Method for preparing gas sensor, gas sensor obtained thereby and application thereof

By using combined buffer layer and UV ozone treatment technology in gas sensors, the problems of insufficient rigidity and graphene flexibility of traditional sensors are solved, and a wearable gas sensor with bending resistance and high sensitivity are realized, suitable for detecting benzene gases.

CN115308269BActive Publication Date: 2024-12-06SHANGHAI INST OF MICROSYSTEM & INFORMATION TECH CHINESE ACAD OF SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210937290.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-05
Publication Date
2024-12-06
Estimated Expiration
2042-08-05

AI Technical Summary

Technical Problem

The rigid structure of traditional gas sensors makes it impossible to achieve bending resistance and wearable applications, and the flexibility of graphene gas sensors cannot meet the needs of wearable devices, especially the problem of performance affected at bending angles.

Method used

Using a combined buffer layer structure, consisting of graphene buffer layer and organic flexible insulating material buffer layer, the mutual repulsion between layers is increased by introducing oxygen-containing functional groups, and the oxidation degree of sensitive material layer is optimized through ultraviolet ozone irradiation, thereby enhancing the resistance of gas sensors. Bending performance and sensitivity.

Benefits of technology

It improves the bending resistance of the gas sensor and the sensitivity to benzene gases, realizes the application of wearable devices, and enhances the elastic deformation ability of the device and the detection ability of harmful gases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115308269B_ABST
    Figure CN115308269B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a gas sensor, comprising providing a substrate; preparing at least one combined buffer layer consisting of a graphene buffer layer and an organic flexible insulating material buffer layer on the substrate; preparing a sensitive material layer on the topmost organic flexible insulating material buffer layer, wherein the sensitive material layer is a graphene sensing layer; forming a source electrode and a drain electrode on the sensitive material layer; and performing post-processing to introduce oxygen-containing functional groups at the contact surface of the graphene buffer layer and the organic flexible insulating material buffer layer to increase the mutual repulsion between the layers and optimize the oxidation degree of the sensitive material layer. The gas sensor according to the present invention and its application are used to detect benzene gases. According to the gas sensor of the present invention, the organic flexible insulating material buffer layer is placed between two graphene layers to offset external forces, and the sliding effect between the graphene layers is increased by simply stacking the graphene layers, thereby enhancing the bending resistance of the graphene gas sensor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to detection, and more specifically to a method for preparing a gas sensor, the gas sensor obtained thereby and applications thereof. Background Art

[0002] Benzene, aldehydes, etc. are organic volatile harmful gases. In a low concentration environment, only a brief contact will cause irritation to the human eyes and respiratory tract, and may cause liver system damage. This type of volatile organic compound has a great impact on human health and the quality of the living environment. Real-time monitoring of harmful gases is particularly important. Gas sensors are an important branch of sensing technology. They can convert information related to gas types and concentrations into electrical signals for detection, monitoring, analysis and alarm. Compared with traditional gas detection instruments, gas sensors have the advantages of low cost, low power consumption and portability, making them an important part of real-time gas monitoring.

[0003] Traditional gas sensors are not resistant to bending and stretching due to the rigid structure of their materials, and cannot be used in wearable applications. Therefore, traditional gas sensors cannot monitor the surrounding environment and health of the human body. In recent years, with the rapid development of flexible electronics, wearable products have enriched and improved people's quality of life due to their advantages of being bendable, portable and wearable. Among them, wearable gas sensors have different bending and stretching properties from traditional gas sensors, which makes it possible to monitor the surrounding environment and health of the human body in real time. However, there are still many problems that need to be solved for wearable gas sensors. Among them, how to improve the bending resistance and sensitivity of wearable gas sensors to benzene gases are problems that need to be solved urgently.

[0004] Graphene is a sp 2 Hybrid connected carbon atoms are tightly stacked into a single-layer two-dimensional honeycomb lattice structure, which has good conductivity, large specific surface area and easy modification. Graphene gas sensors have been widely studied and have achieved many fruitful results, but for wearable device applications, the flexibility of graphene is far from meeting the requirements. At a certain bending angle, the graphene film will break, which has a great impact on the performance of the device. Summary of the invention

[0005] In order to solve the above-mentioned problems of poor bending resistance of graphene gas sensors in the prior art, the present invention provides a method for preparing a gas sensor, a gas sensor obtained thereby and applications thereof.

[0006] According to one aspect of the present invention, a method for preparing a gas sensor is provided, which comprises the following steps: S201, providing a substrate; S202, preparing at least one combined buffer layer on the substrate, the combined buffer layer consisting of a simply stacked graphene buffer layer and an organic flexible insulating material buffer layer; S203, preparing a sensitive material layer on the topmost organic flexible insulating material buffer layer, the sensitive material layer being a graphene sensing layer; S204, forming a source and a drain in the sensitive material layer; S205, performing post-processing, by introducing oxygen-containing functional groups (such as hydroxyl or carboxyl) at the contact surface of the graphene buffer layer and the organic flexible insulating material buffer layer to increase the mutual repulsion between the layers to improve the bending resistance of the gas sensor, and by optimizing the oxidation degree of the sensitive material layer (such as increasing the hydroxyl content) to improve the sensitivity of the gas sensor.

[0007] Preferably, 1 to 10 combined buffer layers are prepared on the substrate.

[0008] Preferably, the post-treatment is ultraviolet ozone irradiation. In a preferred embodiment, the ultraviolet ozone irradiation treatment time is 1 to 30 minutes, and the ultraviolet lamp power is 50-300 W. In a preferred embodiment, the ultraviolet ozone irradiation treatment time is 1200 to 1500 seconds.

[0009] Preferably, the oxygen-containing functional group is a carboxyl group.

[0010] According to another aspect of the present invention, a gas sensor obtained according to the above-mentioned preparation method is provided, which includes a substrate, at least one combined buffer layer, a sensitive material layer, a source electrode and a drain electrode, wherein the combined buffer layer is composed of a simply stacked graphene buffer layer and an organic flexible insulating material buffer layer.

[0011] Preferably, the graphene buffer layer of each combined buffer layer is a single-layer graphene structure.

[0012] Preferably, the thickness of the organic flexible insulating material buffer layer of each combined buffer layer is less than 2 micrometers.

[0013] Preferably, the organic flexible insulating material buffer layer is a polymethyl methacrylate buffer layer or a polydimethylsiloxane buffer layer.

[0014] According to another aspect of the present invention, there is provided an application of the gas sensor described above, which is used to detect benzene or aldehyde gases.

[0015] Preferably, the benzene gas is o-dichlorobenzene. In a preferred embodiment, the content of o-dichlorobenzene is 50 ppm.

[0016] The gas sensor according to the present invention is a flexible gas sensor that is resistant to bending. Based on the characteristics of graphene gas sensors and wearable devices, an organic flexible insulating material (such as polymethyl methacrylate or polydimethylsiloxane) is placed between two graphene layers as a buffer layer (i.e., a flexible buffer layer containing alkyl side chains) to offset external forces. The sliding effect between the graphene layers is increased by simply stacking the graphene layers, thereby enhancing the bending resistance of the graphene gas sensor. In a preferred embodiment, the device is subjected to ultraviolet ozone irradiation on the graphene and the flexible buffer layer containing alkyl side chains. On the one hand, the degree of oxidation of the graphene layer is optimized to enhance the sensitivity of the device to benzene gases. On the other hand, the contact surface of the graphene layer and the flexible buffer layer containing alkyl side chains is hydroxylated to increase the mutual repulsion between the layers, thereby enhancing the elastic deformation capacity of the stacked graphene-polymethyl methacrylate buffer layer, and further enhancing the bending resistance of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0018] Figure 1 FIG. 4 is a schematic structural diagram of a gas sensor according to a preferred embodiment of the present invention.

[0019] Figure 2A Schematic diagram of a single-layer graphene according to a preferred embodiment of the present invention.

[0020] Figure 2B 1 is a structural diagram of polymethyl methacrylate according to a preferred embodiment of the present invention.

[0021] Figure 3 The figure is a schematic flow chart of a method for preparing a gas sensor according to a preferred embodiment of the present invention.

[0022] Figure 4 This is a comparison chart of the response of the gas sensor to 50 ppm o-dichlorobenzene before and after ultraviolet ozone illumination treatment according to a preferred embodiment of the present invention.

[0023] Figure 5 This is a comparison chart of the responses of the gas sensor to 50 ppm o-dichlorobenzene after UV light treatment for different time periods according to a preferred embodiment of the present invention.

[0024] Figure 6This is a comparison chart of the average response of the gas sensor to 50 ppm o-dichlorobenzene before and after ultraviolet ozone illumination treatment according to a preferred embodiment of the present invention.

[0025] Figure 7 This is a graph showing the Fourier transform infrared spectroscopy characterization results of a graphene layer before and after ultraviolet ozone light treatment according to a preferred embodiment of the present invention.

[0026] Figure 8 This is a graph showing the Raman characterization results of a graphene layer before and after ultraviolet ozone irradiation treatment according to a preferred embodiment of the present invention. DETAILED DESCRIPTION

[0027] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure or characteristic that may be included in at least one implementation of the present invention. In the description of the embodiments of the present invention, it should be understood that the orientation or positional relationship indicated by the terms "upper", "lower", "top", "bottom", etc. is based on the orientation or positional relationship shown in the accompanying drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, the terms "first" and "second" are used only for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Moreover, the terms "first", "second", etc. are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein.

[0029] like Figure 1 As shown, the gas sensor according to a preferred embodiment of the present invention is a chemical resistance gas sensor, which adopts a bottom gate top contact structure and includes a substrate 1, a graphene buffer layer 2, a flexible buffer layer of a polymer containing alkyl side chains 3, a sensitive material layer 4, a source 5 and a drain 6.

[0030] The substrate 1 is a flexible substrate, and the material used is PET, PI or silica gel.

[0031] The graphene buffer layer 2 is a simple stack of single-layer graphene layers, which are stacked on the upper surface of the substrate 1, wherein the structure of the graphene is as follows: Figure 2A The simple stacking in this article refers to physical stacking, where no chemical reaction occurs between the layers.

[0032] The alkyl side chain-containing polymer flexible buffer layer 3 is a non-conductive polymer material with elastic deformation ability, also known as an organic flexible insulating material, such as a polymethyl methacrylate or polydimethylsiloxane buffer layer, which is stacked on the upper surface of the graphene buffer layer 2, wherein the structure of the polymethyl methacrylate is as follows: Figure 2B shown.

[0033] The sensitive material layer 4 is a graphene sensing layer, which is stacked on the upper surface of the alkyl side chain-containing polymer flexible buffer layer 3 .

[0034] The source electrode 5 and the drain electrode 6 adopt an interdigitated electrode structure and are arranged on the upper surface of the sensitive material layer 4. In this embodiment, the spacing between the source electrode 5 and the drain electrode 6 is 50 μm, the thickness of the electrode is 20-100 nm, the aspect ratio of the electrode ranges from 10 to 100, the number of channels of the electrode is 5 to 20, and the material of the electrode can be a conductive material with a high work function such as gold, silver or aluminum.

[0035] It should be understood that Figure 1 The two-layer structure formed by stacking the graphene buffer layer 2 and the flexible buffer layer 3 containing alkyl side chains of the gas sensor can be called a combined buffer layer 23, that is, a graphene-flexible buffer layer containing alkyl side chains. The gas sensor of the present invention may include an alternating stacking structure of a graphene buffer layer 2 and a flexible buffer layer 3 containing alkyl side chains, that is, it includes a plurality of combined buffer layers 23, and the sensitive material layer 4 is located on the upper surface of the top flexible buffer layer 3 containing alkyl side chains, so that the flexible buffer layer 3 containing alkyl side chains is always arranged in the interlayer of two graphene layers. It should be understood that the bending resistance of the gas sensor according to the present invention can be regulated by the total number of layers of the combined buffer layer 23, and each combined buffer layer 23 is arranged by a simple stacking method. Preferably, the number of layers of the combined buffer layer 23 is between 1 and 10.

[0036] According to a method for preparing a gas sensor in a preferred embodiment of the present invention, the optional solvents for processing the alkyl side chain polymer flexible buffer layer 3 (for example, a polymethyl methacrylate buffer layer) and the graphene layer (i.e., the graphene buffer layer 2 and the sensitive material layer 4) are acetone, isopropanol, ethanol or chloroform and the like, and the solution transfer method is used to prepare them on a flexible substrate material, and the graphene-polymethyl methacrylate buffer layer and the number of graphene-polymethyl methacrylate layers are regulated by simple stacking to enhance the elastic deformation ability, thereby improving the bending resistance of the gas sensor.

[0037] like Figure 3 As shown, the method for preparing a gas sensor according to a preferred embodiment of the present invention first includes step S201, selecting and cleaning the substrate 1. In the preferred embodiment, PET, PI or silica gel is selected, cut into a desired shape and area, such as a PET sheet of 1 cm×1 cm in size, first ultrasonically cleaned with deionized water for 10 minutes, then ultrasonically cleaned in acetone and isopropanol organic solvents for 15 minutes in turn, and blown dry with nitrogen.

[0038] The method for preparing a gas sensor according to a preferred embodiment of the present invention then includes step S202, preparing a combined buffer layer 23 on the substrate 1. The combined buffer layer 23 is a buffer layer obtained by adjusting the treatment time and releasing the combined buffer layer using acetone, isopropanol, ethanol or chloroform as a solvent. In this embodiment, the combined buffer layer 23 is a graphene-polymethyl methacrylate layer, which includes treating the graphene layer with acetone, isopropanol, ethanol or chloroform to eliminate the protective layer, and forming the graphene layer through a film-forming process of a solution transfer method; it includes treating the polymethyl methacrylate layer with acetone, isopropanol, ethanol or chloroform for 1 to 30 minutes to control the thickness of the flexible buffer layer to be less than 2 microns, and forming a flexible buffer layer containing an alkyl side chain polymer through a film-forming process of a solution transfer method or a spin coating method. In a preferred embodiment, the graphene-polymethyl methacrylate layer grown on the copper foil is immersed in a saturated solution of ferric chloride, and the copper foil is completely removed after full contact, and then the graphene-polymethyl methacrylate layer is treated in acetone, isopropanol, ethanol or chloroform, and treated for 1 to 30 minutes to obtain a graphene-polymethyl methacrylate layer, and transferred to deionized water, and the graphene-polymethyl methacrylate layer is released into the substrate material by a solution transfer method, and finally annealed to obtain a stable graphene-polymethyl methacrylate layer. The simple stacking structure is to stack the released graphene-polymethyl methacrylate layer on the upper surface of the substrate, and then annealed to obtain, and so on, the number of graphene-polymethyl methacrylate layer stacking layers is 1 to 10. It should be understood that the solvent treatment time is less than 1 minute and has no effect. After more than 30 minutes, the material will be over-oxidized, the film will decompose with a high probability, and the device will be damaged.

[0039] The preparation method of the gas sensor according to a preferred embodiment of the present invention then includes step S203, preparing a sensitive material layer 4 on the topmost flexible buffer layer 3 containing alkyl side chains. The sensitive material layer 4 is a graphene layer obtained by adjusting the treatment time using acetone, isopropanol, ethanol or chloroform as a solvent. In a preferred embodiment, the graphene-polymethyl methacrylate layer grown on the copper foil is immersed in a saturated salt solution, and the copper foil is completely removed after sufficient contact, and then the graphene-polymethyl methacrylate layer is treated in acetone, isopropanol, ethanol or chloroform, and the polymethyl methacrylate layer is completely removed after 1 to 30 minutes of treatment to obtain a graphene layer. The graphene layer is transferred to deionized water, released onto the topmost polymethyl methacrylate layer by a solution transfer method, and finally annealed to obtain a stable graphene layer structure.

[0040] The method for preparing a gas sensor according to a preferred embodiment of the present invention then includes step S204, preparing interdigital electrodes on the sensitive material layer 4 by evaporation to form a source electrode 5 and a drain electrode 6. In a preferred embodiment, the device is fixed above an interdigital electrode mask baffle of the same size, and a layer of electrode is evaporated on the surface of the organic semiconductor layer by vacuum evaporation. In order to enable the device to operate at a lower driving voltage and reduce the power consumption of the device as much as possible, the interdigital electrodes need to increase the effective area and aspect ratio of the device as much as possible. Optionally, the interdigital electrodes of the embodiment of the present invention can be 13 channels, with a channel length of 4000μm, a width of 100μm, an electrode aspect ratio of 40, and a minimum operating voltage of the device below 1V.

[0041] The preparation method of a gas sensor according to a preferred embodiment of the present invention then includes step S205, performing ultraviolet ozone irradiation treatment on the gas sensor. Preferably, the ultraviolet ozone irradiation treatment includes adjusting the ultraviolet ozone irradiation time, the ultraviolet ozone irradiation treatment time is 1 to 30 minutes, and the ultraviolet lamp power is 50-300W. It should be understood that the effect is not obvious below 50W, and exceeding 300W will burn the material. In a preferred embodiment, the device is fixed under an ultraviolet lamp and irradiated in an ozone environment for 10 minutes, and the ultraviolet lamp power is 250W. By adjusting the ultraviolet ozone irradiation time, the oxidation degree of graphene and the hydroxylation of graphene and polymethyl methacrylate are optimized, and the elastic deformation capacity of the graphene-polymethyl methacrylate buffer layer is enhanced, thereby further improving the bending / bending resistance of the gas sensor and the sensitivity to benzene gases. Specifically, the bending resistance of the gas sensor can be regulated by the UV-ozone treatment time of the combined buffer layer 23. For example, oxygen-containing functional groups such as hydroxyl or carboxyl can be introduced through UV-ozone treatment, thereby increasing the mutual repulsion between layers, improving the anti-bending space and reducing friction resistance; the gas sensing performance of the gas sensor can be regulated by the UV-ozone treatment time of the sensitive material layer 4 and selecting different functional group modification schemes, thereby increasing the hydroxyl content on the surface of the graphene sensing layer and enhancing the adsorption capacity and signal conversion capacity of harmful gas molecules.

[0042] According to the gas sensor of the present invention, a flexible polymer material containing alkyl side chains such as polymethyl methacrylate and polydimethylsiloxane is added between the stacked monolayer graphene as a buffer layer, and different degrees of ultraviolet ozone treatment are performed to enhance the bending resistance of the device. The characteristics of such flexible polymer materials are that they can be processed in solution, and the polarity of the alkyl side chain and the carbon double bond structure of graphene are similar, which can improve the fit between layers and avoid phase separation. At the same time, by subjecting the graphene sensitive layer to ultraviolet ozone treatment or other functional group modification, the sensitivity of the device to organic volatile harmful gases such as benzene and aldehydes is improved. The resistive graphene sensor provided in the embodiment of the present invention optimizes the oxidation degree of the graphene buffer layer and the flexible buffer layer containing alkyl side chains by regulating the ultraviolet ozone treatment time of the device, thereby enhancing the elastic deformation resistance of the graphene-alkyl side chain polymer flexible buffer layer; by regulating the ultraviolet ozone treatment time of the device or other functional group modification schemes, the adsorption capacity of the graphene sensing layer for organic volatile harmful gases such as benzene and aldehydes is optimized, and the performance of the sensor in detecting organic volatile harmful gases such as benzene and aldehydes is regulated.

[0043] According to the gas sensor of the present invention, the source-drain voltage and gate voltage during operation are both 0.5-50V, the working environment of the device includes but is not limited to air environment, nitrogen environment, etc., and the working environment temperature of the device is 0-50°C. The device preparation process of this structure is simple, and after adding the graphene-polymethyl methacrylate buffer layer and adjusting the number of graphene-polymethyl methacrylate layers, it can offset the external force and enhance the bending resistance of the gas sensor. In addition, after ultraviolet ozone irradiation, hydroxyl groups are introduced at the contact surface of the graphene layer and the polymethyl methacrylate layer, resulting in mutual repulsion between the layers, enhancing the elastic deformation capacity of the graphene-polymethyl methacrylate buffer layer, thereby enhancing the bending resistance of the device; and the oxidation degree of the graphene layer is regulated, thereby enhancing the sensitivity of the gas sensor to benzene gases.

[0044] According to the gas sensor of the present invention, a graphene-polymethyl methacrylate buffer layer is added to protect the graphene layer, thereby enhancing the bending resistance of the gas sensor; the number of graphene-polymethyl methacrylate layers is regulated by a simple stacking method to regulate the flexibility of the gas sensor; the degree of oxidation of graphene and the hydroxylation of graphene and polymethyl methacrylate are optimized by regulating the ultraviolet ozone irradiation time of the device, thereby enhancing the elastic deformation capacity of the graphene-polymethyl methacrylate buffer layer, thereby further improving the bending resistance of the gas sensor and the sensitivity to benzene gases.

[0045] Figure 4 The following is a comparison of the response of the gas sensor to 50ppm o-dichlorobenzene before and after UV-ozone light treatment, where (a) and (b) represent the gas sensor before UV-ozone treatment and the gas sensor after UV-ozone light treatment, respectively. By comparison, it can be found that the response of the gas sensor to o-dichlorobenzene is significantly improved after light treatment.

[0046] First, a graphene-methyl methacrylate buffer layer is stacked on the clean substrate by solution transfer method, and annealed in a nitrogen environment at 60°C for 30 minutes to remove excess solvent, and then treated with ultraviolet ozone for 10 minutes. Then, a graphene-alkyl side chain polymer flexible buffer layer is stacked, and annealed and treated with ultraviolet ozone for the same time. The above steps are repeated three times to form a graphene-methyl methacrylate buffer layer with a thickness of about 6 microns. The gas sensing performance of the gas sensor can be adjusted by the ultraviolet ozone treatment time (1-10 minutes). Figure 5 The following is a comparison of the responses of the gas sensor to 50ppm o-dichlorobenzene after being treated with UV light for different times. By comparison, it can be found that the gas sensor treated with UV light for 1200 to 1500 seconds has the highest sensitivity to o-dichlorobenzene.

[0047] Figure 6 This is a comparison chart of the average response of the gas sensor to 50ppm o-dichlorobenzene before and after ultraviolet ozone light treatment. Through comparison, it can be found that the response of the gas sensor after ultraviolet ozone light treatment is improved by 508% compared with the gas sensor before ultraviolet ozone light treatment.

[0048] Figure 7 This is the Fourier transform infrared spectrum characterization result of the graphene layer before and after UV-ozone irradiation. By comparison, it can be found that the graphene treated with UV-ozone has a high concentration of 1288cm -1 The intensity of the OH characteristic peak at the position increased significantly, revealing that the number of oxygen-containing groups in graphene increased after ultraviolet ozone treatment, thereby improving the sensitivity of the gas sensor.

[0049] Figure 8 The Raman characterization results of graphene layers before and after UV-ozone irradiation. By comparison, it can be found that the peak position of graphene after UV-ozone irradiation moves toward the long-wavelength direction and is located at 2670cm -1 The 2D peaks are located at 1580 cm -1 The peak intensity ratio of the G peak decreases, indicating that graphene after ultraviolet ozone irradiation introduces defects with active sites, thereby improving the sensitivity of the gas sensor.

[0050] In summary, the gas sensor according to the present invention can enhance the elastic deformation ability and optimize the oxidation degree of the graphene layer by adding a graphene-polymethyl methacrylate buffer layer and adjusting the number of graphene-polymethyl methacrylate layers and the ultraviolet ozone irradiation time, thereby improving the bending resistance of the gas sensor and the ability to identify benzene gases.

[0051] The above is only a preferred embodiment of the present invention, and is not intended to limit the scope of the present invention. The above embodiment of the present invention can also be modified in various ways. That is, all simple, equivalent changes and modifications made according to the claims and the contents of the specification of the present invention fall within the scope of protection of the claims of the present invention. The contents not described in detail in the present invention are all conventional technical contents.

Claims

1. A method for preparing a gas sensor, characterized in that: The preparation method comprises the following steps: S201, providing a substrate; S202, preparing at least one combined buffer layer on a substrate, the combined buffer layer consisting of a simply stacked graphene buffer layer and an organic flexible insulating material buffer layer; S203, preparing a sensitive material layer on the topmost organic flexible insulating material buffer layer, wherein the sensitive material layer is a graphene sensing layer; S204, forming a source electrode and a drain electrode on the sensitive material layer; S205, performing ultraviolet ozone post-irradiation treatment, by adjusting the ultraviolet ozone irradiation time, introducing oxygen-containing functional groups at the contact surface of the graphene buffer layer and the organic flexible insulating material buffer layer to increase the mutual repulsion between the layers to improve the bending resistance of the gas sensor, and by optimizing the oxidation degree of the sensitive material layer to improve the sensitivity of the gas sensor.

2. The preparation method according to claim 1, characterized in that: 1 to 10 combined buffer layers are prepared on the substrate.

3. The preparation method according to claim 1, characterized in that: The oxygen-containing functional group is a carboxyl group.

4. A gas sensor obtained by the preparation method according to any one of claims 1 to 3, characterized in that: The gas sensor comprises a substrate, at least one combined buffer layer, a sensitive material layer, a source electrode and a drain electrode. The combined buffer layer is composed of a graphene buffer layer and an organic flexible insulating material buffer layer which are simply stacked.

5. The gas sensor according to claim 4, characterized in that: The graphene buffer layer of each combined buffer layer is a single-layer graphene structure.

6. The gas sensor according to claim 4, characterized in that: The thickness of the organic flexible insulating material buffer layer of each combined buffer layer is less than 2 microns.

7. The gas sensor according to claim 4, characterized in that: The organic flexible insulating material buffer layer is a polymethyl methacrylate buffer layer or a polydimethylsiloxane buffer layer.

8. An application of a gas sensor according to any one of claims 4 to 7, characterized in that: Gas sensors are used to detect benzene or aldehyde gases.

9. The use according to claim 8, characterized in that: The benzene gas is o-dichlorobenzene.

Citation Information

Patent Citations

  • Flexible circuit based on graphene

    CN104333975A

  • Multi-functional graphene flexible sensor having high resistance strain sensitivity coefficient and high deformation capability and preparation method thereof

    CN107655397A

  • Gas-sensitive body for organic gas sensor, organic gas sensor, and solar cell

    JP2020134498A

  • Motion detection sensor and manufacturing method of the same

    KR101753384B1

  • Flexible micro gas sensor using nanostructure array and manufacturing method for the same