A forming method for sheet metal cover parts
By using soft elastic edge compression rings and annealing treatment in the molding of aviation sheet metal cover parts, combined with domestic equipment, the problems of high cost and low efficiency in the existing technology are solved, and more efficient molding and heat treatment are achieved, reducing the number of reductions in the reduction of The parts are broken and deformed, and the production efficiency and yield rate are improved.
Patent Information
- Application Number
- CN202211013564.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-08-23
AI Technical Summary
The existing aviation sheet metal cover part forming technology has problems such as high investment costs, high frequency of equipment use, long processing cycle, low production efficiency, easy breakage of parts and large deformation of heat treatment.
A method of forming a sheet metal cover part is adopted. By installing an upper and lower concave die on the press, using a soft elastic edge ring to press it step by step, and annealing is performed to reduce the number of molding and heat treatments, and the domestically produced 2000T is used. Rubber frame press and air furnace are molded.
It reduces production costs, improves production efficiency, reduces parts fracture phenomena and heat treatment deformation, extends the service life of the equipment, simplifies the process flow, and improves the yield and mechanical properties of the workpiece.
Smart Images

Figure CN115301847B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of aerospace, and in particular relates to a method for forming aviation sheet metal cover parts. Background Art
[0002] At present, the disadvantages of the molding solutions of the existing technology are:
[0003] 1. The equipment used in the prior art for forming aviation sheet metal cover parts is an imported 77000T capsule press and salt bath furnace, which has a high investment cost;
[0004] 2. The equipment is used frequently, which occupies equipment resources for a long time and affects the service life of the equipment;
[0005] 3. The molding process (pressing process, heat treatment process) is complicated, the parts processing cycle is long, and the production efficiency is low;
[0006] 4. During the forming process, the R angle transition of the parts is prone to breakage, resulting in scrapping and high production costs;
[0007] 5. Multiple heat treatments affect the mechanical properties of parts, and the parts are greatly deformed after heat treatment, requiring a lot of work in shaping and reshaping. Summary of the invention
[0008] The invention provides a forming method for sheet metal cover parts, the purpose of which is to reduce the parts forming process, reduce the production cost and improve the production efficiency.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions:
[0010] A method for forming sheet metal cover parts, comprising the following steps:
[0011] Step 1: Install an upper punch and a lower die on the press machine that match the cavity of the cover-type part to be formed;
[0012] Step 2: Place the part blank between the upper punch and the lower die, and place a soft elastic blank holder ring I on the circumference of the upper surface of the part blank to complete the first pressing process;
[0013] Step 3, turn over the blank after the first pressing, set a soft elastic blank holder ring I on the circumference of the upper surface after the turning over, and complete the second pressing;
[0014] Step 4, replace the soft elastic blank holder ring I with soft elastic blank holder ring II, soft elastic blank holder ring III, ... soft elastic blank holder ring N in sequence, wherein N ≥ 2, and each time the soft elastic blank holder ring is replaced, a press forming is completed; wherein, the thickness of the soft elastic blank holder ring I, the soft elastic blank holder ring II, ... the soft elastic blank holder ring N decreases in sequence;
[0015] Step 5: Remove the soft elastic blank holder and complete the last pressing;
[0016] Step 6: Cut off the excess and quench to adjust the shape.
[0017] Furthermore, in step one, a plurality of nest-shaped cavities are formed on the mouth cover-like parts to be formed, and the plurality of nest-shaped cavities are in a symmetrical structure.
[0018] Furthermore, in step 2, after the first pressing, a crack stop hole is opened for each cavity with its center as the center of the circle.
[0019] Furthermore, in step 2, the part blank with the crack stop hole is fully annealed, and the conditions for the full annealing are: keeping the temperature at 413±15°C for at least 2 hours, cooling to 260°C with the furnace, and then cooling in an air environment.
[0020] Furthermore, in step three, for the part blank whose cavity is symmetrically distributed on the left and right sides, first the left and right sides are swapped, and then turned over and pressed back.
[0021] Furthermore, in step 4, the part blank after the third pressing is subjected to intermediate annealing, and the conditions of the intermediate annealing are: at a temperature of 340±10°C, keeping warm for 0.5h-1h, and cooling in an air environment.
[0022] Furthermore, in step four, when N=4, the soft elastic blank holder ring I is replaced with the soft elastic blank holder ring II, the soft elastic blank holder ring III and the soft elastic blank holder ring IV in sequence, and the third, fourth and fifth pressing operations are completed in sequence accordingly.
[0023] Furthermore, the pressure of the first pressing is 800T-1000T, and the pressure is maintained for 10s, the pressure of the second pressing is 800T-1000T, and the pressure is maintained for 10s, the pressure of the third pressing is 1000T-1200T, and the pressure is maintained for 10s, the pressure of the fourth pressing is 1200T-1500T, and the pressure is maintained for 10s, and the pressure of the fifth pressing is 1200T-1500T, and the pressure is maintained for 10s.
[0024] Furthermore, the thicknesses of the soft elastic blank holder ring I, the soft elastic blank holder ring II, the soft elastic blank holder ring III and the soft elastic blank holder ring IV are 25 mm, 10 mm, 5 mm and 3 mm respectively, and their hardness values are all 70°-80°.
[0025] Furthermore, in step five, the quenching condition is 494° C., keeping warm for 30-40 minutes, and quenching and water cooling followed by frozen storage.
[0026] The technical solution of the present invention is used to form aviation sheet metal cover parts, which has the following advantages:
[0027] 1. Use existing equipment (domestic 2000T rubber container frame press, air furnace) for simple transformation, with low investment cost; at the same time, release the production capacity of the imported 77000T capsule press machine to improve parts production efficiency;
[0028] 2. The equipment is used less frequently, occupies less equipment resources, and has a longer service life;
[0029] 3. Reduce the number of parts forming and heat treatment times, reduce the number of pressing and heat treatment processes, save production costs, and significantly improve production efficiency;
[0030] 4. Effectively solve the fracture phenomenon at the R corner transition of parts during the pressing process, reduce production costs, and improve the yield rate of parts;
[0031] 5. Reduce the number of heat treatments, effectively solve the problem of heat treatment deformation, and reduce the workload of shape correction and shaping;
[0032] 6. The process of the present invention is simple and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is an axonometric view of the press;
[0034] Figure 2 It is the front view of the press;
[0035] Figure 3 It is a schematic diagram of forming a double-row eight-hole cover part;
[0036] Figure 4 It is a schematic diagram of forming a single-row three-hole cover part;
[0037] Figure 5 It is a schematic diagram of the installation position of the soft elastic blank holder;
[0038] Figure 6 It is a schematic diagram of the structure of the cover parts after forming;
[0039] In the figure, 1, upper table, 2, lower table, 3, part blank, 4, soft elastic pressure ring, 5, nest cavity, 6, crack stop hole. DETAILED DESCRIPTION
[0040] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Specific implementation method 1
[0042] A method for forming sheet metal cover parts, comprising the following steps:
[0043] Step 1: Pressing machine: Select a domestic 2000T capsule frame press machine, add an upper table 1 and a lower table 2 with T-slots, install an upper punch and a lower die matching the cavity 5 of the cover parts to be formed on the upper table 1 and the lower table 2 with T-slots, respectively, to form aircraft cover parts. The tooling structure is shown in Figure 1 and Figure 2 ; Select the domestic 2000T capsule frame press to replace the imported 77000T capsule press on the single-sided die aviation sheet metal forming method, releasing the production capacity of valuable equipment and machine tools;
[0044] Step 2: Set the part blank 3 between the upper punch and the lower die, set a soft elastic pressure ring I at the circumference of the upper surface of the part blank 3, and complete the first pressing; for each cavity 5, set the center of the circle as the center of the circle to open a crack stop hole 6; fully anneal the part blank 3 with the crack stop hole 6, and the conditions for full annealing are: keep warm at a temperature of 413±15℃ for at least 2h, cool to 260℃ with the furnace, and then cool in air. The reason for choosing full annealing at this time: the material deformation is large after the first pressing of the part, and the stress is too concentrated, and the purpose is to release the stress of the part;
[0045] Step 3, turn over the blank after the first pressing, set a soft elastic blank holder ring I on the circumference of the upper surface after the turning over, and complete the second pressing;
[0046] Step 4, replace the soft elastic blank holder ring I with soft elastic blank holder ring II, soft elastic blank holder ring III, ... soft elastic blank holder ring N in sequence, wherein N ≥ 2, and each time the soft elastic blank holder ring is replaced, a press forming is completed; wherein, the thickness of the soft elastic blank holder ring I, the soft elastic blank holder ring II, ... the soft elastic blank holder ring N decreases in sequence;
[0047] Step 5, cancel the soft elastic blank holder 4 and complete the last pressing;
[0048] Step 6: Cut off the excess and quench to adjust the shape.
[0049] Furthermore, in step one, a plurality of nest-shaped cavities 5 are formed on the mouth cover-like parts to be formed, and the plurality of nest-shaped cavities 5 are in a symmetrical structure.
[0050] Furthermore, in step three, for the part blank 3 whose cavity 5 is symmetrically distributed on the left and right sides, the left and right sides are first swapped and then turned over and pressed back, which not only achieves the purpose of material gathering, but also effectively solves the cracking problem at the excessive R position, greatly reducing the scrap rate.
[0051] Furthermore, in step 4, the part blank 3 after the third pressing is subjected to intermediate annealing, and the conditions of the intermediate annealing are: at a temperature of 340±10°C, keeping warm for 0.5h-1h, and cooling in an air environment.
[0052] Furthermore, in step four, when N=4, the soft elastic blank holder ring I is replaced with the soft elastic blank holder ring II, the soft elastic blank holder ring III and the soft elastic blank holder ring IV in sequence, and the third, fourth and fifth pressing operations are completed in sequence accordingly.
[0053] Furthermore, the material of the soft elastic blank holder ring I, the soft elastic blank holder ring II, the soft elastic blank holder ring III and the soft elastic blank holder ring IV is preferably polyurethane material;
[0054] Furthermore, in step five, the quenching conditions are 494° C., heat preservation for 30-40 minutes, quenching with water cooling, and low-temperature storage before shaping, preferably at a temperature ≤-18° C., and storage at room temperature after shaping.
[0055] Since the depth of the part reinforcement cavity 5 is too large, the upper and lower die structures in the solution of the present invention directly form the part. In order to prevent the uneven feeding of the part from causing wrinkles in the part cavity and its peripheral edges, a soft elastic pressure ring replaces the tooling pressure ring. Figure 3 and Figure 4 The parts are formed by setting a soft elastic blank holder 4 in a manner where the thickness decreases layer by layer.
[0056] The pressure varies according to the characteristics of products of different shapes and the thickness of soft elastic pressure ring pads of different thicknesses. Please see the table below for details.
[0057]
[0058] Reasonable selection of soft elastic blank holder pad plays the most critical role in part forming. This solution solves the problem of no blank holder force in the tooling. At the same time, compared with the metal blank holder of stamping parts in the automotive industry, it simplifies the mold structure and greatly reduces the production cost of the tooling. The price of a set of extended molds for cover types with blank holders is between 500,000 and 700,000 yuan. The cost of mold manufacturing in this solution with a polyurethane pad mold is 15-20% of the above.
[0059] According to the actual formed product, soft elastic pressure rings of different thicknesses are selected, and the number of pressing times can also be determined according to the actual situation.
[0060] ① The present invention adopts a material gathering method of turning over and back pressing (reverse extrusion molding).
[0061] Metal extrusion is a plastic processing method that applies strong pressure to the metal billet placed in the mold cavity, forcing the metal billet to produce directional plastic deformation, and extrude it from the die hole of the extrusion die to obtain parts or semi-finished products with the desired cross-sectional shape, size and certain mechanical properties.
[0062] Back extrusion: The plasticity of the metal parts is improved through the initial forming by forward extrusion, and then back extrusion is performed. The metal flow direction is the same as the movement direction of the punch. During the extrusion process, the extruded metal can obtain a strong and uniform three-dimensional compressive stress state in the deformation zone, which gives full play to the plasticity of the processed metal itself.
[0063] According to the shape characteristics of aviation cover products: for an axially symmetrical single-row cavity, the first step is to use a 25mm thick polyurethane gasket 800-1000T pressure forming, and then completely stress relieve annealing, and the second step is to turn it over and press it back; if it is an even-numbered row cavity with left-right symmetrical distribution, the first step is to use a 25mm thick polyurethane gasket 800-1000T pressure forming, and then completely stress relieve annealing, and the second step is to swap the left and right sides and then turn it over and press it back, so that the purpose of material aggregation is achieved, thereby effectively solving the cracking problem at the excessive R and greatly reducing the scrap rate.
[0064] 2 Reasonable application of one-step forming of aviation sheet metal parts
[0065] The one-step method for aviation aluminum alloy sheet metal parts is to store the quenched aluminum alloy plates at low temperature (≤-18℃) to maintain the good plasticity of the aluminum alloy sheets in the newly quenched state, and to complete the forming and shaping of the newly quenched sheets in one go by mechanized means.
[0066] In the prior art, the workpiece after the final heat treatment (quenching) has a great deformation, and it is difficult for workers to correct the shape and the cycle is long, generally about 6-8 hours for a single piece.
[0067] Preferably, in the steps of the scheme of the present invention, before the last step of forming the part, a 3mm underpressure is selected to be retained, and intermediate annealing is first performed to eliminate stress, and then quenching is performed according to the final use state, and the die is directly pressed to form to the final state after quenching, so that the deformation after heat treatment is basically eliminated after forming, which can effectively solve the problem of increased shaping and shaping workload caused by heat treatment deformation, and the shaping time of workers is generally within 1-2 hours. The shaping efficiency of workers is greatly improved.
[0068] Example 1
[0069] Taking the forming of double-row eight-hole cover parts as an example, the specific steps of the present invention are described in detail.
[0070] This part is formed in the following nine steps, which reduces 3-4 heat treatment (intermediate annealing) processes compared to the original forming solution, greatly improving part production efficiency.
[0071] Step 1: Place a 25mm thick polyurethane blank holder pad I on the circumference of the upper surface of the part blank, with a pressure of 800T and hold the pressure for 10 seconds to complete the first pressing. See the specific on-site photos for details. Figure 1 ;
[0072] Step 2: With the center of the reinforcing cavity as the center, a crack stop hole with a diameter of 80mm is opened, and the part blank is fully annealed. The reason for choosing full annealing at this time is that the material deformation of the part is large after the first step of profiling, and the stress is too concentrated. The purpose of annealing is to release the stress of the part. The specific requirements for full annealing are: the temperature is 413±15℃, the temperature is kept for at least 2h, and the furnace is cooled to 260℃, and then cooled in the air;
[0073] Step 3: Turn over the annealed part blank, place a 25mm thick polyurethane blank holder pad I on the circumference of the upper surface of the part blank, reverse extrude, press 800T, hold the pressure for 10 seconds, and complete the second pressing;
[0074] Step 4: Replace the 25mm thick polyurethane blank holder pad I with a 10mm thick polyurethane blank holder pad II, apply a pressure of 1000T, hold the pressure for 10 seconds, and complete the third pressing;
[0075] Step 5: Intermediate annealing. The specific requirements for intermediate annealing are: temperature of 340±10℃, heat preservation for 0.5h-1h, cooling in air;
[0076] Step 6: Replace the 10mm thick polyurethane pressure ring pad II with a 5mm thick polyurethane pressure ring pad III, with a pressure of 1200T, and hold the pressure for 10 seconds to complete the fourth press;
[0077] Step 7: Replace the 5mm thick polyurethane pressure ring pad III with a 3mm thick polyurethane pressure ring pad IV, apply a pressure of 1400T, hold the pressure for 10 seconds, and complete the fifth pressing;
[0078] Step 8: Remove the polyurethane pressure ring pad IV, pressure 1200T, and maintain pressure for 10 seconds;
[0079] Step 9: Remove excess according to the cutting line and quench and adjust the shape. Specific requirements for quenching: 494℃ insulation for 30-40min quenching and water cooling.
[0080] The schematic diagram of the structure of the cover parts after forming is as follows Figure 6 shown.
[0081] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for forming sheet metal cover parts. Features , including the following steps: Step 1: Install an upper punch and a lower die on the press machine that match the cavity of the cover-type part to be formed; Step 2: The part blank is placed between the upper punch and the lower die, and a soft elastic pressure ring I is placed at the circumference of the upper surface of the part blank to complete the first pressing. After the first pressing, a crack stop hole is opened for each cavity with its center as the center of the circle. Step 3, turn over the blank after the first pressing, set a soft elastic blank holder ring I on the circumference of the upper surface after the turning over, and complete the second pressing; Step 4, replace the soft elastic blank holder ring I with soft elastic blank holder ring II, soft elastic blank holder ring III, ... soft elastic blank holder ring N in sequence, wherein N ≥ 2, and each time the soft elastic blank holder ring is replaced, a press forming is completed; wherein, the thickness of the soft elastic blank holder ring I, the soft elastic blank holder ring II, ... the soft elastic blank holder ring N decreases in sequence; Step 5: Remove the soft elastic blank holder and complete the last pressing; Step 6: Cut off the excess and quench to adjust the shape.
2. A method for forming sheet metal cover parts according to claim 1, Features: In step one, a plurality of nest-shaped cavities are formed on the mouth cover-like parts to be formed, and the plurality of nest-shaped cavities are in a symmetrical structure.
3. A method for forming sheet metal cover parts according to claim 1, Features: In step 2, the part blank with the crack stop hole is fully annealed. The conditions for the full annealing are: keeping the temperature at 413±15°C for at least 2 hours, cooling to 260°C with the furnace, and then cooling in an air environment.
4. A method for forming sheet metal cover parts according to claim 1, Features: In step three, for the part blank whose cavity is symmetrically distributed on the left and right sides, first swap the left and right sides, then turn over and press back.
5. A method for forming sheet metal cover parts according to claim 1, Features: In step 4, the part blank after the third pressing is subjected to intermediate annealing, and the conditions of the intermediate annealing are: at a temperature of 340±10°C, keeping warm for 0.5h-1h, and cooling in an air environment.
6. A method for forming sheet metal cover parts according to claim 1, Features: In step 4, when N=4, the soft elastic blank holder ring I is replaced with the soft elastic blank holder ring II, the soft elastic blank holder ring III and the soft elastic blank holder ring IV in sequence, and the third, fourth and fifth pressing operations are completed in sequence accordingly.
7. A method for forming sheet metal cover parts according to claim 6, Features: The pressure of the first pressing is 800T-1000T, and the pressure is maintained for 10s. The pressure of the second pressing is 800T-1000T, and the pressure is maintained for 10s. The pressure of the third pressing is 1000T-1200T, and the pressure is maintained for 10s. The pressure of the fourth pressing is 1200T-1500T, and the pressure is maintained for 10s. The pressure of the fifth pressing is 1200T-1500T, and the pressure is maintained for 10s.
8. A method for forming sheet metal cover parts according to claim 6, Features: The thicknesses of the soft elastic pressure ring I, soft elastic pressure ring II, soft elastic pressure ring III and soft elastic pressure ring IV are 25 mm, 10 mm, 5 mm and 3 mm respectively, and their hardness values are all 70°-80°.
9. A method for forming sheet metal cover parts according to claim 1, Features: In step 5, the quenching conditions are 494° C., keeping warm for 30-40 minutes, quenching with water cooling, and freezing before calibration.