A novel carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectrocatalytic anode material and preparation method thereof

By using the combination technology of carbon-doped tungsten trioxide, zinc ferrite heterojunction and cobalt-iron oxide passivation layer in traditional photocatalytic materials, the problems of low photocatalytic oxygen evolution reaction efficiency and poor photocorrosion are solved, and high-efficiency photocatalysts are achieved. High performance and stable photoelectrocatalytic materials.

CN115216802BInactive Publication Date: 2024-10-01OCEAN UNIV OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210896338.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-28
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The traditional photocatalytic oxygen evolution reaction has low catalytic efficiency, requires a large overpotential, and the material is poorly corrosive to light, making it difficult to realize high-performance photoelectrocatalytic materials.

Method used

The carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectrocatalytic material was prepared through a precise and orderly three-step hydrothermal method, and loaded with a cobalt-iron oxide passivation layer to improve photocurrent performance and photocorrosion resistance.

Benefits of technology

A high-performance photoelectrocatalytic material has been realized with excellent photocurrent performance and stability. After 8000 seconds of testing, the photocurrent is still maintained at 1.812 mA/cm2, which significantly improves the performance and corrosion resistance of the photoelectrocatalytic material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115216802B_ABST
    Figure CN115216802B_ABST
Patent Text Reader

Abstract

The present invention discloses a novel photoelectric catalyst material and preparation method for a heterojunction formed by carbon-doped tungsten trioxide and zinc ferrite. The experiment prepares a photoelectric catalyst material for a heterojunction formed by carbon-doped tungsten trioxide and zinc ferrite by a precise and orderly three-time hydrothermal and passivation treatment method. The heterojunction preparation method is as follows: first, deionized water, sodium tungstate dihydrate, potassium oxalate, and a quantitative carbon powder are mixed and stirred to prepare a precursor by a hydrothermal method; then, the precursor is dried and sintered to obtain carbon-doped tungsten trioxide; then, ferric chloride hexahydrate, sodium nitrate, and zinc nitrate hexahydrate are mixed and subjected to a secondary hydrothermal method, sintering, and sodium hydroxide soaking to prepare a zinc ferrite film; finally, a cobalt iron oxide passivation layer is loaded by a hydrothermal method. Compared with ordinary zinc ferrite, the heterojunction formed by carbon-doped tungsten trioxide loading the zinc ferrite film has significant advantages such as excellent performance, excellent light corrosion resistance, and stable performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of photoelectric catalytic material chemistry, and specifically relates to a novel carbon-doped tungsten trioxide and zinc ferrite heterojunction novel photoelectric catalyst material and a preparation method thereof. Background Art

[0002] Traditional fossil energy has led to resource shortages due to large-scale and uncontrolled exploitation. At the same time, it is non-renewable and easily causes corresponding environmental pollution. Hydrogen energy is a new type of high-quality energy that is clean and pollution-free, has abundant resource reserves, and has high energy density. Research on hydrogen energy is divided into hydrogen evolution reaction and oxygen evolution reaction. Among them, oxygen evolution reaction is widely used in the preparation and research of pure oxygen, hydrogen energy intermediates, photoelectric materials for sterilization and disinfection equipment, and pollutant degradation materials. The photocatalytic oxygen evolution reaction occurs on the surface of the material, and the catalytic efficiency is often not high. It needs to overcome resistance such as solution and external circuit resistance, and requires a large overpotential. Photocatalysis can effectively separate electrons and holes by applying a bias voltage, thereby improving the photoelectric conversion efficiency. Therefore, the development of new photocatalytic photoanode materials with visible light activity has become an important research topic.

[0003] Literature "Wang Yingjie, Shen Yu, Liu Shuhong, Shi Jinru, et al. 3 / ZnFe 2 O 4 Construction of nanomaterials and their performance in degrading antibiotics. Journal of Dalian Jiaotong University, October 2019, Vol. 40, No. 5, published a process for preparing tungsten trioxide and zinc ferrite composite materials by solid phase grinding. The difference is that the present invention patent has carbon doped the substrate tungsten trioxide, and on this basis, the zinc ferrite heterojunction is prepared by hydrothermal method, and finally the passivation layer is treated to prepare high-performance carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectrocatalytic photoanode materials.

[0004] The present invention prepares a carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectrocatalytic photoanode material by a precise and orderly three-step hydrothermal method. The photoanode catalytic material has significant advantages such as excellent performance, excellent anti-photocorrosion performance and excellent performance stability. Summary of the invention

[0005] The main purpose of the present invention is to provide a photoelectric catalyst with high performance and excellent corrosion resistance.

[0006] In order to achieve the above-mentioned purpose, the present invention provides a novel carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectric catalyst material.

[0007] The preparation method of the present invention is simple and inexpensive. The prepared novel carbon-doped tungsten trioxide and zinc ferrite heterojunction novel photoelectric catalyst has excellent photoelectrochemical performance. Its performance under reversible hydrogen potential is 2.156 mA / cm2. After 8000 seconds of stability test, the photocurrent performance still maintains a high performance of 1.812 mA / cm2.

[0008] The technical solution of the present invention:

[0009] The present invention proposes a novel carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectric catalyst material, characterized in that the photoelectric catalytic photoanode material is prepared by a precise and orderly three-step hydrothermal method to prepare the carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectric catalytic photoanode material, and finally loaded with a cobalt iron oxide passivation layer, so that the photocurrent performance of the photoanode material is greatly improved, while the anti-photocorrosion performance and performance stability are maintained excellent.

[0010] The present invention proposes a novel carbon-doped tungsten trioxide and zinc ferrite heterojunction novel photoelectric catalyst material, which is characterized by comprising the following steps:

[0011] Step (1): deionized water, sodium tungstate dihydrate, potassium oxalate and carbon powder are mixed and stirred evenly, and placed on conductive glass for hydrothermal reaction to prepare a carbon-doped tungsten trioxide precursor; the sample is taken out, washed with ethanol and deionized water for more than three times respectively and vacuum dried; the precursor sample is sintered to obtain a carbon-doped tungsten trioxide sample, and then sealed and stored;

[0012] Step (2): mixing ferric chloride hexahydrate, sodium nitrate, zinc nitrate hexahydrate, and deionized water, and stirring them uniformly, placing a carbon-doped tungsten trioxide conductive glass sample for hydrothermal reaction to obtain a heterojunction precursor, and then drying, sintering, and soaking in sodium hydroxide to obtain a heterojunction, and washing with deionized water and ethanol for more than three times, vacuum drying, and high-temperature sintering;

[0013] Step (3): Finally, place a heterojunction conductive glass sample, load a cobalt iron oxide passivation layer by a hydrothermal method, wash it with deionized water and ethanol for more than three times and vacuum dry it to obtain a new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction.

[0014] A preferred solution is that in step (1), 2.5-4.5 mmol of sodium tungstate dihydrate, 0.4-0.6 mmol of potassium oxalate, 1.2-1.5 mmol of carbon powder and 40-45 ml of deionized water are weighed and placed in a beaker for stirring. The pH value of the solution is adjusted with a 3 mol / L hydrochloric acid solution. The pH value of the solution is adjusted to 0.9-1.3. After stirring for 6 hours, a uniform hydrothermal reaction solution is obtained. The solution is preferably turbid light green. The conductive glass is placed for hydrothermal reaction. The deposition surface of the conductive glass should be placed downward. The transfer volume of the hydrothermal reaction solution needs to be detected so that the conductive glass is not completely immersed. A 2 mm×10 mm unimmersed portion is reserved. The hydrothermal temperature should be set to 170-190 degrees Celsius. The hydrothermal reaction time should be set to 20-30 hours.

[0015] A preferred solution is that in step (2), 4 to 8 mmoles of zinc nitrate hexahydrate, 5 to 10 mmoles of sodium nitrate, and 5 to 10 mmoles of ferric chloride hexahydrate are weighed and mixed with 50 ml of deionized water to dissolve, and stirred for 30 minutes to prepare a uniform hydrothermal reaction solution, into which a carbon-doped tungsten trioxide conductive glass sample is placed for hydrothermal reaction. The deposited surface of the conductive glass should be placed facing downward, leaving a 4 mm × 10 mm unsubmerged portion, the temperature of the hydrothermal reaction should be set to 90 to 115 degrees Celsius, and the time of the hydrothermal reaction should be set to 5 to 8 hours.

[0016] A preferred solution is that in step (3), 20 to 30 mmoles of ferric chloride hexahydrate and 20 to 30 mmoles of cobalt nitrate hexahydrate are weighed, stirred and dissolved, and then placed in a conductive glass for hydrothermal reaction. The deposition surface of the conductive glass should be placed facing downward, leaving a 6 mm × 10 mm unsubmerged part. The hydrothermal temperature should be set to 96 to 100 degrees Celsius, and the hydrothermal reaction time should be set to 30 to 45 minutes. After taking out the sample, vacuum drying is performed to prepare a cobalt iron oxide passivation layer.

[0017] A preferred embodiment is that in the steps (1) to (3), the drying temperature is 60 degrees Celsius and the vacuum drying time is 2 hours.

[0018] A preferred solution is that in steps (1) to (3), the electrolyte solutions used in all sample tests need to be slowly bubbled with nitrogen for 20 to 30 minutes to remove the oxygen component in the electrolyte solution; ice bags need to be placed next to the electrolyte solution or intermittent testing needs to be performed to prevent the electrolyte solution from being irradiated for more than 40 minutes and causing a temperature rise, thereby avoiding inaccurate test results; before testing, an accurate test distance needs to be calculated to ensure the standard sunlight intensity of AM 1.5; and the light intensity is regularly tested every week to avoid the light intensity being weakened due to the long-term use of the xenon lamp, thereby affecting the standard sunlight intensity.

[0019] The beneficial effects of the above scheme are as follows: (1) The present invention uses deionized water, sodium nitrate, ferric chloride hexahydrate, zinc nitrate hexahydrate, potassium oxalate, hydrochloric acid and other raw materials to prepare a heterojunction, which has low cost and excellent performance; (2) The present invention first modifies the tungsten trioxide substrate by carbon doping, and then loads a zinc ferrite film by a hydrothermal method to form a heterojunction, so that the photocurrent catalytic performance is greatly improved, and the photoelectric catalytic stability is very excellent; (3) The present invention treats and loads a cobalt iron oxide passivation layer on the heterojunction, so that the photoelectric catalytic material has excellent anti-photocorrosion performance. After 8000 seconds of stability test, the photocurrent still maintains a high performance of 1.812 mA / cm2.

[0020] In summary, the novel carbon-doped tungsten trioxide and zinc ferrite heterojunction novel photoelectric catalyst material proposed in the present invention has the advantages of excellent photoelectric performance, excellent corrosion resistance, etc.; it has great scientific research and industrial application value in the pure oxygen industry, preparation and research of hydrogen energy intermediates, industrialization of sterilization and disinfection equipment materials, and pollutant degradation industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the X-ray photoelectron spectrum (XPS) of a new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction.

[0022] Figure 2 This is a comparison chart of transient photocurrent tests of a new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction.

[0023] Figure 3 This is a comparison diagram of the mechanism of the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction.

[0024] Figure 4 This is a comparison diagram of the chopped linear sweep voltammetry of the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction.

[0025] Figure 5 This is a stability test comparison chart of the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction.

[0026] Figure 6 This is the X-ray high-resolution photoelectron spectrum of the 2p orbital of zinc element in the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction.

[0027] Figure 7 This is the X-ray high-resolution photoelectron spectrum of the 2p orbital of the iron element in the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction.

[0028] Figure 8This is the X-ray high-resolution photoelectron spectrum of the 2p orbital of the cobalt element in the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction.

[0029] Fig. 9 This is the X-ray high-resolution photoelectron spectrum of the 1s orbit of the oxygen element in the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction. DETAILED DESCRIPTION

[0030] The present invention is described in detail with reference to the following embodiments.

[0031] Example 1

[0032] First, weigh 2.5 mmol of sodium tungstate dihydrate, 0.4 mmol of potassium oxalate, 1.2 mmol of carbon powder and 40 ml of deionized water, put them into a beaker and stir, adjust the pH value of the solution with 3 mol / L hydrochloric acid solution, and the pH value of the solution is adjusted to 0.9. After stirring for 6 hours, a uniform hydrothermal reaction solution is obtained. The solution is best when it is turbid light green. Put it into conductive glass for hydrothermal reaction. The deposition surface of the conductive glass should be placed downward. The transfer volume of the hydrothermal reaction solution needs to be detected so that the conductive glass is not completely immersed. Reserve a 2 mm × 10 mm unimmersed part. The hydrothermal temperature should be set to 170 degrees Celsius, and the hydrothermal reaction time should be set to 20 hours. Then, 4 mmol of zinc nitrate hexahydrate, 5 mmol of sodium nitrate, and 5 mmol of ferric chloride hexahydrate were weighed, mixed, stirred and dissolved with 50 ml of deionized water. After stirring for 30 minutes, a uniform hydrothermal reaction solution was prepared, and a carbon-doped tungsten trioxide conductive glass sample was placed for hydrothermal reaction. The deposition surface of the conductive glass should be placed downward, and a 4 mm × 10 mm unimmersed portion was reserved. The temperature of the hydrothermal reaction should be set to 90 degrees Celsius, and the time of the hydrothermal reaction should be set to 5 hours. Finally, 20 mmol of ferric chloride hexahydrate and 20 mmol of cobalt nitrate hexahydrate were weighed, mixed, stirred and dissolved, and placed in the conductive glass for hydrothermal reaction. The deposition surface of the conductive glass should be placed downward, and a 6 mm × 10 mm unimmersed portion was reserved. The hydrothermal temperature should be set to 96 degrees Celsius, and the time of the hydrothermal reaction should be set to 30 minutes. After taking out the sample, vacuum drying was performed to prepare a cobalt iron oxide passivation layer. Figure 1 This is the X-ray photoelectron spectrum (XPS) of a new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction. From the spectrum, tungsten, oxygen, zinc, iron, cobalt and carbon can be clearly distinguished, which is consistent with "Yayao Lan, Zhifeng Liu, Zhengang Guo, Mengnan Ruan and Xifei Li, Apromising p-type Co-ZnFe 2 O 4nanorod film as a photocathode for photoelectrochemical water splitting, Chem. Commun., 2020, 56, 5279" and "ZhichaoHao, MengnanRuan, ZhengangGuo, WeiguoYan, XiangfengWu and ZhifengLiu, The synergistic role of the photo sensitivity effect and extended space charge region in an inorganic–organic WO 3 / PANIphotoanode for efficient PEC water splitting, Sustainable Energy Fuels, 2021, 5, 2893" and other standard peaks are consistent, proving that the carbon-doped tungsten trioxide and zinc ferrite heterojunction was synthesized in this implementation case.

[0033] Example 2

[0034] First, weigh 4.5 mmol of sodium tungstate dihydrate, 0.6 mmol of potassium oxalate, 1.5 mmol of carbon powder and 45 ml of deionized water, put them into a beaker and stir, adjust the pH value of the solution with 3 mol / L hydrochloric acid solution, and the pH value of the solution is adjusted to 1.3. After stirring for 6 hours, a uniform hydrothermal reaction solution is obtained. The solution is best when it is turbid light green. Put it into conductive glass for hydrothermal reaction. The deposition surface of the conductive glass should be placed downward. The transfer volume of the hydrothermal reaction solution needs to be detected so that the conductive glass is not completely immersed. Reserve 2 mm × 10 mm of unimmersed part. The hydrothermal temperature should be set to 190 degrees Celsius, and the hydrothermal reaction time should be set to 30 hours. Then, 8 mmol of zinc nitrate hexahydrate, 10 mmol of sodium nitrate, 10 mmol of ferric chloride hexahydrate were weighed, mixed and stirred with 50 ml of deionized water to dissolve, and a uniform hydrothermal reaction solution was prepared after stirring for 30 minutes. The carbon-doped tungsten trioxide conductive glass sample was put in for hydrothermal reaction. The deposited surface of the conductive glass should be placed downward, and a 4 mm × 10 mm unimmersed portion was reserved. The temperature of the hydrothermal reaction should be set to 115 degrees Celsius, and the time of the hydrothermal reaction should be set to 8 hours. Finally, 30 mmol of ferric chloride hexahydrate and 30 mmol of cobalt nitrate hexahydrate were weighed, mixed and stirred to dissolve, and put into the conductive glass for hydrothermal reaction. The deposited surface of the conductive glass should be placed downward, and a 6 mm × 10 mm unimmersed portion was reserved. The hydrothermal temperature should be set to 100 degrees Celsius, and the time of the hydrothermal reaction should be set to 45 minutes. After taking out the sample, vacuum drying was performed to prepare a cobalt iron oxide passivation layer. Figure 2 This is a transient photocurrent test comparison chart of the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction. It can be seen from the figure that the light response performance of the photoelectric catalyst prepared in this implementation case is very excellent, and the best photocurrent performance is about 1.756 mA / cm2.

[0035] Example 3

[0036] First, weigh 3.5 mmol of sodium tungstate dihydrate, 0.5 mmol of potassium oxalate, 1.35 mmol of carbon powder and 42.5 ml of deionized water, put them into a beaker and stir, adjust the pH value of the solution with 3 mol / L hydrochloric acid solution, and the pH value of the solution is adjusted to 1.1. After stirring for 6 hours, a uniform hydrothermal reaction solution is obtained. The solution is best when it is turbid light green. Put it into conductive glass for hydrothermal reaction. The deposition surface of the conductive glass should be placed downward. The transfer volume of the hydrothermal reaction solution needs to be detected so that the conductive glass is not completely immersed. Reserve a 2 mm × 10 mm unimmersed part. The hydrothermal temperature should be set to 180 degrees Celsius, and the hydrothermal reaction time should be set to 25 hours. Then, 6 mmol of zinc nitrate hexahydrate, 7.5 mmol of sodium nitrate, 7.5 mmol of ferric chloride hexahydrate were weighed and mixed with 50 ml of deionized water, stirred and dissolved, and a uniform hydrothermal reaction solution was prepared after stirring for 30 minutes. The carbon-doped tungsten trioxide conductive glass sample was put in for hydrothermal reaction. The deposited surface of the conductive glass should be placed downward, and a 4 mm × 10 mm unsubmerged portion was reserved. The temperature of the hydrothermal reaction should be set to 102.5 degrees Celsius, and the time of the hydrothermal reaction should be set to 6.5 hours. Finally, 25 mmol of ferric chloride hexahydrate and 25 mmol of cobalt nitrate hexahydrate were weighed and mixed and stirred and dissolved, and then put into the conductive glass for hydrothermal reaction. The deposited surface of the conductive glass should be placed downward, and a 6 mm × 10 mm unsubmerged portion was reserved. The hydrothermal temperature should be set to 98 degrees Celsius, and the time of the hydrothermal reaction should be set to 37.5 minutes. After taking out the sample, vacuum drying was performed to prepare a cobalt iron oxide passivation layer. Figure 3 This is a comparison diagram of the mechanism of the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction. Figure 4 This is a chopped linear sweep voltammetry comparison diagram of a new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction. It can be seen from the figure that the light response performance of this implementation case is very excellent, and the best photocurrent performance is about 2.089 mA / cm2.

[0037] Example 4

[0038] First, weigh 3 mmol of sodium tungstate dihydrate, 0.45 mmol of potassium oxalate, 1.3 mmol of carbon powder and 42 ml of deionized water, put them into a beaker and stir, adjust the pH value of the solution with 3 mol / L hydrochloric acid solution, and the pH value of the solution is adjusted to 1.0. After stirring for 6 hours, a uniform hydrothermal reaction solution is obtained. The solution is best when it is turbid light green. Put it into conductive glass for hydrothermal reaction. The deposition surface of the conductive glass should be placed downward. The transfer volume of the hydrothermal reaction solution needs to be detected so that the conductive glass is not completely immersed. Reserve 2 mm × 10 mm of unimmersed part. The hydrothermal temperature should be set to 175 degrees Celsius, and the hydrothermal reaction time should be set to 203 hours. Then, 5 mmol of zinc nitrate hexahydrate, 6 mmol of sodium nitrate, and 6 mmol of ferric chloride hexahydrate were weighed, mixed, stirred and dissolved with 50 ml of deionized water, and a uniform hydrothermal reaction solution was prepared after stirring for 30 minutes, and a carbon-doped tungsten trioxide conductive glass sample was put in for hydrothermal reaction. The deposited surface of the conductive glass should be placed downward, and a 4 mm × 10 mm unsubmerged portion was reserved. The temperature of the hydrothermal reaction should be set to 100 degrees Celsius, and the time of the hydrothermal reaction should be set to 6 hours. Finally, 23 mmol of ferric chloride hexahydrate and 23 mmol of cobalt nitrate hexahydrate were weighed, mixed, stirred and dissolved, and put into the conductive glass for hydrothermal reaction. The deposited surface of the conductive glass should be placed downward, and a 6 mm × 10 mm unsubmerged portion was reserved. The hydrothermal temperature should be set to 97 degrees Celsius, and the time of the hydrothermal reaction should be set to 32 minutes. After taking out the sample, vacuum drying was performed to prepare a cobalt iron oxide passivation layer. Figure 5 This is a stability test comparison chart of the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction. In this implementation case, the photocurrent performance of the heterojunction formed by carbon-doped tungsten trioxide and zinc ferrite began to decline at 7000 seconds. However, after loading the passivation layer, not only the photocurrent performance of the catalytic material was greatly improved, but the stability also did not decline, showing excellent stability performance.

[0039] Example 5

[0040] First, weigh 4.2 mmol of sodium tungstate dihydrate, 0.5 mmol of potassium oxalate, 1.4 mmol of carbon powder and 44 ml of deionized water, put them into a beaker and stir, adjust the pH value of the solution with 3 mol / L hydrochloric acid solution, and the pH value of the solution is adjusted to 1.2. After stirring for 6 hours, a uniform hydrothermal reaction solution is obtained. The solution is best when it is turbid light green. Put it into conductive glass for hydrothermal reaction. The deposition surface of the conductive glass should be placed downward. The transfer volume of the hydrothermal reaction solution needs to be detected so that the conductive glass is not completely immersed. Reserve a 2 mm × 10 mm unimmersed part. The hydrothermal temperature should be set to 185 degrees Celsius, and the hydrothermal reaction time should be set to 28 hours. Then, 7 mmol of zinc nitrate hexahydrate, 8 mmol of sodium nitrate, and 8 mmol of ferric chloride hexahydrate were weighed, mixed, stirred and dissolved with 50 ml of deionized water, and a uniform hydrothermal reaction solution was prepared after stirring for 30 minutes, and a carbon-doped tungsten trioxide conductive glass sample was put in for hydrothermal reaction. The deposited surface of the conductive glass should be placed downward, and a 4 mm × 10 mm unimmersed portion was reserved. The temperature of the hydrothermal reaction should be set to 110 degrees Celsius, and the time of the hydrothermal reaction should be set to 7 hours. Finally, 28 mmol of ferric chloride hexahydrate and 28 mmol of cobalt nitrate hexahydrate were weighed, mixed, stirred and dissolved, and put into the conductive glass for hydrothermal reaction. The deposited surface of the conductive glass should be placed downward, and a 6 mm × 10 mm unimmersed portion was reserved. The hydrothermal temperature should be set to 99 degrees Celsius, and the time of the hydrothermal reaction should be set to 43 minutes. After taking out the sample, vacuum drying was performed to prepare a cobalt iron oxide passivation layer. Figure 6 This is the X-ray high-resolution photoelectron spectrum of the 2p orbit of zinc element in the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction. The two characteristic peaks of zinc element at 1046.2 electron volts and 1022.8 electron volts are more obvious. Figure 7This is the X-ray high-resolution photoelectron spectrum of the 2p orbital of the iron element of the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction. The two characteristic peaks of the iron element at 724.3 electron volts and 710.8 electron volts are very obvious, and the satellite peaks accompanying the two characteristic peaks are also relatively obvious. The appearance of the characteristic peaks and satellite peaks of zinc and iron elements is consistent with the position of the characteristic peaks and satellite peaks of zinc ferrite in many literatures such as "Jianhua Han, Yayao Lan, Qinggong Song, Huiyu Yan, Jianhai Kang, Yanrui Guo and Zhifeng Liu, Zinc ferrite-based pn homojunction with multi-effect for efficient photoelectrochemical water splitting, Chem. Commun., 2020, 56, 13205", proving that the zinc ferrite film was synthesized in this implementation case. Figure 8 This is the X-ray high-resolution photoelectron spectrum of the 2p orbit of the cobalt element in the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction. The two characteristic peaks of the cobalt element at 797.1 electron volts and 780.9 electron volts are more obvious. In addition, the satellite peaks accompanying the two characteristic peaks of the cobalt element are also more obvious. Fig. 9 This is the X-ray high-resolution photoelectron spectrum of the 1s orbit of oxygen element in the new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction. The characteristic peak of 531.2 electron volts is more obvious. The appearance of the characteristic peak of the interaction between cobalt and oxygen elements confirms the existence of the cobalt iron oxygen passivation layer.

[0041] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field, within the technical scope disclosed by the present invention, can make equivalent replacements or changes based on the technical scheme and inventive concept of the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectrocatalytic anode material, characterized in that: The photoelectrocatalytic photoanode material is prepared by three precise and orderly hydrothermal reactions, and finally passivated, which greatly improves the photocurrent performance of the photoanode material. At the same time, the catalyst has excellent anti-photocorrosion performance and excellent photocurrent stability. The method for manufacturing the carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectric catalyst material comprises the following steps: Step (1): Mix deionized water, sodium tungstate dihydrate, potassium oxalate and carbon powder and stir them evenly, place conductive glass for the first hydrothermal reaction to prepare a carbon-doped tungsten trioxide precursor; take out the sample, wash it with ethanol and deionized water for more than three times respectively and vacuum dry it; sinter the precursor sample to obtain a carbon-doped tungsten trioxide sample, and seal it for storage; Step (2): mixing ferric chloride hexahydrate, sodium nitrate, zinc nitrate hexahydrate, and deionized water, and stirring them uniformly, placing a carbon-doped tungsten trioxide conductive glass sample for a second hydrothermal reaction to obtain a heterojunction precursor, and then drying, sintering, and soaking in sodium hydroxide to obtain a heterojunction, and washing with deionized water and ethanol for more than three times, vacuum drying, and high-temperature sintering; Step (3): Finally, place a heterojunction conductive glass sample, load a cobalt iron oxide passivation layer through the third hydrothermal reaction, wash it with deionized water and ethanol for more than three times and vacuum dry it to obtain a new photoelectric catalyst material of carbon-doped tungsten trioxide and zinc ferrite heterojunction.

2. The carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectrocatalytic anode material according to claim 1, characterized in that: In the step (1), 2.5-4.5 mmol of sodium tungstate dihydrate, 0.4-0.6 mmol of potassium oxalate, 1.2-1.5 mmol of carbon powder and 40-45 ml of deionized water are weighed and placed in a beaker for stirring. The pH value of the solution is adjusted with a 3 mol / L hydrochloric acid solution. The pH value of the solution is adjusted to 0.9-1.

3. After stirring for 6 hours, a uniform hydrothermal reaction solution is obtained. The solution is turbid light green. A conductive glass is placed for hydrothermal reaction. The deposition surface of the conductive glass should be placed downward. The transfer volume of the hydrothermal reaction solution needs to be detected so that the conductive glass is not completely immersed. A 2 mm×10 mm unimmersed portion is reserved. The hydrothermal temperature should be set to 170-190 degrees Celsius. The hydrothermal reaction time should be set to 20-30 hours.

3. The carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectrocatalytic anode material according to claim 1, characterized in that: In the step (2), 4 to 8 mmoles of zinc nitrate hexahydrate, 5 to 10 mmoles of sodium nitrate, and 5 to 10 mmoles of ferric chloride hexahydrate are weighed and mixed with 50 ml of deionized water to dissolve. After stirring for 30 minutes, a uniform hydrothermal reaction solution is prepared, and a carbon-doped tungsten trioxide conductive glass sample is placed in the solution for hydrothermal reaction. The deposited surface of the conductive glass should be placed downward, leaving a 4 mm × 10 mm unsubmerged portion. The temperature of the hydrothermal reaction should be set to 90 to 115 degrees Celsius, and the time of the hydrothermal reaction should be set to 5 to 8 hours.

4. The carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectrocatalytic anode material according to claim 1, characterized in that: In the steps (1) to (3), the drying temperature is 60 degrees Celsius and the vacuum drying time is 2 hours.

5. The carbon-doped tungsten trioxide and zinc ferrite heterojunction photoelectrocatalytic anode material according to any one of claims 3 to 4, characterized in that: The electrolyte solutions used in all sample tests need to be slowly bubbled with nitrogen for 20 to 30 minutes to remove the oxygen content in the electrolyte solution; ice bags need to be placed next to the electrolyte solution or intermittent testing should be performed to prevent the electrolyte solution from being exposed to light for more than 40 minutes, which would cause the temperature to rise and thus avoid inaccurate test results; the accurate test distance needs to be calculated before testing to ensure the standard sunlight intensity of AM 1.5; the light intensity should be checked regularly every week to avoid the weakening of light intensity due to the long-term use of xenon lamps, which would in turn affect the standard sunlight intensity.