A method for preparing a liquid-phase synthesized n-butanol gas sensor

The preparation of LaFeO3 gas sensors loaded with Au nanoparticles by one-step hydrothermal method solves the problems of poor selectivity and high working temperature of n-butanol gas sensors in the prior art, and achieves high selectivity and low detection lower limits for n-butanol. Improves sensor sensitivity and stability.

CN115326888BActive Publication Date: 2024-11-15HEBEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210915725.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-01
Publication Date
2024-11-15
Estimated Expiration
2042-08-01

AI Technical Summary

Technical Problem

The existing n-butanol gas-sensitive sensors have problems such as poor selectivity, high operating temperature, high detection limit and insufficient long-term stability.

Method used

A one-step hydrothermal method is used to prepare a LaFeO3 gas sensor loaded with trace precious metals. The citrate ions are used as complexing agent and reducing agent to generate nano Au particles and form a core-shell structure. Au nanoparticles loaded with 0 valence state are on the surface of LaFeO3 to form a Zodiac Teki junction improves the sensitivity and stability of the sensor.

Benefits of technology

It achieves high selectivity, low detection lower limit and good long-term stability for n-butanol, and has a 5-fold increase in sensitivity. It can efficiently detect n-butanol gas at a lower working temperature, with a lower limit of 500ppb.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115326888B_ABST
    Figure CN115326888B_ABST
Patent Text Reader

Abstract

The present invention is a preparation method of a liquid-phase synthesized n-butanol gas sensor. The method adopts a simple one-step hydrothermal method, using citrate ions to simultaneously play the role of a complexing agent and a reducing agent, and then by the addition of chloroauric acid, an Au source is provided to generate nano Au particles, and then the nano particles will adhere to the crystallized LaFeO3 crystal surface, inhibiting the further growth of the crystal nucleus so that LaFeO3 develops into a core-shell structure, and annealing. By controlling the parameters such as load ratio, reaction temperature, annealing temperature, stirring rate, the porous LaFeO3 surface of the core-shell structure is loaded with Au nanoparticles in a 0-valent state, forming a Schottky junction, and obtaining an Au-LaFeO3 composite material, and a gas-sensitive element is obtained after coating. The present invention overcomes the problems of poor selectivity of existing devices, high operating temperature, etc., improves the sensitivity to n-butanol, and the detection lower limit reaches 500ppb, and the long-term stability and repeatability are good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to a gas-sensitive sensor device, which is suitable for preparing an Au-LaFeO3 gas sensor with high selectivity for n-butanol at a relatively low working temperature (225°C). Background technology:

[0002] In the chemical industry, n-butanol can be used as a raw material for organic synthesis, used to make n-butyl ester plasticizers of phthalic acid, aliphatic dibasic acids and phosphoric acid, which are widely used in various plastics and rubber products, and are also raw materials for making butyraldehyde, butyric acid, butylamine and butyl lactate. As an additive for alkyd resin coatings, it is used to produce melamine resins, acrylic acid, epoxy varnishes, etc. It is widely used in the production of urea-formaldehyde resins, cellulose resins, alkyd resins and coatings. It can also be used as a commonly used inactive diluent in adhesives, used to make esters, plastic plasticizers, spray paints, etc. It is a good solvent system for esterification reactions. As a solvent in nail polish, paint, coatings, and pigments, it helps dissolve colorants and adjusts the evaporation rate and viscosity of the solvent. It can also be used as a solvent and dewaxing agent for organic dyes and printing inks, and as a defoaming agent for ink preparation in silk screen printing.

[0003] In the laboratory, it is used to prepare solvents such as slow-drying water, beakers, test tubes, washing of nanopowders, extraction of some organic matter, etc. In addition, n-butanol has a special pungent odor and is easy to volatilize. Trace amounts of n-butanol have been used to detect olfactory thresholds to evaluate the recovery of olfaction.

[0004] However, exposure to high concentrations of n-butanol may cause adverse reactions such as headaches, dizziness, and drowsiness, and direct contact with n-butanol may cause dermatitis. The vapor emitted by a large amount of n-butanol is harmful to the respiratory and nervous systems. According to the latest requirements of the National Occupational Health Standard of the People's Republic of China GBZ 2.1-2019, the exposure limit of n-butanol is not more than 100 mg / m 3 , that is, the volume fraction should be below 123ppm. Therefore, in chemical synthesis, large-scale dye printing or as a standard gas for olfactory testing, in order to prevent the harm of n-butanol gas in the air to the human body, it is very important to monitor the gas concentration of n-butanol in real time.

[0005] However, the n-butanol sensors currently developed have disadvantages such as poor selectivity, high operating temperature, and high detection limit, while metal oxide semiconductor (MOS) gas sensors have attracted much attention in the sensor field due to their high sensitivity, fast response, simple structure, low price, simple operation, and small detection device. Among them, LaFeO3 has excellent photoelectric properties, fast charge transfer rate, simple preparation process, low cost, and environmental friendliness. The Au-LaFeO3-based sensor prepared has a simple synthesis method, fast response recovery, good stability, excellent long-term stability, and a low operating temperature, which brings convenience to its application in actual production. Summary of the invention:

[0006] The present invention aims at the shortcomings of the current n-butanol gas sensor, such as high operating temperature, poor selectivity, and long-term stability, and proposes a preparation method of a LaFeO3 n-butanol gas sensor loaded with trace precious metals. The method adopts a simple one-step hydrothermal method, uses citrate ions to simultaneously play the role of a complexing agent and a reducing agent, and then provides an Au source by adding chloroauric acid to generate nano Au particles, and then the nano particles will adhere to the surface of the crystallized LaFeO3 crystal, inhibit the further growth of the crystal nucleus, so that LaFeO3 develops into a core-shell structure, and annealing. By controlling the parameters such as the load ratio, reaction temperature, annealing temperature, stirring rate, etc., the surface of the porous LaFeO3 of the core-shell structure is loaded with Au nanoparticles in the 0-valent state to form a Schottky junction, and obtain an Au-LaFeO3 composite material, and a gas-sensitive element is obtained after coating. The element overcomes the problems of poor selectivity and high operating temperature of the existing device, improves the sensitivity to n-butanol, and the detection lower limit reaches 500ppb, and has good long-term stability and repeatability. The material powder obtained by the present invention has the characteristics of simple preparation, large specific surface area, multiple active sites, etc. The prepared sensor has the advantages of excellent selectivity for n-butanol, good repeatability and long-term stability, low detection limit, high sensitivity, etc.

[0007] The technical solution of the present invention is:

[0008] A method for preparing a liquid phase synthesized n-butanol gas sensor, the method comprising the following steps:

[0009] (1) adding lanthanum nitrate and ferric nitrate to deionized water, and magnetically stirring for 1-5 minutes to obtain a mixed solution;

[0010] The molar ratio is lanthanum nitrate: iron nitrate = 1:1; the concentration of lanthanum nitrate in the mixed solution is 0.015-0.018 mol / L; the stirring rate is 800-1000 rpm;

[0011] (2) under magnetic stirring, citric acid and hexamethylenetetramine are added to the mixed solution; after stirring for 0.5-1 hour, HAuCl4 solution is added dropwise to the transparent light yellow solution, and stirring is continued for 0.5-1 hour to obtain a precursor;

[0012] Wherein, 0.45-0.55mmol of citric acid and 0.17-0.19g of hexamethylenetetramine are added to every 30-40mL of the mixed solution; 0.0006-0.001mol of HAuCl4 is added dropwise to every liter of the mixed solution; the molar ratio is lanthanum nitrate: citric acid = 1:1; the stirring rate is 800-1000rpm;

[0013] The concentration of the HAuCl4 solution used for dropwise addition was 0.015-0.025 g / mL.

[0014] (3) transferring the precursor to a stainless steel autoclave lined with Teflon, keeping it at 170-190° C. for 22-26 hours after sealing, then taking it out and cooling it naturally to room temperature;

[0015] (4) collecting the brown precipitate by centrifugation, washing it with deionized water and ethanol alternately for 6-8 times, and drying the obtained powder at 70-80° C. for 10-12 h;

[0016] (5) collecting the dried powder and placing it in a ceramic boat, placing it in a muffle furnace, heating it to 750-850° C. in an air atmosphere, annealing it for 2-2.5 hours, and then naturally cooling it to room temperature to obtain a powder;

[0017] (6) The powder obtained above is mixed with deionized water to form a paste, and the paste is evenly coated on the surface of the ceramic tube; wherein the coating thickness is 10-20 μm and the solid-liquid ratio is 0.08-0.12 g / ml.

[0018] (7) The ceramic tube coated with the powder is placed in a muffle furnace, annealed at 440-460° C. for 2-2.5 hours at a heating rate of 1-3° C. / min, and then naturally cooled to room temperature. The annealed ceramic tube is welded to a base to make a gas sensor.

[0019] The heating rate in steps (5) and (7) is 1-3°C / min.

[0020] The essential features of the present invention are:

[0021] Existing noble metal-loaded gas-sensitive materials require the addition of additional reducing agents such as sodium borohydride and sodium citrate. These additional reagents may cause more pollution, increase the washing steps, and introduce impurity ions (such as sodium ions). The present invention utilizes the reducing property of citrate ions in the liquid phase, so that most of the Au in the liquid phase reaction is reduced to chlorauric acid. 3+has been reduced; at the same time, by utilizing the high temperature annealing required for LaFeO3, while generating LaFeO3, a small portion of chloroauric acid that may still exist is decomposed to form Au in a single substance state, further ensuring the existence of Au in a single substance form.

[0022] High temperature annealing, ① makes the hydroxide ligand generated after the hydrothermal reaction decompose and crystallize into LaFeO3 ② makes the organic template hexamethylenetetramine added in the solution decompose and volatilize, and the position originally occupied by it becomes the porous core-shell structure of the product ③ ensures that the residual chloroauric acid decomposes and finally leaves Au element.

[0023] Generate nano-Au particles, increasing the gas-sensitive response to 5 times that of pure LaFeO3 materials; the generated nano-particles will adhere to the surface of the crystallized LaFeO3 crystals, inhibiting the further growth of the crystal nucleus so that LaFeO3 develops into a core-shell structure instead of a simply grown porous sphere;

[0024] The present invention adopts a liquid phase synthesis method to prepare an Au-LaFeO3-based sensor. The prepared LaFeO3 powder loaded with zero-valent Au nanoparticles is a nanopowder with a core-shell structure. The material surface is rough, the specific surface area is large, the grain size is about 800-900nm, and the thermal stability is good, which can greatly improve the selectivity of the gas sensor. After annealing, the LaFeO3 powder obtains a porous ball with a core-shell structure, the specific surface area is unchanged, the shell layer formed on the surface has more active contact sites with oxygen molecules, the response value is higher, the selectivity is also better, and a Schottky junction is formed between the nanoparticles of Au atoms existing in a single substance and the LaFeO3, so that the sensitivity of the sensor is improved and the stability is better.

[0025] Compared with the prior art, the present invention has the following advantages:

[0026] (1) A core-shell structured LaFeO3 nanomaterial loaded with Au nanoparticles was prepared by a one-step hydrothermal method. The preparation method is simple and the obtained gas-sensitive material has more active sites, good selectivity, stable long-term performance, and excellent repeatability.

[0027] (2) Au nanoparticles are loaded on the surface of LaFeO3 material, and the valence state is controlled to be a single substance. The Schottky junction formed between the noble metal and LaFeO3 significantly improves its gas sensing performance.

[0028] (3) The present invention prepares Au-LaFeO3 material by hydrothermal method, and completes the loading of zero-valent Au nanoparticles for the first time by one-step hydrothermal method, requiring only a single annealing and without the need for a reducing atmosphere. When detecting n-butanol vapor, the gas sensor prepared with this material can show a higher sensitivity (110-120, concentration is 100 ppm n-butanol vapor) at a lower operating temperature (220-250°C). In the best case, the core-shell structure LaFeO3 loaded with Au (Example 1) has a sensitivity that is 5 times (115 / 20) higher than that of the unloaded LaFeO3 (Example 5), such as Figure 5 The detection limit reaches 500 ppb (the response is 1.2 at this time), which can realize the detection of trace n-butanol concentration. In the concentration gradient test, the response of the sensor prepared in Example 1 to n-butanol shows a positive correlation trend with the gas concentration, such as Figure 6 In addition, for Example 1, the response to n-butanol is the highest among all gases at an operating temperature of 225-275°C, such as Figure 3 . Description of the drawings:

[0029] Figure 1 Shown is a structural diagram of the sensor in the present invention;

[0030] Among them, 1-resistance wire, 2-metal electrode, 3-sensitive material, 4-ceramic tube, 5-platinum wire, 6-base;

[0031] Figure 2 Shown is a scanning electron microscope photograph of Au-LaFeO3 obtained in Example 1;

[0032] Figure 3 The figure shows the corresponding relationship between the sensitivity of the gas sensor obtained in Example 1 and different working temperatures and different gases;

[0033] Figure 4 The figure shows the single response curve of the Au-LaFeO3 gas sensor obtained in Example 1 to 100 ppm n-butanol.

[0034] Figure 5 Shown is the sensitivity of Examples 1, 2, 3, and 5 to 100 ppm n-butanol at the optimal operating temperature.

[0035] Figure 6 The figure shows the sensitivity response curve of the sensor prepared in Example 1 to n-butanol at concentrations ranging from 500 ppb to 100 ppm. Figure 6 (a) is the sensitivity response curve of the prepared sensor to 500ppb~10ppm concentration of n-butanol. Figure 6 (b) is the sensitivity response curve of the prepared sensor to n-butanol with a concentration of 20ppm to 100ppm. Specific implementation method:

[0036] Au-LaFeO3 gas-sensitive material was prepared by hydrothermal method by selecting appropriate process parameters (such as load ratio, hydrothermal temperature, hydrothermal time, annealing temperature, stirring speed, etc.), and Au-LaFeO3 film was coated on the surface of Al2O3 ceramic tube. Ni-Cr heating wire was inserted into Al2O3 ceramic tube, and the current passing through the heating wire was adjusted to heat Al2O3 ceramic tube. The electrodes led out from the heating wire and the platinum wire on the Au-LaFeO3 film were connected to the lead-out loop and the test circuit respectively. The resistance changed with the change of the test gas concentration in the environment, so as to determine whether the test gas existed. The components showed high selectivity, high sensitivity and short response-recovery time for n-butanol.

[0037] The gas-sensing characteristics of gas sensors are usually characterized by sensitivity. For p-type semiconductor gas-sensitive materials, the sensitivity is defined as the resistance value R of the sensor in a certain concentration of the measured gas atmosphere. g The resistance value R of the sensor in the atmosphere s Ratio:

[0038] S=R g / R s

[0039] Sensitivity test method: By adjusting the working voltage to heat the resistance wire in the sensor, the heat is indirectly transferred to the surface of the Al2O3 ceramic tube. z Phase in series, with the test voltage V supplied to both ends c The voltage across R is taken as the output voltage V out . Resistance of the sensor: R z =V c / V out (1-R). In atmospheric atmosphere R z =R s , under the test gas atmosphere, R z =R g According to R z The changes in the test gas in the environment can be used to understand the changes in the test gas in the environment.

[0040] The test conditions are: temperature 25±2°C, relative humidity RH 40±5%. The test gas is the volatile gas corresponding to the volatile organic compounds (n-butanol, ethanol, acetone, toluene, formaldehyde, methanol) in the gas-sensitive test system.

[0041] The invention prepares a gas sensor sensitive to n-butanol, which can detect the vapor of n-butanol in a variety of mixed gases by adjusting the working temperature. The process is simple and has excellent properties such as low working temperature, high sensitivity and high selectivity.

[0042] Embodiment 1:

[0043] (1) The experimental equipment was repeatedly cleaned with deionized water and dried in an oven. A certain amount of lanthanum nitrate and a certain amount of iron nitrate were respectively dissolved in 30 mL of deionized water at a constant temperature of 20°C, and stirred evenly. The concentrations of lanthanum nitrate and iron nitrate were both 0.0167 mol / L. The mixture was magnetically stirred for 1 minute. The stirring rate was 1000 rpm.

[0044] (2) Under magnetic stirring, add citric acid in the same amount as lanthanum nitrate to the solution, and add 0.18 g of hexamethylenetetramine (i.e., the concentration of hexamethylenetetramine in the mixed solution is 0.043 mol / L). The resulting mixed solution is magnetically stirred at room temperature for 0.5 hour, and 0.020 g / mL of chloroauric acid solution is added dropwise to the mixed solution until the concentration of chloroauric acid in the mixed solution is 0.0008 mol / L, and stirring is continued for 0.5 hour. The stirring rate is 1000 rpm.

[0045] (3) The mixed solution precursor was transferred into a 50 mL Teflon-lined stainless steel autoclave, sealed, and placed in an oven at 180 °C for 24 h, then taken out and naturally cooled to room temperature.

[0046] (4) The brown material precipitate was collected by centrifugation, and then washed with deionized water and ethanol alternately by centrifugation for 6 times. The material was placed in an oven and dried at 80°C for 12 hours.

[0047] (5) The collected material powder is placed in a ceramic boat and annealed in a muffle furnace. The heating rate is 2°C / min, the annealing temperature is 800°C, and the annealing time is 2 hours. It is naturally cooled to room temperature to obtain a powder.

[0048] (6) The powder obtained above and the deionized water sample are mixed into a paste with a solid-liquid ratio of 1 g:10 ml, and evenly coated on the surface of the ceramic tube with a coating thickness of 15 μm.

[0049] (7) The evenly coated ceramic tube is placed in a muffle furnace for annealing at a heating rate of 2°C / min, an annealing temperature of 450°C, and an annealing time of 2 hours. The annealed ceramic tube is then welded to a dedicated base. The structure of the sensor is shown in FIG1 (here, the commercially available Al2O3 ceramic tube is coated with the prepared material).

[0050] (8) The sensor was aged for 48 hours at a relative humidity of 40% RH and a temperature of 25°C using a gas sensor aging station. The gas sensing properties of the gas sensor were tested using a gas sensing test system (WS-30B). The SEM image of the prepared Au-LaFeO3 material is shown in Figure 2. Figure 2 As shown in the figure, it can be observed that the morphology is a core-shell structure, and the surface of the material is relatively rough. The organic template linker in the crystal is decomposed by high temperature to form porous spheres inside. The addition of chloroauric acid affects the further crystallization process of the LaFeO3 crystal, and a loose shell layer appears on the surface, forming a core-shell structure.

[0051] The test results are as follows Figure 3 As shown in the figure, it can be seen that the element has the highest sensitivity when the working temperature is 225°C, and the sensitivity to 100ppm of n-butanol, ethanol, acetone, toluene, formaldehyde and methanol are respectively: S=115, 37.6, 35.5, 47, 4.52 and 5.21. This shows that the gas sensor of the present invention has a strong selectivity for n-butanol and can eliminate the interference of other common organic vapors in the measurement atmosphere.

[0052] Embodiment 2:

[0053] (1) The experimental equipment was repeatedly washed with deionized water and dried in an oven. At a constant temperature of 20°C, a certain amount of lanthanum nitrate and a certain amount of iron nitrate were dissolved in 30 mL of deionized water respectively, and stirred evenly, wherein the concentrations of lanthanum nitrate and iron nitrate were both 0.0167 mol / L, and magnetic stirring was performed for 1 minute. The stirring rate was 1000 rpm.

[0054] (2) Under magnetic stirring, add citric acid in the same amount as lanthanum nitrate to the solution, and add 0.18 g of hexamethylenetetramine (i.e., the concentration of hexamethylenetetramine in the mixed solution is 0.043 mol / L). The resulting mixed solution is magnetically stirred at room temperature for 0.5 hour. Add chloroauric acid solution dropwise to the mixed solution until the concentration of chloroauric acid in the solution is 0.001 mol / L, and continue stirring for 0.5 hour, wherein the stirring rate is 1000 rpm.

[0055] (3) The mixed solution was transferred into a 50 mL Teflon-lined stainless steel autoclave, sealed, and placed in an oven at 180 °C for 24 h, then taken out and naturally cooled to room temperature.

[0056] (4) The brown material precipitate was collected by centrifugation, and then washed alternately with deionized water and ethanol for 6 times, and the material was placed in an oven at 80°C for 12 hours.

[0057] (5) The collected material powder is placed in a ceramic boat and annealed in a muffle furnace. The heating rate is 2°C / min, the annealing temperature is 800°C, the annealing time is 2 hours, and then naturally cooled to room temperature to obtain a powder.

[0058] (6) The powder obtained above and the deionized water sample are mixed into a paste with a solid-liquid ratio of 1 g:10 ml, and evenly coated on the surface of the ceramic tube with a coating thickness of 15 μm.

[0059] (7) The evenly coated ceramic tube is placed in a muffle furnace for annealing at a heating rate of 2°C / min, an annealing temperature of 450°C, and an annealing time of 2 hours. The annealed ceramic tube is then welded to a dedicated base to form a gas sensor. The sensor is aged at a relative humidity of 40% RH and a temperature of 25°C for 48 hours on a gas sensor aging station.

[0060] (8) The gas-sensing characteristics of the gas sensor were tested using a gas-sensing test system (WS-30B). The prepared sensor was tested for n-butanol gas-sensing characteristics at 200°C. The device working time was 1200 seconds, of which the response time was 50 seconds and the recovery time was 30 seconds. It can be seen that the device response characteristics and recovery performance are good. The device sensitivity S reached 58.9, which is relatively high.

[0061] Embodiment 3:

[0062] (1) The experimental equipment was repeatedly cleaned with deionized water and dried in an oven. A certain amount of lanthanum nitrate and a certain amount of iron nitrate were respectively dissolved in 30 mL of deionized water at a constant temperature of 20°C, and stirred evenly. The concentrations of lanthanum nitrate and iron nitrate were both 0.0167 mol / L. The mixture was magnetically stirred for 1 minute. The stirring rate was 1000 rpm.

[0063] (2) Under magnetic stirring, add citric acid in the same amount as lanthanum nitrate to the solution, and add 0.18 g of hexamethylenetetramine (i.e., the concentration of hexamethylenetetramine in the mixed solution is 0.043 mol / L). The resulting mixed solution is magnetically stirred at room temperature for 1 hour, and chloroauric acid solution is added dropwise to the mixed solution until the concentration of chloroauric acid in the solution is 0.0006 mol / L, and stirring is continued for 1 hour. The stirring rate is 1000 rpm.

[0064] (3) The mixed solution precursor was transferred into a 50 mL Teflon-lined stainless steel autoclave, sealed, and placed in an oven at 180 °C for 26 h, then taken out and naturally cooled to room temperature.

[0065] (4) The brown material precipitate was collected by centrifugation, and then washed 8 times by alternating centrifugation with deionized water and ethanol. The material was placed in an oven and dried at 80°C for 12 hours.

[0066] (5) The collected material powder is placed in a ceramic boat and annealed in a muffle furnace. The heating rate is 2°C / min, the annealing temperature is 800°C, the annealing time is 2 hours, and then naturally cooled to room temperature to obtain a powder.

[0067] (6) The powder obtained above is mixed with deionized water to form a paste with a solid-liquid ratio of 1 g:10 ml, and evenly coated on the surface of the ceramic tube with a coating thickness of 15 μm.

[0068] (7) The evenly coated ceramic tube is placed in a muffle furnace for annealing at a heating rate of 2°C / min, an annealing temperature of 450°C, and an annealing time of 2 hours. The annealed ceramic tube is then welded to a dedicated base to make a gas sensor. The sensor is aged at a relative humidity of 40% RH and a temperature of 25°C for 48 hours on a gas sensor aging station.

[0069] (8) The gas-sensing characteristics of the gas sensor were tested using a gas-sensing test system (WS-30B). The prepared sensor was tested for its n-butanol gas-sensing characteristics at 200°C. The device working time was 1100 seconds, of which the response time was 20 seconds and the recovery time was 45 seconds. It can be seen that the device response characteristics and recovery performance were good. The device sensitivity S reached 34, which is a relatively high sensitivity value. At this time, the responses of other gases were ethanol 15.61, acetone 11.09, toluene 17.62, formaldehyde 1.76, and methanol 5.578, and the selectivity was also good.

[0070] Embodiment 4:

[0071] (1) The experimental equipment was repeatedly washed with deionized water and dried in an oven. At a constant temperature of 20°C, a certain amount of lanthanum nitrate and a certain amount of iron nitrate were dissolved in 30 mL of deionized water respectively, and stirred evenly, wherein the concentrations of lanthanum nitrate and iron nitrate were both 0.0167 mol / L, and magnetic stirring was performed for 1 minute. The stirring rate was 1000 rpm.

[0072] (2) Under magnetic stirring, add citric acid in the same amount as lanthanum nitrate to the solution, and add 0.18 g of hexamethylenetetramine (i.e., the concentration of hexamethylenetetramine in the mixed solution is 0.043 mol / L). The resulting mixed solution is magnetically stirred at room temperature for 0.5 hour, and chloroauric acid solution is added dropwise to the mixed solution until the concentration of chloroauric acid in the solution is 0.0008 mol / L, and stirring is continued for 0.5 hour. The stirring rate is 1000 rpm.

[0073] (3) The mixed solution precursor was transferred into a 50 mL Teflon-lined stainless steel autoclave, sealed, and placed in an oven at 180 °C for 24 h, then taken out and naturally cooled to room temperature.

[0074] (4) The brown material precipitate was collected by centrifugation, and then washed with deionized water and ethanol alternately by centrifugation for 6 times. The material was placed in an oven and dried at 80°C for 12 hours.

[0075] (5) The collected material powder is placed in a ceramic boat and annealed in a muffle furnace. The heating rate is 2°C / min, the annealing temperature is 800°C, the annealing time is 2 hours, and then naturally cooled to room temperature to obtain a powder.

[0076] (6) The powder obtained above is mixed with deionized water to form a paste with a solid-liquid ratio of 1 g:10 ml, and evenly coated on the surface of the ceramic tube with a coating thickness of 15 μm.

[0077] (7) The evenly coated ceramic tube is placed in a muffle furnace for annealing at a heating rate of 2°C / min, an annealing temperature of 450°C, and an annealing time of 2 hours. The annealed ceramic tube is then welded to a dedicated base to make a gas sensor. The sensor is aged at a relative humidity of 40% RH and a temperature of 25°C for 48 hours on a gas sensor aging station.

[0078] (8) The gas-sensing characteristics of the gas sensor were tested using a gas-sensing test system (WS-30B). The prepared sensor was tested for its n-butanol gas-sensing characteristics at 250°C. The device working time was 1200 seconds, of which the response time was 46 seconds and the recovery time was 35 seconds. It can be seen that the device response characteristics and recovery performance were good. The device sensitivity S reached 42, which is a relatively high sensitivity value. At this time, the responses of other gases were ethanol 10.11, acetone 13.927, toluene 21.968, formaldehyde 4.761, and methanol 23.18, and the selectivity was relatively good.

[0079] Example 5: (Comparative Example)

[0080] (1) The experimental equipment was repeatedly cleaned with deionized water and dried in an oven. A certain amount of lanthanum nitrate and a certain amount of iron nitrate were respectively dissolved in 30 mL of deionized water at a constant temperature of 20°C, and stirred evenly. The concentrations of lanthanum nitrate and iron nitrate were both 0.0167 mol / L. The mixture was magnetically stirred for 1 minute. The stirring rate was 1000 rpm.

[0081] (2) Under magnetic stirring, add citric acid in the same amount as lanthanum nitrate to the solution, and add 0.18 g of hexamethylenetetramine (i.e., the concentration of hexamethylenetetramine in the mixed solution is 0.043 mol / L). The resulting mixed solution is magnetically stirred at room temperature for 0.5 hour. The stirring rate is 1000 rpm.

[0082] (3) The mixed solution precursor was transferred into a 50 mL Teflon-lined stainless steel autoclave, sealed, and placed in an oven at 180 °C for 24 h, then taken out and naturally cooled to room temperature.

[0083] (4) The brown material precipitate was collected by centrifugation, and then washed with deionized water and ethanol alternately by centrifugation for 6 times. The material was placed in an oven and dried at 80°C for 12 hours.

[0084] (5) The collected material powder is placed in a ceramic boat and annealed in a muffle furnace. The heating rate is 2°C / min, the annealing temperature is 800°C, and the annealing time is 2 hours. It is naturally cooled to room temperature to obtain a powder.

[0085] (6) The powder obtained above and the deionized water sample are mixed into a paste with a solid-liquid ratio of 1 g:10 ml, and evenly coated on the surface of the ceramic tube with a coating thickness of 15 μm.

[0086] (7) The evenly coated ceramic tube is placed in a muffle furnace for annealing at a heating rate of 2°C / min, an annealing temperature of 450°C, and an annealing time of 2 hours. The annealed ceramic tube is then welded to a dedicated base. The structure of the sensor is shown in FIG1 (here, the commercially available Al2O3 ceramic tube is coated with the prepared material).

[0087] (8) The sensor was aged at a relative humidity of 40% RH and a temperature of 25°C for 48 hours using a gas sensor aging station. The gas sensing properties of the gas sensor were tested using a gas sensing test system (WS-30B). The sensitivity and selectivity of the prepared LaFeO3 material without Au loading were as follows: Figure 5 As shown, compared with Example 1, the sensitivity is very low and the selectivity is poor.

[0088] The above embodiments illustrate that the gas sensors prepared in embodiments 1-4 within the scope of the claims all have good response characteristics to n-butanol gas and relatively high sensitivity. Among them, embodiment 1 has the highest sensitivity, reaching 115. And embodiment 5 (comparative example) illustrates that when too high a concentration of chloroauric acid (0.002 mol / L) is added and the stirring rate is 400 rpm, chloroauric acid cannot be evenly distributed in the precursor solution, and the resulting Au particles will be locally agglomerated rather than evenly diffused; when the hydrothermal time is short, the crystal development is poor, which is not enough to allow the metal cations to form a uniform morphology. The negative side proves that the present invention has the characteristics of uniform distribution of Au particles, high response, uniform and good crystal development.

[0089] The above embodiments are for illustration only and are not intended to be limiting. Any equivalent modifications or changes made thereto without departing from the spirit and scope of the present invention shall be included in the scope of the claims of this application.

[0090] Matters not covered by the present invention are known technologies.

Claims

1. A method for preparing a liquid phase synthesized n-butanol gas sensor, characterized in that the method comprises the following steps: (1) adding lanthanum nitrate and ferric nitrate to deionized water, and stirring magnetically for 1-5 minutes to obtain a mixed solution; in, The molar ratio is lanthanum nitrate: ferric nitrate = 1:1; in the mixed solution, the concentration of lanthanum nitrate is 0.015-0.018 mol / L; (2) under magnetic stirring, citric acid and hexamethylenetetramine are added to the mixed solution; after stirring for 0.5-1 hour, HAuCl4 solution is added dropwise to the transparent light yellow solution, and stirring is continued for 0.5-1 hour to obtain a precursor; Wherein, 0.45-0.55mmol of citric acid and 0.17-0.19g of hexamethylenetetramine are added to every 30-40mL of the mixed solution; 0.0006-0.001mol of HAuCl4 is added dropwise to every liter of the mixed solution; the stirring rate is 800-1000rpm; the molar ratio is lanthanum nitrate: citric acid = 1:1; (3) transferring the precursor to a stainless steel autoclave lined with Teflon, keeping it at 170-190° C. for 22-26 hours after sealing, then taking it out and cooling it naturally to room temperature; (4) collecting the brown precipitate by centrifugation, washing it alternately with deionized water and ethanol, and drying the resulting powder at 70-80° C. for 10-12 h; (5) collecting the dried powder and placing it in a muffle furnace, heating it to 750-850° C. in an air atmosphere at a heating rate of 1-3° C. / min, annealing it for 2-2.5 hours, and then naturally cooling it to room temperature to obtain a powder; (6) The powder obtained above is prepared into a paste with deionized water and evenly coated on the surface of the ceramic tube; wherein the coating thickness is 10-20 μm and the solid-liquid ratio is 0.08-0.12 g / ml; (7) The ceramic tube coated with the powder is placed in a muffle furnace, annealed at 440-460° C. for 2-2.5 hours at a heating rate of 1-3° C. / min, and then naturally cooled to room temperature. The annealed ceramic tube is welded to a base to make a gas sensor.

2. The method for preparing a liquid phase synthesized n-butanol gas sensor as claimed in claim 1, characterized in that The heating rate in steps (5) and (7) is 1-3°C / min.

3. The method for preparing the liquid phase synthesized n-butanol gas sensor according to claim 1, characterized in that The stirring rate in steps (1) and (2) is 800-1000 rpm.

4. The method for preparing a liquid phase synthesized n-butanol gas sensor as claimed in claim 1, characterized in that The concentration of the HAuCl4 solution added dropwise in step (2) is 0.015-0.025 g / mL.