A crystal growth device and method with controllable temperature gradient

By setting up a controllable melt and crystal temperature gradient control mechanism in the crystal growth device, the problem of low yield in vertical gradient solidification method and Bridgeman method is solved, and high-quality and high-yield crystal growth is achieved, reducing the number of crystals The cost.

CN115216831BActive Publication Date: 2024-11-15THE 13TH RES INST OF CHINA ELECTRONICS TECH GRP CORP
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202210829102.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-15
Publication Date
2024-11-15
Estimated Expiration
2042-07-15

AI Technical Summary

Technical Problem

The vertical gradient solidification method and the vertical Bridgeman method have low yield problems in crystal growth, which leads to the crystal being prone to twinning and polycrystalline defects and stresses, and high costs.

Method used

A crystal growth device and method with controllable temperature gradient is adopted, including setting a melt temperature gradient control mechanism and a crystal temperature gradient control mechanism in the crucible, and accurately controlling the temperature of the melt and crystal through a lifting rod, a heating plate, and a constant temperature chiller. Gradient ensures stable growth interface.

Benefits of technology

By accurately controlling the temperature gradient, the emergence of twins and polycrystals can be reduced, the yield and quality of the crystals can be improved, stress and dislocation defects can be reduced, and production costs can be reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115216831B_ABST
    Figure CN115216831B_ABST
Patent Text Reader

Abstract

A crystal growth device and method with controllable temperature gradient, relating to the fields of semiconductor, optical crystal and metal crystal preparation, the crystal growth device comprises a crucible and supporting components, a melt temperature gradient control mechanism, and a crystal temperature gradient control mechanism; the melt temperature gradient control mechanism is arranged inside the crucible, comprising a lifting rod and a heating plate; the crystal temperature gradient control mechanism comprises a constant temperature chiller and a cold water circulation pipeline. The growth method comprises gradually increasing the water supply flow of the constant temperature chiller during crystal growth until it increases to 30L / min; raising the melt temperature gradient control mechanism, and the pulling speed is 2-5mm / h. The present invention arranges a movable heating device in the melt, improves the temperature gradient in the melt by accurately controlling the position and temperature of the heating device; passes cooling water with accurate flow and basically constant temperature into the crucible rod to control the temperature gradient at the seed crystal, so as to achieve high-quality and high-yield growth of crystals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor, optical crystal and metal crystal preparation, and in particular to a device and method for preparing high-yield, low-cost and low-stress crystals by using a vertical Bridgman method and a vertical gradient solidification method. Background Art

[0002] The main growth methods used for the preparation of semiconductor and optical crystals are: Czochralski method, vertical gradient solidification method (VGF), vertical Bridgman method (VB), etc.

[0003] The Czochralski method is a more traditional single crystal preparation method, which is characterized by a high growth temperature gradient and a high single crystal yield. However, the crystals prepared by this method have high stress, high density of defects such as dislocations, and are easy to break. The vertical gradient solidification method and the vertical Bridgman method growth method are characterized by a low growth temperature gradient and a small temperature gradient for the prepared crystals. However, since the temperature gradient is too low during growth, it is easy to cause instability of the growth interface, growth of crystal defects such as twins and polycrystals, resulting in a reduction in the yield of the crystals. The cost of crystals prepared by these two growth methods remains high, especially for crystals such as indium phosphide, gallium phosphide, phosphorus germanium zinc, indium antimonide, etc., which are prone to defects such as twins and polycrystals or are easy to break.

[0004] Among all the parameters of crystal growth, the temperature gradient during the growth process has the greatest impact on the quality of the crystal. The temperature gradient in the crystal determines the magnitude of the crystal stress and the level of the dislocation density. The greater the temperature gradient in the crystal, the greater the crystal stress and the higher the dislocation density. The temperature gradient in the melt determines whether the crystal growth interface is unstable, which is especially important for long-sized compound materials and single-element materials containing dopants. The temperature gradient in the melt is small, which can easily cause the components to be overcooled due to the deviation of the components at the front of the solid-liquid interface, thus leading to interface instability and the appearance of twins and polycrystals.

[0005] The traditional way to control the temperature gradient is to set up segmented heaters outside the crucible, and each segment can independently control the heating temperature. However, the fluidity of the melt is very good under high temperature conditions, which leads to very good uniformity, especially in devices with good insulation conditions. The uniformity of temperature caused by thermal convection is easy to maintain. For deep crucibles, there will be a lot of eddies, which may be rotating or circulating in a large direction, making it difficult to establish a temperature gradient. Summary of the invention

[0006] The purpose of the present invention is to solve the problem of low yield of crystal growth by vertical gradient solidification method (VGF) and vertical Bridgman method (VB).

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] A crystal growth device with controllable temperature gradient comprises a crucible, a crucible holder, a crucible rod, heaters I, II and III on the periphery of the crucible and matching thermocouples, a seed crystal groove is arranged at the bottom of the crucible, and the key point is that the growth device also comprises a melt temperature gradient control mechanism and a crystal temperature gradient control mechanism.

[0009] The melt temperature gradient control mechanism is arranged inside the crucible, and comprises a lifting rod, a heating plate connected to the lifting rod, and a heating wire and a thermocouple IV are built in the heating plate.

[0010] The crystal temperature gradient control mechanism comprises a constant temperature water chiller and a cold water circulation pipeline connected to the constant temperature water chiller, wherein the cold water circulation pipeline is close to the bottom of the seed crystal tank.

[0011] Furthermore, the heating plate is a downwardly concave arc surface.

[0012] Furthermore, the cold water circulation pipeline includes an outlet pipe and a return pipe connected to a constant temperature water chiller, the crucible rod is a hollow tube, the outlet pipe enters the crucible rod and extends to the top of the crucible rod, and the return pipe connects the crucible rod and the constant temperature water chiller.

[0013] Based on the above device, the present invention also proposes a crystal growth method with controllable temperature gradient, the growth method comprising the following steps:

[0014] Step 1: Use deionized water to clean the material to ensure that the surface of the material is free of contamination;

[0015] Step 2, placing the seed crystal into the seed crystal slot at the bottom of the crucible;

[0016] Step 3, lowering the melt temperature gradient control mechanism to the bottom of the crucible;

[0017] Step 4: Load the material into the crucible;

[0018] Step 5: Turn on the constant temperature chiller and set the chiller flow rate to 10L / min;

[0019] Step 6, turn on heater I, heater II, and heater III, and set the temperatures to be 30°C, 20°C, and 10°C higher than the melting point of the material, respectively;

[0020] Step 7, turn on the heating wire so that the temperature of thermocouple IV reaches 3-15°C above the melting point of the material;

[0021] Step 8: Maintain the temperature for 30-60 minutes to ensure that all the materials in the crucible are melted;

[0022] Step 9, reduce the power of heater I, heater II, and heater III, and set the temperature to be 20°C, 10°C, and 5°C higher than the melting point of the material respectively;

[0023] Step 10, gradually increase the water flow rate of the constant temperature chiller until it increases to 30L / min, and the water flow rate increase rate is 0.1L / min;

[0024] Step 11, the melt temperature gradient control mechanism is raised, and the pulling speed is 2-5 mm / h; the cooling rate of heater I, heater II, and heater III is set to 1-3°C / h;

[0025] Step 12, the melt temperature gradient control mechanism leaves the melt, and the crystal growth ends;

[0026] Step 13: Heater I, heater II, and heater III are cooled at a rate of 100°C / h to complete the cooling of the crystal.

[0027] Furthermore, in step 11, the distance between the heating plate and the solid-liquid interface is maintained at 5-15 mm.

[0028] The present invention adds a melt temperature gradient control mechanism and a crystal temperature gradient control mechanism in the device, and achieves the purpose of the invention through precise control.

[0029] Beneficial effects: The present invention sets a movable heating device in the melt, improves the temperature gradient in the melt by precisely controlling the position and temperature of the heating device, stabilizes the crystal growth interface, and reduces the probability of twins and polycrystals; cooling water with precise flow and basically constant temperature is introduced into the crucible rod, and the temperature gradient at the seed crystal can be controlled by adjusting the water flow. The precise control of the temperature gradient in the melt and at the seed crystal enables the growth of high-quality and high-yield crystals. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the device composition diagram after loading is completed.

[0031] Figure 2 This is the device status diagram after the material is completely melted.

[0032] Figure 3 is the device state diagram during the crystal growth process,

[0033] Figure 4 is a schematic diagram of the melt temperature gradient control mechanism.

[0034] Figure 5 The figure is a comparison of the temperature gradient curves at the solid-liquid interface front when synthesizing indium phosphide by the present invention and the traditional method.

[0035] Among them: 1 is thermocouple I, 2 is thermocouple II, 3 is thermocouple III, 4 is heater I, 5 is heater II, 6 is heater III, 7 is crucible, 8 is seed crystal slot, 9 is material, 10 is seed crystal, 11 is return pipe, 12 is crucible rod, 13 is cooling water, 14 is outlet pipe, 15 is thermocouple IV, 16 is lifting rod, 17 is heating wire, 18 is constant temperature chiller, 19 is growing crystal, and 20 is crucible support. DETAILED DESCRIPTION

[0036] A crystal growth device with controllable temperature gradient, see Figure 1 , including a crucible 7, a crucible support 20, a crucible rod 12, heaters Ⅰ4, Ⅱ5, and Ⅲ6 on the periphery of the crucible, and matching thermocouples Ⅰ1, Ⅱ2, and Ⅲ3; a seed crystal groove 8 is arranged at the bottom of the crucible 7.

[0037] The heater and thermocouple are a coupled control pair, and the power of the corresponding heater is adjusted by the thermocouple test temperature.

[0038] The crucible 7 is made of materials such as quartz and boron nitride and is used to place seed crystals, crystals, melts and covering agents.

[0039] The crucible support is made of alumina insulation cotton, carbon felt and other materials, which can keep the bottom of the crucible and the seed crystal warm.

[0040] The growth device also includes a melt temperature gradient control mechanism and a crystal temperature gradient control mechanism.

[0041] The melt temperature gradient control mechanism is arranged inside the crucible 7, including a lifting rod 16 and a heating plate connected to the lifting rod 16, which is made of quartz or boron nitride material; the heating plate has a built-in heating wire 17 and a thermocouple IV 15, such as Figure 4 shown.

[0042] The heating plate is circular when viewed from below. Figure 4 As shown, the diameter is close to the inner diameter of the crucible 7; the heating plate is a downwardly concave arc surface, and the shape is similar to the expected shape of the crystal solid-liquid interface.

[0043] The heating wire 17 and the thermocouple IV 15 are a coupling control pair. The power of the corresponding heating wire is adjusted by the thermocouple test temperature so that the thermocouple reaches the preset temperature. The lifting rod 16 is connected to the driving device (not shown in the figure) to enable the heating plate to move up and down at a speed of 1-50mm / h, and the speed is adjustable.

[0044] The crystal temperature gradient control mechanism includes a constant temperature water chiller 18 and a cold water circulation pipeline connected to the constant temperature water chiller 18. The cold water circulation pipeline is close to the bottom of the seed crystal groove 8, with a distance of 3-10 mm.

[0045] The constant temperature chiller 18 provides cold water at 14-17°C, with a water temperature control accuracy of ±0.5°C, a maximum water flow rate of 100L / min, an adjustable flow rate in the range of 10-100L / min, and a flow control accuracy of ±0.1L / min.

[0046] The cold water circulation pipeline includes an outlet pipe 14 and a return pipe 11 connected to a constant temperature water chiller 18. The crucible rod 12 is a part of the cold water circulation pipeline and is a hollow pipe. The outlet pipe 14 enters the crucible rod 12 and extends to the top of the crucible rod 12. The return pipe 11 connects the crucible rod 12 and the constant temperature water chiller 18.

[0047] During operation, cooling water 13 is pumped out from the constant temperature water chiller 18, enters the crucible rod 12 through the water outlet pipe 14 and reaches the top of the crucible rod 12, and then flows into the constant temperature water chiller 18 through the return pipe 11 from the middle position between the crucible rod 12 and the water outlet pipe 14.

[0048] The water outlet pipe 14 and the water return pipe 11 are made of stainless steel and covered with heat-insulating materials, and the inner diameter of the pipe is 10-20 mm.

[0049] The distance between the top end of the hollow part of the crucible rod 12 and the seed crystal groove 8 is 3-10 mm.

[0050] Based on the above device, the present invention also proposes a crystal growth method with controllable temperature gradient, the growth method comprising the following steps:

[0051] Step 1: Use deionized water to clean the material 9 to ensure that the surface of the material 9 is free of contamination.

[0052] The material 9 here is a semiconductor compound, such as indium phosphide, gallium phosphide, phospho-zinc-germanium, indium antimonide, and the like.

[0053] Step 2: Place the seed crystal 10 into the seed crystal groove 8 at the bottom of the crucible.

[0054] Step 3: The lifting rod 16 is driven by the driving device to lower the melt temperature gradient control mechanism to the bottom of the crucible 7.

[0055] Step 4: Load the material 9 into the crucible 7.

[0056] Step 5: Turn on the constant temperature water chiller 18, and set the flow rate of the water chiller to 10 L / min.

[0057] At this time, the status of the device is Figure 1 shown.

[0058] Step 6: Turn on heater I4, heater II5 and heater III6, and set the temperatures to be 30°C, 20°C and 10°C higher than the melting point of material 9 respectively.

[0059] Step 7: Turn on the heating wire 17 so that the temperature of the thermocouple IV 15 reaches 3-15° C. above the melting point of the material 9.

[0060] Step 8: When the temperatures displayed by thermocouple Ⅰ1, thermocouple Ⅱ2 and thermocouple Ⅲ3 reach the set temperatures respectively, keep the temperature constant for 30-60 minutes to ensure that all the material 9 in the crucible 7 is melted.

[0061] At this time, the status of the device is Figure 2 shown.

[0062] Step 9, reduce the power of heater Ⅰ4, heater Ⅱ5, and heater Ⅲ6, and set the temperature to be 20°C, 10°C, and 5°C higher than the melting point of material 9 respectively. At this time, it can still ensure that the melt remains in a molten state.

[0063] Step 10: Gradually increase the water supply flow of the constant temperature chiller until it increases to 30 L / min, and the water flow increase rate is 0.1 L / min to meet the requirements for latent heat release of crystallization.

[0064] At this time, the melt 9 near the seed crystal 10 begins to adhere to the seed crystal 10 and solidify according to the seed crystal lattice arrangement.

[0065] Step 11: The melt temperature gradient control mechanism is raised, and the pulling speed is 2-5 mm / h. The cooling rate of heater I4, heater II5, and heater III6 is set to 1-3°C / h, so that the melt is gradually solidified.

[0066] The pulling speed determines the growth rate of the crystal 19 to a certain extent, and can increase the temperature gradient in the melt at the solid-liquid interface front, ensuring that the melt thickness at the interface front is at a low value (generally, the temperature gradient control mechanism is required to be 5-15mm away from the solid-liquid interface), thereby ensuring the stability of crystal growth. The temperature gradient in the melt can be easily controlled and data obtained, temperature gradient = (control unit thermocouple temperature - material melting point) / distance between the solid-liquid interface and the temperature gradient control unit. In the traditional method of controlling the temperature gradient, the heater is outside the crucible, and the temperature gradient of the melt is difficult to control and obtain actual gradient data.

[0067] The solid-liquid interface refers to the contact surface between the upper surface of the crystal 19 (solid) and the melt, and is the interface for crystal growth.

[0068] During the growth of the crystal 19, while pulling, the distance between the heating plate and the solid-liquid interface is ensured to be maintained at 5-15 mm.

[0069] In existing crystal growth technology, especially for relatively deep melts, due to the temperature differences and composition differences in various parts of the melt, strong turbulence is often caused. The turbulence may be rotating or may circulate in the entire melt. The existence of turbulence makes it difficult to control the temperature gradient. In addition, the heater that controls the temperature gradient at the far end often heats and controls the melt through the atmosphere and the crucible. The control process is not direct enough and the control effect is poor. In addition, the complex convection in the deeper melt makes gradient control even more difficult. In addition, in the existing growth technology, as the crystal grows, the solid-liquid interface gradually advances toward the melt, and the effect of the surrounding fixed heaters on it also changes accordingly, and the temperature gradient control effect has a large uncertainty.

[0070] In this embodiment, there is a very narrow gap between the heating plate and the solid-liquid interface, which limits the range of turbulence in space, and the temperature control unit is close to the growth interface, and has a very strong control ability over the solid-liquid interface, so the temperature gradient is easier to maintain and control than the prior art. In addition, in the process of the solid-liquid interface advancing toward the melt, the distance between the solid-liquid interface and the temperature control unit can be kept unchanged, thereby ensuring the stability of the temperature gradient control effect during the entire crystal growth period. At the same time, during the crystal growth process, the heater outside the crucible is cooled synchronously with the rise of the heating plate (1-3°C / h), which also ensures the control of the temperature gradient.

[0071] See also Figure 5 Taking the synthesis of indium phosphide as an example, the temperature of the solid-liquid interface (the position where the horizontal axis is 0) is the melting point of indium phosphide (1062°C). Using the traditional method, assuming that heating is also performed at the same position and the same temperature, since the heater is set outside the crucible, the temperature change at different positions is not large, and the temperature gradient is not obvious; using the device and method of the present invention, a basically linear temperature gradient is established between the heating plate and the solid-liquid interface (in this embodiment, the heating plate is 9mm away from the solid-liquid interface and the temperature is set to 11°C).

[0072] In the figure, the curve using the traditional method is an ideal situation: the external heater is located at the solid-liquid interface. In actual operation, there are usually several external heaters, and they are in fixed positions. It is difficult to achieve precise position control throughout the crystal growth process.

[0073] If the external heater is below the solid-liquid interface, increasing the heater temperature will heat the crystal at the same time, causing crystal regeneration; if it is above the solid-liquid interface, it is easy to increase the stirring effect of the melt due to buoyancy convection (the hot melt has a low density and naturally floats up), making the temperature field chaotic and difficult to establish a gradient; if it is above the melt, it is often difficult to control the temperature because it is too far away, and there is often an atmosphere space above the melt, making it difficult to heat the melt through the atmosphere.

[0074] At this time, the status of the device is Figure 3 shown.

[0075] Step 12: The melt temperature gradient control mechanism leaves the melt, the melt is completely solidified, and the crystal growth ends.

[0076] Step 13, heater I4, heater II5, and heater III6 are cooled at a rate of 100°C / h to complete the cooling of the crystal.

[0077] After cooling, the crystal 19 is taken out.

[0078] For volatile materials, such as indium phosphide, in step 4, a covering agent with a density lower than that of the material and which does not contaminate the material may be loaded, typically boron oxide (not shown in the figure).

[0079] The method of the present invention is used to grow SI-type indium phosphide crystals, which significantly improves the yield rate of the crystals, and the grown crystals have lower stress and dislocation defects, which has a very good effect on improving the yield rate of the crystals. The specific comparison is shown in the following table.

[0080]

Claims

1. A method for crystal growth with controllable temperature gradient, which is implemented based on a crystal growth device with controllable temperature gradient, the device comprising a crucible (7), a crucible support (20), a crucible rod (12), a heater I (4), a heater II (5), a heater III (6) and a matching thermocouple on the periphery of the crucible, a seed crystal groove (8) being arranged at the bottom of the crucible (7), characterized in that: The heater I (4), heater II (5), and heater III (6) are arranged from top to bottom along the periphery of the crucible, and the growth device also includes a melt temperature gradient control mechanism and a crystal temperature gradient control mechanism; The melt temperature gradient control mechanism is arranged inside the crucible (7), and comprises a lifting rod (16), a heating plate connected to the lifting rod (16), the heating plate having a built-in heating wire (17) and a thermocouple IV (15), and the heating plate presents a downwardly concave arc surface; The crystal temperature gradient control mechanism comprises a constant temperature water chiller (18) and a cold water circulation pipeline connected to the constant temperature water chiller (18), wherein the cold water circulation pipeline is close to the bottom of the seed crystal tank (8); The growth method comprises the following steps: Step 1: Clean the material (9) with deionized water to ensure that the surface of the material (9) is free of contamination; Step 2, placing the seed crystal (10) into the seed crystal groove (8) at the bottom of the crucible; Step 3, lowering the melt temperature gradient control mechanism to the bottom of the crucible (7); Step 4, loading the material (9) into the crucible (7); Step 5: Turn on the constant temperature water chiller (18), and set the flow rate of the water chiller to 10 L / min; Step 6, turn on heater I (4), heater II (5), and heater III (6), and set the temperatures to be 30°C, 20°C, and 10°C higher than the melting point of the material (9), respectively; Step 7, turning on the heating wire (17) so that the temperature of the thermocouple IV (15) reaches 3-15°C above the melting point of the material (9); Step 8, maintaining the temperature for 30-60 minutes to ensure that the material (9) in the crucible (7) is completely melted; Step 9, reduce the power of heater I (4), heater II (5), and heater III (6), and set the temperature to be 20°C, 10°C, and 5°C higher than the melting point of material (9), respectively; Step 10, gradually increase the water flow rate of the constant temperature chiller until it increases to 30L / min, and the water flow rate increase rate is 0.1L / min; Step 11, the melt temperature gradient control mechanism is raised, and the pulling speed is 2-5 mm / h; the cooling rate of heater I (4), heater II (5), and heater III (6) is set to 1-3°C / h; the distance between the heating plate and the solid-liquid interface is maintained at 5-15 mm; Step 12, the melt temperature gradient control mechanism leaves the melt, and the crystal growth ends; Step 13: Heater I (4), heater II (5), and heater III (6) are cooled at a rate of 100°C / h to complete the cooling of the crystal.

2. The crystal growth method according to claim 1, characterized in that The cold water circulation pipeline comprises a water outlet pipe (14) and a water return pipe (11) connected to a constant temperature water chiller (18); the crucible rod (12) is a hollow tube; the water outlet pipe (14) enters the crucible rod (12) and extends to the top of the crucible rod (12); and the water return pipe (11) connects the crucible rod (12) and the constant temperature water chiller (18).

3. The crystal growth method according to claim 2, characterized in that: The constant temperature chiller (18) provides cold water at 14-17°C, with a water temperature control accuracy of ±0.5°C, a maximum water flow rate of 100L / min, an adjustable flow rate in the range of 10-100L / min, and a flow control accuracy of ±0.1L / min.

4. The crystal growth method according to claim 2, characterized in that: The water outlet pipe (14) and the water return pipe (11) are made of stainless steel and covered with heat-insulating material, and the inner diameter of the pipe is 10-20 mm.

5. The crystal growth method according to claim 2, characterized in that: The distance between the top end of the hollow part of the crucible rod (12) and the seed crystal groove (8) is 3-10 mm.

6. The crystal growth method with controllable temperature gradient according to claim 1, characterized in that: Step 4: Load the material (9) and the covering agent into the crucible (7).

Citation Information

Patent Citations

  • Device for growing large-size and high-temperature crystals with real-time adjustable temperature gradient method and method

    CN102766901A

  • Growth method of large-size zinc germanium phosphide crystal for increasing heat transfer

    CN110042461A

  • Low-stress crystal growth method

    CN112746312A

  • GaAs single crystal growth equipment and GaAs single crystal growth process

    CN114686963A

  • Growth apparatus for large-areaed crystal by temperature gradient technique and crystal growth method thereof

    CN1485467A