A method for preparing ceramic insulated aluminum winding
Through microarc oxidation/thermoelectrochemical oxidation technology and specific device design, ceramic insulated aluminum wires are directly wound on the winding coil, solving the scrapping problem of ceramic insulated aluminum wires due to large bending in traditional winding preparation, and simplifying the process and The effect of reducing costs.
Patent Information
- Application Number
- CN202210970949.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-14
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-08-14
AI Technical Summary
Ceramic insulated aluminum conductors are prone to falling off due to large bends during the preparation of traditional windings, resulting in scrapping of ceramic film. There are many links and high costs in the existing technology.
Microarc oxidation/thermoelectrochemical oxidation technology is used to process aluminum wires in the oxidation tank to generate ceramic insulated aluminum wires. Through specific device design and process flow, it is directly wound on the winding coil to form a winding to reduce bending and intermediate links.
The production process from wires to windings is simplified, the production difficulty and cost of ceramic insulated aluminum windings is reduced, and the damage to the ceramic film layer is avoided.
Smart Images

Figure CN115274294B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a winding, and in particular to a method for preparing an aluminum winding by using a ceramic insulated aluminum wire. Background Art
[0002] In the conventional winding preparation process, the wire manufacturer produces insulated wires, and then the transformer manufacturer uses the insulated wires to produce windings and assemble them into transformers. From a roll of wire to a finished winding, it needs to go through multiple links such as unwinding-insulation treatment-rewinding-transporting to the transformer manufacturer-unwinding-winding. Aluminum wire with a ceramic insulating film layer is a new type of insulating wire, but the insulating film layer on the surface of this ceramic insulated aluminum wire is relatively fragile and cannot withstand large bends. When using this ceramic insulated aluminum wire to prepare windings using traditional methods, the winding, unwinding and winding processes can easily cause the ceramic film layer on the surface of the ceramic insulated aluminum wire to fall off and become scrapped. Summary of the invention
[0003] The object of the present invention is to provide a method for preparing an aluminum winding using a ceramic insulated aluminum wire, which can unwind, insulate and wind the aluminum wire in one step without significantly bending the ceramic insulated aluminum wire, thereby significantly reducing the intermediate links from the wire to the winding and overcoming the defects of the prior art.
[0004] To achieve the above-mentioned purpose, the technical solution of the present invention is as follows:
[0005] A method for preparing a ceramic insulated aluminum winding comprises the steps of:
[0006] (1) An oxidation trough with an arc surface and an arc plate with a guide groove are arranged opposite to each other, and the relative positions of the oxidation trough and the arc plate are adjusted so that the arc surface and the arc plate are coaxial; the side walls of the oxidation trough on both sides of the arc surface are surrounded by electrode plates, and inlet and outlet holes are provided on the side walls of the oxidation trough at both ends of the arc surface;
[0007] (2) unwinding and leading out the aluminum wire from the aluminum wire coil, guiding the aluminum wire into the arc plate with the guide groove by the guide wheel, allowing the aluminum wire to slide along the guide groove and then pass through the inlet and outlet holes into one end of the oxidation tank, and passing the aluminum wire out of the inlet and outlet holes at the other end of the oxidation tank by the lead-out wheel, and adjusting the length of the aluminum wire in the oxidation tank so that the aluminum wire in the guide groove and the aluminum wire in the oxidation tank are located on the same circular ring;
[0008] (3) The electrolyte is injected into the oxidation tank, and the electrode plate and the aluminum wire are respectively connected to a micro-arc oxidation / thermo-electrochemical oxidation power source, so that the aluminum wire in the oxidation tank undergoes a micro-arc oxidation / thermo-electrochemical oxidation reaction while passing through the oxidation tank, and the aluminum wire generates an arc-shaped ceramic insulated aluminum wire after passing through the oxidation tank.
[0009] Furthermore, step (1) comprises:
[0010] The oxidation groove with arc surface and the arc plate with guide groove are relatively enclosed around the insulating cylinder, the insulating cylinder is fixed on the winding winding mechanism, and the relative positions of the oxidation groove and the arc plate are adjusted so that the arc surface and the arc plate are coaxial; the side walls of the oxidation groove on both sides of the arc surface are enclosed by electrode plates, and inlet and outlet holes are opened on the side walls of the oxidation groove at both ends of the arc surface;
[0011] Step (3) includes:
[0012] (3) The electrolyte is injected into the oxidation tank, and the electrode plate and the aluminum wire are respectively connected to the micro-arc oxidation / thermoelectrochemical oxidation power supply, so that the aluminum wire in the oxidation tank undergoes micro-arc oxidation / thermoelectrochemical oxidation reaction while passing through the oxidation tank. After passing through the oxidation tank, the aluminum wire generates an arc-shaped ceramic insulated aluminum wire and is wound around the insulating tube.
[0013] Furthermore, step (2) includes:
[0014] The aluminum wire is unwound and led out from the aluminum wire coil, and the aluminum wire is guided into the arc plate with the guide groove by the conductive copper wheel, so that the aluminum wire slides along the guide groove and then passes through the inlet and outlet holes into one end of the oxidation tank, and the aluminum wire is passed out from the inlet and outlet holes at the other end of the oxidation tank by the lead-out wheel, and the length of the aluminum wire in the oxidation tank is adjusted so that the aluminum wire in the guide groove and the aluminum wire in the oxidation tank are located on the same ring;
[0015] Step (3) includes:
[0016] The electrolyte is injected into the oxidation tank, and the electrode plate and the conductive copper wheel are respectively connected to the micro-arc oxidation / thermal electrochemical oxidation power supply, so that the aluminum wire in the oxidation tank undergoes micro-arc oxidation / thermal electrochemical oxidation reaction while passing through the oxidation tank, and the aluminum wire generates an arc-shaped ceramic insulated aluminum wire after passing through the oxidation tank.
[0017] Furthermore, step (1) comprises:
[0018] An oxidation tank with an arc surface and an arc plate with a guide groove are arranged opposite to each other, and the relative positions of the oxidation tank and the arc plate are adjusted so that the arc surface and the arc plate are coaxial; the side walls of the oxidation tank on both sides of the arc surface are surrounded by electrode plates, and inlet and outlet holes and water inlet and outlet holes are provided on the side walls of the oxidation tank at both ends of the arc surface;
[0019] Step (3) includes:
[0020] The water inlet and outlet holes are externally connected to an electrolyte circulation system, and the electrolyte is injected into the oxidation tank through the electrolyte circulation system. The electrode plate and the aluminum wire are respectively connected to a micro-arc oxidation / thermal electrochemical oxidation power source, so that the aluminum wire in the oxidation tank undergoes a micro-arc oxidation / thermal electrochemical oxidation reaction while passing through the oxidation tank. The aluminum wire generates an arc-shaped ceramic insulated aluminum wire after passing through the oxidation tank.
[0021] Furthermore, step (1) includes: arranging an oxidation groove having an arc surface and an arc plate having a guide groove relative to each other, adjusting the relative positions of the oxidation groove and the arc plate so that the arc surface and the arc plate are coaxial; enclosing the side walls of the oxidation groove on both sides of the arc surface with electrode plates, opening inlet and outlet holes on the side walls of the oxidation groove at both ends of the arc surface, plugging the inlet and outlet holes with sealing plugs, and wrapping the aluminum wire with the sealing plugs.
[0022] Compared with the prior art, the beneficial technical effects of the present invention are:
[0023] The ceramic insulated aluminum winding preparation method of the present invention simplifies the existing unwinding-insulation treatment-rewinding-transportation to the transformer manufacturer-unwinding-winding process to unwinding-insulation treatment-winding, and can avoid large bending of the ceramic insulated aluminum wire, which can greatly reduce the production difficulty and cost of the ceramic insulated aluminum winding. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the structure of part of the device of the present invention;
[0025] Figure 2 It is a schematic diagram of the arc plate structure of the present invention;
[0026] Figure 3 It is a schematic structural diagram of the oxidation tank of the present invention. DETAILED DESCRIPTION
[0027] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Embodiment 1:
[0029] like Figure 1-3As shown, the device of the present invention comprises a vertically arranged arc plate 1 and an oxidation tank 2, one end of the arc plate 1 is fixed together with one end of the oxidation tank 2. The oxidation tank 2 contains electrolyte, one end of the oxidation tank 2 has a wire inlet 201 and a water inlet 202, and the other end of the oxidation tank 2 has a wire outlet 203 and a water outlet 204. The wire inlet 201 and the wire outlet 203 are provided with sealing plugs 206 that wrap the aluminum wire 3 (for the setting method, material and function of the sealing plug, please refer to patent CN2021116747753, title: Conductor wire thermal electrochemical oxidation treatment device, the sealing plug is made of a silicone pad or a polyurethane foam pad wrapped around the aluminum wire and then clamped on the wire inlet and outlet holes. The sealing plug blocks the wire inlet and outlet holes to prevent the electrolyte from flowing out of the oxidation tank. At the same time, since it is clamped on the wire inlet and outlet holes, the aluminum wire can slide through the wound silicone pad or polyurethane foam pad), and the water inlet 203 and the water outlet 204 are respectively connected to the water outlet pipe and the water inlet pipe of the electrolyte circulation system. One side of the oxidation tank 2 is an arc surface 205, which is coaxial with the arc plate 1 and is located between the inlet hole 201 and the outlet hole 203. The sides of the oxidation tank on both sides of the arc surface 205 are surrounded by electrode plates made of stainless steel. The arc plate 1 has a guide groove 101, which is made of PVC. It also includes a pair of introduction wheels 6 and a pair of export wheels 7, the introduction wheel 6 is located at the other end of the arc plate 1, and the export wheel 7 is located at the other end of the oxidation tank 2. The introduction wheel 6 is a conductive copper wheel.
[0030] The aluminum wire 3 is fed into the arc plate 1 along the guide groove 101 by rotating the introduction wheel 6. After the aluminum wire 3 slides into the arc plate 1 along the guide groove 101, it passes through the wire inlet hole 201 and the wire outlet hole 203 in sequence and passes through the oxidation tank 2. The aluminum wire 3 in the guide groove 101 and the aluminum wire in the oxidation tank 2 are located on the same ring. The electrode plate and the conductive copper wheel are respectively connected to the thermoelectrochemical oxidation power supply. After the power supply is turned on, the aluminum wire immersed in the electrolyte in the oxidation tank 2 undergoes a thermoelectrochemical oxidation reaction to generate a ceramic insulated aluminum wire 3'. The lead-out wheel 7 clamps the ceramic insulated aluminum wire 3' and leads the ceramic insulated aluminum wire 3' out by rotating the lead-out wheel 7. The aluminum wire 3 is concave into a ring when passing through the guide groove 101. At the same time, the wire inlet hole 201, the wire outlet hole 203, the introduction wheel 6 and the lead-out wheel 7 also play an auxiliary shaping role to keep the aluminum wire 3 in a ring shape.
[0031] The ceramic insulated aluminum wire 3' slides out of the outlet hole 203 and takes a circular ring shape. The aluminum wire 3 continuously enters the oxidation tank 2. During the whole process, the wire enters and oxidizes while exiting, so that a single aluminum wire 3 can be directly oxidized into a circle of circular ceramic insulated aluminum wires 3'.
[0032] As a preferred embodiment, the ceramic insulated aluminum wire 3' is directly wound on the insulating cylinder 4 after sliding out of the outlet hole 203 to directly form a winding. Specifically, the insulating cylinder 4 is arranged horizontally and driven to rotate by the winding mechanism, and the arc plate 1 and the oxidation groove 3 surround the insulating cylinder 4. The ceramic insulated aluminum wire 3' is directly wound on the insulating cylinder 4 after passing through the oxidation groove, and the rotation direction of the insulating cylinder 4 is consistent with the direction in which the ceramic insulated aluminum wire 3' slides out of the outlet hole 203. The ceramic insulated aluminum wire 3' between the insulating cylinder 4 and the outlet hole 204, the aluminum wire in the guide groove 101 and the aluminum wire in the oxidation groove 2 are kept on the same ring as much as possible, and the ceramic insulated aluminum wire 3' is kept tangent to the outer periphery of the insulating cylinder 4 to minimize the bending of the ceramic insulated aluminum wire 3'. Further, it also includes an elastic pressure roller 5, which is located at the tangent point between the ceramic insulated aluminum wire 3' and the outer periphery of the insulating cylinder 4. The elastic pressure roller 5 makes the ceramic insulated aluminum wire 3' always close to the outer periphery of the insulating cylinder 4 during winding, so that the formed winding is more compact. The setting method of the elastic pressure roller 5 is the existing technology, and the specific setting can be referred to the lower pressure roller in patent CN202121354504.5.
Claims
1. A method for preparing a ceramic-insulated aluminum winding, It is characterized in that Includes steps: (1) An oxidation groove with an arc surface and an arc plate with a guide groove are relatively enclosed around an insulating cylinder, the insulating cylinder is fixed on a winding winding mechanism, and the relative positions of the oxidation groove and the arc plate are adjusted so that the arc surface and the arc plate are coaxial; the side walls of the oxidation groove on both sides of the arc surface are enclosed by electrode plates, and inlet and outlet holes and water inlet and outlet holes are provided on the side walls of the oxidation groove at both ends of the arc surface; (2) unwinding and leading out the aluminum wire from the aluminum wire coil, guiding the aluminum wire into the arc plate with the guide groove by means of a conductive copper wheel, allowing the aluminum wire to slide along the guide groove and then pass through the inlet and outlet holes at one end of the oxidation tank, and passing the aluminum wire out of the inlet and outlet holes at the other end of the oxidation tank by means of a lead-out wheel, adjusting the length of the aluminum wire in the oxidation tank so that the aluminum wire in the guide groove and the aluminum wire in the oxidation tank are located on the same circular ring; plugging the inlet and outlet holes with a sealing plug, the sealing plug wrapping the aluminum wire; (3) The water inlet and outlet holes are connected to an electrolyte circulation system, and the electrolyte is injected into the oxidation tank through the electrolyte circulation system. The electrode plate and the conductive copper wheel are respectively connected to a micro-arc oxidation / thermal electrochemical oxidation power source, so that the aluminum wire in the oxidation tank undergoes a micro-arc oxidation / thermal electrochemical oxidation reaction while passing through the oxidation tank. After passing through the oxidation tank, the aluminum wire generates an arc-shaped ceramic insulated aluminum wire and is directly wound on the insulating cylinder.