Preparation method of modified calcium hydroxide sulfur-fixing material and application of modified calcium hydroxide sulfur-fixing material in adsorbing sulfur trioxide in flue gas
By adding sodium hydroxide or sodium carbonate to calcium hydroxide to form a modified calcium hydroxide sulfur-fixing material, the problem of low efficiency of calcium hydroxide absorbing sulfur trioxide is solved, and the effect of efficient absorption of sulfur trioxide in flue gas is achieved. , and the process is simple and economical.
Patent Information
- Application Number
- CN202210944961.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-08-08
AI Technical Summary
The existing calcium hydroxide is not efficient in absorbing sulfur trioxide, making it difficult to effectively deal with sulfur trioxide pollution emitted by coal-fired power plants.
By adding a certain proportion of sodium hydroxide or sodium carbonate to calcium hydroxide, a sintered modified or impregnated modified calcium hydroxide sulfur-fixing material is formed, forming a network structure or increasing the specific surface area, and improving its absorption of sulfur trioxide ability.
The efficiency of calcium hydroxide absorbs sulfur trioxide is significantly improved, and the efficiency of absorbing sulfur trioxide in flue gas is achieved. The process is simple, the raw materials are easy to obtain, and the price is low.
Smart Images

Figure CN115228280B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adsorption materials, and in particular relates to a method for preparing a modified calcium hydroxide sulfur-fixing material for sulfur trioxide in flue gas. Background Art
[0002] Sulfur trioxide has serious harm to human health, environmental quality, and safe operation of power plants. The harm of sulfur trioxide to the human body is mainly reflected in the following aspects: sulfur trioxide is highly irritating and corrosive. After sulfur trioxide is discharged into the atmosphere through the chimney of a power plant, it will naturally settle and gradually enter the lower atmosphere. It will enter the human body through the respiratory system. After entering the human body, sulfur trioxide will easily combine with the water in the human body to form sulfuric acid, which will stick to the respiratory tract, causing the pH of the human respiratory tract to decrease. In severe cases, it will corrode the respiratory tract and affect the normal lung function of the human body. Therefore, the prevention and control of sulfur trioxide is very important.
[0003] SO3 not only causes great environmental pollution but also affects the normal operation of power plants. In order to respond to the development concept of ecological civilization and green mountains and clear waters, how to reduce the emission of pollutants from coal-fired power plants, especially the treatment of sulfur trioxide, has become the focus of research by scholars at home and abroad. There is an urgent need for efficient and affordable absorbents to treat sulfur trioxide produced by coal combustion.
[0004] Traditional calcium-based adsorbent calcium hydroxide has the advantages of being widely distributed in nature, having many ways to obtain it, and being affordable, but its efficiency in absorbing sulfur trioxide is not high. Summary of the invention
[0005] The purpose of the present invention is to solve the problem that the existing calcium hydroxide has low efficiency in absorbing sulfur trioxide, and to provide a preparation method of a modified calcium hydroxide sulfur-fixing material and its application in absorbing sulfur trioxide in flue gas.
[0006] The preparation method of the sintered modified calcium hydroxide sulfur-fixing material of the present invention is achieved by the following steps:
[0007] 1. Grinding the solid materials of calcium hydroxide and sodium hydroxide respectively, and obtaining calcium hydroxide powder and sodium hydroxide powder after sieving;
[0008] 2. Adding sodium hydroxide powder to the calcium hydroxide powder, wherein the sodium hydroxide powder accounts for 1.5wt% to 5wt% of the calcium hydroxide powder, and stirring and mixing the mixture to obtain a mixed powder;
[0009] 3. Put the mixed powder obtained in step 2 into a muffle furnace and calcine it at a temperature of 550°C to 650°C. After calcination, cool it to room temperature under closed conditions to obtain a sintered modified calcium hydroxide sulfur-fixing material.
[0010] The preparation method of the sintered modified calcium hydroxide sulfur-fixing material of the present invention is to add a certain proportion of sodium hydroxide additive, so that a network structure beneficial to the absorption of sulfur trioxide can be formed in the sulfur-fixing process, and the sodium ions can slow down the decomposition of the product after the absorption reaction, thereby improving the effect of the calcium hydroxide absorbent in absorbing sulfur trioxide.
[0011] The preparation method of the impregnated modified calcium hydroxide sulfur-fixing material of the present invention is achieved by the following steps:
[0012] 1. Grinding the solid materials of calcium hydroxide and sodium carbonate respectively, and obtaining calcium hydroxide powder and sodium carbonate powder after sieving;
[0013] 2. Adding sodium carbonate powder to calcium hydroxide powder, wherein the sodium carbonate powder accounts for 1.5wt% to 5wt% of the calcium hydroxide powder, stirring and mixing uniformly to obtain a mixed powder, and stirring and mixing the mixed powder and deionized water uniformly to obtain a mixed solution;
[0014] 3. Evaporating the water in the mixed solution at a temperature of 110°C to 120°C, and collecting the solid phase mixed material after drying;
[0015] Fourth, the solid phase mixed material is calcined at 450° C. to 550° C., and cooled to room temperature in a closed environment to obtain an impregnated modified calcium hydroxide sulfur-fixing material.
[0016] The application of the modified calcium hydroxide sulfur-fixing material of the present invention is to use the sintered modified calcium hydroxide sulfur-fixing material or the impregnated modified calcium hydroxide sulfur-fixing material as an adsorbent to adsorb sulfur trioxide in flue gas.
[0017] The preparation method of the impregnated modified calcium hydroxide sulfur-fixing material of the present invention is to add a certain proportion of sodium carbonate additive to change the surface structure of calcium hydroxide, increase its specific surface area, and rearrange the molecular structure of calcium hydroxide to generate holes that are conducive to the adsorption of sulfur trioxide, thereby improving the effect of the calcium hydroxide absorbent in absorbing sulfur trioxide.
[0018] The preparation methods of the two modified calcium hydroxide sulfur-fixing materials of the invention are simple and reliable, the raw materials are easily available, the price is low, and the efficiency of absorbing sulfur trioxide in flue gas is relatively high. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a comparison chart of the effects of modified calcium hydroxide sulfur-fixing material prepared in Example 1 and modified calcium hydroxide materials prepared in Comparative Examples 2-5 on absorbing sulfur trioxide under the same experimental conditions;
[0020] Figure 2 This is a comparison chart of the effects of modified calcium hydroxide prepared in Example 2 and modified calcium hydroxide prepared in Comparative Examples 6-9 on absorbing sulfur trioxide under the same experimental conditions. DETAILED DESCRIPTION
[0021] Specific implementation method 1: The preparation method of the sintered modified calcium hydroxide sulfur-fixing material in this implementation method is achieved by the following steps:
[0022] 1. Grinding the solid materials of calcium hydroxide and sodium hydroxide respectively, and obtaining calcium hydroxide powder and sodium hydroxide powder after sieving;
[0023] 2. Adding sodium hydroxide powder to the calcium hydroxide powder, wherein the sodium hydroxide powder accounts for 1.5wt% to 5wt% of the calcium hydroxide powder, and stirring and mixing the mixture to obtain a mixed powder;
[0024] 3. Put the mixed powder obtained in step 2 into a muffle furnace and calcine it at a temperature of 550°C to 650°C. After calcination, cool it to room temperature under closed conditions to obtain a sintered modified calcium hydroxide sulfur-fixing material.
[0025] In this embodiment, a certain proportion of additives are added to calcium hydroxide to modify it so that it can efficiently absorb sulfur trioxide, thereby improving the absorption efficiency of sulfur trioxide.
[0026] Specific implementation method 2: This implementation method is different from the specific implementation method 1 in that in step 1, the powder is sieved through a 300-mesh screen after grinding.
[0027] Specific embodiment 3: This embodiment is different from specific embodiment 1 or 2 in that in step 2, the sodium hydroxide powder accounts for 2wt% of the calcium hydroxide powder.
[0028] Specific implementation method 4: This implementation method is different from any one of specific implementation methods 1 to 3 in that in step 3, the calcination treatment is performed at a temperature of 600° C. for 0.5 h.
[0029] Specific implementation method 5: The preparation method of the impregnated modified calcium hydroxide sulfur-fixing material in this implementation method is implemented according to the following steps:
[0030] 1. Grinding the solid materials of calcium hydroxide and sodium carbonate respectively, and obtaining calcium hydroxide powder and sodium carbonate powder after sieving;
[0031] 2. Adding sodium carbonate powder to calcium hydroxide powder, wherein the sodium carbonate powder accounts for 1.5wt% to 5wt% of the calcium hydroxide powder, stirring and mixing uniformly to obtain a mixed powder, and stirring and mixing the mixed powder and deionized water uniformly to obtain a mixed solution;
[0032] 3. Evaporating the water in the mixed solution at a temperature of 110°C to 120°C, and collecting the solid phase mixed material after drying;
[0033] Fourth, the solid phase mixed material is calcined at 450° C. to 550° C., and cooled to room temperature in a closed environment to obtain an impregnated modified calcium hydroxide sulfur-fixing material.
[0034] Specific implementation method 6: This implementation method is different from specific implementation method 5 in that in step 1, the powder is sieved through a 300-mesh screen after grinding.
[0035] Specific embodiment 7: The difference between this embodiment and specific embodiment 5 or 6 is that in step 2, the sodium carbonate powder accounts for 2wt% of the calcium hydroxide powder.
[0036] Specific embodiment eight: This embodiment differs from any one of specific embodiments five to seven in that in step two, 25 to 35 g of mixed powder is stirred and mixed evenly with 90 to 110 mL of deionized water.
[0037] Specific embodiment 9: This embodiment is different from any one of specific embodiments 5 to 8 in that in step 3, the water in the mixed liquid is evaporated at a temperature of 110°C.
[0038] Specific embodiment ten: This embodiment is different from any one of specific embodiments five to nine in that in step four, the solid phase mixed material is calcined at 500° C. for 2 hours.
[0039] Example 1: The preparation method of the sintered modified calcium hydroxide sulfur-fixing material of this example is implemented according to the following steps:
[0040] 1. Grind the solid materials of calcium hydroxide and sodium hydroxide respectively, and obtain calcium hydroxide powder and sodium hydroxide powder after passing through a 300-mesh sieve;
[0041] 2. Adding sodium hydroxide powder to the calcium hydroxide powder, wherein the sodium hydroxide powder accounts for 2.0wt% of the calcium hydroxide powder, and stirring and mixing uniformly to obtain a mixed powder;
[0042] 3. Put the mixed powder obtained in step 2 into a muffle furnace and calcine it at 600° C. for 0.5 h. After calcination, cool it to room temperature under closed conditions to obtain a sintered modified calcium hydroxide sulfur-fixing material.
[0043] The absorption test experiment of sulfur trioxide by the sintered modified calcium hydroxide sulfur-fixing material in this embodiment is as follows:
[0044] (1) SO3 production: About 4 L / min of O2 was introduced into the ozone generator to generate O3. A glass rotor flowmeter was used to set 50 mL / min of O3 and 70 mL / min of SO2 to be introduced into a three-necked flask. SO3 was generated by reaction at 80°C, and the SO3 content generated was measured at the outlet.
[0045] (2) Flue gas composition simulation: The SO3 content generated was measured and a flue gas flow rate of 1 L / min was simulated. The generated SO3 was introduced into a four-necked flask. NH3, N2, SO2, NO and O2 were introduced into the four-necked flask through a dynamic gas distribution cabinet. N2 was introduced into a conical flask filled with 80°C deionized water, and then introduced into the four-necked flask using N2 to carry water mist. All the gases introduced were fully mixed in the four-necked flask at 70°C, and the sulfuric acid mist content generated by the simulated flue gas at the outlet was measured.
[0046] (3) SO3 absorption: 10 g of modified calcium hydroxide sulfur-fixing material was added to a U-shaped tube, which was connected to the outlet of a four-necked flask. The modified material was absorbed in the U-shaped tube, and the remaining SO3 was absorbed with isopropanol at the outlet.
[0047] (4) Determination of residual SO3 content: The absorbance is determined by thorium reagent spectrophotometry and the residual SO3 concentration is calculated. The removal rate is calculated by calculating the difference between the residual amount and the initial amount.
[0048] The absorption (efficiency) of sulfur trioxide by the sintered modified calcium hydroxide sulfur-fixing material obtained in this embodiment is 85.61%.
[0049] Comparative Example 2: This embodiment differs from Example 1 in that the sodium hydroxide powder in step 2 accounts for 5.0wt% of the calcium hydroxide powder.
[0050] The absorption efficiency of the sintered modified calcium hydroxide sulfur-fixing material for sulfur trioxide obtained in this embodiment is 76.02%.
[0051] Comparative Example 3: This embodiment is different from Example 1 in that the sodium hydroxide powder in step 2 accounts for 8.0wt% of the calcium hydroxide powder.
[0052] The absorption efficiency of the sintered modified calcium hydroxide sulfur-fixing material for sulfur trioxide obtained in this embodiment is 68.82%.
[0053] Comparative Example 4: The preparation method of the sintered modified calcium hydroxide sulfur-fixing material of this embodiment is implemented according to the following steps:
[0054] 1. Grind the barium chloride and calcium hydroxide solid materials respectively, and obtain calcium hydroxide powder and sodium hydroxide powder after passing through a 300-mesh sieve;
[0055] 2. Add barium chloride powder to calcium hydroxide powder, wherein the barium chloride powder accounts for 2.0wt% of the calcium hydroxide powder, and stir to mix evenly to obtain a mixed powder;
[0056] 3. Put the mixed powder obtained in step 2 into a muffle furnace and calcine it at 600° C. for 0.5 h. After calcination, cool it to room temperature under closed conditions to obtain a sintered modified calcium hydroxide sulfur-fixing material.
[0057] The absorption efficiency of the sintered modified calcium hydroxide sulfur-fixing material for sulfur trioxide obtained in this example is 40.05%.
[0058] Comparative Example 5: The preparation method of the sintered modified calcium hydroxide sulfur-fixing material of this embodiment is implemented according to the following steps:
[0059] 1. Grind the zinc oxide and calcium hydroxide solid materials respectively, and obtain calcium hydroxide powder and sodium hydroxide powder after passing through a 300-mesh sieve;
[0060] 2. Add zinc oxide powder to calcium hydroxide powder, wherein the zinc oxide powder accounts for 2.0wt% of the calcium hydroxide powder, and stir and mix evenly to obtain a mixed powder;
[0061] 3. Put the mixed powder obtained in step 2 into a muffle furnace and calcine it at 600° C. for 0.5 h. After calcination, cool it to room temperature under closed conditions to obtain a sintered modified calcium hydroxide sulfur-fixing material.
[0062] The absorption efficiency of the sintered modified calcium hydroxide sulfur-fixing material for sulfur trioxide obtained in this embodiment is 56.89%.
[0063] Calcium hydroxide is widely present in nature. As a raw calcium-based material, it has the advantages of easy availability and low price. However, its efficiency in absorbing sulfur trioxide in flue gas is not high, so it needs to be modified to improve its absorption efficiency of sulfur trioxide.
[0064] The alkali-modified calcium hydroxide prepared by sintering and doping with 2 wt % sodium hydroxide in Example 1 can absorb sulfur dioxide in flue gas very well. Sodium ions make the product after absorption difficult to decompose and change the structure of calcium hydroxide, so that it can better absorb sulfur dioxide in flue gas.
[0065] Example 2: The preparation method of the impregnated modified calcium hydroxide sulfur-fixing material of this example is implemented according to the following steps:
[0066] 1. Grinding the solid materials of calcium hydroxide and sodium carbonate respectively, and obtaining calcium hydroxide powder and sodium carbonate powder after sieving;
[0067] 2. Add sodium carbonate powder to the calcium hydroxide powder, wherein the sodium carbonate powder accounts for 2wt% of the calcium hydroxide powder, and stir and mix uniformly to obtain a mixed powder. Stir and mix 30g of the mixed powder with 100mL of deionized water to obtain a mixed solution.
[0068] 3. Evaporate the water in the mixed solution at a temperature of 110° C. in an electric blast drying oven, and collect the solid phase mixed material after drying for 12 hours;
[0069] 4. The solid phase mixed material is calcined at 500° C. for 2 h in a box-type resistance furnace, and cooled to room temperature in a closed environment to obtain an impregnated modified calcium hydroxide sulfur-fixing material.
[0070] The absorption efficiency of the impregnated modified calcium hydroxide sulfur-fixing material for sulfur trioxide obtained in this embodiment is 91.85%.
[0071] Comparative Example 6: This embodiment is different from Example 2 in that sodium carbonate powder is added to the calcium hydroxide powder, and the sodium carbonate powder accounts for 5wt% of the calcium hydroxide powder.
[0072] The absorption efficiency of the impregnated modified calcium hydroxide sulfur-fixing material for sulfur trioxide obtained in this embodiment is 75.54%.
[0073] Comparative Example 7: This embodiment is different from Example 2 in that sodium carbonate powder is added to the calcium hydroxide powder, and the sodium carbonate powder accounts for 8wt% of the calcium hydroxide powder.
[0074] The absorption efficiency of the impregnated modified calcium hydroxide sulfur-fixing material for sulfur trioxide obtained in this embodiment is 71.70%.
[0075] Comparative Example 8: The preparation method of the impregnated modified calcium hydroxide sulfur-fixing material of this embodiment is implemented according to the following steps:
[0076] 1. Grinding calcium hydroxide and potassium hydroxide solid materials respectively, and obtaining calcium hydroxide powder and potassium hydroxide powder after sieving;
[0077] 2. Add potassium hydroxide powder to calcium hydroxide powder, the potassium hydroxide powder accounts for 2wt% of calcium hydroxide powder, stir and mix evenly to obtain a mixed powder, stir and mix 30g of the mixed powder with 100mL of deionized water to obtain a mixed solution;
[0078] 3. Evaporate the water in the mixed solution at a temperature of 110° C. in an electric blast drying oven, and collect the solid phase mixed material after drying for 12 hours;
[0079] 4. The solid phase mixed material is calcined at 500° C. for 2 h in a box-type resistance furnace, and cooled to room temperature in a closed environment to obtain an impregnated modified calcium hydroxide sulfur-fixing material.
[0080] The absorption efficiency of the impregnated modified calcium hydroxide sulfur-fixing material for sulfur trioxide obtained in this embodiment is 72.66%.
[0081] Comparative Example 9: The preparation method of the impregnated modified calcium hydroxide sulfur-fixing material of this embodiment is implemented according to the following steps:
[0082] 1. Grinding calcium hydroxide and sodium chloride solid materials respectively, and obtaining calcium hydroxide powder and sodium chloride powder after sieving;
[0083] 2. Add sodium chloride powder to the calcium hydroxide powder, wherein the sodium chloride powder accounts for 2wt% of the calcium hydroxide powder, and stir and mix uniformly to obtain a mixed powder. Stir and mix 30g of the mixed powder with 100mL of deionized water to obtain a mixed solution.
[0084] 3. Evaporate the water in the mixed solution at a temperature of 110° C. in an electric blast drying oven, and collect the solid phase mixed material after drying for 12 hours;
[0085] 4. The solid phase mixed material is calcined at 500° C. for 2 h in a box-type resistance furnace, and cooled to room temperature in a closed environment to obtain an impregnated modified calcium hydroxide sulfur-fixing material.
[0086] The absorption efficiency of sulfur trioxide by the impregnated modified calcium hydroxide sulfur-fixing material obtained in this embodiment is 66.91%.
[0087] The alkali-modified calcium hydroxide prepared by the impregnation method with 2 wt% sodium carbonate doped in Example 2 can absorb sulfur dioxide in flue gas very well. After adding sodium carbonate, the surface structure of the absorbent changes, and the specific surface area of the new absorbent is larger than that of the original absorbent, so that the desulfurization efficiency is improved. When the added sodium carbonate content is too high, such as the attached Figure 2 Comparing the desulfurization effects of Example 2 and Comparative Examples 6-9, the desulfurization efficiency is reduced because the main components of the absorbent are changed, resulting in a reduction in the desulfurization efficiency. At the same time, adding sodium carbonate to calcium hydroxide rearranges the molecular structure of the calcium-based material, generating many holes that are conducive to the adsorption of sulfur trioxide, and sodium carbonate itself also has an absorption effect on sulfur trioxide, which makes sodium carbonate significantly improve the desulfurization performance of the calcium-based material.
Claims
1. A method for preparing a sintered modified calcium hydroxide sulfur-fixing material, characterized in that The preparation method is achieved by the following steps:
1. Grinding the solid materials of calcium hydroxide and sodium hydroxide respectively, and obtaining calcium hydroxide powder and sodium hydroxide powder after sieving; 2. Adding sodium hydroxide powder to the calcium hydroxide powder, wherein the sodium hydroxide powder accounts for 2wt% of the calcium hydroxide powder, and stirring and mixing uniformly to obtain a mixed powder; 3. Put the mixed powder obtained in step 2 into a muffle furnace and calcine it at a temperature of 550° C. to 650° C. After calcination, cool it to room temperature under closed conditions to obtain a sintered modified calcium hydroxide sulfur-fixing material.
2. The method for preparing the sintered modified calcium hydroxide sulfur-fixing material according to claim 1, characterized in that After grinding in step 1, pass through a 300-mesh sieve.
3. The method for preparing the sintered modified calcium hydroxide sulfur-fixing material according to claim 1, characterized in that In step 3, the calcination treatment is carried out at a temperature of 600° C. for 0.5 h.
4. A method for preparing a modified calcium hydroxide sulfur-fixing material by impregnation, characterized in that The preparation method is achieved by the following steps:
1. Grinding the solid materials of calcium hydroxide and sodium carbonate respectively, and obtaining calcium hydroxide powder and sodium carbonate powder after sieving; 2. Adding sodium carbonate powder to the calcium hydroxide powder, wherein the sodium carbonate powder accounts for 2wt% of the calcium hydroxide powder, stirring and mixing uniformly to obtain a mixed powder, and stirring and mixing the mixed powder and deionized water uniformly to obtain a mixed solution; 3. Evaporating the water in the mixed solution at a temperature of 110°C to 120°C, and collecting the solid phase mixed material after drying; Fourth, the solid phase mixed material is calcined at 450° C. to 550° C., and cooled to room temperature in a closed environment to obtain an impregnated modified calcium hydroxide sulfur-fixing material.
5. The method for preparing the impregnated modified calcium hydroxide sulfur-fixing material according to claim 4, characterized in that In step 2, 25 to 35 g of the mixed powder is stirred and mixed evenly with 90 to 110 mL of deionized water.
6. The method for preparing the impregnated modified calcium hydroxide sulfur-fixing material according to claim 4, characterized in that In step 3, the water in the mixed solution is evaporated at a temperature of 110°C.
7. The method for preparing the impregnated modified calcium hydroxide sulfur-fixing material according to claim 4, characterized in that In step 4, the solid phase mixed material is calcined at 500° C. for 2 h.
8. The use of the modified calcium hydroxide sulfur-fixing material prepared as claimed in claim 1 or 4, characterized in that Modified calcium hydroxide sulfur-fixing material is used as an adsorbent to adsorb sulfur trioxide in flue gas.
Citation Information
Patent Citations
Flue gas desulfurizing agent, preparation method and application thereof
CN112295395A
Acidic gas absorbent and production thereof
JP1996206443A
Calcium oxide particulate matter, its manufacturing process and acidic-gas absorbent comprising the same
JP2004161513A