Matt polyvinyl chloride resin and preparation method thereof

By incorporating modified zeolite powder into the suspension polymerization process, matte polyvinyl chloride resin was prepared, resolving the contradiction between matting and processing performance, achieving better matting effect and processing performance, while also improving thermal stability.

CN115286729BActive Publication Date: 2024-11-22SHANGHAI CHLOR ALKALI CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211114508.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-14
Publication Date
2024-11-22
Estimated Expiration
2042-09-14

AI Technical Summary

Technical Problem

While existing matting polyvinyl chloride resins improve the matting effect, their processing performance and mechanical properties are often affected, making it difficult to achieve excellent matting and processing performance at the same time.

Method used

Zeolite powder was added during the polymerization process and modified to prepare matte polyvinyl chloride resin through suspension polymerization. The zeolite was enriched on the surface of monomer droplets to provide mechanical isolation, thereby reducing the gloss of the resin and improving its processing performance.

Benefits of technology

The prepared matting polyvinyl chloride resin has better matting effect and processing performance, while also possessing better thermal stability, overcoming the problem of processing difficulties for resins with high gel content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003844897810000101
    Figure BDA0003844897810000101
Patent Text Reader

Abstract

Matt polyvinyl chloride resin and preparation method thereof. A matte polyvinyl chloride resin and preparation method thereof are provided. The matte polyvinyl chloride is prepared as follows: (1) adding vinyl chloride monomer, initiator, zeolite, crosslinking agent and dispersant to an aqueous solvent to obtain a dispersion; and (2) performing suspension polymerization in the dispersion to obtain the matte polyvinyl chloride.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a matte polyvinyl chloride resin and a preparation method thereof, and more specifically to a matte polyvinyl chloride resin with better comprehensive performance and a preparation method thereof. The obtained matte polyvinyl chloride resin has better matte property and better processing performance. Background Art

[0002] Polyvinyl chloride resin is one of the five general-purpose resins. It has many advantages such as high physical properties, good processing performance, corrosion resistance and low price.

[0003] Matt polyvinyl chloride resin is one of the common polyvinyl chloride specialty resins. Compared with ordinary polyvinyl chloride resin, matte polyvinyl chloride resin contains some tetrahydrofuran (THF) insoluble parts (gel). During the processing of this resin, the gel structure deforms, rotates and orients in the continuous phase, and then as the temperature decreases, the material changes from a viscous flow state to a highly elastic state and a glassy state. Due to the structural difference between gel and sol, during the transition process, the relaxation and viscoelasticity of the gel structure are very different from those of the sol continuous phase, resulting in tiny bumps and depressions on the surface of the product, thus producing matte properties.

[0004] Generally speaking, the main method to enhance the matte effect of polyvinyl chloride resin is to increase the amount of crosslinking agent and improve the gel content. However, this method will seriously affect the processing performance of the matte resin, making it difficult to use in practice. Another method is from a pure processing perspective. In the actual processing formula, a large amount of inorganic fillers are added. However, doing so will seriously affect the mechanical properties of the finished product.

[0005] Therefore, there is an urgent need for a new matte polyvinyl chloride resin in the art, which has both excellent matte properties and processing properties (mechanical properties). Summary of the invention

[0006] The purpose of the present application is to provide a matte polyvinyl chloride resin and a preparation method thereof, wherein the resin has both excellent matte properties and processing properties (mechanical properties).

[0007] After extensive research, the inventors of the present application have found that zeolite can be added during the polymerization of polyvinyl chloride resin. Zeolite is a tiny solid powder that is insoluble in water. It is enriched on the surface of monomer droplets and plays a role in mechanical isolation. At the same time, the addition of zeolite can also effectively reduce the glossiness of the finished resin, and the matte effect is more obvious than adding inorganic fillers during post-processing. In addition, zeolite can be modified to make it more effectively integrated with PVC resin, so as to further improve the processing performance of the resulting matte polyvinyl chloride resin.

[0008] Based on the above findings, the present application provides a matte polyvinyl chloride resin on one hand, wherein the matte polyvinyl chloride is prepared as follows:

[0009] (1) adding vinyl chloride monomer, initiator, zeolite, crosslinking agent and dispersant into an aqueous solvent to obtain a dispersion; and

[0010] (2) Suspension polymerization is carried out in the dispersion to obtain matte polyvinyl chloride.

[0011] On the other hand, the present application provides a method for preparing a matte polyvinyl chloride resin, the method comprising the following steps:

[0012] (1) adding vinyl chloride monomer, initiator, zeolite, crosslinking agent and dispersant into an aqueous solvent to obtain a dispersion; and

[0013] (2) Suspension polymerization is carried out in the dispersion to obtain matte polyvinyl chloride. DETAILED DESCRIPTION

[0014] Compared with ordinary matting resins, the matting polyvinyl chloride prepared by using zeolite in the present application has better matting effect and better processing performance. At the same time, due to the characteristics of zeolite, the matting resin of the present application has better thermal stability. Therefore, the present application provides a matting polyvinyl chloride resin with better comprehensive performance, while overcoming the problem of difficulty in processing high gel content resins.

[0015] On one hand, the present application provides a matte polyvinyl chloride resin, wherein the matte polyvinyl chloride is prepared as follows:

[0016] (1) adding vinyl chloride monomer, initiator, zeolite, crosslinking agent and dispersant into an aqueous solvent to obtain a dispersion; and

[0017] (2) Suspension polymerization is carried out in the dispersion to obtain matte polyvinyl chloride.

[0018] Unless otherwise stated herein, the reactions are all carried out at room temperature and pressure.

[0019] In this document, unless otherwise specified, the amounts of materials are all based on weight.

[0020] Herein, unless otherwise specified, the reaction steps may be performed sequentially, in any order or simultaneously.

[0021] In this document, unless otherwise specified, the term "zeolite" or "zeolite powder" has the same meaning.

[0022] In the method of the present application, the vinyl chloride monomer can be any vinyl chloride monomer commonly used in the art, and can be a product derived from petroleum cracking, or a product derived from calcium carbide gas. Generally, the vinyl chloride monomer refers to 1-vinyl chloride, which can be easily synthesized by a method commonly used in the art (such as the addition reaction of hydrogen chloride and acetylene), or can be obtained commercially.

[0023] The initiator suitable for the present application can adopt high, medium and low active organic peroxide initiators according to different polymerization temperatures. Preferably, an organic peroxide composite initiation system can be used, such as cumyl peroxyneodecanoate (Tx99), 2,4,4-trimethylpentyl peroxyneodecanoate (Tx423), bis-(2-ethylhexyl peroxydicarbonate) (EHP), tert-butyl peroxyneodecanoate (Tx23), tert-butyl peroxyneoheptanoate (Tx257), tert-pentyl peroxypivalate (Tx125), tert-butyl peroxypivalate (Tx25), bis-(3,5,5-trimethylhexanoyl peroxide) (Tx36), dilauroyl peroxide (LPO) or a combination thereof.

[0024] In the present application, the amount of the initiator is conventional. In a preferred embodiment, based on 100 parts by weight of vinyl chloride monomer, the amount of the initiator added is 0.01 to 4.5 parts by weight, such as 0.05 to 2.5 parts by weight, more preferably 0.05 to 0.5 parts by weight, and even more preferably 0.08 to 0.2 parts by weight.

[0025] The zeolite suitable for this application can use the common zeolite powder on the market, for example, zeolite powder of 100-400 mesh (for example, 100-300 mesh, preferably 150-250 mesh) can be used. The zeolite powder can be but is not limited to clinoptilolite, mordenite, analcime, chabazite or a combination thereof. In one example of the present application, the zeolite powder can be purchased from, for example, the Z-PVC heat stabilizer special zeolite of Chalco Shandong Co., Ltd., and the 4A special zeolite for PVC stabilization of Zibo Wandou New Materials Co., Ltd. In a preferred example, the zeolite powder can be physically modified or grafted to improve the comprehensive performance of the matte polyvinyl chloride resin. Generally, the physical modification includes stirring the zeolite powder under heating conditions (for example, 70-200°C, preferably 80-180°C, more preferably 100-150°C); the grafting modification method includes surface grafting modification of the zeolite powder with a surface modifier. The surface modifier may include but is not limited to fatty acid glycerides (e.g., C6-C20 fatty acid glycerides, including but not limited to C6-C20 fatty acid monoglycerides), polyvinyl alcohol or a combination thereof. In one example of the present application, the C6-C20 fatty acid monoglycerides include but are not limited to glyceryl monostearate, glyceryl monolaurate, glyceryl monooleate or a combination thereof. In a preferred embodiment, the surface modifier and zeolite powder are mixed in a weight ratio of 1:1 to 1:10 (e.g., 1:1 to 1:6, preferably 1:1 to 1:4, more preferably 1:2 to 1:3), and then stirred evenly under heating (e.g., 40-150°C, preferably 50-120°C, more preferably 60-100°C), and finally dried to obtain modified zeolite powder.

[0026] In one embodiment of the present application, zeolite powder and surface modifier are stirred and mixed in heated water (e.g., 40-150° C., preferably 50-120° C., more preferably 60-100° C.) The stirring and mixing time can be, for example, 1-20 hours, preferably 2-15 hours, more preferably 5-12 hours, and most preferably 8-10 hours.

[0027] In the present application, the amount of the zeolite can be determined according to the desired performance. In a preferred embodiment, based on 100 parts by weight of vinyl chloride monomer, the amount of the zeolite added is 0.1 parts by weight to 30 parts by weight, such as 1 part by weight to 20 parts by weight, more preferably 2 parts by weight to 15 parts by weight, and even more preferably 5 parts by weight to 10 parts by weight.

[0028] The dispersant applicable to the present application may be a commonly used dispersant in the art to carry out suspension polymerization of vinyl chloride monomer. Generally, the dispersant includes but is not limited to a binary PVA composite dispersion system (optionally a third component dispersant may be used); a PVA and cellulose ether (such as hydroxypropyl methyl cellulose ether, etc.) composite dispersion system (optionally used together with a third component PVA dispersant). Examples of dispersants that can be used include PVA dispersant KH20 with a higher degree of polymerization of 2000 and a degree of alcoholysis of about 80 mol%; hydroxypropyl methylcellulose dispersant E50 from DOW Chemical Company of the United States; PVA dispersant B72 with a degree of polymerization of 700 and a degree of alcoholysis of 72 mol% from Harco Company of the United Kingdom; PVA dispersant L-9-78 with a higher "cloud point" and a degree of alcoholysis of 76.5-79.0 mol% from Kuraray Company of Japan; PVA dispersant LM22 with a degree of polymerization of 250 and a degree of alcoholysis of 47.0-53.0 mol% from Kuraray Company of Japan; PVA dispersant LW300 with a degree of polymerization of 250 and a degree of alcoholysis of 53.0-60.0 mol% from Synthetic Chemical Company of Japan, and the like.

[0029] In the present application, the amount of the dispersant is conventional. In a preferred embodiment, based on 100 parts by weight of vinyl chloride monomer, the amount of the dispersant added is 0.01 to 5 parts by weight, such as 0.05 to 2 parts by weight, more preferably 0.1 to 1 part by weight, and even more preferably 0.2 to 0.5 parts by weight.

[0030] In the method of the present application, the aqueous solvent may be an aqueous solvent commonly used in the art, including but not limited to water, such as deionized water, desalted water, distilled water, and the like.

[0031] In the method of the present application, a cross-linking agent is further added to the aqueous solvent. The cross-linking agent may be a cross-linking agent commonly used in the art, including but not limited to one or more of diallyl phthalate, ethylene glycol diacrylate, glycerol diglycidyl ether diacrylate, dimethyl diacrylate, ethylene glycol dimethacrylate, maleic acid diallyl ester, trimethylolpropane trimethacrylate, trimethylolpropane acrylate, pentaerythritol triacrylate, and pentaerythritol tetraacrylate.

[0032] In the present application, the amount of the crosslinking agent is conventional. In a preferred embodiment, based on 100 parts by weight of vinyl chloride monomer, the amount of the crosslinking agent added is 0.01 parts by weight to 10 parts by weight, such as 0.1 parts by weight to 6 parts by weight, more preferably 0.5 parts by weight to 4 parts by weight, and even more preferably 0.8 parts by weight to 0.2 parts by weight. The preferred addition amount range of the crosslinking agent can be determined according to the type of crosslinking agent and the polymerization temperature. The gel content of the resin thus obtained is 0.5 to 50%, and the optimal content is 10 to 40%. If the gel content is too low, the matte effect of the product will be affected; if it is too high, the processing performance of the resin will be affected.

[0033] The crosslinking agent can be added within a certain period of time after the polymerization reaction starts, or before the polymerization reaction starts. The crosslinking agent can be added all at once, or added in batches or by using a metering pump. Different addition times and addition methods determine the range of gel content and degree of polymerization of the matting resin.

[0034] During the suspension polymerization of vinyl chloride, the pH value of the system affects the polymerization rate and the dispersing effect of the dispersant. The pH value of the system is generally controlled to be neutral to alkaline, so it is preferred to add a pH adjuster to adjust the pH value of the reaction system. The pH adjuster suitable for this application can be an alkaline substance, such as an inorganic acid alkali metal salt, such as NaHCO3, or a NH4 + The pH buffering agent. The film structure of the resin particles can be improved by adding a pH adjusting agent. The amount of the pH adjusting agent added is conventional, for example, the amount added is 0.001-1 parts by weight, preferably 0.01-0.5 parts by weight.

[0035] In a preferred embodiment of the present application, the present application provides a matte polyvinyl chloride resin, and the matte polyvinyl chloride is prepared as follows:

[0036] (1) providing a modified zeolite;

[0037] (2) Add vinyl chloride monomer, initiator, modified zeolite, crosslinking agent and dispersant into an aqueous solvent to obtain a dispersion.

[0038] (3) Suspension polymerization is carried out in the dispersion to obtain matte polyvinyl chloride.

[0039] The zeolite suitable for the present application can use the common zeolite powder on the market, for example, zeolite powder of 100-400 mesh (for example, 100-300 mesh, preferably 150-250 mesh) can be used. The zeolite powder can be but is not limited to clinoptilolite, mordenite, analcime, chabazite or a combination thereof. In one example of the present application, the zeolite powder can be purchased from, for example, the Z-PVC heat stabilizer special zeolite of Chalco Shandong Co., Ltd., and the 4A special zeolite for PVC stabilization of Zibo Wandou New Materials Co., Ltd. Preferably, the step of providing a modified zeolite includes physically modifying the zeolite powder or surface grafting the zeolite powder with a surface modifier. Typically, the physical modification includes stirring the zeolite powder under heating conditions (for example, 70-200°C, preferably 80-180°C, and more preferably 100-150°C). The surface modifier may include but is not limited to fatty acid glycerides (e.g., C6-C20 fatty acid glycerides, including but not limited to C6-C20 fatty acid monoglycerides), polyvinyl alcohol or a combination thereof. In one example of the present application, the C6-C20 fatty acid monoglycerides include but are not limited to glyceryl monostearate, glyceryl monolaurate, glyceryl monooleate or a combination thereof. In a preferred embodiment, the surface modifier and zeolite powder are mixed in a weight ratio of 1:1 to 1:10 (e.g., 1:1 to 1:6, preferably 1:1 to 1:4, more preferably 1:2 to 1:3), and then stirred evenly under heating (e.g., 40-150°C, preferably 50-120°C, more preferably 60-100°C), and finally dried to obtain modified zeolite powder.

[0040] In one embodiment of the present application, the zeolite powder and the surface modifier are stirred and mixed in water heated (e.g., 40-150° C., preferably 50-120° C., more preferably 60-100° C.) for 1-20 hours, preferably 2-15 hours, more preferably 5-12 hours, and most preferably 8-10 hours.

[0041] On the other hand, the present application provides a method for preparing a matte polyvinyl chloride resin, the method comprising:

[0042] (1) Vinyl chloride monomer, initiator, zeolite, crosslinking agent and dispersant are added to an aqueous solvent to obtain a dispersion.

[0043] (2) Suspension polymerization is carried out in the dispersion to obtain matte polyvinyl chloride.

[0044] In a preferred embodiment of the present application, the method comprises the following steps:

[0045] (1) providing a modified zeolite;

[0046] (2) Add vinyl chloride monomer, initiator, modified zeolite, crosslinking agent and dispersant into an aqueous solvent to obtain a dispersion.

[0047] (3) Suspension polymerization is carried out in the dispersion to obtain matte polyvinyl chloride.

[0048] The modified zeolite is obtained by physically modifying or grafting the zeolite powder or a combination thereof in a barrel to improve the comprehensive performance of the matte polyvinyl chloride resin. Generally, the physical modification includes stirring the zeolite powder under heating conditions (e.g., 70-200°C, preferably 80-180°C, more preferably 100-150°C); the grafting modification method includes surface grafting modification of the zeolite powder with a surface modifier. The surface modifier may include but is not limited to fatty acid glycerides (e.g., C6-C20 fatty acid glycerides, including but not limited to C6-C20 fatty acid monoglycerides), polyvinyl alcohol or a combination thereof. In one example of the present application, the C6-C20 fatty acid monoglycerides include but are not limited to glyceryl monostearate, glyceryl monolaurate, glyceryl monooleate or a combination thereof. In a preferred embodiment, the surface modifier and zeolite powder are mixed in a weight ratio of 1:1 to 1:10 (e.g., 1:1 to 1:6, preferably 1:1 to 1:4, more preferably 1:2 to 1:3), then stirred evenly under heating (e.g., 40-150°C, preferably 50-120°C, more preferably 60-100°C), and finally dried to obtain the modified zeolite powder.

[0049] In one embodiment of the present application, zeolite powder and surface modifier are stirred and mixed in heated water (e.g., 40-150° C., preferably 50-120° C., more preferably 60-100° C.) The stirring and mixing time can be, for example, 1-20 hours, preferably 2-15 hours, more preferably 5-12 hours, and most preferably 8-10 hours.

[0050] Compared with common matt resins, the matt polyvinyl chloride resin obtained by the present invention has better matt effect, better processing performance and better comprehensive performance, and can effectively improve the comprehensive performance of the resin.

[0051] In order to make the technical means, creative features, objectives and effects of the present application easier to understand, the present invention is further described below in conjunction with specific embodiments, but the following embodiments are only preferred embodiments of the present invention, and the protection scope of the present application is not limited thereto.

[0052] Example 1

[0053] The following raw materials were provided: 100 kg of vinyl chloride monomer, 0.25 kg of dispersant (KH20 / E50 / LM22), 5 kg of modified zeolite, 0.1 kg of initiator (EHP), 0.02 kg of pH adjuster (sodium bicarbonate), 1.2 kg of cross-linking agent (polyethylene glycol diallyl ester), and 240 kg of desalted water.

[0054] First, zeolite modification is performed. Pour 5 kg of zeolite powder (zeolite for Z-PVC heat stabilizer produced by Shandong Chalco Co., Ltd.) into the kettle, and then pour in 50 kg of water and stir. The stirring speed is 200 rpm. While stirring, add 2.5 kg of glyceryl monostearate. At the same time, raise the water temperature to 80°C and mix the molten glyceryl monostearate and zeolite powder thoroughly in a ratio of 1:2. After stirring for 8 hours, a mixture is obtained. After that, after drying at an air temperature of 90°C for 2 hours, the final product is obtained.

[0055] Afterwards, the obtained modified zeolite, dispersant, pH adjuster, crosslinking agent and water are added into the polymerization kettle, and vacuum is applied after the addition.

[0056] Add vinyl chloride monomer into the polymerization kettle and start stirring. After stirring for 10 minutes, add the initiator. Then, raise the temperature to 57°C until the reaction is completed. The reaction time is 5.25 hours.

[0057] After the reaction was completed, 0.5 kg of acetone thiosemicarbazone was added as a terminator to terminate the reaction, and the material was discharged after the pressure dropped to 0.15 MPa.

[0058] Example 2

[0059] The following raw materials were provided: 100 kg of vinyl chloride monomer, 0.25 kg of dispersant (KH20 / E50 / LM22), 10 kg of modified zeolite, 0.1 kg of initiator (EHP), 0.02 kg of pH adjuster (sodium bicarbonate), 1.2 kg of cross-linking agent (polyethylene glycol diallyl ester), and 240 kg of desalted water.

[0060] First, zeolite modification was performed. 10 kg of zeolite powder (zeolite for Z-PVC heat stabilizer produced by Shandong Chalco Co., Ltd.) was poured into the kettle, and then 100 kg of water was poured in and stirred at 200 rpm. While stirring, 3.33 kg of glyceryl monostearate was added. At the same time, the water temperature was raised to 80°C, and the molten monoglyceride and zeolite powder were fully mixed in a ratio of 1:3. After stirring for 10 hours, a mixture was obtained. After that, it was dried at an air temperature of 90°C for 3 hours to obtain the final product. .

[0061] Afterwards, the obtained modified zeolite, dispersant, pH adjuster, crosslinking agent and water are added into the polymerization kettle, and vacuum is applied after the addition.

[0062] Add vinyl chloride monomer into the polymerization kettle and start stirring. After stirring for 15 minutes, add the initiator. Then, raise the temperature to 57°C until the reaction is completed. The reaction time is 5.38 hours.

[0063] After the reaction was completed, 0.5 kg of acetone thiosemicarbazone was added as a terminator to terminate the reaction, and the material was discharged after the pressure dropped to 0.15 MPa.

[0064] Example 3

[0065] The following raw materials were provided: 100 kg of vinyl chloride monomer, 0.25 kg of dispersant (KH20 / E50 / LM22), 5 kg of modified zeolite, 0.1 kg of initiator (EHP), 0.02 kg of pH adjuster (sodium bicarbonate), 1.2 kg of cross-linking agent (polyethylene glycol diallyl ester), and 240 kg of desalted water.

[0066] First, zeolite modification is performed. First, 5 kg of zeolite powder (zeolite for Z-PVC heat stabilizer of Chalco Shandong Co., Ltd.) is poured into the kettle, and then 50 kg of water is poured in and stirred. The stirring speed is 200 rpm. While stirring, 2.5 kg of glyceryl monostearate is added. At the same time, the water temperature is raised to 80°C, and the molten monoglyceride and zeolite powder are fully mixed in a ratio of 1:2. After stirring for 8 hours, a mixture is obtained. After that, after drying at an air temperature of 90°C for 2 hours, the final product is obtained.

[0067] Afterwards, the obtained modified zeolite, dispersant, pH adjuster, crosslinking agent and water are added into the polymerization kettle, and vacuum is applied after the addition.

[0068] Add vinyl chloride monomer into the polymerization kettle and start stirring. After stirring for 10 minutes, add the initiator. Then, raise the temperature to 57°C until the reaction is completed. The reaction time is 5.30 hours.

[0069] After the reaction was completed, 0.5 kg of acetone thiosemicarbazone was added as a terminator to terminate the reaction, and the material was discharged after the pressure dropped to 0.15 MPa.

[0070] Example 4

[0071] The following raw materials were provided: 100 kg of vinyl chloride monomer, 0.25 kg of dispersant (KH20 / E50 / LM22), 5 kg of modified zeolite, 0.1 kg of initiator (EHP), 0.02 kg of pH adjuster (sodium bicarbonate), 1.2 kg of cross-linking agent (polyethylene glycol diallyl ester), and 240 kg of desalted water.

[0072] First, zeolite modification was performed. 5 kg of zeolite powder (zeolite for Z-PVC heat stabilizer produced by Chalco Shandong Co., Ltd.) was poured into a mixing kettle for direct physical modification. The stirring speed was 500 rpm. After the temperature was raised to 130°C, it was directly cooled to obtain the final product.

[0073] Afterwards, the obtained modified zeolite, dispersant, pH adjuster, crosslinking agent and water are added into the polymerization kettle, and vacuum is applied after the addition.

[0074] Add vinyl chloride monomer into the polymerization kettle and start stirring. After stirring for 10 minutes, add the initiator. Then, raise the temperature to 57°C until the reaction is completed. The reaction time is 5.50 hours.

[0075] After the reaction was completed, 0.5 kg of acetone thiosemicarbazone was added as a terminator to terminate the reaction, and the material was discharged after the pressure dropped to 0.15 MPa.

[0076] Example 5

[0077] The following raw materials were provided: 100 kg of vinyl chloride monomer, 0.25 kg of dispersant (KH20 / E50 / LM22), 5 kg of zeolite, 0.1 kg of initiator (EHP), 0.02 kg of pH adjuster (sodium bicarbonate), 1.2 kg of cross-linking agent (polyethylene glycol diallyl ester), and 240 kg of desalted water.

[0078] 5 kg of unmodified ordinary zeolite powder (zeolite for Z-PVC heat stabilizer produced by Chalco Shandong Co., Ltd.), dispersant, pH adjuster, crosslinking agent and water were added into the polymerization kettle, and vacuum was applied after the addition.

[0079] Add vinyl chloride monomer into the polymerization kettle and start stirring. After stirring for 10 minutes, add the initiator. Then, raise the temperature to 57°C until the reaction is completed. The reaction time is 5.50 hours.

[0080] After the reaction was completed, 0.5 kg of acetone thiosemicarbazone was added as a terminator to terminate the reaction, and the material was discharged after the pressure dropped to 0.15 MPa.

[0081] Comparative Example 1

[0082] The following raw materials were provided: 100 kg of vinyl chloride monomer, 0.25 kg of dispersant (KH20 / E50 / LM22), 0.1 kg of initiator (EHP), 0.02 kg of pH adjuster (sodium bicarbonate), 1.2 kg of cross-linking agent (polyethylene glycol diallyl ester), and 240 kg of desalted water.

[0083] Add dispersant, pH adjuster, crosslinking agent and water into the polymerization kettle, and then evacuate the kettle.

[0084] Add vinyl chloride monomer into the polymerization kettle and start stirring. After stirring for 10 minutes, add the initiator. Then, raise the temperature to 57°C until the reaction is completed. The reaction time is 5.47 hours.

[0085] After the reaction was completed, 0.5 kg of acetone thiosemicarbazone was added as a terminator to terminate the reaction, and the material was discharged after the pressure dropped to 0.15 MPa.

[0086] The polymers obtained in Examples 1-5 and Comparative Example 1 were analyzed and tested. Test resin particles were prepared according to the proportions in the following table, and then the plasticization time of the resins obtained in the Examples and Comparative Examples was tested by a HAKKE rheometer. The processing temperature was 160°C. The units of the amounts of each component in the following table are kg. The stabilizer was Rohm and Haas organotin TM181, the plasticizer was Qilu Petrochemical DOP, and the titanium dioxide was DuPont r105.

[0087] Then, the glossiness of the resin products obtained in the examples and comparative examples was tested by a Triumph YG60S gloss meter, and the mechanical properties were tested by a Chengde Jinjian UTM1422 electronic universal testing machine.

[0088]

[0089] It can be seen from the experimental results that compared with the common matting resin (Comparative Example 1), the matting effect of Examples 1-5 is significantly better. At the same time, compared with the case where the zeolite is not modified in advance (Example 5), the physical properties and plasticizing properties of Examples 1-4 are significantly better.

Claims

1. A matte polyvinyl chloride resin, wherein the matte polyvinyl chloride is prepared as follows: (1) adding vinyl chloride monomer, initiator, zeolite, crosslinking agent and dispersant into an aqueous solvent to obtain a dispersion; and (2) Suspension polymerization is carried out in the dispersion to obtain matte polyvinyl chloride.

2. The matte polyvinyl chloride resin according to claim 1, wherein The zeolite is 100-400 mesh.

3. The matte polyvinyl chloride resin according to claim 1, wherein The zeolite is zeolite powder with a mesh size of 100-300.

4. The matte polyvinyl chloride resin according to claim 1, wherein The zeolite is 150-250 mesh zeolite powder.

5. The matte polyvinyl chloride resin according to claim 1, wherein The zeolite is physically modified or graft-modified.

6. The matte polyvinyl chloride resin according to claim 5, wherein The physical modification includes stirring the zeolite powder under heating conditions; the grafting modification method includes performing surface grafting modification on the zeolite powder using a surface modifier.

7. The matte polyvinyl chloride resin according to claim 6, wherein The physical modification involves stirring the zeolite powder at 70-200°C.

8. The matte polyvinyl chloride resin according to claim 6, wherein The physical modification involves stirring the zeolite powder at 80-180°C.

9. The matte polyvinyl chloride resin according to claim 6, wherein The physical modification involves stirring the zeolite powder at 100-150°C.

10. The matte polyvinyl chloride resin according to claim 6, wherein The surface modifier includes fatty acid glyceride, polyvinyl alcohol or a combination thereof.

11. The matte polyvinyl chloride resin according to claim 10, wherein The fatty acid glyceride is a C6-C20 fatty acid glyceride.

12. The matte polyvinyl chloride resin according to claim 10, wherein The fatty acid glyceride is C6-C20 fatty acid monoglyceride.

13. The matte polyvinyl chloride resin according to claim 12, wherein The C6-C20 fatty acid monoglyceride includes glyceryl monostearate, glyceryl monolaurate, glyceryl monooleate or a combination thereof.

14. The matte polyvinyl chloride resin according to claim 1, wherein The delustering polyvinyl chloride is prepared as follows: (1) providing a modified zeolite; (2) adding vinyl chloride monomer, initiator, modified zeolite, crosslinking agent and dispersant into an aqueous solvent to obtain a dispersion; and (3) Suspension polymerization is carried out in the dispersion to obtain matte polyvinyl chloride.

15. A method for preparing a matte polyvinyl chloride resin, the method comprising: (1) adding vinyl chloride monomer, initiator, zeolite, crosslinking agent and dispersant into an aqueous solvent to obtain a dispersion; as well as (2) Suspension polymerization is carried out in the dispersion to obtain matte polyvinyl chloride.

16. The method of claim 15, wherein: The zeolite is physically modified or graft-modified.

17. The method of claim 16, wherein: The physical modification includes stirring the zeolite powder under heating conditions; the grafting modification method includes performing surface grafting modification on the zeolite powder using a surface modifier.

18. The method of claim 17, wherein: The physical modification involves stirring the zeolite powder at 70-200°C.

19. The method of claim 17, wherein: The physical modification involves stirring the zeolite powder at 80-180°C.

20. The method of claim 17, wherein: The physical modification involves stirring the zeolite powder at 100-150°C.

21. The method of claim 17, wherein: The surface modifier includes fatty acid glyceride, polyvinyl alcohol or a combination thereof.

22. The method of claim 21, wherein: The fatty acid glyceride is a C6-C20 fatty acid glyceride.

23. The matte polyvinyl chloride resin according to claim 21, wherein The fatty acid glyceride is C6-C20 fatty acid monoglyceride.

24. The matte polyvinyl chloride resin according to claim 23, wherein The C6-C20 fatty acid monoglyceride includes glyceryl monostearate, glyceryl monolaurate, glyceryl monooleate or a combination thereof.

25. The method of claim 15, wherein: The method comprises the following steps: (1) providing a modified zeolite; (2) adding vinyl chloride monomer, initiator, modified zeolite, crosslinking agent and dispersant into an aqueous solvent to obtain a dispersion; and (3) Suspension polymerization is carried out in the dispersion to obtain matte polyvinyl chloride.