Oxygen carrier with oxygen decoupling-catalysis dual functions and preparation method thereof

By designing the MnCaFeO-based composite metal oxygen carrier, controlling the Mn doping ratio and calcination treatment, the problem of limited oxygen decoupling performance of the Ca-Fe-based oxygen carrier is solved, an efficient chemical chain gasification reaction is achieved, and the gas efficiency is improved. It improves the chemical efficiency and carbon conversion rate and avoids the degradation of syngas quality caused by excessive oxidation.

CN115301250BActive Publication Date: 2024-10-18TIANJIN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210777115.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-30
Publication Date
2024-10-18
Estimated Expiration
2042-06-30

AI Technical Summary

Technical Problem

The existing Ca-Fe-based oxygen carriers have problems with limited oxygen decoupling performance and low syngas quality in chemical chain gasification reactions. The excessive oxidation of Mn-based oxygen decoupling materials leads to reduced syngas quality and is difficult to use. Effectively improve its catalytic performance.

Method used

Using MnCaFeO-based composite metal oxygen carrier, by regulating the Mn doping ratio and the temperature rise rate of the calcination treatment, an oxygen carrier with oxygen decoupling and catalysis dual functions is formed, and the release of lattice oxygen is used to realize the gas-solid reaction and improve the reaction performance. , and improve the CO2 catalytic conversion ability by regulating the mass ratio of biomass and oxygen carrier.

Benefits of technology

The oxygen decoupling performance and catalytic performance of the oxygen carrier are improved, the gasification efficiency is increased to more than 70%, and the carbon conversion rate reaches more than 90%, avoiding the degradation of syngas quality caused by excessive oxidation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115301250B_ABST
    Figure CN115301250B_ABST
Patent Text Reader

Abstract

The present disclosure provides an oxygen carrier with oxygen decoupling-catalysis dual functions and a preparation method. The oxygen carrier with oxygen decoupling-catalysis dual functions is a MnCaFeO-based composite metal oxygen carrier, wherein the metal component of the oxygen carrier is composed of Mn, Fe, and Ca elements, wherein the molar percentage content of Mn, Fe, and Ca is (10%-40%): (30%-45%): (30%-45%), and the content of Fe and Ca is the same. The present disclosure also provides a chemical chain gasification method, wherein the method includes an oxygen carrier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure belongs to the field of energy chemical industry and material technology, and in particular relates to an oxygen carrier with dual functions of oxygen decoupling and catalysis, a preparation method, and a chemical chain gasification method. Background Art

[0002] With the continuous progress of industry and society, fossil energy, mainly coal, has been consumed in large quantities, accompanied by serious resource shortages and increasingly severe environmental pollution problems. Therefore, the development of renewable energy to replace traditional fossil fuels has become an inevitable trend. As a green, clean and renewable energy source, biogas reduces greenhouse gas (GHG) emissions while meeting energy needs; and biogas production through anaerobic fermentation can also achieve solid waste treatment. However, the large amount of sludge, a by-product of anaerobic fermentation, is difficult to handle, which limits the development of the industry. Currently, the utilization of sludge includes organic fertilizer and soilless cultivation. However, problems such as high transportation costs, poor dosage controllability, and mediocre results limit its large-scale application.

[0003] Chemical looping gasification (CLG) is a novel thermal conversion technology based on chemical looping combustion that produces syngas from solid fuels. Syngas is widely used for power generation and as a feedstock for Fischer-Tropsch synthesis, fuels, and chemicals. Chemical looping gasification uses lattice oxygen as the gasification medium, replacing traditional gasifiers to provide the oxygen required for the reaction. This avoids direct contact between the reactants and air, fundamentally eliminating nitrogen dilution and increasing the calorific value of the syngas. It also eliminates the need for equipment such as air separators, reducing costs and energy consumption.

[0004] The preparation of oxygen carriers plays a key role in chemical looping gasification technology. Fe-based oxygen carriers are widely used due to their acceptable reactivity, high-temperature stability, cost-effectiveness, and environmental friendliness. However, their reactivity is limited and they suffer from issues such as sintering and agglomeration. CaO is a promising chemical looping material as a CO2 carrier, reducing CO2 production while increasing CO and H2 production. The addition of CaO can effectively inhibit the agglomeration and sintering of Fe-based oxygen carriers. Using Ca2Fe2O5 as a matrix can also effectively modulate the redox and migration activity of lattice oxygen, achieving uniform lattice oxygen release. However, the chemical looping gasification reaction of conventional oxygen carriers is easily limited by solid-solid reactions between lattice oxygen and the feedstock. Therefore, the use of materials with oxygen decoupling properties to modify Ca-Fe-based oxygen carriers has been proposed. This can convert solid-solid reactions into gas-solid reactions between molecular oxygen and the feedstock, promoting the chain gasification reaction and improving reaction performance. Commonly used materials with oxygen decoupling properties include Co- and Cu-based materials.

[0005] Although Co- and Cu-based oxygen decoupling materials have been used in Ca-Fe-based oxygen carriers, these oxygen decoupling materials are expensive and have high oxidizing properties and oxygen release rates, resulting in low syngas quality. Compared to Co- and Cu-based modified oxygen carriers, Mn-based modified oxygen carriers offer advantages such as slow oxygen decoupling rates, better activity, and a richer oxidation state, effectively improving the oxygen decoupling performance of oxygen carriers. However, how to further enhance the oxygen decoupling and catalytic performance of Mn-based oxygen carriers using Mn-based oxygen decoupling materials is an urgent issue. Summary of the Invention

[0006] In response to the above technical problems, the present disclosure provides an oxygen carrier with dual oxygen decoupling and catalysis functions, a preparation method, and a chemical chain gasification method, in order to at least partially solve the above technical problems.

[0007] In order to solve the above technical problems, as one aspect of the present disclosure, an oxygen carrier with oxygen decoupling-catalysis dual functions is provided, wherein the above oxygen carrier is a MnCaFeO-based composite metal oxygen carrier, wherein the metal components of the oxygen carrier are composed of Mn, Fe, and Ca elements, wherein the molar percentage content of Mn, Fe, and Ca is (10%-40%): (30%-45%): (30%-45%), and the content of Fe and Ca is the same.

[0008] In one embodiment, the oxygen carrier has a perovskite structure.

[0009] As another aspect of the present disclosure, a method for preparing an oxygen carrier is provided, the method comprising:

[0010] Mixing ferric nitrate, calcium nitrate and manganese nitrate to prepare a nitrate solution;

[0011] Adding a complexing agent to the above nitrate solution, adjusting the pH value of the solution, and heating to form a gel;

[0012] The dried gel is calcined to obtain an oxygen carrier;

[0013] The molar percentage content of Mn, Fe and Ca metal ions in the nitrate solution is (10%-40%): (30%-45%): (30%-45%).

[0014] In another embodiment, the molar ratio of the complexing agent to the metal ions in the nitrate is 0.5:1-1.5:1, wherein the complexing agent comprises citric acid.

[0015] In another embodiment, the pH value of the solution is adjusted to 1.9-2.1.

[0016] In another embodiment, the parameters of the calcination process include:

[0017] The temperature of the calcination treatment includes: 850-950°C;

[0018] The heating rate of the calcination treatment includes: 5-10°C / min.

[0019] In another embodiment, the method further comprises grinding the calcined oxygen carrier into a powder with a particle size less than 0.2 mm.

[0020] As another aspect of the present disclosure, a chemical looping gasification method is also provided, which includes using the above-mentioned oxygen carrier.

[0021] In another embodiment, the chemical chaining gasification is biomass chemical chaining gasification, wherein the mass ratio of the oxygen carrier to the biomass is 0.2-0.7.

[0022] In another embodiment, during the chemical looping gasification reaction, the lattice oxygen of the oxygen carrier releases oxygen, resulting in the generation of oxygen vacancies caused by the reduction of the oxygen carrier and oxygen decoupling.

[0023] Based on the above technical solution, the present disclosure provides an oxygen carrier with oxygen decoupling and catalytic dual functions, a preparation method, and a chemical looping gasification method, which have at least one of the following beneficial effects:

[0024] (1) In the embodiments of the present disclosure, the interaction between metals can be regulated by adjusting the ratio of Mn doping, so that the oxygen carrier has better oxygen decoupling performance and catalytic performance.

[0025] (2) In the embodiments disclosed herein, the oxygen decoupling performance and catalytic performance of the oxygen carrier can be controlled by regulating the Mn doping ratio and the heating rate during the calcination treatment, and at the same time, the reduction in the quality of the synthesis gas caused by the excessive oxidizing property of the oxygen carrier can be effectively avoided.

[0026] (3) In the embodiments of the present disclosure, by adjusting the mass ratio of biomass to oxygen carrier during the chain gasification reaction, a higher oxygen decoupling ability of the oxygen carrier can be obtained and the oxygen carrier can have a higher CO2 catalytic conversion ability. By regulating the Mn doping ratio, the heating rate during calcination treatment and the mass ratio of biomass to oxygen carrier, the gasification efficiency of chemical chain gasification is increased to more than 70%, and the carbon conversion rate is increased to more than 90%. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 3. The thermogravimetric curves of the composite oxygen carriers with different Mn doping amounts after decoupling and regeneration treatment in Examples 1, 3, 6, and 9 of the present disclosure;

[0028] Figure 2This is a full spectrum of X-ray photoelectron spectra of composite metal oxygen carriers with different Mn doping amounts in Examples 1, 3, 6, and 9 of the present disclosure;

[0029] Figure 3A is a Mn 2p 3 / 2 diagram of the X-ray photoelectron spectrum of the composite metal oxygen carrier with different Mn doping amounts in Examples 1, 3, 6, and 9 of the present disclosure;

[0030] Figure 3B is an O1s diagram of the X-ray photoelectron spectrum of the composite metal oxygen carrier with different Mn doping amounts in Examples 1, 3, 6, and 9 of the present disclosure;

[0031] Figure 3C is the Fe 2p diagram of the X-ray photoelectron spectrum of the composite metal oxygen carrier with different Mn doping amounts in Examples 1, 3, 6, and 9 of the present disclosure;

[0032] Figure 4A -D is a transmission electron micrograph of the composite metal oxygen carriers with different Mn doping contents in Examples 1, 3, 6, and 9 of the present disclosure;

[0033] Figure 5 is a temperature-programmed reduction diagram of the composite metal oxygen carrier with different Mn doping contents in Examples 1, 3, 6, and 9 of the present disclosure;

[0034] Figure 6 is a Raman spectrum of the composite metal oxygen carrier with different Mn doping contents in Examples 1, 3, 6, and 9 of the present disclosure;

[0035] Figure 7 is a Fourier transform infrared spectrum of the composite metal oxygen carrier with different Mn doping contents in Examples 1, 3, 6, and 9 of the present disclosure;

[0036] Figure 8 3 are X-ray diffraction patterns of composite metal oxygen carriers with different Mn doping contents in Examples 1, 3, 6, and 9 of the present disclosure. DETAILED DESCRIPTION

[0037] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.

[0038] Based on the advantages of Mn-based oxygen carriers, such as slow oxygen decoupling rate, good activity and rich oxidation states, and Ca-Fe-based oxygen carriers, which have the advantages of uniform lattice oxygen release, Mn-based oxygen decoupling materials are used to modify Ca-Fe-based oxygen carriers. An oxygen carrier with dual oxygen decoupling and catalytic functions, as well as a preparation method and a chemical chain gasification method are proposed. By regulating the Mn doping ratio, the interaction between metals can be achieved, so that the Mn-based oxygen carrier has good oxygen decoupling performance and good catalytic performance at the same time, which can avoid the extremely strong oxidizing property of the oxygen carrier that reduces the quality of the synthesis gas.

[0039] According to an embodiment of the present disclosure, an oxygen carrier having the dual functions of oxygen decoupling and catalysis is provided, wherein the oxygen carrier is a MnCaFeO-based composite metal oxygen carrier, wherein the metal components of the oxygen carrier are composed of Mn, Fe, and Ca elements, wherein the molar percentage content of Mn, Fe, and Ca is (10%-40%): (30%-45%): (30%-45%), and the content of Fe and Ca is the same.

[0040] According to an embodiment of the present disclosure, the molar percentage content of Mn, Fe and Ca is (10%-40%):(30%-45%):(30%-45%), among which it can be selected as 10%:45%:45%, 20%:40%:40%, 30%:35%:35%, 40%:30%:30%, etc.

[0041] According to the embodiments of the present disclosure, by regulating the ratio of Mn doping, regulation between metals can be achieved, so that the oxygen carrier has better oxygen decoupling and catalytic conversion capabilities, while also avoiding the extremely strong oxidizing properties caused by Mn doping.

[0042] According to an embodiment of the present disclosure, the oxygen carrier has a perovskite structure, which has certain catalytic properties.

[0043] According to an embodiment of the present disclosure, a method for preparing an oxygen carrier includes: mixing ferric nitrate, calcium nitrate, and manganese nitrate to prepare a nitrate solution; adding a chelating agent to the nitrate solution, adjusting the pH of the solution, and heating to form a gel; and calcining the dried gel to obtain an oxygen carrier; wherein the molar percentage of Mn, Fe, and Ca metal ions in the nitrate solution is (10%-40%):(30%-45%):(30%-45%).

[0044] According to an embodiment of the present disclosure, the iron nitrate, calcium nitrate and manganese nitrate are Fe(NO3)3·9H2O, Ca(NO3)2·4H2O and Mn(NO3)2·4H2O, respectively.

[0045] According to an embodiment of the present disclosure, the molar ratio of the complexing agent to the metal ions in the nitrate is 0.5:1-1.5:1, wherein the complexing agent includes citric acid.

[0046] According to an embodiment of the present disclosure, the pH of the solution is adjusted to 1.9-2.1.

[0047] In the embodiments disclosed herein, the molar ratio of the complexing agent to the metal ions in the nitrate is limited to a range of 0.5-1 to 1.5:1, allowing the nitrate solution and the complexing agent to fully complex, forming a sol. The solution is then adjusted to a pH of 1.9-2.1 using aqueous ammonia, heated in a water bath at 80°C, and continuously stirred until a gel forms. If the pH of the solution is too high, precipitation is likely to form. If the pH of the solution is too low, the complexing effect between the metal ions in the nitrate and the complexing agent will be poor, making gel formation difficult.

[0048] According to an embodiment of the present disclosure, the gel is dried at 105° C. for 48 hours to remove moisture from the gel, and then the dried gel is placed in a reactor for calcination to obtain an oxygen carrier. A forced air drying oven can be used to dry the gel, and a tubular furnace can be used to calcine the gel.

[0049] According to an embodiment of the present disclosure, the temperature of the calcination treatment includes: 850-950°C, wherein it can be selected as 850°C, 900°C, 950°C, etc.; the calcination heating rate includes: 5-10°C / min, wherein it can be selected as 5, 6, 8, 10°C / min; the calcination atmosphere includes air, and the gas flow rate is 100mL / min.

[0050] In the embodiments of the present disclosure, the dried gel is calcined at a slow heating rate, which can activate the oxygen carrier and improve the crystal structure of the oxygen carrier, thereby increasing the surface activity of the oxygen carrier crystal, thereby affecting the oxygen decoupling performance and catalytic performance of the oxygen carrier. At the same time, limiting the calcination temperature of the oxygen carrier to this range can avoid sintering of the oxygen carrier due to excessively high temperature.

[0051] According to an embodiment of the present disclosure, the calcined oxygen carrier is further ground into a powder with a particle size of less than 0.2 mm, so that the powder can fully contact with the oxygen carrier during the subsequent chemical chain gasification reaction, thereby improving the reaction efficiency.

[0052] According to an embodiment of the present disclosure, a chemical looping gasification method is further provided, including using the oxygen carrier in the above embodiment, where the oxygen carrier is a MnCaFeO-based composite metal oxygen carrier.

[0053] According to an embodiment of the present disclosure, the above-mentioned chemical chain gasification is biochemical chain gasification, wherein the mass ratio of oxygen carrier to biomass is 0.2-0.7, which can be selected from 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, etc., preferably 0.4-0.6, and more preferably 0.5.

[0054] In the embodiments of the present disclosure, the mass ratio of the oxygen carrier to the biomass is limited to 0.2-0.7, so that the oxygen carrier and the biomass can fully react to generate synthesis gas with H2 and CO as the main components, reducing the occurrence of other side reactions and the waste of oxygen carriers.

[0055] According to an embodiment of the present disclosure, before the chemical chain gasification reaction, the reaction temperature in the reactor is preheated to 600-1000°C, and N2 is introduced at 100 mL / min for 10 minutes to ensure an inert atmosphere in the reactor; then, a certain mass of biomass is evenly mixed with an oxygen carrier and sent into the reactor for a chemical chain gasification reaction to prepare synthesis gas, wherein the reaction duration is preferably 30 minutes, and the reaction temperature in the reactor is preferably 800°C.

[0056] In the embodiments disclosed herein, the reactor temperature is limited to 600-1000°C, allowing the oxygen carrier to fully react with the biomass to produce syngas primarily composed of CO and H2. Excessively high reaction temperatures can lead to sintering of the oxygen carrier and shift the reaction in the forward direction, reducing the quality of the syngas. Excessively low reaction temperatures can lead to incomplete reaction between the oxygen carrier and the biomass, and the oxygen carrier cannot exhibit oxygen decoupling properties at lower temperatures, affecting syngas production. Therefore, to achieve higher syngas quality and yield, the reaction temperature is preferably limited to 800°C.

[0057] According to the embodiments of the present disclosure, by utilizing an oxygen-decoupling oxygen carrier under certain temperature and oxygen partial pressure conditions, the oxygen released from the lattice oxygen of the oxygen carrier will lead to the reduction of the oxygen carrier and the generation of oxygen vacancies due to oxygen decoupling, thereby converting the traditional solid-solid reaction into a gas-solid reaction of molecular oxygen and biomass, promoting coke cracking, realizing the conversion of CO2 to CO, and making the synthesis gas have higher selectivity for CO and H2; and lower selectivity for CO2.

[0058] According to embodiments of the present disclosure, the oxygen-decoupled oxygen carrier after the reaction can be regenerated in an oxygen-containing atmosphere to enable reuse of the oxygen carrier. The oxygen carrier regeneration method includes converting the atmosphere in the chemical looping gasification reactor to air to regenerate the oxygen carrier. The regeneration temperature ranges from 700°C to 900°C, with options including 700°C, 800°C, and 900°C, preferably 800°C, and the regeneration time is 30 minutes.

[0059] In order to make the purpose, technical solution and effect of the present disclosure more clear, the present disclosure is further described below in conjunction with specific embodiments and drawings. It should be noted that the examples listed are only used to explain the present disclosure and are not used to limit the scope of the present disclosure.

[0060] The biomass residue used in this disclosure was obtained from an anaerobic digestion plant for food waste in Beijing. It served as feedstock for chemical chaining gasification and was dried, crushed, and sieved to a particle size less than 0.2 mm. The industrial analysis, elemental analysis, and lower heating value of the residue are shown in Table 1.

[0061] Table 1. Industrial analysis, elemental analysis and lower heating value (LHV) of biogas residue

[0062]

[0063] Example

[0064] Example 1

[0065] The sol-gel method was used to prepare the oxygen carrier 20MnCaFe with oxygen decoupling and catalysis dual functions. The specific preparation method is as follows:

[0066] 10.04g of Mn(NO3)2·4H2O, 18.89g of Ca(NO3)2·4H2O, and 32.32g of Fe(NO3)3·9H2O were dissolved in 100mL of deionized water at a molar ratio of 20%:40%:40% (1:2:2) of metal cations, respectively, and stirred continuously until completely dissolved. Next, 38.424g of citric acid was added as a complexing agent at a molar ratio of 1:1 to the metal ions in the nitrate. Ammonia was then slowly added dropwise to the nitrate solution with continuous stirring until the solution reached a pH of 2. The solution was then heated in an 80°C water bath with continuous stirring until a gel formed. The wet gel was dried in a forced-air drying oven at 105°C for 48 hours to form a xerogel. The xerogel was calcined in an air atmosphere at a rate of 5°C / min to fully decompose the nitrate in the xerogel and regulate the oxygen decoupling and catalytic conversion properties of the oxygen carrier. The calcination temperature was raised from room temperature to 900°C and then calcined for 4 hours to fully activate the oxygen carrier. The calcined oxygen carrier was ground into a powder with a particle size of less than 0.2 mm, resulting in an oxygen carrier with both oxygen decoupling and catalytic properties, designated 20MnCaFe.

[0067] The oxygen-decoupling-catalytic dual-functional oxygen carrier 20MnCaFe prepared by the above method was uniformly mixed with biomass and fed into a reactor for chemical looping gasification. The biomass-to-oxygen carrier mass ratio was 2:1, the chemical looping gasification reaction temperature was 800°C, and the reaction lasted for 30 minutes. The oxygen-decoupling property of the oxygen carrier facilitated gas-solid reactions by releasing oxygen from lattice oxygen, promoting coke cracking and tar gasification. Furthermore, the catalytic performance of the oxygen carrier resulted in the formation of oxygen vacancies, which, when released from lattice oxygen, led to the catalytic conversion of CO2 to CO, improving CO yield and selectivity (Table 2). After the reaction, the reactor atmosphere was switched to air, simultaneously regenerating the oxygen vacancies and further demonstrating oxygen-decoupling properties. The specific method for regenerating the oxygen carrier includes: oxidizing and regenerating the oxygen carrier 20MnCaFe with the dual functions of oxygen decoupling and catalysis at 800°C for 30 minutes, then adding an amount of biomass equal to that in the first chemical chain gasification reaction to the reactor for a second chemical chain gasification reaction. After the regeneration treatment, the oxygen vacancies in the oxygen carrier can be regenerated and the oxygen decoupling performance can be further exhibited, thereby realizing the recycling of the oxygen carrier.

[0068] Table 2. Implementation results of chemical looping gasification based on oxygen decoupling-catalysis dual-functional oxygen carrier 20MnCaFe

[0069]

[0070] Example 2

[0071] The preparation method and chemical looping gasification method in Example 2 are the same as those in Example 1. The only difference is that during the chemical looping gasification reaction, the mass ratio of biomass to oxygen carrier is 5:2. The implementation results of Example 2 are shown in Table 3.

[0072] Table 3. Implementation results of chemical looping gasification based on oxygen decoupling-catalysis dual-functional oxygen carrier 20MnCaFe

[0073]

[0074] Example 3

[0075] The sol-gel method was used to prepare the oxygen carrier 10MnCaFe with oxygen decoupling and catalysis dual functions. The specific preparation method is as follows:

[0076] 5.02g of Mn(NO3)2·4H2O, 21.25g of Ca(NO3)2·4H2O, and 36.36g of Fe(NO3)3·9H2O were dissolved in 100mL of deionized water at a molar ratio of 10%:45%:45% (1:4.5:4.5) of metal cations, respectively, and stirred continuously until completely dissolved. 38.424g of citric acid was added at a molar ratio of 1:1 to the metal ions in the nitrate solution and used as a complexing agent. Ammonia was then slowly added dropwise to the nitrate solution with continuous stirring until the solution reached a pH of 2. The solution was then heated in an 80°C water bath with continuous stirring until a gel formed. The wet gel was dried in a forced-air drying oven at 105°C for 48 hours to form a xerogel. The xerogel was calcined in an air atmosphere at a rate of 5°C / min to fully decompose the nitrate in the xerogel and regulate the oxygen decoupling and catalytic conversion properties of the oxygen carrier. The calcination temperature was raised from room temperature to 900°C and then calcined for 4 hours to fully activate the oxygen carrier. The calcined oxygen carrier was ground into a powder with a particle size of less than 0.2 mm, resulting in an oxygen carrier with both oxygen decoupling and catalytic properties, designated 10MnCaFe.

[0077] The oxygen carrier 10MnCaFe prepared by the above method was uniformly mixed with biomass and introduced into a reactor for a chemical looping gasification reaction. The biomass-to-oxygen carrier mass ratio was 2:1, the chemical looping gasification reaction temperature was 800°C, and the reaction lasted for 30 minutes. At this point, the oxygen carrier's oxygen decoupling property enabled the release of oxygen from lattice oxygen to achieve a gas-solid reaction, promoting coke cracking and tar gasification. The oxygen carrier's catalytic performance also enabled the release of oxygen from lattice oxygen to form oxygen vacancies, which were then utilized to catalytically convert CO2 to CO, increasing CO yield and selectivity. After the reaction, the atmosphere in the reactor was converted to air, simultaneously regenerating the oxygen vacancies and further demonstrating oxygen decoupling properties. The specific method for oxygen carrier regeneration included oxidative regeneration of the oxygen carrier at 800°C for 30 minutes, followed by the addition of an equal amount of biomass to the first reaction into the chemical looping gasification reactor for a second chemical looping gasification reaction. The regenerated oxygen carrier achieved cyclic reuse. The specific implementation results of this example are shown in Table 4.

[0078] Table 4. Implementation results of chemical looping gasification based on oxygen decoupling-catalysis dual-functional oxygen carrier 10MnCaFe

[0079]

[0080] Example 4

[0081] The preparation method and chemical looping gasification method in Example 4 are the same as those in Example 3. The only difference is that during the chemical looping gasification reaction, the mass ratio of biomass to oxygen carrier is 5:2. The implementation results in this example are shown in Table 5.

[0082] Table 5. Implementation results of chemical looping gasification based on oxygen decoupling-catalysis dual-functional oxygen carrier 10MnCaFe

[0083]

[0084] Example 5

[0085] The preparation method and chemical looping gasification method in Example 5 are the same as those in Example 3. The only difference is that during the chemical looping gasification reaction, the mass ratio of biomass to oxygen carrier is 5:3. The implementation results in this example are shown in Table 6.

[0086] Table 6. Implementation results of chemical looping gasification based on oxygen decoupling-catalysis dual-functional oxygen carrier 10MnCaFe

[0087]

[0088] Example 6

[0089] The sol-gel method was used to prepare the oxygen carrier 30MnCaFe with oxygen decoupling and catalysis dual functions. The specific preparation method is as follows:

[0090] 15.06g of Mn(NO3)2·4H2O, 16.53g of Ca(NO3)2·4H2O, and 28.28g of Fe(NO3)3·9H2O were dissolved in 100mL of deionized water at a molar ratio of 30%:35%:35% (3:3.5:3.5) of metal cations, respectively, and stirred continuously until completely dissolved. Next, 38.424g of citric acid was added as a complexing agent at a molar ratio of 1:1 to the metal ions in the nitrate. Ammonia water was then slowly added dropwise to the nitrate solution with continuous stirring until the solution reached a pH of 2. The solution was then heated in an 80°C water bath with continuous stirring until a gel formed. The wet gel was dried in a forced-air drying oven at 105°C for 48 hours to form a xerogel. The xerogel was calcined in an air atmosphere at a rate of 5°C / min to fully decompose the nitrate in the xerogel and regulate the oxygen decoupling and catalytic conversion properties of the oxygen carrier. The calcination temperature was raised from room temperature to 900°C and then calcined for 4 hours to fully activate the oxygen carrier. The calcined oxygen carrier was ground into a powder with a particle size of less than 0.2 mm, resulting in an oxygen carrier with both oxygen decoupling and catalytic properties, designated 30MnCaFe.

[0091] The oxygen carrier 30MnCaFe, prepared by the above method and having both oxygen decoupling and catalytic functions, was uniformly mixed with biomass and fed into a reactor for a chemical looping gasification reaction. The biomass: oxygen carrier mass ratio was 2:1, the reaction temperature was 800°C, and the reaction duration was 30 minutes. The oxygen decoupling property of the oxygen carrier facilitated gas-solid reactions by releasing oxygen from lattice oxygen, promoting coke cracking and tar gasification. The catalytic properties of the oxygen carrier also facilitated the catalytic conversion of CO2 to CO by releasing oxygen from lattice oxygen, creating oxygen vacancies. These oxygen vacancies were then utilized to catalyze the conversion of CO2 to CO, improving CO yield and selectivity. After the reaction was completed, the atmosphere in the chemical looping gasification reactor was switched to air, and the oxygen carrier 30MnCaFe, which had both oxygen decoupling and catalytic functions, was oxidatively regenerated at 800°C for 30 minutes. Then, an amount of biomass equal to that in the first chemical chain gasification reaction was added to the reactor for a second chemical chain gasification reaction. This indicates that after the regeneration treatment, the oxygen vacancies in the oxygen carrier can be regenerated and further exhibit oxygen decoupling performance, thereby realizing the recycling of the oxygen carrier. The specific implementation results are shown in Table 7.

[0092] Table 7. Implementation results of chemical looping gasification based on oxygen decoupling-catalysis dual-functional oxygen carrier 30MnCaFe

[0093]

[0094] Example 7

[0095] The preparation method and chemical looping gasification method in Example 7 are the same as those in Example 6, with the only difference being that during the chemical looping gasification reaction, the mass ratio of biomass to oxygen carrier is 5:2. The implementation results in this example are shown in Table 8.

[0096] Table 8. Implementation results of chemical looping gasification based on oxygen decoupling-catalysis dual-functional oxygen carrier 30MnCaFe

[0097]

[0098] Example 8

[0099] The preparation method and chemical looping gasification method in Example 8 are the same as those in Example 6. The only difference is that during the chemical looping gasification reaction, the mass ratio of biomass to oxygen carrier is 5:3. The implementation results in this example are shown in Table 9.

[0100] Table 9. Implementation results of chemical looping gasification based on oxygen decoupling-catalysis dual-functional oxygen carrier 30MnCaFe

[0101]

[0102] Example 9

[0103] The sol-gel method was used to prepare the oxygen carrier 40MnCaFe with oxygen decoupling and catalysis dual functions. The specific preparation method is as follows:

[0104] 20.08g of Mn(NO3)2·4H2O, 14.169g of Ca(NO3)2·4H2O, and 24.24g of Fe(NO3)3·9H2O were dissolved in 100mL of deionized water at a molar ratio of 40%:30%:30% (1:0.75:0.75) of metal cations, respectively, and stirred continuously until completely dissolved. Next, 38.424g of citric acid was added as a complexing agent at a molar ratio of 1:1 to the metal ions in the nitrate. Ammonia was then slowly added dropwise to the nitrate solution with continuous stirring until the solution reached a pH of 2. The solution was then heated in an 80°C water bath with continuous stirring until a gel formed. The wet gel was dried in a forced-air drying oven at 105°C for 48 hours to form a xerogel. The xerogel was calcined in an air atmosphere at a rate of 5°C / min to fully decompose the nitrate in the xerogel and regulate the oxygen decoupling and catalytic conversion properties of the oxygen carrier. The calcination temperature was raised from room temperature to 900°C and then calcined for 4 hours to fully activate the oxygen carrier. The calcined oxygen carrier was ground into a powder with a particle size of less than 0.2 mm, resulting in an oxygen carrier with both oxygen decoupling and catalytic properties, designated 40MnCaFe.

[0105] The oxygen-decoupling-catalytic dual-functional oxygen carrier 40MnCaFe prepared by the above method was uniformly mixed with biomass and introduced into a reactor for a chemical chain gasification reaction, wherein the mass ratio of biomass to oxygen carrier was 2:1. The chemical chain gasification reaction temperature was 800°C and the reaction lasted for 30 minutes. During this time, the oxygen-decoupling property of the oxygen carrier enabled the gas-solid reaction by releasing oxygen from lattice oxygen, promoting coke cracking and tar gasification. The catalytic property of the oxygen carrier also enabled the catalytic conversion of CO2 to CO by releasing oxygen from lattice oxygen, thereby increasing CO yield and selectivity. After the reaction was completed, the atmosphere in the reactor was switched to air, and the oxygen carrier was oxidatively regenerated at 800°C for 30 minutes. Then, an equal amount of biomass as in the first reaction was added to the reactor for a second chemical chain gasification reaction, achieving the recycling and reuse of the oxygen carrier. The specific implementation results of this example are shown in Table 10.

[0106] Table 10. Implementation results of chemical looping gasification based on oxygen decoupling-catalytic dual-functional oxygen carrier 40MnCaFe

[0107]

[0108] Example 10

[0109] The preparation method and chemical looping gasification method in Example 10 are the same as those in Example 9, with the only difference being that the mass ratio of biomass to oxygen carrier during the chemical looping gasification reaction is 5:2. The implementation results in this example are shown in Table 11.

[0110] Table 11. Implementation results of chemical looping gasification based on oxygen decoupling-catalytic dual-functional oxygen carrier 40MnCaFe

[0111]

[0112] Example 11

[0113] The preparation method and chemical looping gasification method in Example 11 are the same as those in Example 9, with the only difference being that during the chemical looping gasification reaction, the mass ratio of biomass to oxygen carrier is 5:3. The implementation results in this example are shown in Table 12.

[0114] Table 12. Implementation results of chemical looping gasification based on oxygen decoupling-catalytic dual-functional oxygen carrier 40MnCaFe

[0115]

[0116] By comparing Examples 1, 3, 6, and 9, it can be seen that during the chemical chain gasification reaction under the same conditions, as the Mn doping content increases, such as the Mn doping content increases from 10% to 20%, the quality of the synthesis gas after the oxygen carrier undergoes the chemical chain gasification reaction is continuously increasing, that is, the output of H2, CO, and CH4 is continuously increasing, and the gasification efficiency and carbonization efficiency are also increasing synchronously; and when the Mn doping content is further increased, that is, the Mn doping content increases from 20% to 40%, the oxygen carrier undergoes the chemical chain gasification reaction. After the reaction, the quality of the syngas continues to decline, namely the production of H2 and CO continues to decrease, and the gasification efficiency and carbonization efficiency also continue to decline. Among them, the most significant changes in the chain gasification reaction of the oxygen carrier 40MnCaFe with a Mn doping content of 40% are mainly due to the fact that with the increase of Mn doping content, the oxidizing properties of the oxygen carrier continue to increase. The highly oxidizing lattice oxygen mainly participates in the conversion of CO to CO2 and H2 to H2O in the syngas reaction, resulting in a decrease in syngas quality. Although gaseous oxygen can also oxidize syngas, it can better promote the cracking of tar and coke, so the benefits and disadvantages are offset.

[0117] When the oxygen carrier has the same Mn doping content, as the mass ratio of biomass to oxygen carrier increases during the chemical chain gasification reaction, that is, when the mass ratio of oxygen carrier to biomass increases from 0.4 to 0.5, the gasification efficiency and carbonization efficiency of the oxygen carrier continue to increase. The main reason is that the biomass and the oxygen carrier fully react. However, when the mass of the oxygen carrier to biomass further increases from 0.5 to 0.6, the gasification efficiency and carbonization efficiency of the oxygen carrier continue to decrease. The main reason is that the oxygen carrier with strong oxidizing properties participates in other side reactions (such as the conversion of CO to CO2 and H2 to H2O), affecting the selective conversion of H2 and CO.

[0118] It can be seen that the method in the embodiment of the present disclosure has been proved through relevant experiments that by regulating the Mn doping content and the ratio of biomass / oxygen carrier in the chain gasification reaction, the oxygen decoupling performance of the oxygen carrier is achieved through the oxygen released by lattice oxygen to realize gas-solid reaction, thereby promoting coke cracking and tar gasification. At the same time, the catalytic performance of the oxygen carrier is achieved when the lattice oxygen releases oxygen to form oxygen vacancies for oxygen decoupling. The oxygen vacancies of the oxygen carrier can be used to realize the catalytic conversion of CO2 into CO, thereby increasing the gasification efficiency of the oxygen carrier to more than 70%, and the carbon conversion efficiency to more than 90%, thereby improving the CO yield and selectivity in the chemical chain gasification reaction.

[0119] Figure 1 3 is a thermogravimetric graph of the composite metal oxygen carriers with different Mn doping amounts in Examples 1, 3, 6, and 9 of the present disclosure after decoupling and regeneration treatment.

[0120] A thermogravimetric reactor was used to simulate inert gas to investigate the oxygen decoupling and regeneration performance of the composite metal oxygen carrier. Figure 1 As shown, within the first 10 minutes, the composite metal oxygen carriers with different Mn doping amounts all showed obvious weight loss, and this part of the weight loss was caused by the components adsorbed in the oxygen carrier. Under Ar atmosphere, the oxygen carrier continued to lose weight, indicating that the oxygen carrier released lattice oxygen during the reaction, indicating that the oxygen carrier had a certain oxygen decoupling performance. Among them, the weight loss phenomenon of 20MnCaFe oxygen carrier was the most serious and the oxygen release rate of the oxygen carrier was slow, indicating that it had strong oxygen decoupling performance. Then, air (containing oxygen) was introduced into the oxygen carrier after the reaction, and under oxygen-rich conditions, the composite metal oxygen carrier would adsorb oxygen to regenerate it. In addition, it can be seen from the figure that the oxygen decoupling oxygen carrier provided in the embodiment of the present disclosure has a faster oxygen absorption rate, which makes it have a faster regeneration rate, which is conducive to the preparation of synthesis gas by chemical chain gasification reaction; it can also be seen that after 5 oxygen decoupling and regeneration reactions, the quality of the composite metal oxygen carrier provided in the embodiment of the present disclosure did not show any significant loss, and still maintained a high oxygen decoupling ability, indicating that it has a high cycle stability.

[0121] Figure 2This is a full spectrum of the X-ray photoelectron spectrum of the composite metal oxygen carrier with different Mn doping amounts in Examples 1, 3, 6, and 9 of the present disclosure.

[0122] like Figure 2 As shown, the oxygen carrier mainly contains Fe, Mn, O, and Ca, and composite metal oxygen carriers with different Mn contents are obtained.

[0123] Figure 3A 3 / 2 diagram of the X-ray photoelectron spectrum of the composite metal oxygen carrier with different Mn doping amounts in Examples 1, 3, 6, and 9 of the present disclosure.

[0124] like Figure 3A As shown, the Mn element in Examples 1, 3, 6, and 9 is mainly in the form of Mn 4+ 、Mn 3+ The 20MnCaFe oxygen carrier has a higher binding energy, and the higher binding energy of Mn means that the oxygen carrier has a higher charge, which in turn makes it have higher OER performance and oxygen activity, thereby making the oxygen carrier have stronger oxygen decoupling performance.

[0125] Figure 3B It is the O1s diagram of the X-ray photoelectron spectrum of the composite metal oxygen carrier with different Mn doping amounts in Examples 1, 3, 6, and 9 of the present disclosure.

[0126] like Figure 3B As shown in the figure, with the increase of Mn, the lattice oxygen (O lat ) continuously increases, which means that the oxidizing performance of the oxygen carrier continues to increase. However, excessive oxidizing property of the oxygen carrier will reduce the quality of the synthesis gas in the chemical chaining gasification reaction.

[0127] Figure 3C 2p diagrams of the X-ray photoelectron spectrum of the composite metal oxygen carriers with different Mn doping amounts in Examples 1, 3, 6, and 9 of the present disclosure.

[0128] like Figure 3C As shown, the Fe in the composite metal oxygen carrier is mainly Fe 2+ and Fe 3+ exists in the form of, and with the increase of Mn doping content, Fe 2+ and Fe 3+ The binding energy is constantly increasing, indicating that there are more high-charge Fe in the oxygen carrier, making the oxygen carrier more oxidizing.

[0129] Figure 4A -D is a transmission electron micrograph of the composite metal oxygen carrier with different Mn doping contents in Examples 1, 3, 6, and 9 of the present disclosure.

[0130] like Figure 4A -D shows that with the increase of Mn doping content, the oxygen lattice spacing first increases and then decreases. The decrease in oxygen lattice spacing will affect the diffusion ability of lattice oxygen and reduce the oxygen decoupling ability of oxygen carriers. For example, when the Mn doping content increases from 20% to 40%, the oxygen lattice spacing decreases from 3.5057nm to 1.8736nm.

[0131] Figure 5 It is a temperature-programmed reduction diagram of the composite metal oxygen carrier with different Mn doping contents in Examples 1, 3, 6, and 9 of the present disclosure.

[0132] like Figure 5 As shown in the figure, with the increase of Mn content, the peak area of ​​hydrogen consumption in the low temperature section continues to increase, which means that the oxidizing property of the oxygen carrier is constantly increasing and the oxygen decoupling performance is constantly decreasing.

[0133] Figure 6 is a Raman spectrum of the composite metal oxygen carrier with different Mn doping contents in Examples 1, 3, 6, and 9 of the present disclosure; Figure 7 3 is a Fourier transform infrared spectrum of the composite metal oxygen carrier with different Mn doping contents in Examples 1, 3, 6, and 9 of the present disclosure.

[0134] like Figure 6 and Figure 7 As shown in the figure, with the increase of Mn content, the displacement of the optical spectrum changes, among which the change of 20MnFeCa is the most significant, indicating that the structure of the Fe-O bond in the 20MnFeCa octahedron is distorted.

[0135] Figure 8 3 are X-ray diffraction patterns of composite metal oxygen carriers with different Mn doping contents in Examples 1, 3, 6, and 9 of the present disclosure.

[0136] like Figure 8 As shown in the figure, with the increase of Mn content, the structure of the oxygen carrier realizes the transition transformation from Ca2Fe2O5 (JCPDS Card no71-2264) to CaMnO3 (JCPDS Card no 50-1746), realizing B site doping, affecting the OER performance of the material, and then affecting the oxygen decoupling performance of the oxygen carrier.

[0137] In summary, with the increase of Mn doping content (10% to 40%), the oxidizing property of the oxygen carrier gradually increases, while the oxygen decoupling performance of the oxygen carrier is strongest when the Mn doping content is 20% (20MnCaFe). It can be seen that the oxygen decoupling performance and oxidation performance of the present invention are relatively independent, which effectively avoids the quality reduction of oxygen decoupling into gas due to the excessive oxidizing property of the oxygen carrier. The 20MnCaFe oxygen carrier formed when the Mn doping content is 20% will lead to structural distortion of the Fe-O bond in the octahedral structure of the oxygen carrier and stronger adsorption capacity of carbon oxides, so that it has the strongest CO2 adsorption catalytic conversion ability and oxygen decoupling performance.

[0138] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above are only specific embodiments of the present disclosure and are not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the scope of protection of the present disclosure.

Claims

1. A chemical chain gasification method, characterized in that: The method comprises: During the biomass chemical chain gasification reaction, the lattice oxygen of the oxygen carrier releases oxygen, resulting in the generation of oxygen vacancies for oxygen carrier reduction and oxygen decoupling, and the oxygen vacancies of the oxygen carrier are used to realize the conversion of CO2 into CO, wherein the mass ratio of the oxygen carrier to the biomass is 0.5; The oxygen carrier is a MnCaFeO-based composite metal oxygen carrier, wherein the metal component of the oxygen carrier is composed of Mn, Fe, and Ca elements, wherein the molar percentage content of Mn, Fe, and Ca is 20%:40%:40%, and the structure of the Fe-O bond in the formed oxygen carrier octahedron is distorted, and it has oxygen decoupling performance and catalytic performance, and the oxygen decoupling performance and oxidation performance are relatively independent, and the catalytic performance is CO2 adsorption catalytic conversion capability.

2. The method according to claim 1, characterized in that The oxygen carrier is prepared by the following method: Mixing iron nitrate, calcium nitrate and manganese nitrate to prepare a nitrate solution; Adding a complexing agent to the nitrate solution, adjusting the pH value of the solution, and heating to form a gel; The dried gel is calcined to obtain an oxygen carrier; Wherein, the molar percentage content of Mn, Fe and Ca metal ions in the nitrate solution is 20%:40%:40%.

3. The method according to claim 2, wherein the molar ratio of the complexing agent to the metal ions in the nitrate is 0.5:1-1.5:1, wherein The complexing agent includes citric acid.

4. The method according to claim 2, characterized in that: The pH of the solution was adjusted to 1.9-2.

1.

5. The method according to claim 2, characterized in that: The parameters of the calcination process include: The temperature of the calcination treatment includes: 850-950°C; The heating rate of the calcination treatment includes: 5-10 ℃ / min.

6. The method according to claim 3, characterized in that The method also includes grinding the calcined oxygen carrier into powder with a particle size less than 0.2 mm.