The general structural formula of the proton type co-catalyst is: X-(CH2) n -OH Wherein, n is selected from an integer of 1-10; X is selected from one of a nitro group, a halogen group, a sulfonic acid group and a carboxyl group; The molar ratio of boron trifluoride to proton type co-catalyst is 0.1 to 3.0; The catalyst composition for α-olefin polymerization is prepared by at least the following steps: mixing the proton-type co-catalyst and boron trifluoride, reacting at a predetermined temperature for a predetermined time, wherein the predetermined temperature is from -30°C to 50°C, to obtain the catalyst composition.
2. The catalyst composition according to claim 1, wherein The proton type co-catalyst is selected from 2-nitroethanol, 3-nitropropanol, 2-chloroethanol, 3-chloro-1-propanol, 4-chloro-1-butanol, 5-chloro-1-pentanol, 6-chloro-1-hexanol, 7-chloro-1-heptanol, 8-chloro-1-octanol, 9-chloro-1-nonanol, 10-chloro-1-decanol, 2-fluoroethanol, 3-fluoro-1-propanol, 4-fluoro-1-butanol, 5-fluoro-1-pentanol, 6-fluoro-1-hexanol, 7-fluoro-1-heptanol, 8-fluoro-1-octanol, 9-fluoro-1-nonanol, 10-fluoro-1-decanol, 2-bromoethanol, 3-bromo-1-propanol, 4-bromo-1-butanol, 5-bromo-1-pentanol, 6-bromo-1-hexanol, 7-bromo-1-heptanol, 8-bromo-1-octanol, 9-bromo-1-nonanol, 10-bromo-1-decanol, 2-iodoethanol, 3-iodo-1-propanol, 4-iodo-1-butanol, 5-iodo-1-pentanol, 6-iodo-1-hexanol, 7-iodo-1-heptanol, 8-iodo-1-octanol, 9-iodo-1-nonanol, 10-iodo-1-decanol, 2-hydroxyethylsulfonic acid, 3-hydroxypropanesulfonic acid, 4-hydroxybutanesulfonic acid, glycolic acid, 3-hydroxypropionic acid, 4-hydroxybutyric acid, 6-hydroxyhexanoic acid, 7-hydroxyheptanoic acid, 8-hydroxyoctanoic acid, 9-hydroxynonanoic acid and 10-hydroxydecanoic acid, or a combination of two or more thereof.
3. The catalyst composition according to claim 1, wherein The proton-type co-catalyst is selected from one or a combination of two or more of 4-fluoro-1-butanol, 3-chloro-1-propanol, 3-iodo-1-propanol, 4-bromo-1-butanol, 6-hydroxyhexanoic acid, 3-nitropropanol, 2-hydroxyethanesulfonic acid, 4-hydroxybutanesulfonic acid, 8-hydroxyoctanoic acid and 10-hydroxydecanoic acid.
4. The catalyst composition according to claim 1, wherein X is selected from one of halogen and carboxyl.
5. The catalyst composition according to claim 4, wherein The proton type co-catalyst is selected from one or a combination of two or more of 4-fluoro-1-butanol, 4-bromo-1-butanol and 8-hydroxyoctanoic acid.
6. The catalyst composition according to claim 1, wherein The molar ratio of the boron trifluoride to the proton type co-catalyst is 0.5-2.
0.
7. The catalyst composition according to claim 1, wherein The molar ratio of the boron trifluoride to the proton type co-catalyst is 0.8 to 1.
5.
8. The catalyst composition according to claim 1, wherein The proton type co-catalyst is selected from one or a combination of two or more of 4-fluoro-1-butanol, 4-bromo-1-butanol and 8-hydroxyoctanoic acid, and the molar ratio of boron trifluoride to the proton type co-catalyst is 1 to 1.
2.
9. A method for preparing the catalyst composition according to any one of claims 1 to 8, wherein: The preparation method comprises: mixing the proton type co-catalyst and boron trifluoride, reacting at a predetermined temperature for a predetermined time, wherein the predetermined temperature is from -30°C to 50°C, to obtain the catalyst composition.
10. The preparation method according to claim 9, wherein: The process of mixing the proton type catalyst and boron trifluoride includes: firstly, using nitrogen to heat purge the catalyst to prepare the reaction kettle, adding the proton type catalyst after nitrogen purge, starting stirring at the same time, raising the temperature to a predetermined temperature, and adding boron trifluoride in proportion.
11. The preparation method according to claim 9, wherein: The predetermined temperature is -10°C to 30°C.
12. The preparation method according to claim 9, wherein: The predetermined time is 0.5 h to 4.0 h.
13. The preparation method according to claim 12, wherein: The predetermined time is 0.5 h to 3.0 h.
14. The preparation method according to claim 9, wherein: The proton type co-catalyst is refined.
15. The preparation method according to claim 14, wherein: The refining treatment includes distillation and / or adsorbent removal method, and the water content of the proton-type promoter after the refining treatment is less than 100 ppm.
16. The preparation method according to claim 9, wherein: The preparation method comprises: firstly, using nitrogen to heat purge a catalyst preparation reactor for 5 min to 10 min, adding a refined proton type co-catalyst after nitrogen purge, and simultaneously starting stirring, and controlling the temperature to be -30°C to 50°C; adding boron trifluoride in proportion, reacting for 0.5 h to 4.0 h, and obtaining the catalyst composition.
17. Use of the catalyst composition according to any one of claims 1 to 8 in synthesizing poly-alpha-olefin synthetic oil base oil.
18. The use according to claim 17, wherein: The application includes the following steps: The raw material α-olefin is added into a kettle polymerization reactor, and the catalyst composition is continuously added into the kettle polymerization reactor, and the reaction temperature is controlled at 20° C. to 50° C. and the residence time is 20 min to 100 min. After the reaction is completed, the catalyst is separated and hydrogenated to obtain the polyα-olefin synthetic oil base oil.
19. The use according to claim 18, wherein: The catalyst composition is added in an amount of 0.1% to 2.0% of the mass of the raw α-olefin.