A kind of water-based binder and its preparation method and application

The tragacanth gum and polyacrylic acid water-based binder prepared through crosslinking reaction solve the problem of insufficient cycle stability and rate performance of the positive electrode of lithium sulfur battery. By improving adhesion and dispersion and preventing the shuttle effect, it significantly improves the Cycle stability and rate performance of the battery.

CN115275203BActive Publication Date: 2024-12-03SUN YAT SEN UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210986117.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-16
Publication Date
2024-12-03
Estimated Expiration
2042-08-16

AI Technical Summary

Technical Problem

The current water-based binders of the positive electrode of lithium-sulfur batteries have shortcomings in terms of cycle stability and rate performance, especially due to the performance degradation caused by oxidation, which limits the application potential of the battery.

Method used

The aqueous binder prepared by crosslinking reaction is mainly composed of tragacanth and polyacrylic acid. It uses its hydroxyl and carboxylic active functional groups to improve adhesion and dispersion, and binds to polysulfides through ether bonds to prevent the shuttle effect. Enhance the wetting and ionic conductivity of the electrode and electrolyte.

Benefits of technology

The cycle stability and rate performance of lithium-sulfur batteries are significantly improved, the stability and capacity retention of the battery at high voltages are ensured, and the mechanical integrity and electronic conductivity of the electrodes are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115275203B_ABST
    Figure CN115275203B_ABST
Patent Text Reader

Abstract

The invention discloses an aqueous binder and a preparation method and application thereof, and relates to the technical field of lithium-sulfur batteries. The aqueous binder of the invention is prepared by cross-linking tragacanth gum and polyacrylic acid, and the amount of tragacanth gum and polyacrylic acid added is controlled to obtain an aqueous binder with good adhesion and dispersibility. The aqueous binder is particularly suitable for preparing a positive electrode of a lithium-sulfur battery, can effectively prevent the shuttle effect of the lithium-sulfur battery, and improve the cycle stability and rate performance of the corresponding lithium-sulfur battery. The capacity retention rate of the obtained lithium-sulfur battery is above 89.1%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium-sulfur batteries, and more specifically, to an aqueous binder and a preparation method and application thereof. Background Art

[0002] Lithium-sulfur battery refers to a secondary battery that uses metallic lithium as the negative electrode and sulfur-containing materials as the positive electrode. It has the advantages of high energy density, long cycle life, high safety, and low cost. Therefore, lithium-sulfur batteries are considered to be one of the most promising new generation high-energy storage systems. Sulfur positive electrode materials are mainly composed of three parts, namely active substances, binders, and conductive agents. Although the amount of binder used is very small, it plays a vital role in the performance of the battery. The main function of the binder is to maintain the integrity of the electrode structure. Adding an appropriate amount of binder with excellent performance can obtain a larger capacity and a longer cycle life, and can also reduce the internal resistance of the battery, which has a promoting effect on improving the battery's discharge platform and large current discharge capacity, reducing the internal resistance during low-rate charging, and improving the battery's fast charging ability.

[0003] At present, the commonly used binder for commercial battery positive electrode materials is mainly polyvinylidene fluoride, which has the advantages of easy dispersion, good thermal stability, good electrochemical and chemical stability, and not easy to deteriorate. However, polyvinylidene fluoride has a semi-crystalline structure and a low electrolyte absorption rate, which hinders the circulation of lithium ions in the electrolyte and increases the internal resistance of the battery. In addition, it is a linear binder with poor adhesion. Secondly, the solvent of polyvinylidene fluoride is N-methylpyrrolidone (NMP), which is toxic, and because organic solvents easily absorb moisture, they also have high requirements for air humidity. At present, water-based binders are widely used in new negative electrode materials in the lithium battery industry, but due to the high positive electrode voltage, water-based binders are easily oxidized, resulting in a decrease in the cycle stability and rate performance of the battery. Therefore, the application of water-based binders in the positive electrode needs further development, and it is urgent to develop water-based binders suitable for the positive electrode to improve the rate and cycle performance of the battery.

[0004] The prior art discloses a binder, which includes a lignin derivative and polyacrylic acid. The binder can be prepared and used using deionized water as a solvent, avoiding the use of toxic and highly polluting organic solvents. The binder is an aqueous binder and is suitable for the production of positive electrodes for lithium-ion batteries. However, the cycle stability and rate performance of batteries assembled with positive electrodes prepared using the aqueous binder still need to be improved. Summary of the invention

[0005] In view of the defects and shortcomings of the prior art, the present invention provides an aqueous binder which is applied to the positive electrode of a lithium-sulfur battery, thereby effectively improving the cycle stability and rate performance of the battery.

[0006] Another object of the present invention is to provide a method for preparing a water-based binder.

[0007] Another object of the present invention is to provide an application of an aqueous binder in the preparation of lithium-sulfur battery electrodes.

[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0009] A water-based adhesive is mainly prepared by cross-linking reaction of the following raw materials calculated by weight: 20-45 parts of tragacanth gum and 55-80 parts of polyacrylic acid.

[0010] The inventors found that tragacanth gum contains abundant hydroxyl active functional groups, while polyacrylic acid contains a large number of carboxyl groups. During the cross-linking reaction, the hydroxyl groups of tragacanth gum and the carboxyl groups of polyacrylic acid will be connected to each other, and finally a water-based binder with strong adhesion and dispersibility is obtained. Since the hydroxyl group is a hydrophilic group, the obtained binder is used in the electrode to improve the wettability of the electrode with the electrolyte, ensuring that the inside of the electrode can be infiltrated by the electrolyte, thereby improving the ionic conductivity of the electrode. In addition, when the water-based binder is used as a binder for the positive electrode of a lithium-sulfur battery, since the cross-linked product of tragacanth gum and polyacrylic acid contains a large number of active functional groups such as ether bonds, hydroxyl groups and carboxyl groups, it can adsorb polysulfides, effectively prevent the shuttle effect of the lithium-sulfur battery, and avoid the polysulfide intermediates generated by the positive electrode during the charge and discharge process from dissolving into the electrolyte, and diffusing through the diaphragm to the negative electrode, and directly reacting with the negative electrode metal lithium, resulting in the irreversible loss of active substances in the battery, thereby improving the cycle stability and rate performance of the lithium-sulfur battery.

[0011] In addition, when the amount of tragacanth gum and polyacrylic acid added is too much or too little, the degree of cross-linking will be reduced, resulting in reduced adhesion of the aqueous binder and reduced dispersibility in the electrode, affecting the use effect of the aqueous binder. Therefore, it is necessary to reasonably control the amount of tragacanth gum and polyacrylic acid added.

[0012] Preferably, the weight proportion of tragacanth gum in the raw materials is 30-40 parts, and the weight proportion of polyacrylic acid is 65-75 parts, more preferably, 35 parts of tragacanth gum and 70 parts of polyacrylic acid.

[0013] Preferably, the number average molecular weight of the tragacanth gum is 600,000-1,000,000, and the number average molecular weight of the polyacrylic acid is 300,000-600,000. More preferably, the number average molecular weight of the tragacanth gum is 800,000-900,000, and the number average molecular weight of the polyacrylic acid is 400,000-500,000.

[0014] The molecular weight of tragacanth gum and polyacrylic acid will affect the compatibility of tragacanth gum and polyacrylic acid, further affect the degree of cross-linking between the two, and ultimately affect the performance of the water-based adhesive. In addition, the larger the molecular weight, the worse the solubility of tragacanth gum and polyacrylic acid in water, which affects the mixing during the preparation process.

[0015] Preferably, the number average molecular weight of the tragacanth gum is 800,000, and the number average molecular weight of the polyacrylic acid is 450,000.

[0016] The present invention also specifically protects a method for preparing the water-based binder, comprising the following steps:

[0017] S1. dissolving tragacanth gum and polyacrylic acid in water and mixing them evenly to obtain a mixed solution, wherein the volume ratio of the total mass of the tragacanth gum and polyacrylic acid to water is 0.1 g: (2 to 4) mL;

[0018] S2. Place the mixed solution in S1 in a vacuum environment at 100-160°C for cross-linking reaction, the reaction time is not less than 0.5h, and fully dry after the reaction to obtain a water-based adhesive, wherein the vacuum degree of the vacuum environment is not less than -0.06MPa.

[0019] It should be noted that:

[0020] In S1, the mass volume ratio of the mixture of tragacanth gum and polyacrylic acid to water needs to be controlled to avoid problems of insufficient dissolution or uneven mixing, which will affect the effect of the cross-linking reaction of tragacanth gum and polyacrylic acid in S2.

[0021] When the temperature of the cross-linking reaction in S2 is too low, the cross-linking reaction will be slow or even non-existent. When the temperature is too high, the reaction will be too intense, destroying the structure of the polymer and affecting the use effect of the water-based binder. The obtained water-based binder cannot improve the cycle stability and rate performance of the battery. When the cross-linking reaction time is too short, the cross-linking of tragacanth gum and polyacrylic acid is not sufficient, affecting the performance of the water-based binder.

[0022] The dissolution temperature in S1 is 30 to 100°C, more preferably 60 to 80°C, and even more preferably 60°C.

[0023] When the dissolution temperature is too low, tragacanth gum and polyacrylic acid dissolve slowly, while when the dissolution temperature is too high, water evaporates quickly, affecting the mixing effect of the solution.

[0024] Preferably, the reaction temperature in S2 is 110-130°C, more preferably 120°C.

[0025] Wherein, the reaction time is preferably 0.5 to 2 hours.

[0026] Preferably, the vacuum degree of the vacuum environment is -0.06 to -0.1 MPa.

[0027] If the vacuum is too large, the reaction will be too intense, posing a threat to experimental safety.

[0028] The present invention also protects a use of the aqueous binder in preparing lithium-sulfur battery electrodes.

[0029] The operating voltage range of commonly used lithium-sulfur batteries is 1.5 to 3V, while the applicable voltage of the aqueous binder of the present invention is 0 to 4.6V. The wide range of applicable voltages ensures the use of the aqueous binder in the positive and negative electrodes without reducing the performance of the battery due to oxidation.

[0030] The present invention particularly protects a lithium-sulfur battery positive electrode sheet, comprising a sulfur active material, a conductive additive and a binder, wherein the binder used is the aqueous binder described in the present invention.

[0031] Preferably, the mass ratio of the sulfur active material, the conductive additive and the aqueous binder is (70-95):(3-15):(2-15), more preferably (75-85):(10-17):(5-8), and even more preferably 80:15:5.

[0032] The preparation method of the lithium-sulfur battery positive electrode sheet and the lithium-sulfur battery comprises the following steps:

[0033] S1. The sulfur active material, the conductive additive and the aqueous binder are mixed with water to obtain a mixed slurry, and the mixed slurry is evenly coated on the current collector to obtain a positive electrode sheet;

[0034] S2. Dry and remove water from the positive electrode sheet obtained in S1, cut and weigh the pieces, and then assemble them into lithium-sulfur batteries.

[0035] Wherein, the sulfur active material is one of elemental sulfur, lithium polysulfide, sulfur-based composite materials, organic sulfide, and carbon-sulfur material.

[0036] The conductive additive is one or more of acetylene black, Super P, superconductive carbon black, carbon nanotubes, graphene, and Ketjen black.

[0037] The current collector is one of aluminum foil, aluminum mesh, carbon-coated aluminum foil, nickel mesh, nickel foam, and conductive carbon paper.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] The invention obtains a water-based binder with strong adhesion and dispersibility through a cross-linking reaction of tragacanth gum and polyacrylic acid. The water-based binder has a variety of active groups, can provide multi-directional reaction sites, improve the electronic conductivity of the electrode material, effectively alleviate the volume change of the active material during the charge and discharge process, and maintain the mechanical integrity of the electrode structure.

[0040] The aqueous binder of the present invention is particularly suitable for the positive electrode of lithium-sulfur batteries. The ether bond, hydroxyl group and carboxyl group in tragacanth gum are combined with polysulfide to effectively prevent the shuttle effect in the lithium-sulfur battery, improve the cycle stability and rate performance of the battery, and the capacity retention rate of the obtained lithium-sulfur battery is above 89.1%, and the discharge specific capacity at 2C rate is 656 mAh g -1 When the discharge rate is switched to 0.2C again, the discharge capacity is 853 mAh g -1 above. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 The scanning electron microscope images of electrodes prepared with water-based binders of Example 1 and Comparative Example 4;

[0042] Figure 2 This is a test diagram of electrode adhesion prepared with the aqueous binder of Example 1 and Comparative Example 4;

[0043] Figure 3 The cycle performance test diagram of the battery assembled with the electrodes prepared with the water-based binder of Example 1 and Comparative Example 4;

[0044] Figure 4 The rate performance test diagram of the battery assembled with the electrodes prepared with the aqueous binder of Example 1 and Comparative Example 4;

[0045] Figure 5 The test diagram of the contact angle between the electrode and the electrolyte prepared by the water-based binder of Example 1 and Comparative Example 4;

[0046] Figure 6 This is a diagram of the voltage range of the electrode prepared with the aqueous binder of Example 1. DETAILED DESCRIPTION

[0047] The molecular weight of the tragacanth gum used in the examples and comparative examples of the present invention is 800,000, and the molecular weight of the polyacrylic acid is 450,000, both of which were purchased from the official website of Maclean.

[0048] The present invention will be further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form.

[0049] Example 1

[0050] A water-based adhesive comprises the following raw materials by weight: 35 parts of tragacanth gum and 70 parts of polyacrylic acid.

[0051] The preparation method of the water-based binder comprises the following steps:

[0052] S1. Add tragacanth gum and polyacrylic acid into a sample bottle, add water to dissolve at 60°C, and mix well to obtain a mixed solution, wherein the volume ratio of the total mass of tragacanth gum and polyacrylic acid to water is 0.1 g:3 mL;

[0053] S2. The mixed solution in S1 is placed in a vacuum environment at 120°C for a cross-linking reaction. The reaction time is 1 hour and the vacuum degree is -0.08MPa. After the reaction, the reaction product is dried at 80°C for 24 hours to obtain a water-based adhesive.

[0054] Embodiments 2 to 16

[0055] A water-based binder, the preparation method is the same as that of Example 1, and the differences are shown in Table 1.

[0056] Table 1. Parameters of water-based binders for Examples 1 to 16

[0057]

[0058]

[0059] Comparative Example 1

[0060] A water-based adhesive, the preparation method is the same as that of Example 1, except that the weight portion of tragacanth gum is 10 parts.

[0061] Comparative Example 2

[0062] A water-based adhesive, the preparation method is the same as that of Example 1, except that the weight portion of tragacanth gum is 55 parts.

[0063] Comparative Example 3

[0064] A water-based adhesive, the preparation method is the same as that of Example 1, except that the weight portion of polyacrylic acid is 45 parts.

[0065] Comparative Example 4

[0066] A water-based adhesive, the preparation method is the same as that of Example 1, except that the weight percentage of polyacrylic acid is 90 parts.

[0067] Comparative Example 5

[0068] A water-based adhesive, the preparation method is the same as that of Example 1, except that the weight portion of tragacanth gum is 0 part.

[0069] Comparative Example 6

[0070] A water-based adhesive, the preparation method is the same as that of Example 1, except that the weight portion of polyacrylic acid is 0 part.

[0071] Comparative Example 7

[0072] A method for preparing a water-based binder, the steps are the same as those of Example 1, except that the reaction temperature in S2 is 80°C.

[0073] Comparative Example 8

[0074] A method for preparing a water-based binder, the steps are the same as those of Example 1, except that the vacuum degree in S2 is -0.03 MPa.

[0075] Results

[0076] The aqueous binders of the above examples and comparative examples are used to prepare lithium-sulfur batteries, and the preparation method is as follows:

[0077] S1. Weigh 0.8 g of elemental sulfur, 0.15 g of carbon nanotubes and 0.05 g of an aqueous binder, add water and mix to obtain a mixed slurry, and evenly coat the mixed slurry on a carbon-coated aluminum foil to obtain a positive electrode sheet;

[0078] S2. Dry the positive electrode sheet obtained in S1 to remove water, cut it into pieces, weigh it, and assemble it into a lithium-sulfur battery.

[0079] The cycle stability of the lithium-sulfur battery is tested in the following manner:

[0080] Test 1: The battery's charge and discharge cycle performance was tested at a voltage range of 1.7-2.8V and a rate of 0.5C, expressed as the capacity retention rate after 300 cycles.

[0081] Test 2: The voltage range is 1.7-2.8V. The discharge rate is switched in the order of 0.2C, 0.5C, 1C, 2C, and 0.2C to test the discharge capacity of the battery. The rate performance is evaluated. At the same rate, the larger the discharged capacity, the better the rate performance.

[0082] The test results are shown in Table 2.

[0083] Table 2. Performance test results of lithium-sulfur batteries assembled with the aqueous binder

[0084]

[0085]

[0086] From the data in Table 2, it can be seen that the capacity retention rate of the battery assembled with the electrodes prepared with the aqueous binder in Examples 1 to 16 is above 89.1%, and the discharge specific capacity at a rate of 0.2C is 912 mAh g -1 The discharge capacity at 0.5C rate is 788 mAh g -1 The discharge capacity at 1C rate is 713 mAh g -1The discharge capacity at 2C rate is 656 mAh g -1 When the discharge rate is switched to 0.2C again, the discharge capacity is still 853 mAh g -1 The above results show good rate performance. Comparative Examples 1-2 and Comparative Examples 3-4 are the results of exceeding the range of the amount of tragacanth gum added and the range of the amount of polyacrylic acid added, respectively. It can be seen that when the amount of tragacanth gum and polyacrylic acid is too much or too little, the positive electrode prepared by the obtained aqueous binder is assembled into a lithium-sulfur battery. The battery capacity retention rate and rate performance are significantly reduced. This is because tragacanth gum and polyacrylic acid are both polymers, and the amount of the two has good compatibility within a certain range, so that they can achieve full cross-linking and obtain a water-based binder with better effect. However, when the amount exceeds the range described in the present invention, the cross-linking effect is significantly reduced, and the performance of the water-based binder is also reduced.

[0087] Figure 1 Shown are scanning electron microscope images of electrodes prepared with water-based binders of Example 1 and Comparative Example 4. It can be seen that the electrode prepared with the water-based binder in Example 1 has a complete structure, the active material is evenly distributed, and no cracks are generated. However, it can be clearly seen that the electrode prepared with the water-based binder in Comparative Example 4 has an uneven surface, poor dispersion of the active material, and cracks. This is because the amount of polyacrylic acid added to the water-based binder is too large, resulting in a low degree of crosslinking between tragacanth gum and polyacrylic acid, which reduces the adhesion and dispersibility of the water-based binder.

[0088] Comparison of the adhesion of electrodes prepared with aqueous binders of Example 1 and Comparative Example 4 Figure 2 As shown, the ordinate represents the adhesion of the aqueous binder to the active material and the current collector. It can be seen that the adhesion of the aqueous binder obtained in Example 1 to the active material and the current collector is stronger than that of Comparative Example 4. Therefore, the positive electrode sheet made of the aqueous binder in Example 1 can better maintain the integrity of the electrode structure during the battery cycle, which further illustrates that excessive addition of polyacrylic acid will affect the adhesion of the aqueous binder.

[0089] Figure 3 The cycle performance test diagram of the battery assembled with the electrodes prepared with the aqueous binder of Example 1 and Comparative Example 4, from which the initial discharge specific capacity and capacity retention rate of the battery can be obtained, it can be seen that the initial specific capacity and capacity retention rate of the battery corresponding to the electrode prepared with the aqueous binder of Example 1 are better than those of Comparative Example 4. In addition, Figure 4It can be seen from the rate performance test results of the batteries assembled with the electrodes prepared with the aqueous binders of Example 1 and Comparative Example 4 that at the rates of 0.2C, 0.5C, 1C, 2C, and 0.2C, the discharge specific capacity of the lithium-sulfur battery finally obtained with the aqueous binder of Example 1 is higher than that of Comparative Example 4 at different rates, indicating that after the electrodes prepared with the aqueous binder in Example 1 are assembled into a lithium-sulfur battery, the cycle stability and rate performance of the battery are improved.

[0090] Figure 5 The test diagram of the contact angle between the electrode and the electrolyte prepared by the aqueous binder of Example 1 and Comparative Example 4. The smaller the contact angle, the better the wettability between the electrode and the electrolyte. As can be seen from the figure, the contact angle between the electrode and the electrolyte of Example 1 is 16°, which is much lower than the contact angle (47°) of Comparative Example 4, indicating that the aqueous binder obtained by the technical solution of the present invention can make the positive electrode sheet and the electrolyte have good wettability, thereby improving the electrochemical performance.

[0091] Figure 6 This is a voltage range diagram of the electrode prepared with the aqueous binder of Example 1. It can be seen from the figure that the electrode is stable in the voltage range of 0 to 4.6 V and no electrochemical reaction occurs, indicating that the electrode prepared with the aqueous binder of the present invention has a wide applicable voltage range and can be applied to lithium-sulfur battery electrodes.

[0092] It should be noted that, although the remaining embodiments do not provide corresponding scanning electron microscope images, wettability images and voltage range images, the electrodes prepared therefrom also have complete structures and uniform distribution of active materials, and the obtained positive electrode sheets and electrolytes also have good wettability and also have a wide voltage range; adhesion images and discharge specific capacity images are also not provided, but it can be seen from Table 2 that the remaining embodiments also have the effect of improving the cycle stability and rate performance of the assembled lithium-sulfur battery.

[0093] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A water-based adhesive, characterized in that: The invention is mainly prepared by cross-linking reaction of the following raw materials calculated by weight: 20-45 parts of tragacanth gum and 55-80 parts of polyacrylic acid. The temperature of the cross-linking reaction is 100-160 DEG C and the vacuum degree of the cross-linking reaction is not less than -0.06MPa.

2. The water-based adhesive according to claim 1, characterized in that: The weight proportion of tragacanth gum in the raw materials is 30-40 parts, and the weight proportion of polyacrylic acid is 65-75 parts.

3. The water-based adhesive according to claim 1, characterized in that: The number average molecular weight of the tragacanth gum is 600,000-1,000,000, and the number average molecular weight of the polyacrylic acid is 300,000-600,000.

4. The water-based adhesive according to claim 3, characterized in that: The number average molecular weight of the tragacanth gum is 800,000, and the number average molecular weight of the polyacrylic acid is 450,000.

5. The method for preparing the water-based binder according to any one of claims 1 to 4, characterized in that: The steps include: S1. dissolving tragacanth gum and polyacrylic acid in water and mixing them evenly to obtain a mixed solution, wherein the volume ratio of the total mass of the tragacanth gum and polyacrylic acid to water is 0.1 g: (2 to 4) mL; S2. Place the mixed solution in S1 in a vacuum environment at 100-160°C for cross-linking reaction, the reaction time is not less than 0.5h, and fully dry after the reaction to obtain a water-based adhesive, wherein the vacuum degree of the vacuum environment is not less than -0.06MPa.

6. The preparation method according to claim 5, characterized in that: The reaction temperature in S2 is 110-130°C.

7. The preparation method according to claim 5, characterized in that: The vacuum degree of the vacuum environment is -0.06 to -0.1 MPa.

8. Use of the aqueous binder according to any one of claims 1 to 4 in the preparation of lithium-sulfur battery electrodes.

9. A lithium-sulfur battery positive electrode sheet, comprising a sulfur active material, a conductive additive and a binder, characterized in that: The binder is the water-based binder according to any one of claims 1 to 4.

10. The positive electrode sheet of a lithium-sulfur battery as claimed in claim 9, characterized in that: The mass ratio of the sulfur active material, the conductive additive and the aqueous binder is (70-95):(3-15):(2-15).

Citation Information

Patent Citations

  • Preparation method for positive plate of lithium-sulfur battery

    CN102569730A

  • Polymer solution and cosmetic article for cleaning and nursing skin

    CN1262921A

  • Method for producing radical material composition, active material for secondary battery, electrode for the secondary battery, and the secondary battery

    JP2013184981A

  • Crosslinking agent, crosslinked polymer, and their applications

    JP2014205826A

  • Binder for lithium ion secondary battery negative electrode

    JP2014209469A