Cooling process for medium and thick steel plate production
Through precise positioning and cooling area partition management, the cooling water volume and roller speed are adjusted, the problem of poor cooling uniformity in the length direction of medium and thick steel plates is solved, and the cooling uniformity and stable performance of the head and tail of the steel plate are improved.
Patent Information
- Application Number
- CN202211027841.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-08-25
AI Technical Summary
In the production of medium and thick steel plates, the difference in cooling uniformity in the length direction of the steel plate leads to uneven performance of the steel plate, especially the inconsistent cooling strength at the head and tail parts, which is difficult for the prior art to effectively solve this problem.
The cooling control equipment receives the steel plate size and water inlet temperature information, sets the water volume of the cooling header, the initial cooling roller speed and the roller acceleration, and uses the head shading and cooling roller acceleration mode to adjust the cooling water volume and roller speed to ensure the steel plate head The cooling uniformity of the tail is adopted, and the independent cooling area and water volume compensation strategy are used to accurately locate the steel plate position to avoid fluctuations caused by water volume adjustment.
The cooling uniformity of the head and tail of the steel plate and the stability of the length direction performance are achieved, the problem of excessive cooling strength of the steel plate is avoided, and the overall mechanical properties of the steel plate are ensured.
Smart Images

Figure CN115318844B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and relates to a control method for improving the cooling uniformity of a medium and thick steel plate in a length direction after rolling. Background Art
[0002] When steel mills produce medium and thick steel plates with low alloy, high strength and high toughness, they usually need to adopt controlled rolling and controlled cooling processes to ensure the comprehensive mechanical properties of the steel plates. The controlled cooling process has a decisive influence on the performance of the final steel plates. Especially when the steel plates use low carbon and low alloy components, the process control window for steel plate cooling is narrow, and the contradiction between the uniformity of steel plate performance and the controlled cooling process is more prominent.
[0003] The problem of cooling uniformity in the length direction of medium and thick plates is mainly affected by two aspects: first, the unstable water flow state at the head and tail of the steel plate will cause poor cooling intensity stability, resulting in strength differences at the head and tail of the steel plate; second, the difference in water entry time at different positions in the length direction of the steel plate causes differences in cooling effects, resulting in uneven release performance along the length of the steel plate.
[0004] In the existing steel plate cooling technology, the problem of excessive cooling intensity at the head is solved by using the head shielding method, such as tracking the head and tail positions of the steel plate and reducing the water volume adjustment valve in the quick cooling zone as a whole to reduce the head and tail cooling intensity and ensure the consistency of the steel plate's red-return temperature. When the head and tail of the steel plate pass through the cooling zone, the water volume returns to normal. The usual approach to cooling uniformity in the length direction of the steel plate is to shorten the length of the rolled steel plate and increase the conveying speed of the roller during the cooling process.
[0005] On the one hand, the adjustment of the water valve in the quick cooling zone has a certain hysteresis. In order to complete the water volume adjustment in a short time, the water valve adjustment requires extremely high sensitivity and accuracy. In the entire water adjustment process, there will be a problem of large water volume fluctuations caused by over-adjustment; on the other hand, the temperature difference at the head and tail of the steel plate caused by the water entry time difference in the length direction of the steel plate will directly affect the cooling phase change of the steel plate. Even if the red-return temperature of the head and tail of the final steel plate is consistent, it is difficult to ensure the uniform performance of the final steel plate. Summary of the invention
[0006] The purpose of the present invention is to provide a cooling control method in the production of medium and thick steel plates, so as to solve the problem in the prior art that the performance difference of the controlled cooling steel plates in the length direction is large, while avoiding the large performance difference between the head and the tail, especially the problem of excessive strength caused by excessive cooling intensity at the head of the steel plate.
[0007] The technical solution of the present invention:
[0008] The cooling process for the production of medium and thick steel plates includes the following steps:
[0009] (1) The cooling control equipment receives the process information of the cooling steel plate size, water inlet temperature, and red-return temperature;
[0010] (2) Setting the cooling manifold water volume, initial cooling roller speed, head shielding length and mode, cooling roller speed acceleration, manifold water volume increment setting after acceleration, and tail water volume compensation process parameters;
[0011] (3) The position of the cooling steel plate head is corrected, the steel plate position signal is tracked and turned on throughout the process, the head shield is turned on, and the water volume in the cooling area is adjusted to the correct position;
[0012] (4) The cooling steel plate head passes through zone A, the head shielding ends, and the cooling roller acceleration mode is turned on;
[0013] (5) After the cooling roller is accelerated, the water volume in the cooling device B, C, and D zones increases;
[0014] (6) The tail of the cooling steel plate enters the cooling area and the tail flow compensation is turned on;
[0015] (7) All cooled steel plates pass through the cooling area and controlled cooling is completed.
[0016] In the step (1), the cooling control equipment is a conveyor cooling device with a total length of 24 m, including a steel plate cooling conveying roller, a steel plate position tracking device, a steel plate inlet and outlet pyrometer, and a cooling control device for the steel plate cooling conveying area. The steel plate position tracking device includes a roller speed position encoder and a heat detection device before and after the cooling device for correcting the steel plate position. The device includes four independent cooling areas, A, B, C, and D. Each cooling area is composed of 6 groups of cooling headers in the upper and lower parts, wherein the 6 groups of headers in the upper and lower parts of the A area can be opened or closed separately, and the upper and lower headers in the B, C, and D areas are opened or closed by a unified water valve.
[0017] The process parameters in step (2) can be input into the cooling device manually or automatically, wherein the process parameter setting values of the initial cooling roller speed and the cooling roller speed acceleration are set according to the target difference in the head and tail water entry time of the steel plate, and the calculation formula is:
[0018]
[0019] In the formula, a represents the cooling roller speed acceleration, v 0 represents the initial cooling roller speed, t Indicates the time difference between the head and tail of the steel plate entering the water. l Indicates the length of the steel plate, l 0 The time difference between the head and tail of the steel plate entering the water can be determined according to the structure and performance of the CCT curve of the steel grade. The time difference between the head and tail of the steel plate of the present invention is preferably controlled within 20 to 35 seconds.
[0020] The head shielding in step (3) uses head cooling water compensation to reduce the cooling rate of the head of the steel plate in the rapid cooling section, and is characterized in that: the opening mode of the 6 groups of independent cooling headers in zone A is m+n mode, where m+n=6. Specifically, before the steel plate enters the cooling device, m groups of headers in zone A are opened for cooling, and after the steel plate head shielding area passes through zone A, the other n groups of headers in zone A are opened.
[0021] Preferably, when zone A adopts 3+3 mode, the headers that are first opened are 1, 4, and 6, or when zone A adopts 4+2 mode, the headers that are first opened are 1, 3, 4, and 6.
[0022] The cooling roller acceleration mode in step (4) is characterized in that the cooling roller acceleration is determined by the system or manually according to the steel plate specifications, and the acceleration is accumulated with the initial speed of the cooling steel plate as the current speed of the steel plate cooling roller until the tail of the steel plate leaves the water cooling area.
[0023] The maximum roller speed of the steel plate cooling, i.e., the speed from the tail of the steel plate to the outlet of the cooling equipment, is limited by the capacity of the cooling equipment. The maximum roller speed in the present invention is 2.5 m / s, which can be calculated according to formula (2). max When >2.5m / s, v0 and a must be adjusted until the calculated v max ≤2.5m / s.
[0024]
[0025] In the formula, v max Indicates the speed of the steel plate tail leaving the cooling equipment. v 0 represents the initial cooling roller speed, a represents the cooling roller speed acceleration, l Indicates the length of the steel plate, l 0 Indicates the head occlusion length, L Indicates the length of the cooling equipment.
[0026] Preferably, the speed of the steel plate tail out of the cooling equipment is preferably in the range of v max 1.5~2.2m / s.
[0027] The increase in water volume in zones B, C, and D in step (5) is to compensate for the reduction in cooling time in the middle and tail of the cooling steel plate due to roller acceleration, and is characterized in that: the water volume in the cooling zone is adjusted according to the length of the steel plate and the total cooling time of the steel plate, and the cooling water volume is increased from the time the cooling steel plate enters the acceleration mode. The water valve adjustment mode when the water volume is increased should adopt a small flow rate slow increase mode to avoid overshoot during the water volume adjustment process, which causes excessive local cooling intensity of the steel plate.
[0028] Preferably, the increase in water volume in zones B, C, and D can be calculated according to formula (3).
[0029]
[0030] In the formula, β is the compensation coefficient, the value range is 0.5-0.9; v 0 represents the initial cooling roller speed, a represents the cooling roller speed acceleration, l Indicates the length of the steel plate, l 0 Indicates the head occlusion length, L Indicates the length of the cooling equipment.
[0031] The tail flow compensation in step (6) is to compensate for the insufficient cooling intensity caused by the long air cooling time before the tail of the cooled steel plate enters the cooling device, and is characterized in that: the water volume compensation in zone A at the tail of the steel plate is determined according to the CCT curve of the steel grade, the target structure and the degree and time of cooling at the tail of the steel plate, and the water volume increment in the present invention is 10% to 20%.
[0032] The beneficial effects of the present invention are as follows: by accurately positioning each section of the steel plate in the cooling area, using head shielding at the head of the steel plate, and using a mode of pre-adjusting a fixed flow rate of a partial header to stabilize the head shielding effect, the cooling fluctuation caused by the water valve adjustment in the entire cooling zone during the cooling process is avoided; by using the roller acceleration mode in the cooling zone, the cooling water entry time of the head and tail of the steel plate is shortened, and the temperature difference between the head and tail of the steel plate is reduced; by adjusting the cooling water volume at different positions of the steel plate, the cooling intensity of the middle and tail of the steel plate is increased, and the insufficient cooling of the middle and tail of the steel plate caused by the increase in roller speed and the low water entry temperature is compensated. The present invention is suitable for the production of controlled-cooling low-alloy high-strength and high-toughness medium and thick plates, and has the advantage of uniform and stable performance for controlled-cooling medium and thick plates with a longer length. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The figure is a schematic diagram of the CCT curve of a certain type of steel and the cooling curve of the head, middle and tail of the steel plate under the existing process conditions.
[0034] Figure 2 The figure is a schematic diagram of the CCT curve of a certain type of steel and the head, middle and tail cooling curve of a steel plate using the technical solution of the present invention. DETAILED DESCRIPTION
[0035] The technical principle and specific implementation methods of the present invention are described below in comparison with the existing technology. Figure 1It is the CCT curve of a certain type of steel and the cooling curve of the head, middle and tail of the steel plate under the existing process conditions. Curve 1 represents the cooling curve of the head of the steel plate, curve 2 is the cooling curve of the middle of the steel plate, and curve 3 is the cooling curve of the tail of the steel plate. For the process with fixed water volume and fixed cooling roller speed, different cooling paths are formed in the head, middle and tail of the steel plate due to the air cooling effect before the steel plate enters the cooling equipment at different positions, which leads to the difference in the organizational properties of the steel plate at the head, middle and tail. For the process with fixed water volume and accelerated cooling roller speed, the cooling roller speed acceleration method is adopted to reduce the water temperature drop in the middle and tail of the steel plate, but it also reduces the time the steel plate stays in the cooling area, resulting in insufficient cooling in the middle and tail of the steel plate. For the existing head and tail shielding process, when the head and tail shielding areas of the steel plate enter the cooling area of area A, the water valve is activated to reduce the water volume in the shielding area. After the shielding area passes, the water valve is activated again to increase the water volume, but the shielding duration is generally short. The frequent operation of the water valve leads to poor temperature accuracy in the shielding area, and it also affects other cooling areas. The specific implementation of the existing process is shown in Example 1.
[0036] The present invention reduces the temperature difference of the steel plate entering the water by simultaneously adjusting the roller speed and the water volume in the cooling area, compensates for the insufficient cooling strength in the middle and tail of the steel plate, and improves the uniformity of the structural performance of the cooling of the head, middle and tail of the steel plate. Figure 2 The CCT curve of a certain type of steel and the cooling curve of the head, middle and tail of the steel plate using the technical solution of the present invention are shown. For the head shielding of the cooling steel plate, the A zone headers are opened in groups, and the head shielding effect is further stabilized by the mode of the pre-adjustment group and the subsequent opening group. When the head of the steel plate enters the cooling zone, the pre-adjustment group is opened and the subsequent opening group is closed to reduce the cooling intensity of the head and prevent the head of the steel plate from being overcooled and causing excessive strength. That is, the cooling curve is changed from Figure 1 Curve 1 in the figure becomes Figure 2 Curve 1' in the figure. When the head of the steel plate passes through zone A, on the one hand, the subsequent opening group of zone A is opened; on the other hand, the cooling roller is opened and accelerated, and the cooling water volume in zone BCD is increased at the same time. The increase in the water volume in zone BCD is to compensate for the shortened cooling time of the steel plate in the cooling zone caused by the acceleration of the roller. The cooling curve corresponds to Figure 2 When the tail of the steel plate is about to enter the cooling area, the water volume in zone A is increased by 10-20% to compensate for the insufficient cooling intensity of the tail of the steel plate caused by the long air cooling space before the tail enters the cooling area. That is, the cooling curve is changed from Figure 1 Curve 3 in the figure becomes Figure 2 The specific embodiment of the present invention is shown in Example 2.
[0037] The present invention will be further described below in conjunction with the embodiments.
[0038] The cooling process equipment of the present invention is a conveying cooling device with a total length of 24m, including a steel plate cooling and conveying roller, steel plate position tracking, steel plate inlet and outlet pyrometers and a cooling control device in the steel plate cooling and conveying area. The steel plate position tracking includes a roller speed position encoder and a heat detection device before and after the cooling device to correct the steel plate position; it includes four independent cooling areas A, B, C, and D, each cooling area is composed of 6 groups of cooling manifolds in the upper and lower parts, wherein the 6 groups of manifolds in the upper and lower parts of the A area can be opened or closed separately, and the upper and lower manifold groups in the B, C, and D areas are opened or closed by a unified water valve.
[0039] Example 1: The cooling process for producing medium and thick steel plates in the prior art comprises the following steps:
[0040] (1) The specifications of the controlled cooling steel plate are 18mm×3880mm×40000mm. The temperature of the steel plate before entering the water is 800℃, and the target red-return temperature is 400℃.
[0041] (2) The cooling water volume setting is shown in Table 1. The cooling roller speed is set to 1.4 m / s. Based on this, it is calculated that the time for the steel plate to completely pass through the cooling zone is about 46 s, the time difference between the head and tail entering the water is about 28 s, and the head and tail entering water temperature difference is about 20~40℃. The head shielding is set to 2m, and the head shielding mode is that the 6 groups of headers in area A are proportionally reduced by 50%.
[0042] (3) When the heat inspection at the entrance of the cooling equipment detects the head of the steel plate, the position of the head of the steel plate is corrected, and then the position signal of the cooling steel plate is tracked according to the speed position encoder of the cooling roller. Before the head of the steel plate enters the cooling equipment, the cooling water valve is opened in advance and reaches the set water volume. When the head of the steel plate enters area A, the head shielding function is activated, and the 6 groups of manifold water valves in area A are adjusted to reduce the water volume by 15% in turn according to the position tracking of the head of the steel plate, and the water valve opening is adjusted according to the water valve calibration value.
[0043] (4) Based on the head shielding length of 3m, the shielding time is calculated to be 2s, that is, the water valve returns to the original set opening after being adjusted down for 2s.
[0044] However, due to the influence of the water valve action time and response curve, the head water volume fluctuates greatly and has poor stability. After the cooling steel plate head shielding area passes through each group of headers in area A one by one, the water volume of each header in area A is adjusted back to the original setting value one by one.
[0045] (5) The cooled steel plates all pass through the cooling area at a uniform speed, and the controlled cooling is completed.
[0046] Embodiment 2: The cooling process for producing medium and thick steel plates of the present invention comprises the following steps:
[0047] (1) The specifications of the controlled cooling steel plate are 18mm×3880mm×40000mm. The temperature of the steel plate before entering the water is 800℃, and the target red-return temperature is 400℃.
[0048] (2) First, the cooling process parameters are designed. See Table 1 for setting 1. The initial cooling roller speed is set to 1.2 m / s, the head shielding length is set to 3 m, the head shielding is set to 4+2 mode (the pre-adjusted headers in zone A are 1, 3, 4, and 6), the head shielding length is set to 6 m, and the target value of the head and tail steel plate water entry time difference is set to 25 s. According to the relationship between the cooling roller speed and the cooling roller speed acceleration (1), the cooling roller speed acceleration is calculated to be 0.05 m / s 2 , calculated according to formula (2) v max =2.69m / s, the calculated maximum roller speed of the steel plate exceeds the maximum roller speed of the cooling equipment.
[0049] The cooling process parameters were redesigned, see Table 1 Setting 2, the initial cooling roller speed was set to 1.4 m / s, the head shielding length was set to 3 meters, the head shielding was set to 4+2 mode (the pre-adjusted headers in zone A were 1, 3, 4, and 6), the head shielding length was set to 6 m, the target value of the head and tail steel plate water entry time difference was set to 26 s, and the cooling roller speed acceleration was calculated according to the relationship between the cooling roller speed and the cooling roller speed acceleration (1) to be 0.015 m / s 2 , calculated according to formula (2) v max =1.92m / s, which meets the requirements. At the same time, the tail water compensation length is set to 10m.
[0050] (3) When the heat inspection at the entrance of the cooling equipment detects the head of the steel plate, the position of the head of the steel plate is corrected, and then the position signal of the cooling steel plate is tracked according to the speed position encoder of the cooling roller. Before the head of the steel plate enters the cooling equipment, the cooling water valve is opened in advance and reaches the water volume setting value (except for the 2nd and 5th group of headers in area A). Because the shielding mode of the head of the steel plate is set to 4+2 mode, the 2nd and 5th group of headers in area A are closed.
[0051] (4) According to the set head shielding length of 6m, that is, after the head of the steel plate enters the cooling zone for 6m, the water valves of the 2nd and 5th group of headers in zone A are opened to the set opening. At the same time, the cooling roller is opened and accelerated, with an acceleration of 0.018m / s 2 .
[0052] (5) After the cooling roller is opened and accelerated, the water volume in the cooling device B, C, and D zones is increased and opened. The increase in water volume is calculated according to formula (3), where the compensation coefficient is taken as β= 0.8, =12%.
[0053] (6) After the cooling steel plate enters the cooling area at a distance of 10m from the tail, the tail flow compensation is turned on in zone A, and the tail water volume increases by 12%~15%, that is, the water volume of the upper and lower headers in zone A increases from 70 / 80L / s to 80 / 90L / s.
[0054] (7) All cooled steel plates pass through the cooling area and controlled cooling is completed.
[0055] The mechanical properties of the steel plate after cooling are shown in Table 2. Compared with Example 1, the uniformity of the head, middle and tail performance of Example 2 is significantly improved.
[0056] Table 1 Cooling process settings
[0057] .
[0058] Table 2 Mechanical properties of steel plate after cooling
[0059] .
Claims
1. The cooling process for the production of medium and thick steel plates is characterized by The steps include: (1) The cooling control equipment receives the process information of the cooling steel plate size, water inlet temperature, and red-return temperature; (2) Set the cooling manifold water volume, initial cooling roller speed, head shielding length and mode, cooling roller speed acceleration, manifold water volume increment setting after acceleration, and tail water volume compensation process parameters, and input them into the cooling equipment by manual setting or automatic setting. The process parameters of initial cooling roller speed and cooling roller speed acceleration are set according to the target difference of the head and tail water entry time of the steel plate, and the relationship is: Where a is the acceleration of the cooling roller speed, v0 is the initial cooling roller speed, l is the length of the steel plate, and l0 is the head shielding length; t is the time difference between the head and tail of the steel plate entering the water, and t is determined to be 20 to 35s according to the structure and performance of the CCT curve of the steel grade; (3) The position of the cooling steel plate head is corrected, the steel plate position signal is tracked and turned on throughout the process, the head shield is turned on, and the water volume in the cooling area is adjusted to the right level; (4) When the head of the cooling steel plate passes through zone A, the head shielding ends and the cooling roller acceleration mode is turned on. The cooling roller acceleration is determined by the system or manually according to the steel plate specifications. The acceleration is accumulated with the initial speed of the cooling steel plate as the current speed of the steel plate cooling roller until the tail of the steel plate leaves the water cooling area. The maximum roller speed of the steel plate cooling, that is, the speed from the tail of the steel plate to the outlet of the cooling equipment, is calculated as follows: In the formula, v max represents the speed of the steel plate tail exiting the cooling device, v0 represents the initial cooling roller speed, a represents the cooling roller speed acceleration, l represents the steel plate length, l0 represents the head shielding length, and L represents the cooling device length; (5) After the cooling roller is accelerated and opened, the water volume in the cooling device B, C, and D zones increases. The increase in water volume in the B, C, and D zones is calculated as follows: In the formula, β is the compensation coefficient, ranging from 0.5 to 0.9; v0 represents the initial cooling roller speed, a represents the cooling roller speed acceleration, l represents the steel plate length, l0 represents the head shielding length, and L represents the cooling equipment length; (6) The tail of the cooling steel plate enters the cooling area and the tail flow compensation is turned on; (7) All the cooled steel plates pass through the cooling area and controlled cooling is completed.
2. The cooling process for producing medium and thick steel plates according to claim 1, characterized in that: The head shielding in step (3) uses head cooling water compensation to reduce the cooling rate of the head of the steel plate in the rapid cooling section. The opening mode of the 6 groups of independent cooling headers in zone A is m+n mode, where m+n=6. Before the steel plate enters the cooling device, m groups of headers in zone A are opened for cooling. After the steel plate head shielding area passes through zone A, the other n groups of headers in zone A are opened.
3. The cooling process for producing medium and thick steel plates according to claim 2, characterized in that: When zone A adopts 3+3 mode, the first headers opened are 1, 4, and 6. Or when zone A adopts 4+2 mode, the first headers opened are 1, 3, 4, and 6.
4. The cooling process for producing medium and thick steel plates according to claim 1, characterized in that: In the cooling roller acceleration mode in step (4), the speed value v of the steel plate tail exiting the cooling device is max =1.5~2.2m / s.
5. The cooling process for producing medium and thick steel plates according to claim 1, characterized in that: In step (6), the water volume compensation of zone A at the tail of the steel plate is determined according to the CCT curve of the steel grade, the target structure, and the degree and time of cooling at the tail of the steel plate, and the water volume increment is 10% to 20%.