A method for evaluating the burning loss and pulverization of semi-coke in the ferrosilicon charge surface

By evaluating the burning and pulverization of orchid carbon on the ferrosilicon furnace surface, the burning and pulverization rate and pulverization rate are calculated, the burning and pulverization problem of orchid carbon on the ferrosilicon furnace surface is solved, and theoretical guidance for optimizing ferrosilicon smelting is provided. , improves furnace surface performance and output.

CN115290498BActive Publication Date: 2024-12-06XI'AN UNIVERSITY OF ARCHITECTURE AND TECHNOLOGY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210931741.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-04
Publication Date
2024-12-06
Estimated Expiration
2042-08-04

AI Technical Summary

Technical Problem

The prior art has failed to effectively evaluate and solve the burning problem of orchid carbon on the ferrosilicon furnace surface, resulting in high furnace surface temperature, small crucible in the reaction area, reduced output and increased power consumption.

Method used

An evaluation method is adopted, including raw material pretreatment, heating furnace body preparation, burn loss determination and pulverization rate determination. By calculating the burn loss and pulverization rate of orchid, a quality grading basis is provided to optimize the performance of the ferrosilicon furnace surface.

Benefits of technology

Accurately determine the burning and pulverization performance parameters of orchid carbon, provide theoretical guidance to improve the reduction performance of ferrosilicon smelting, reduce furnace surface temperature and electricity consumption, and improve output.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115290498B_ABST
    Figure CN115290498B_ABST
Patent Text Reader

Abstract

The invention discloses a method for evaluating the burning loss and pulverization of blue coke in a ferrosilicon furnace charge surface, comprising the following steps: 1) raw material pretreatment: select 10 kg of representative blue coke small material, reduce it into four parts of about 2.5 kg each, then sieve a 2.5 kg blue coke small material sample with a round sieve, then dry it in a drying oven, and sieve it with a round sieve again; 2) device preparation before measurement: place a heating furnace body on the right side of the entire slide rod, weighing step 1) a dried blue coke sample of 60±0.5 g is placed in a sample boat, the initial mass is recorded as m0 (g), close the lid and seal it, and the gas cylinder is a mixed gas of CO:O2:N2; 3) heating the furnace body: heat the furnace temperature, keep the temperature, slowly push the furnace body to the left sample position, let the sample porcelain boat be in the middle of a constant temperature zone and start timing; 4) burning loss measurement: 5) measuring the pulverization rate: the invention can accurately measure the blue coke material surface burning loss and pulverization performance parameters, and provide a basis for the quality classification of blue coke for ferrosilicon through horizontal comparison.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ferroalloy process technology, and in particular to a method for evaluating the burning loss and pulverization of blue coke in a ferrosilicon charge surface. Background Art

[0002] In the process of smelting ferrosilicon in submerged arc furnace, semi-coke has largely replaced traditional reducing agents such as metallurgical coke and gas coal coke. Compared with traditional reducing agents, semi-coke has the advantages of high specific resistivity, high reactivity, low ash, low aluminum, low phosphorus, low price and other raw material advantages, and the application process significantly reduces power consumption. However, some production units have found that after semi-coke enters the ferrosilicon furnace, the material collapse and abnormal noise increase, the furnace surface is seriously burned, there are many stabs, the furnace surface temperature is high, the crucible in the reaction zone is small, the carbon content increases, the manual intervention of the furnace increases, the output decreases, and the power consumption increases. Experimental and operating experience show that these phenomena are mainly caused by the properties of semi-coke. Since semi-coke is prepared by low-temperature dry distillation of low-rank coal with high volatile matter, the release of volatile matter leads to the development of semi-coke pores and the disorder of carbon lattice is further increased. Semi-coke with too low ignition point will burn rapidly after entering the ferrosilicon furnace and contacting with air and reaching the ignition temperature, causing the material surface temperature to rise and the heat loss to increase, which in turn leads to carbon deficiency in the reduction area.

[0003] When the same coal rank is used as the raw coal for dry distillation, the high-temperature reduction reactivity of the semi-coke obtained is basically the same. This is mainly because the reduction temperature has greatly exceeded the dry distillation temperature. In the range of 700-1100℃ on the material surface, the combustion performance of different types of semi-coke is different due to the difference in dry distillation process parameters. The traditional view is that improving the reactivity of the reducing agent should be based on high-temperature reduction performance rather than medium- and low-temperature combustion performance, which has caused some misleading in the smelting process of many ferrosilicon furnaces. The degree of burnout of semi-coke on the material surface is closely related to the volatile content. Some views believe that in order to improve the reducibility of semi-coke, the lower limit of the volatile content of semi-coke should be specified, while the upper limit of the volatile content is relatively loose, which further increases the burnout rate of semi-coke on the material surface. Of course, the higher reactivity of semi-coke on the material surface can indeed adsorb SiO gas and react with it to generate SiC or Si. When O2 and SiO gas are present at the same time, inhibiting the reaction of semi-coke with O2 may theoretically ensure that sufficient reactive sites react with SiO gas, thereby reducing the loss of Si raw materials and improving the product yield.

[0004] However, there are currently no regulations on the evaluation and methods of the burning loss of lignite on the ferrosilicon charge surface. Summary of the invention

[0005] In order to overcome the deficiencies of the above-mentioned prior art, the object of the present invention is to provide a method for evaluating the burning loss and pulverization of lignite in the charge surface of ferrosilicon furnace, which can accurately determine the charge surface burning loss and pulverization performance parameters of lignite, and provide a basis for the quality grading of lignite for ferrosilicon through horizontal comparison.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for evaluating the burning loss and pulverization of blue carbon in a ferrosilicon charge surface comprises the following steps:

[0008] 1) Raw material pretreatment: 10 kg of representative semi-coke was selected and divided into four portions of about 2.5 kg each. Then, a 2.5 kg semi-coke sample was sieved with a round sieve, dried in a drying oven, and sieved again with a round sieve;

[0009] 2) Preparation of the device before measurement: Place the heating furnace on the right side of the entire slide, weighing step 1) Place a portion of dried blue carbon sample 60±0.5g in the sample boat, the initial mass is recorded as m0 (g), close the lid and seal, the gas cylinder is a mixture of CO:O2:N2;

[0010] 3) Heating the furnace body: Heat the furnace temperature, keep it warm, slowly push the furnace body to the left sample position, let the sample porcelain boat be in the middle of the constant temperature zone and start timing;

[0011] 4) Burning loss determination: After heating for 20 minutes, the temperature began to decrease with the furnace, and N2 was switched to flow at a flow rate of 1L / min until the furnace temperature dropped below 50°C. The reaction tube was opened to take out the semi-coke sample, and the mass of the semi-coke remaining in the porcelain boat was weighed, recorded as m1 (g);

[0012] The calculation formula of blue carbon burning loss rate is:

[0013]

[0014] 5) Determination of pulverization rate: The blue carbon is sieved through a 6 mm round sieve to separate the material on the sieve and weigh it, and the mass is calculated as m2;

[0015] The calculation formula of blue carbon pulverization rate is:

[0016]

[0017] The blue carbon small material sample in step 1) is screened with a round sieve to obtain particles of 6-10 mm, and then dried in a drying oven at 105° C. for 5 hours, and screened with a round sieve again to obtain particles of 6-10 mm.

[0018] In the step 2), the mixed gas of CO:O2:N2 has a ratio of 20%:15%:65%, and the air in the ventilation replacement tube is ventilated for 10 minutes with a flow rate of 1.5 L / min.

[0019] In the step 3), the furnace body is heated to 800° C. at a rate of 10° C. / min and kept at this temperature for 5 minutes.

[0020] Beneficial effects of the present invention:

[0021] The present invention can accurately measure the material surface burning loss and pulverization performance parameters of blue coke. The higher the blue coke burning loss rate, the greater the loss of blue coke on the material surface, which generally corresponds to a high material surface temperature, and vice versa. The higher the blue coke differentiation rate, the higher the degree of blue coke crushing after the material surface is burned. Under the same blue coke raw material particle size conditions, it generally corresponds to a decrease in the air permeability in the furnace and an increase in the piercing phenomenon, and vice versa. The above two parameters and their determination steps provide theoretical guidance for the smelting reduction blue coke required for the optimization of ferrosilicon.

[0022] In step 1, small semi-coke with a particle size of 6-10 mm is first oxidized and burned after entering the ferrosilicon furnace charge surface.

[0023] Step 2 sets the ratio of the mixed gas and the ratio of the ventilation replacement zone to simulate the gas composition of the ferrosilicon furnace charge surface. The ventilation replacement can simulate the rapid oxidation and combustion reaction process of the blue coke after it enters the charge surface.

[0024] The temperature of about 800° C. in step 3 is the actual ferrosilicon charge surface temperature.

[0025] The temperature in step 4 and the introduction of N2 can prevent the further oxidation and combustion of the blue carbon, thus achieving the purpose of comparison at the same level. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the evaluation device for the burning loss and pulverization of blue coke in the ferrosilicon charge surface of the present invention. DETAILED DESCRIPTION

[0027] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0028] like Figure 1 As shown, the measuring device is a sliding tubular heating furnace. The heating furnace adopts a sliding rod design, and the heating furnace can move freely left and right on the supporting sliding rod.

[0029] A method for evaluating the burning loss and pulverization of blue coke in a ferrosilicon charge surface, comprising the following steps;

[0030] 1) Raw material pretreatment: 10 kg of representative semi-coke was selected and divided into four portions of about 2.5 kg each. Then, a 2.5 kg semi-coke sample was sieved with a round sieve to obtain 6-10 mm particles, and then dried in a drying oven at 105 ° C for 5 hours, and sieved with a round sieve again to obtain 6-10 mm particles;

[0031] 2) Preparation of the device before measurement: Figure 1The heating furnace body is placed on the right side of the entire slide rod. Weighing step 1) A portion of dried lignite sample 60±0.5g is placed in the sample boat, and the initial mass is recorded as m0 (g). The lid is closed and sealed. The gas cylinder is a mixture of CO:O2:N2 in a ratio of 20%:15%:65%. The air in the ventilation replacement tube is 10 minutes, and the flow rate is 1.5L / min.

[0032] 3) Heat the furnace. Heat the furnace to 800°C at 10°C / min, keep warm for 5 minutes, and then Figure 1 Slowly push the middle furnace body to the sample position on the left side, place the sample porcelain boat in the middle of the constant temperature zone and start timing.

[0033] 4) Burning loss measurement: After heating for 20 minutes, the temperature began to drop with the furnace, and N2 was switched to flow at a flow rate of 1L / min until the furnace temperature dropped below 50°C. The reaction tube was opened to take out the semi-coke sample, and the mass of the semi-coke remaining in the porcelain boat was weighed and recorded as m1 (g).

[0034] The calculation formula of blue carbon burning loss rate is:

[0035]

[0036] 5) Determine the pulverization rate. The blue carbon is taken out and sieved through a 6 mm round sieve to separate the material on the sieve and weigh it. The mass is calculated as m2.

[0037] The calculation formula of blue carbon pulverization rate is:

[0038] Example:

[0039] Provide the evaluation process and results of the burning loss rate and pulverization rate of 3 kinds of semi-coke. The 3 kinds of semi-coke are small semi-coke materials from different manufacturers. The test process is as follows:

[0040] The sample was sieved with a round sieve to obtain particles of 6-10 mm, and then dried in a drying oven at 105° C. for 5 hours, and sieved with a round sieve again to obtain particles of 6-10 mm.

[0041] Preparation of the device before measurement: Place the heating furnace body on the right side, weighing step 1) Place a 60±0.5g medium blue carbon sample in the sample boat, the initial mass is recorded as m0 (g), close the lid and seal it, the gas cylinder is a mixture of CO:O2:N2 in the ratio of 20%:15%:65%, and the air in the ventilation tube is replaced for 10 minutes, with a flow rate of 1.5L / min.

[0042] Heat the furnace body. Heat the furnace to 800℃ at 10℃ / min. After keeping the temperature for 5 minutes, slowly push the furnace body to the left sample position, place the sample boat in the middle of the constant temperature zone and start timing.

[0043] Burn-out measurement. After heating for 20 minutes, the furnace temperature began to cool down and N2 was switched to flow at a flow rate of 1 L / min until the furnace temperature dropped below 50°C. The reaction tube was opened to take out the semi-coke sample and the remaining semi-coke mass in the porcelain boat was weighed and recorded as m1 (g). The burn-out rate was calculated according to formula (1).

[0044] Determine the pulverization rate. The blue carbon is taken out and passed through a 6mm round sieve. The sieve material is sieved with a vibrating sieve machine and weighed as m2.

[0045] The powdering rate was calculated according to formula (2).

[0046] The burnout rate and pulverization rate of the three enterprises are shown in Table 1. From the results, it can be seen that the burnout rate and pulverization rate of 2# semi-coke are both higher, while the burnout rate and pulverization rate of 1# semi-coke are both lower, which is consistent with the actual process.

[0047] Table 1 Evaluation results of the burning loss rate and pulverization rate of semi-coke on the ferrosilicon charge surface of three enterprises

[0048]

[0049] It can be seen from the above examples that the method can accurately measure the material surface burning loss and pulverization performance parameters of semi-coke, and provide theoretical guidance for the smelting and reduction of semi-coke required for the optimization of ferrosilicon.

Claims

1. A method for evaluating the burning loss and pulverization of blue coke in a ferrosilicon charge surface, characterized in that: The steps include: 1) Raw material pretreatment: 10 kg of representative semi-coke was selected and divided into four portions of about 2.5 kg each. Then, a 2.5 kg semi-coke sample was sieved with a round sieve, dried in a drying oven, and sieved again with a round sieve; 2) Preparation of the device before measurement: Place the heating furnace on the right side of the entire slide, weighing step 1) Place a portion of dried semi-coke sample 60±0.5g in the sample boat, the initial mass is recorded as m0 (g), close the lid and seal, the gas cylinder is a mixture of CO:O2:N2; 3) Heating the furnace body: Heat the furnace temperature, keep it warm, slowly push the furnace body to the left sample position, let the sample porcelain boat be in the middle of the constant temperature zone and start timing; 4) Burning loss determination: After heating for 20 minutes, the temperature began to decrease with the furnace, and N2 was switched to flow at a flow rate of 1L / min until the furnace temperature dropped below 50°C. The reaction tube was opened to take out the semi-coke sample, and the mass of the semi-coke remaining in the porcelain boat was weighed, recorded as m1 (g); The calculation formula of blue carbon burning loss rate is: 5) Determination of pulverization rate: The blue carbon is sieved through a 6 mm round sieve to separate the sieve material and weigh it, and the mass is calculated as m2; The calculation formula of blue carbon pulverization rate is:

2. The method for evaluating burning loss and pulverization of blue coke in a ferrosilicon charge surface according to claim 1, characterized in that: The blue carbon small material sample in step 1) is screened with a round sieve to obtain particles of 6-10 mm, and then dried in a drying oven at 105° C. for 5 hours, and screened with a round sieve again to obtain particles of 6-10 mm.

3. The method for evaluating burning loss and pulverization of blue coke in a ferrosilicon charge surface according to claim 1, characterized in that: In the step 2), the mixed gas of CO:O2:N2 has a ratio of 20%:15%:65%, and the air in the ventilation replacement tube is ventilated for 10 minutes with a flow rate of 1.5 L / min.

4. The method for evaluating burning loss and pulverization of blue coke in a ferrosilicon charge surface according to claim 1, characterized in that: In the step 3), the furnace body is heated to 800° C. at a rate of 10° C. / min and kept at this temperature for 5 minutes.

Citation Information

Patent Citations

  • Iron ore concentrate for increasing low-temperature reduction pulverization rate of iron ore sinter and preparation method

    CN112301215A

  • Method for measuring high-temperature pulverization performance of ferrocoke

    CN112903513A

  • A method for estimating quality of coal in coal basediron making

    KR1020020015787A