A device and method for magnetically controlled arc variable temperature gradient melting

Through the magnetron arc-changing temperature gradient smelting equipment, the problems of uneven tissue and uncontrollable temperature gradient in vacuum non-consumable arc smelting are solved, and uniform smelting and structural morphology of high melting point alloys are achieved, and uniform composition of alloys is improved. and mechanical properties.

CN115265189BActive Publication Date: 2024-10-15HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210644052.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-03-05
Filing Date
2022-06-08
Publication Date
2024-10-15
Estimated Expiration
2042-06-08

AI Technical Summary

Technical Problem

During vacuum non-consumable arc smelting, the ingot structure is uneven and the temperature gradient is uncontrollable, resulting in uneven alloy structure and difficult to accurately control the components.

Method used

A magnetron arc-variable temperature gradient smelting equipment is designed, including arc and coil controllers, arc gun control rods, arc magnetron components, smelting furnaces, crucibles, vacuum extraction mechanisms and control cabinets, through induction coils and permanent magnet components Under the action of magnetic field, the current and frequency of the arc gun are controlled, and the temperature gradient and structure of high-melting alloys are controlled.

Benefits of technology

The uniform melting of high-melting alloys is achieved, and the structure and temperature gradient of metal ingots can be adjusted, dendrite or columnar crystals can be formed, and the composition uniformity and mechanical properties of the alloy are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115265189B_ABST
    Figure CN115265189B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of high melting point alloy material smelting, and relates to a device and method for magnetically controlled arc variable temperature gradient smelting, including an arc and coil controller, an arc gun control rod, an arc magnetic control assembly, a smelting furnace, a crucible, an arc gun, a vacuum pumping mechanism and a control cabinet, wherein the arc magnetic control assembly includes a magnetic head, an electromagnetic shielding cover, an induction coil and a permanent magnet assembly, and the bottom end height of the permanent magnet assembly is consistent with the bottom end height of the tungsten level of the arc gun. Advantages of the present invention: the device and method for magnetically controlled arc variable temperature gradient smelting can be used to melt high melting point alloy melts, and at the same time, the alloy temperature gradient and the arc action range can be controlled by controlling the size of the sharp angle magnetic field, and the obtained metal material structure can be adjusted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high melting point alloy material smelting, and relates to a device and method for magnetically controlled arc variable temperature gradient smelting. Background Art

[0002] High melting point alloys are widely used in aviation, aerospace, civil and other fields. Since high melting point alloys refer to alloys with a melting point temperature of more than 1000K, and some high melting point alloys are very active, smelting is more difficult. At present, the main smelting method of high melting point alloys is a vacuum non-consumable arc furnace, which has controllable temperature and can melt multiple alloy ingots at a time, with high smelting efficiency. However, the temperature gradient generated by melting alloys in a vacuum non-consumable arc furnace is large, which makes the alloy's organizational gradient large and the organization uneven. In addition, during the smelting process, the arc blowing force is large, and the alloy powder is easy to blow away, which is not conducive to the precise control of the composition. Therefore, there is an urgent need for a magnetically controlled arc variable temperature gradient melting device and method. Summary of the invention

[0003] Purpose of the Invention

[0004] The technical problem to be solved by the present invention is to overcome the problems of uneven ingot structure and uncontrollable temperature gradient in vacuum non-consumable arc melting, provide a device and method for magnetically controlled arc variable temperature gradient melting, build a device for magnetically controlled arc variable temperature gradient melting, and obtain a smelted ingot with controllable structure.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A device for magnetically controlled arc variable temperature gradient melting, characterized in that it comprises an arc and coil controller, an arc gun control rod, an arc magnetic control assembly, a melting furnace, a crucible, an arc gun, a vacuum pumping mechanism and a control cabinet, wherein the arc and coil controller is arranged above the melting furnace, and the arc and coil controller is connected to the control cabinet through a power connection line; the top end of the arc gun control rod is connected to the arc and coil controller, and the bottom end of the arc gun control rod extends into the melting furnace; the arc magnetic control assembly comprises a magnetic head, an electromagnetic shielding cover, an induction coil and a permanent magnet assembly, wherein the magnetic head is fixed to the inner top wall of the melting furnace through a magnetic head connecting column, and the magnetic head has an introduction channel, and the induction coil is wound around the magnetic head. The electromagnetic shielding cover is wound around the magnetic head, the upper part of which is fixed on the magnetic head, and the electromagnetic shielding cover is arranged on the outside of the induction coil, and the bottom end height of the electromagnetic shielding cover is consistent with the bottom end height of the induction coil; the upper part of the permanent magnet assembly is fixed on the magnetic head, and the permanent magnet assembly is arranged on the outside of the electromagnetic shielding cover, and the bottom end height of the permanent magnet assembly is consistent with the bottom end height of the tungsten level of the arc gun; the crucible is arranged in the smelting furnace; one end of the arc gun is connected to the bottom end of the arc gun control rod, and the other end of the arc gun passes through the introduction channel, and the tungsten pole of the arc gun is located above the crucible; the vacuum mechanism is connected to the smelting furnace; the induction coil and the arc gun are both electrically connected to the arc and coil controller.

[0007] As a further description of the above solution, the crucible is a water-cooled crucible, and the crucible is arranged in the smelting furnace through a supporting base.

[0008] As a further description of the above scheme, the permanent magnet assembly includes a first permanent magnet unit and a second permanent magnet unit, there are two first permanent magnet units and two second permanent magnet units, each of the first permanent magnet units and the second permanent magnet units are staggered and equidistantly arranged on the magnetic head, the length of the second permanent magnet unit is greater than the length of the first permanent magnet unit, and the bottom end of each of the first permanent magnet unit and the second permanent magnet unit is flush with the bottom end of the tungsten pole of the arc gun.

[0009] As a further description of the above scheme, it also includes a drive motor, and the drive motor is arranged in the arc and coil controller;

[0010] As a further description of the above scheme, the arc gun control rod includes an outer rod, a telescopic rod and a center rod, the top end of the outer rod is connected to the arc and coil controller, and the bottom end of the outer rod is fixedly connected to the top wall of the smelting furnace; the diameter of the telescopic rod is smaller than that of the outer rod, and there is a cavity between the outer diameter of the telescopic rod and the inner wall of the outer rod, and the bottom end of the telescopic rod extends into the smelting furnace; one end of the center rod is connected to the driving motor, and the center rod is threadedly connected to the inner wall of the telescopic rod, and the arc gun is arranged at the bottom end of the telescopic rod.

[0011] It also includes a protective gas pressurizing mechanism, which is connected to the smelting furnace.

[0012] A smelting method for preparing a high melting point alloy ingot using the above-mentioned magnetic arc variable temperature gradient smelting equipment comprises the following steps:

[0013] Step 1: Place the high melting point alloy to be melted in the crucible, and adjust the tungsten level of the arc gun to a position where the arc can be struck;

[0014] Step 2: Turn on the vacuum pumping mechanism, then turn on the protective gas pressurizing mechanism to control the vacuum degree in the smelting furnace to 0.05MPa, turn on the arc gun for smelting, and fully melt the metal particles of the high melting point alloy;

[0015] Step 3: Use the arc gun again for smelting, the arc current of the arc gun increases from 0 to 500 A, the high melting point alloy in the smelting furnace is fully melted, the induction coil is started, and the arc gun melts the high melting point alloy under the action of the magnetic field;

[0016] Step 4: Keep the set time under the magnetic field of the induction coil in step 3, then reduce the current of the arc gun to 0, turn off the power, and obtain the alloy ingot under a small temperature gradient.

[0017] As a further description of the above scheme, the tungsten level of the arc gun in step one is no more than 5 mm away from the metal to be melted.

[0018] As a further description of the above scheme, in step 2, the melting temperature of the electric welding gun is greater than or equal to the liquidus line of the high melting point alloy solution, 100°C; in step 4, the arc current of the arc gun is reduced by 50A every 10s, and the current is gradually reduced to 0.

[0019] As a further description of the above scheme, the setting time of step 4 is 70-90s.

[0020] As a further description of the above scheme, in step 3, the current and frequency of the induction coil are controlled by the arc and coil controller, and when the high melting point alloy forms a dendrite structure, the high melting point alloy is controlled to be less than 5*10 4 K / m for melting and cooling, the induction coil frequency is 60-100Hz, the induction coil current is 50-150A; when the high melting point alloy forms a columnar crystal structure, the high melting point alloy is controlled to be greater than 1.0*10 5 Melting and cooling are carried out under a large temperature gradient of K / m, the frequency of the induction coil is 20-60Hz, and the current of the induction coil is 200-300A.

[0021] Advantages and effects

[0022] 1. The present invention adopts a device and method for magnetically controlled arc variable temperature gradient melting, which can melt high melting point alloy melts. At the same time, the alloy temperature gradient and the arc action range can be controlled by controlling the size of the sharp-angle magnetic field, and the obtained metal material structure can be adjusted.

[0023] 2. In the present invention, the metal ingot is repeatedly melted four times under the action of the electric arc to obtain a uniform structure. During the last melting, the temperature gradient is changed by the magnetic control device to adjust the structure of the ingot. The magnetic control device can change the melting depth and adjust the structure morphology. The melting depth is shallow, that is, the arc acts on the melt in a shallow distance along the height direction, and the temperature gradient is less than 5*10 4 K / m, it is easy to form dendrites; the melting depth, that is, the distance the arc acts on the melt along the height direction, the temperature gradient is greater than 1.0*10 5 K / m, it is easy to form columnar crystals. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A front view of a device for magnetically controlled arc variable temperature gradient melting according to an embodiment of the present invention;

[0025] Figure 2 It is a schematic diagram of the structure of the equipment for magnetically controlled arc variable temperature gradient melting according to an embodiment of the present invention;

[0026] Figure 3 A schematic structural diagram of an arc gun control rod according to an embodiment of the present invention;

[0027] Figure 4 for Figure 1 Cross-sectional view of the middle DD;

[0028] Figure 5 This is the microstructure picture of Nb-Si-Ti-ZrC-Sc alloy with variable temperature gradient under scanning electron microscope;

[0029] Figure 6 This is the microstructure picture of Nb-Si-Ti-ZrC-Sc alloy with variable temperature gradient under scanning electron microscope.

[0030] Description of reference numerals:

[0031] 1-arc and coil controller; 2-arc gun control rod; 21-drive motor; 22-center rod; 23-telescopic rod; 24-outer rod; 3-head furnace body connecting column; 4-arc magnetron assembly; 41-magnetic head; 42-induction coil; 43-electromagnetic shielding cover; 44 permanent magnet assembly; 5-smelting furnace; 6-arc gun; 7-crucible; 701-crucible water inlet pipe; 702-crucible water outlet pipe; 8-power connection line; 9-power control cabinet; 10-vacuum extraction mechanism; 11-protective gas pressurization mechanism. DETAILED DESCRIPTION

[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.

[0033] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] The components of the embodiments of the present invention generally described and shown in the drawings herein may be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention.

[0035] The high melting point alloy of the present invention refers to an alloy having a melting point temperature of 1000K or above.

[0036] A device for magnetically controlled arc variable temperature gradient melting, comprising an arc and coil controller 1, an arc gun control rod 2, an arc magnetic control assembly 4, a melting furnace 5, a crucible 7, an arc gun 6, a vacuum pumping mechanism 10 and a control cabinet 11, wherein the arc and coil controller 1 is arranged above the melting furnace 5, and the arc and coil controller 1 is connected to the control cabinet 11 through a power connection line 10; the top end of the arc gun control rod 2 is connected to the arc and coil controller 1, and the bottom end of the arc gun control rod 2 extends into the melting furnace 5; the arc magnetic control assembly comprises a magnetic head 41, an electromagnetic shielding cover 43, an induction coil 42 and a permanent magnet assembly 44, the magnetic head 41 is fixed on the inner top wall of the melting furnace 5 through a magnetic head connecting column 3, and the magnetic head 41 has an introduction channel, the induction coil 42 Wrapped on the magnetic head 41, the upper part of the electromagnetic shielding cover 43 is fixed on the magnetic head 41, and the electromagnetic shielding cover 43 is arranged on the outer side of the induction coil 42, and the bottom end height of the electromagnetic shielding cover 43 is consistent with the bottom end height of the induction coil 42; the upper part of the permanent magnet assembly is fixed on the magnetic head 41, and the permanent magnet assembly is arranged on the outer side of the electromagnetic shielding cover 43, and the bottom end height of the permanent magnet assembly is consistent with the bottom end height of the tungsten grade of the arc gun 6; the crucible 7 is arranged in the smelting furnace 5; one end of the arc gun is connected to the bottom end of the arc gun control rod 2, and the other end of the arc gun passes through the introduction channel, and the tungsten pole of the arc gun 6 is located above the crucible 7; the vacuum mechanism 10 is connected to the smelting furnace 5; the induction coil 42 and the arc gun 6 are both electrically connected to the arc and coil controller 1.

[0037] The permanent magnet assembly of the embodiment of the present invention is composed of four first permanent magnet units, which are arranged on the magnetic head 41 at equal intervals, and the bottom end of the first permanent magnet unit is flush with the bottom end of the tungsten pole of the arc gun 6. The design that the bottom end of a permanent magnet unit of the present invention is flush with the bottom end of the tungsten pole of the arc gun 6 can strengthen the control of the magnetic field on the arc, thereby more accurately controlling the arc shape and the molten pool melting depth, and generating a sharp magnetic field.

[0038] The crucible 7 of the embodiment of the present invention is a water-cooled crucible having a crucible water inlet pipe 701 and a crucible water outlet pipe 702 . The crucible 7 is arranged in the smelting furnace 5 via a supporting base.

[0039] The permanent magnet assembly of the embodiment of the present invention comprises a first permanent magnet unit and a second permanent magnet unit, there are two first permanent magnet units, there are two second permanent magnet units, each of the first permanent magnet unit and the second permanent magnet unit is staggered and arranged at equal distances on the magnetic head 41, the length of the second permanent magnet unit is greater than the length of the first permanent magnet unit, and the bottom end of each of the first permanent magnet unit and the second permanent magnet unit is flush with the bottom end of the tungsten pole of the arc gun 6; specifically, the first permanent magnet unit is fixed to the side wall of the lower part of the magnetic head 41 by a connecting member, and the second permanent magnet unit is fixed to the side wall of the upper part of the magnetic head 41 by bolts, and the height of the top end of the first permanent magnet unit is lower than the height of the top end of the second permanent magnet unit. The design that the bottom end of the second permanent magnet unit of the present invention is flush with the bottom end of the tungsten pole of the arc gun 6 can strengthen the control of the magnetic field on the arc, thereby more accurately controlling the arc shape and the melting depth of the molten pool, and generating a sharp magnetic field.

[0040] The above-mentioned device also includes a drive motor 21, which is arranged in the arc and coil controller 1;

[0041] The arc gun control rod 2 includes an outer rod 24, a telescopic rod 23 and a center rod 22. The top of the outer rod 24 is connected to the arc and coil controller 1, and the bottom of the outer rod 24 is fixedly connected to the top wall of the smelting furnace 5. The diameter of the telescopic rod 23 is smaller than that of the outer rod 24, and there is a cavity between the outer diameter of the telescopic rod 23 and the inner wall of the outer rod 24. The bottom end of the telescopic rod 23 extends into the smelting furnace. One end of the center rod 22 is connected to the driving motor, and the center rod 22 is threadedly connected to the inner wall of the telescopic rod 23. The arc gun 6 is arranged at the bottom end of the telescopic rod 23. The present invention fixes the arc and coil controller 1 above the smelting furnace 5 through the outer rod 24, and controls the distance between the tungsten pole of the arc gun 6 and the metal to be smelted by the cooperation of the driving motor 21 and the telescopic rod 23. In this design, each component can be disassembled and repaired separately, which is convenient for later maintenance and improves the practicality of the equipment.

[0042] The above-mentioned equipment further includes a protective gas pressurizing mechanism 11 , which is connected to the smelting furnace 5 .

[0043] A smelting method for preparing a high melting point alloy ingot using the above-mentioned magnetic arc variable temperature gradient smelting equipment comprises the following steps:

[0044] Step 1: placing the high melting point alloy to be smelted inside the crucible 7, and adjusting the tungsten level of the arc gun 6 to a position capable of striking an arc;

[0045] Step 2: Turn on the vacuum pumping mechanism 10, then turn on the protective gas pressurizing mechanism 11 to control the vacuum degree in the smelting furnace 5 to 0.05MPa, turn on the arc gun 6 for smelting, and fully melt the metal particles of the high melting point alloy; specifically, the arc gun 6 is used to melt the high melting point alloy, and the smelting process is: the arc current increases from 0 to 500A, and is maintained at 500A for 1 minute, and then the current is slowly reduced, the current of the arc gun 6 is reduced by 50A every 10s, and is reduced to 0, the metal particles of the high melting point alloy are fully melted, and the high melting point alloy is turned over after smelting; and then the above smelting process is repeated four times.

[0046] Step 3: The arc gun 6 is used again for smelting. The arc current of the arc gun 6 increases from 0 to 500 A. The high melting point alloy in the smelting furnace 5 is fully melted. The induction coil 42 is started. Under the action of the magnetic field, the arc gun 6 melts the high melting point alloy. In this smelting, in order to control the organization of the solidification process, the magnetic control is turned on to change the melting depth, which can regulate the organization morphology. The melting depth is shallow, that is, the arc acts on the melt in a shallow distance along the height direction, and the temperature gradient is less than 5*10 4 K / m, it is easy to form dendrites; the melting depth, that is, the distance the arc acts on the melt along the height direction, the temperature gradient is greater than 1.0*10 5 K / m, tends to form columnar crystals;

[0047] The above step 4: in step 3, the magnetic field of the induction coil 42 is maintained for 70-90 seconds, and then the current of the arc gun 6 is reduced to 0, and the power is turned off to obtain an alloy ingot with a small temperature gradient.

[0048] The tungsten level of the arc gun 6 in the above step 1 is no more than 5 mm away from the metal to be smelted.

[0049] In the above step 2, the melting temperature of the welding gun 6 is greater than or equal to the liquidus line of the high melting point alloy solution 100° C.; in step 4, the arc current of the arc gun 6 is reduced by 50A every 10s and gradually reduced to 0.

[0050] In step 3, the current and frequency of the induction coil 42 are controlled by the arc and coil controller 1, and when the high melting point alloy forms a dendrite structure, the high melting point alloy is controlled to be less than 5*10 4K / m, the melting and cooling are performed at a small temperature gradient, the frequency of the induction coil 42 is 60-100 Hz, and the current of the induction coil 42 is 50-150 A; when the high melting point alloy forms a columnar crystal structure, the high melting point alloy is controlled to be greater than 1.0*10 5 K / m for melting and cooling, the frequency of the induction coil 42 is 20-60 Hz, and the current of the induction coil 42 is 200-300A.

[0051] In the present invention, the metal ingot is repeatedly melted four times under the action of the electric arc to obtain a uniform structure. During the last melting, the temperature gradient is changed by the magnetic control device to adjust the structure of the ingot. The magnetic control device can change the melting depth and adjust the structure morphology. The melting depth is shallow, that is, the arc acts on the melt in a shallow distance along the height direction, and the temperature gradient is less than 5*10 4 K / m, it is easy to form dendrites; the melting depth, that is, the distance the arc acts on the melt along the height direction, the temperature gradient is greater than 1.0*10 5 K / m, it is easy to form columnar crystals. Example

[0052] A smelting method for preparing Nb-Si-Ti-ZrC-Sc ingots using the above-mentioned equipment:

[0053] Step 1: placing a high melting point alloy inside the crucible 7, and adjusting the tungsten level of the arc gun 6 to a position capable of striking an arc;

[0054] Step 2: Turn on the vacuum pumping mechanism 10, and then turn on the protective gas pressurizing mechanism 11, control the vacuum degree in the smelting furnace 5 to 0.05MPa, turn on the arc gun 6, and melt the high melting point alloy. The smelting process is: the arc current increases from 0 to 600A, and is maintained at 600A for 1 minute, and the current of the arc gun 6 is slowly reduced, reducing 50A every 10s to 0, so that the metal particles of the high melting point alloy are fully melted, and the high melting point alloy is turned over after smelting; then repeat the above smelting process four times, so that the elements of the high melting point alloy are evenly distributed. Step 3: Perform the fifth smelting, arc melt the high melting point alloy in step 2, and the arc current increases from 0 to 500A. After the metal is fully melted, a stable flow is formed, and the induction coil 42 is turned on. When the high melting point alloy needs to obtain a dendrite structure, the current of the induction coil 42 is adjusted to 100A, and the frequency of the induction coil 42 is 80Hz. Under the action of the magnetic field, the high melting point alloy is controlled to be less than 5*10 4 Melting and cooling occur under a small temperature gradient of 1.34°C / min.

[0055] Step 4: Maintain the current and frequency of the induction coil 42 for 70 seconds, reduce the current of the arc gun 6 to 0, and turn off the power of the arc gun 6 and the induction coil 42.

[0056] Step 5: Conduct tissue testing on the obtained ingot, and the tissue is uniform. Example

[0057] A smelting method for preparing Nb-Si-Ti-ZrC-Sc ingots using the above-mentioned equipment:

[0058] Step 1: placing a high melting point alloy inside the crucible 7, and adjusting the tungsten level of the arc gun 6 to a position capable of striking an arc;

[0059] Step 2: Turn on the vacuum pumping mechanism 10, then turn on the protective gas pressurizing mechanism 11, control the vacuum degree in the smelting furnace 5 to 0.05MPa, turn on the arc gun 6, and melt the high melting point alloy. The smelting process is: the arc current increases from 0 to 600A, and is maintained at 600A for 1min, and the current of the arc gun 6 is slowly reduced, reducing 50A every 10s to 0, so that the metal particles of the high melting point alloy are fully melted, and the high melting point alloy is turned over after smelting; then repeat the above smelting process four times, so that the elements of the high melting point alloy are evenly distributed. Step 3: Perform the fifth smelting, arc melt the high melting point alloy in step 2, and the arc current increases from 0 to 500A. After the metal is fully melted, a stable flow is formed, and the induction coil 42 is turned on. When the high melting point alloy needs to obtain a dendrite structure, the current of the induction coil 42 is adjusted to 50A, and the frequency of the induction coil 42 is 60Hz. Under the action of the magnetic field, the high melting point alloy is controlled to be less than 5*10 4 Melting and cooling occur under a small temperature gradient of 1.34°C / min.

[0060] Step 4: Maintain the current and frequency of the induction coil 42 for 70 seconds, reduce the current of the arc gun 6 to 0, and turn off the power of the arc gun 6 and the induction coil 42.

[0061] Step 5: Conduct tissue testing on the obtained ingot, and the tissue is uniform. Example

[0062] A smelting method for preparing Nb-Si-Ti-ZrC-Sc ingots using the above-mentioned equipment:

[0063] Step 1: placing a high melting point alloy inside the crucible 7, and adjusting the tungsten level of the arc gun 6 to a position capable of striking an arc;

[0064] Step 2: Turn on the vacuum pumping mechanism 10, then turn on the protective gas pressurizing mechanism 11, control the vacuum degree in the smelting furnace 5 to 0.05MPa, turn on the arc gun 6, and melt the high melting point alloy. The smelting process is: the arc current increases from 0 to 600A, and is maintained at 600A for 1min, and the current of the arc gun 6 is slowly reduced, decreasing by 50A every 10s until it reaches 0, so that the metal particles of the high melting point alloy are fully melted, and the high melting point alloy is turned over after melting; then repeat the above steps. The melting process is repeated four times to make the elements of the high melting point alloy evenly distributed. Step three: the fifth melting is performed, the high melting point alloy in step two is arc melted, the arc current increases from 0 to 500A, after the metal is fully melted, a stable flow is formed, the induction coil 42 is turned on, and when the high melting point alloy needs to obtain a dendrite structure, the current of the induction coil 42 is adjusted to 150A, and the frequency of the induction coil 42 is 100Hz. Under the action of the magnetic field, the high melting point alloy is controlled to be less than 5*10 4 Melting and cooling occur under a small temperature gradient of 1.34°C / min.

[0065] Step 4: Maintain the current and frequency of the induction coil 42 for 70 seconds, reduce the current of the arc gun 6 to 0, and turn off the power of the arc gun 6 and the induction coil 42.

[0066] Step 5: Conduct tissue testing on the obtained ingot, and the tissue is uniform.

[0067] The current and frequency of the induction coil (42) are regulated to control the high melting point alloy to be less than 5*10 4 K / m, the melting and cooling are performed at a small temperature gradient, the frequency of the induction coil (42) is 60-100 Hz, and the current of the induction coil (42) is 50-150 A; when the high melting point alloy forms a columnar crystal structure, the high melting point alloy is controlled to be greater than 1.0*10 5 Melting and cooling are performed under a large temperature gradient of 200 K / m, the frequency of the induction coil (42) is 20-60 Hz, and the current of the induction coil (42) is 200-300 A. Example

[0068] A smelting method for preparing Nb-Si-Ti-ZrC-Sc ingots using the above-mentioned equipment:

[0069] Step 1: placing a high melting point alloy inside the crucible 7 and adjusting the tungsten level of the arc gun 6 to a position that facilitates arc ignition;

[0070] Step 2: After the vacuum pumping mechanism 10 is turned on, the protective gas pressurizing mechanism 11 is turned on to control the vacuum degree in the smelting furnace 5 to 0.05MPa, and the arc gun 6 is turned on to melt the high melting point alloy. The smelting process is as follows: the arc current increases from 0 to 600A, and is maintained at 600A for 1min, and the current of the arc gun 6 is slowly reduced, reducing 50A every 10s to 0, so that the metal particles of the high melting point alloy are fully melted, and the high melting point alloy is turned over after smelting; then the above smelting process is repeated four times, so that the elements of the high melting point alloy are evenly distributed; Step 3: The high melting point alloy in step 2 is arc melted. After the metal is fully melted, a stable flow is formed, and the induction coil 42 is turned on, and the current of the induction coil 42 is adjusted to 240A, and the frequency of the induction coil 42 is 40Hz. Under the action of the magnetic field, the high melting point alloy is controlled to be greater than 1.0*10 5 K / m large temperature gradient for melting and cooling, high melting point alloys need to obtain columnar crystal structure.

[0071] Step 4: Maintain the current and frequency of the induction coil 42 for 90 seconds, slowly turn off the arc power supply, turn off the power of the arc gun 6 and the induction coil 42, and obtain a Nb-Si-Ti-ZrC-Sc ingot with a small temperature gradient.

[0072] Step 5: Conduct tissue testing on the obtained ingot, and the tissue is uniform. Example

[0073] A smelting method for preparing Nb-Si-Ti-ZrC-Sc ingots using the above-mentioned equipment:

[0074] Step 1: placing a high melting point alloy inside the crucible 7 and adjusting the tungsten level of the arc gun 6 to a position that facilitates arc ignition;

[0075] Step 2: After the vacuum pumping mechanism 10 is turned on, the protective gas pressurizing mechanism 11 is turned on to control the vacuum degree in the smelting furnace 5 to 0.05MPa, and the arc gun 6 is turned on to melt the high melting point alloy. The smelting process is as follows: the arc current increases from 0 to 600A, and is maintained at 600A for 1min, and the current of the arc gun 6 is slowly reduced, reducing 50A every 10s to 0, so that the metal particles of the high melting point alloy are fully melted, and the high melting point alloy is turned over after smelting; then the above smelting process is repeated four times, so that the elements of the high melting point alloy are evenly distributed; Step 3: The high melting point alloy in step 2 is arc melted. After the metal is fully melted, a stable flow is formed, and the induction coil 42 is turned on, and the current of the induction coil 42 is adjusted to 200A, and the frequency of the induction coil 42 is 20Hz. Under the action of the magnetic field, the high melting point alloy is controlled to be greater than 1.0*10 5 K / m large temperature gradient for melting and cooling, high melting point alloys need to obtain columnar crystal structure.

[0076] Step 4: Maintain the current and frequency of the induction coil 42 for 90 seconds, slowly turn off the arc power supply, turn off the power of the arc gun 6 and the induction coil 42, and obtain a Nb-Si-Ti-ZrC-Sc ingot with a small temperature gradient.

[0077] Step 5: Conduct tissue testing on the obtained ingot, and the tissue is uniform. Example

[0078] A smelting method for preparing Nb-Si-Ti-ZrC-Sc ingots using the above-mentioned equipment:

[0079] Step 1: placing a high melting point alloy inside the crucible 7 and adjusting the tungsten level of the arc gun 6 to a position that is easy to strike an arc;

[0080] Step 2: After the vacuum pumping mechanism 10 is turned on, the protective gas pressurizing mechanism 11 is turned on to control the vacuum degree in the smelting furnace 5 to 0.05MPa, and the arc gun 6 is turned on to melt the high melting point alloy. The smelting process is as follows: the arc current increases from 0 to 600A, and is maintained at 600A for 1min, and the current of the arc gun 6 is slowly reduced, reducing 50A every 10s to 0, so that the metal particles of the high melting point alloy are fully melted, and the high melting point alloy is turned over after smelting; then the above smelting process is repeated four times, so that the elements of the high melting point alloy are evenly distributed; Step 3: The high melting point alloy in step 2 is arc melted. After the metal is fully melted, a stable flow is formed, and the induction coil 42 is turned on, and the current of the induction coil 42 is adjusted to 300A. The frequency of the induction coil 42 is 60Hz. Under the action of the magnetic field, the high melting point alloy is controlled to be greater than 1.0*10 5 K / m large temperature gradient for melting and cooling, high melting point alloys need to obtain columnar crystal structure.

[0081] Step 4: Maintain the current and frequency of the induction coil 42 for 90 seconds, slowly turn off the arc power supply, turn off the power of the arc gun 6 and the induction coil 42, and obtain a Nb-Si-Ti-ZrC-Sc ingot with a small temperature gradient.

[0082] Step 5: Conduct tissue testing on the obtained ingot, and the tissue is uniform.

[0083] Figure 5 The microstructure of the Nb-Si-Ti-ZrC-Sc alloy with variable temperature gradient under a scanning electron microscope is shown in the figure. The microstructure of the Nb-Si-Ti-ZrC-Sc alloy prepared by the device and method of the present invention for magnetic arc variable temperature gradient melting is in the form of dendrites, wherein the size of the dendrites is mostly 100-300 μm. The maximum size of the Nbss phase in the figure reaches 50 μm. Nbss / Nb is also formed in the middle of some dendrites. 5 Si 3Eutectic structure, the eutectic structure is very fine, wherein the Nbss phase reaches the micron level. It can be seen that the magnetically controlled arc variable temperature gradient melting equipment of the present invention is beneficial to improving the room temperature fracture toughness of high melting point alloys.

[0084] Figure 6 The Nb-Si-Ti-ZrC-Sc alloy microstructure under a scanning electron microscope is shown in Figure 1. The microstructure of the Nb-Si-Ti-ZrC-Sc alloy prepared by the device and method for magnetic arc variable temperature gradient melting according to the present invention is small equiaxed crystals. The microstructure is relatively small. 5 Si 3 The size of the phase is mostly 5-10 μm in island shape, dispersedly distributed on the Nbss phase matrix. It can be seen that the magnetic arc variable temperature gradient melting equipment of the present invention is conducive to changing and increasing the crack extension path in the high melting point alloy, thereby having the effect of improving the mechanical properties.

[0085] Obviously, the above-mentioned embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the embodiments of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made on the basis of the above description. It is impossible to list all the embodiments here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A device for magnetically controlled arc variable temperature gradient melting, characterized in that: It comprises an arc and coil controller (1), an arc gun control rod (2), an arc magnetic control assembly (4), a smelting furnace (5), a crucible (7), an arc gun (6), a vacuum pumping mechanism (10) and a power supply control cabinet (9). The arc and coil controller (1) is arranged above the smelting furnace (5), and the arc and coil controller (1) is connected to a power control cabinet (9) via a power connection line; the top end of the arc gun control rod (2) is connected to the arc and coil controller (1), and the bottom end of the arc gun control rod (2) extends into the smelting furnace (5); The arc magnetron assembly (4) comprises a magnetic head (41), an electromagnetic shielding cover (43), an induction coil (42) and a permanent magnet assembly (44); the magnetic head (41) is fixed to the inner top wall of the smelting furnace (5) through a magnetic head connecting column (3), and the magnetic head (41) has an introduction channel; the induction coil (42) is wound on the magnetic head (41); the upper part of the electromagnetic shielding cover (43) is fixed to the magnetic head (41), and the electromagnetic shielding cover (43) is arranged on the outside of the induction coil (42); the bottom end height of the electromagnetic shielding cover (43) is consistent with the bottom end height of the induction coil (42); the upper part of the permanent magnet assembly is fixed to the magnetic head (41), and the permanent magnet assembly is arranged on the outside of the electromagnetic shielding cover (43); the bottom end height of the permanent magnet assembly is consistent with the bottom end height of the tungsten grade of the arc gun (6); the crucible (7) is arranged in the smelting furnace (5); One end of the arc gun is connected to the bottom end of the arc gun control rod (2), the other end of the arc gun passes through the introduction channel, and the tungsten pole of the arc gun (6) is located above the crucible (7); the vacuum pumping mechanism (10) is connected to the smelting furnace (5); The induction coil (42) and the arc gun (6) are both electrically connected to the arc and coil controller (1); The crucible (7) is a water-cooled crucible, and the crucible (7) is arranged in the smelting furnace (5) via a supporting base; The permanent magnet assembly comprises a first permanent magnet unit and a second permanent magnet unit, the first permanent magnet unit has two strips, the second permanent magnet unit has two strips, each of the first permanent magnet unit and the second permanent magnet unit is staggered and arranged at an equal distance on the magnetic head (41), the length of the second permanent magnet unit is greater than the length of the first permanent magnet unit, and the bottom end of each of the first permanent magnet unit and the second permanent magnet unit is flush with the bottom end of the tungsten pole of the arc gun (6); The magnetically controlled arc variable temperature gradient smelting device further comprises a drive motor (21), wherein the drive motor (21) is arranged in the arc and coil controller (1); The arc gun control rod (2) comprises an outer rod (24), a telescopic rod (23) and a center rod (22); the top end of the outer rod (24) is connected to the arc and coil controller (1), and the bottom end of the outer rod (24) is fixedly connected to the top wall of the smelting furnace (5); the diameter of the telescopic rod (23) is smaller than that of the outer rod (24), and a cavity is provided between the outer diameter of the telescopic rod (23) and the inner wall of the outer rod (24), and the bottom end of the telescopic rod (23) extends into the smelting furnace; one end of the center rod (22) is connected to the driving motor, and the center rod (22) is threadedly connected to the inner wall of the telescopic rod (23); the arc gun (6) is arranged at the bottom end of the telescopic rod (23); The magnetically controlled arc variable temperature gradient smelting device further comprises a shielding gas pressurizing mechanism (11), wherein the shielding gas pressurizing mechanism (11) is connected to the smelting furnace (5); and the induction coil (42) is an AC induction coil.

2. A method for preparing a high melting point alloy ingot using the magnetic arc variable temperature gradient melting device as claimed in claim 1, characterized in that: The following steps are involved: Step 1: placing the high melting point alloy to be smelted inside the crucible (7), and adjusting the tungsten level of the arc gun (6) to a position capable of striking an arc; Step 2: starting the vacuum pumping mechanism (10), then starting the protective gas pressurizing mechanism (11) to control the vacuum degree in the smelting furnace (5) to 0.05 MPa, starting the arc gun (6) to carry out smelting, and fully melting the metal particles of the high melting point alloy; Step 3: The arc gun (6) is used again for smelting, and the arc current of the arc gun (6) is increased from 0 to 500 A. The high melting point alloy in the smelting furnace (5) is fully melted, and the induction coil (42) is started. Under the action of the magnetic field, the arc gun (6) melts the high melting point alloy; Step 4: maintaining the magnetic field of the induction coil (42) in step 3 for a set time, then reducing the current of the arc gun (6) to 0, turning off the power supply, and obtaining an alloy ingot with a small temperature gradient; the set time of step 4 is 70-90 seconds; In the step 3, the current and frequency of the induction coil (42) are controlled by the arc and coil controller (1), and when the high melting point alloy forms a dendrite structure, the high melting point alloy is controlled to be less than 5*10 4 K / m, the melting and cooling are performed at a small temperature gradient, the frequency of the induction coil (42) is 60-100 Hz, and the current of the induction coil (42) is 50-150 A; when the high melting point alloy forms a columnar crystal structure, the high melting point alloy is controlled to be greater than 1.0*10 5 Melting and cooling are performed under a large temperature gradient of 200 K / m, the frequency of the induction coil (42) is 20-60 Hz, and the current of the induction coil (42) is 200-300 A.

3. The method for preparing high melting point alloy ingots by using the magnetic controlled arc variable temperature gradient melting equipment according to claim 2, characterized in that: The tungsten level of the arc gun (6) in step 1 is no more than 5 mm away from the metal to be smelted.

4. The method for preparing high melting point alloy ingots by using the magnetic controlled arc variable temperature gradient melting equipment according to claim 2, characterized in that: In the step 2, the melting temperature of the electric welding gun (6) is greater than or equal to 100° C., which is the liquidus line of the high melting point alloy solution; and in the step 4, the arc current of the arc gun (6) is reduced by 50A every 10 seconds, and the current is gradually reduced to 0.