A Li2SO4 coated and Al-doped composite layered positive electrode material and its application
Through Li2SO4 coated and Al doped composite layered positive electrode material, the problem of poor stability of layered oxide positive electrode material under high pressure conditions is solved, high specific capacity and cycle stability is achieved, the preparation process is simplified, and it is suitable for large-scale production. .
Patent Information
- Application Number
- CN202210847848.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-07-19
AI Technical Summary
The existing layered oxide cathode materials have poor stability under high pressure conditions, and the existing doping coating modification methods are complex and not suitable for large-scale production, resulting in limited commercial applications.
Using Li2SO4 coated and Al doped composite layered cathode material, mixed precursor powder, lithium source and aluminum source in anhydrous ethanol, followed by decomposition of sulfate at high temperature to produce sulfur trioxide gas coated and doped , a uniform Li2SO4 coating and Al doping are formed, simplifying the preparation process and improving the morphological uniformity of the material.
It significantly improves the specific capacity and cycle stability under high charging cutoff voltage, reduces side reactions, is suitable for large-scale production, has good morphology and is cheap.
Smart Images

Figure CN115332497B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a composite layered cathode material coated with Li2SO4 and doped with Al and its application, belonging to the technical field of lithium-ion batteries. Background Art
[0002] With the gradual development of mankind, energy and environment have become two key issues that people are concerned about, as they are closely related to people's lives. Energy is related to all aspects of people's production and life, and the environment is even more crucial for human survival. Therefore, when studying and developing energy systems, we must necessarily consider environmental issues, and only by taking both into account can we meet the strategic requirements of global sustainable development. Lithium-ion batteries that are green, sustainable, and have excellent electrochemical performance have developed rapidly in recent decades and have gradually occupied the energy storage market. However, with the development of energy storage devices, the energy density and other properties of these commercial lithium-ion batteries can no longer meet people's needs. A high cut-off voltage can bring a higher specific energy and better meet people's needs. Therefore, researchers are committed to developing cathode materials that can exhibit excellent electrochemical performance under high-voltage conditions. Layered oxide cathode materials such as Li(Ni x A y M 1-x-y )O2) (where A is a transition metal Co or Fe, M is one or more of Mn, Al, and W, 0 < x < 1, 0 ≤ y < 1, 0 ≤ 1 - x - y < 1) are considered to be one of the most promising high-voltage cathode materials.
[0003] Under high-voltage conditions, layered oxide cathode materials can provide a higher specific energy to meet people's needs. However, under high-voltage conditions, due to the extraction of more lithium ions from the layered cathode materials, the material structure is damaged to a greater extent and at a faster rate, and the stability of the material is worse. This problem has attracted the attention of many scientific researchers and a large number of studies have been carried out. However, the solutions to solve the problem are relatively complex and not suitable for large-scale production, which also greatly limits the commercial application of high-voltage layered oxide cathode materials.
[0004] Doping and coating are common modification methods for layered oxide cathode materials. At present, it has been found that doping and coating the materials simultaneously can better improve the performance of layered cathode materials under high-voltage conditions. Among them, Al element doping can effectively inhibit cation mixing and prevent structural phase transformation caused by complete de-lithiation, thus well improving the electrochemical performance of layered materials. Lithium sulfate, as a lithium-ion conductor, coated on the surface of layered materials can not only isolate the electrode material from the electrolyte, play a role in reducing side reactions and protecting the layered cathode material, but also increase the conductivity and improve the lithium-ion transport efficiency. However, at present, most of the modification methods of doping and coating simultaneously are complex, difficult to commercialize, and the obtained materials have poor morphological uniformity and poor high-voltage stability. Summary of the invention
[0005] In view of this, an object of the present invention is to provide a Li2SO4 coated and Al-doped composite layered positive electrode material and its application.
[0006] To achieve the above object, the technical solution of the present invention is as follows:
[0007] A Li2SO4-coated and Al-doped composite layered positive electrode material is prepared by the following method, wherein the steps are as follows:
[0008] (1) grinding and mixing layered cathode material precursor powder, lithium source and aluminum source in anhydrous ethanol to obtain a mixed powder;
[0009] (2) placing the mixed powder into crucible I, placing sulfate into crucible II, placing the two crucibles into a tube furnace or a muffle furnace, first heating to 480° C. to 520° C. for pre-calcination for 4 h to 6 h in an air or oxygen atmosphere, then heating to 600° C. to 900° C. for calcination for 10 h to 12 h, and cooling after calcination to obtain a Li2SO4-coated and Al-doped composite layered positive electrode material in crucible I;
[0010] Among them, the molar ratio of the layered positive electrode material precursor powder to the lithium source is 1:1.05~1.2, the amount of the aluminum source is 0.5%~10% of the amount of the layered positive electrode material precursor powder, and more preferably 1%~3%; when it is a tubular furnace; the amount of sulfate ion in the sulfate is 20%~50% of the amount of the layered positive electrode material precursor powder, when it is a muffle furnace, the amount of sulfate ion in the sulfate is 5~20% of the amount of the layered positive electrode material precursor powder.
[0011] The sulfate is a sulfate that decomposes at 520-900° C. to produce sulfur trioxide gas.
[0012] Preferably, in step (1), the layered cathode material precursor powder is (Ni x A y M 1-x-y )(OH)2、(Ni x A y M 1-x-y )CO3 or (Ni x A y M 1-x-y )C2O4, wherein A is Co or Fe, M is Mn, Al or W, 0 <x<1,0≤y<1,0≤1-x-y<1。
[0013] Preferably, in step (1), the lithium source is lithium hydroxide, lithium carbonate or lithium oxalate.
[0014] Preferably, in step (1), the aluminum source is aluminum acetate, aluminum oxalate, aluminum carbonate, aluminum hydroxide or aluminum sulfate.
[0015] Preferably, in step (1), during grinding, the relative humidity is 5% to 20%, the temperature is 30° C. to 60° C., and the grinding time is 0.5 h to 2 h. When the lithium source or aluminum source is a moisture-sensitive substance such as lithium hydroxide or aluminum hydroxide, the material can be effectively prevented from absorbing water by controlling the grinding conditions.
[0016] Preferably, in step (2), the sulfate is copper sulfate or aluminum sulfate.
[0017] Preferably, in step (2), when the high temperature heating device is a tube furnace, the crucible II is placed at the air inlet end of the tube furnace to ensure that the crucible I is in a sulfur oxide atmosphere during the high temperature reaction.
[0018] Preferably, in step (2), the heating rate is 2°C / min to 15°C / min, and the cooling rate is 1°C / min to 10°C / min.
[0019] Preferably, when the nickel content in the layered cathode material precursor powder is greater than 0.8 in step (1), the high temperature heating device in step (2) is a tube furnace, the atmosphere is oxygen, and the gas flow rate is 50 cfm to 300 cfm. Otherwise, a muffle furnace is used, and the atmosphere is air.
[0020] Preferably, the particle diameter of the Li2SO4 coated and Al-doped composite layered positive electrode material is 1 μm to 15 μm, the coating amount of Li2SO4 is 1% to 5% of the amount of the layered positive electrode material, and the doping of the Al element is 0.5% to 10% of the amount of the layered positive electrode material.
[0021] Preferably, the coating amount of Li2SO4 is 2-3% of the amount of the layered positive electrode material, and the doping amount of the Al element is 1-3% of the amount of the layered positive electrode material.
[0022] A lithium ion battery, wherein the positive electrode material of the battery adopts the Li2SO4 coated and Al doped composite layered positive electrode material described in the present invention.
[0023] Beneficial Effects
[0024] The present invention provides a Li2SO4 coated and Al-doped composite layered positive electrode material, wherein a precursor is mixed with a lithium source and an aluminum source to obtain a mixed powder, and sulfate is used as a coating source material. When the mixed powder is not in contact with the coating source material, sulfur trioxide gas is generated by decomposing the sulfate, and is wrapped around the layered positive electrode material particles, thereby reacting with the residual lithium on the surface of the particles to generate a uniform Li2SO4 coating layer, and Al doping is achieved at the same time. Li2SO4 coating and Al doping can reduce side reactions such as oxygen generation on the surface of the high-voltage positive electrode through synergistic effects, and can also increase the lithium ion transmission rate and stabilize the internal lattice structure of the positive electrode in a high-delithiation state, thereby significantly improving the specific capacity and cycle stability of the single-crystal layered positive electrode material under a high charging cut-off voltage.
[0025] The present invention provides a Li2SO4 coated and Al-doped composite layered positive electrode material, which achieves both coating and doping effects by a one-step synthesis method using a chemical vapor deposition (CVD) method. The method is simple and effective, low-cost, and the prepared material has good morphology uniformity and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The X-ray diffraction (XRD) diagrams of the positive electrode materials prepared in Example 1 and Comparative Example 1 are shown.
[0027] Figure 2 This is the energy spectrum (EDS) diagram of the composite layered positive electrode material prepared in Example 1.
[0028] Figure 3 The electrochemical cycle performance diagram of the batteries assembled in Example 1 and Comparative Example 1.
[0029] Figure 4 This is the XRD pattern of the material prepared in Comparative Example 2. DETAILED DESCRIPTION
[0030] The present invention will be further described in detail below in conjunction with specific embodiments.
[0031] In the following examples or comparative examples:
[0032] (1) XRD test: UltimatⅣ-185 powder diffractometer.
[0033] (2) EDS test: Hitachi S-4800 scanning electron microscope.
[0034] (3) Button cell assembly and electrochemical performance testing: The electrochemical performance test was performed using CR2025 button cell batteries at room temperature. The working electrode preparation process is as follows: first, the material prepared in the embodiment or comparative example and acetylene black are mixed, and polyvinylidene fluoride (PVDF) / N-methyl-2-pyrrolidone (NMP) solution is added dropwise to the mixed sample so that the mass ratio of the material prepared in the embodiment or comparative example, acetylene black and PVDF is 8:1:1, and a uniform slurry is obtained; then, the obtained slurry is evenly scraped onto an aluminum foil with a scraper, and vacuum dried at 100°C for 12 hours to remove the solvent; finally, a small disc with a diameter of 1.1 cm is pressed out of the aluminum foil coated with the sample with a punching machine as a positive electrode, a lithium sheet is used as a negative electrode material, and a 1.0MLiPF6 carbonate electrolyte (the volume ratio of ethylene carbonate (EC): diethyl carbonate (DEC): dimethyl carbonate (DMC) is 1:1:1). The charge and discharge test is completed under the blue battery test system, the test voltage range is 3.0-4.6V, the test temperature is room temperature, and the test current density is 1C (1C = 200mA / g).
[0035] Example 1
[0036] The precursor (Ni 0.9 Co 0.05 Mn 0.05 )(OH)2, LiOH and (CH3COO)3Al are mixed in a molar ratio of 0.98:1.07:0.02, and ground for 0.5h at a relative humidity of 10% and a temperature of 45°C to obtain a mixed powder, which is loosely spread into crucible No. 1, and CuSO4 powder accounting for 50% of the amount of the precursor material is weighed and put into crucible No. 2, and then the two crucibles are put into a tubular furnace in the order of crucible No. 2 close to the air inlet end, and the temperature is first raised to 500°C for pre-calcination for 5h, and then raised to 750°C for calcination for 12h, the heating rate is 5°C / min, the atmosphere is oxygen, the gas flow rate is 200cfm, and finally the temperature is lowered at a rate of 2°C / min to obtain a Li2SO4-coated and Al-doped composite layered positive electrode material, recorded as Al 0.02 -Li(Ni 0.9 Co 0.05 Mn 0.05 )O2@Li2SO4.
[0037] The XRD test results of the composite layered positive electrode material are as follows Figure 1 As shown in the figure, it can be seen that the layered structure of the composite layered positive electrode material has not changed compared with the bulk positive electrode material of Comparative Example 1.
[0038] The EDS test results of the composite layered cathode material are as follows Figure 2As shown, the results show that Al and S elements are distributed in the composite material. Combined with the reaction process, it can be determined that the S element is coated on the surface of the layered positive electrode material in the form of Li2SO4. The amount of the substance in the Li2SO4 coating layer is calculated to be 2.5% of the layered positive electrode material body.
[0039] The electrochemical cycling results of the assembled battery are shown in Figure 3 As shown in the figure, it can be seen that the layered composite material described in this embodiment still has a specific capacity of 176.0 mAh / g after 200 cycles, and the capacity retention rate is 90.7%.
[0040] Example 2
[0041] The precursor (Ni 0.7 Co 0.1 Al 0.2 )(OH)2, LiOH and (CH3COO)3Al are mixed in a molar ratio of 0.99:1.07:0.01, and ground for 0.5 h at a relative humidity of 10% and a temperature of 60°C to obtain a mixed powder, which is loosely spread into crucible No. 1, and CuSO4 powder accounting for 30% of the amount of the precursor material is weighed and put into crucible No. 2, and then the two crucibles are placed in a muffle furnace and first heated to 500°C for pre-calcination for 5h, and then heated to 850°C for calcination for 12h, with a heating rate of 5°C / min, and the atmosphere is air, and finally cooled at a rate of 2°C / min to obtain a Li2SO4-coated and Al-doped composite layered positive electrode material, denoted as Al 0.01 -Li(Ni 0.7 Co 0.1 Mn 0.2 )O2@Li2SO4.
[0042] The XRD test result of the composite layered positive electrode material shows that the layered structure of the composite layered positive electrode material is not changed compared with the bulk positive electrode material of Comparative Example 1.
[0043] The EDS test results of the composite layered positive electrode material show that Al and S elements are distributed in the composite material. Combined with the reaction process, it can be determined that the S element is coated on the surface of the layered positive electrode material in the form of Li2SO4. By calculation, the amount of the Li2SO4 coating layer is 5% of the layered positive electrode material body.
[0044] After 200 cycles, the assembled battery still has a specific capacity of 176.3 mAh / g, and the capacity retention rate is 86.3%.
[0045] Example 3
[0046] The precursor (Ni 0.8 Fe 0.1 Mn0.1 )(OH)2, LiOH and (CH3COO)3Al are mixed in a molar ratio of 0.98:1.07:0.02, and ground for 0.5h under the conditions of relative humidity of 10% and temperature of 45°C to obtain a mixed powder, which is loosely spread into crucible No. 1, and Al2(SO4)3 powder accounting for 20% of the amount of the precursor material is weighed and put into crucible No. 2, and then the two crucibles are placed in a muffle furnace and first heated to 480°C for pre-calcination for 5h, and then heated to 850°C for calcination for 12h, with a heating rate of 5°C / min, and the atmosphere is air, and finally cooled at a rate of 2°C / min to obtain a Li2SO4-coated and Al-doped composite layered positive electrode material, denoted as Al 0.02 -Li(Ni 0.8 Fe 0.1 Mn 0.1 )O2@Li2SO4.
[0047] The XRD test result of the composite layered positive electrode material shows that the layered structure of the composite layered positive electrode material is not changed compared with the bulk positive electrode material of Comparative Example 1.
[0048] The EDS test results of the composite layered positive electrode material show that Al and S elements are distributed in the composite material. Combined with the reaction process, it can be determined that the S element is coated on the surface of the layered positive electrode material in the form of Li2SO4. By calculation, the amount of the Li2SO4 coating layer is 3% of the layered positive electrode material body.
[0049] After 200 cycles, the assembled battery still has a specific capacity of 174.2 mAh / g, and the capacity retention rate is 84.4%.
[0050] Example 4
[0051] The precursor (Ni 0.7 Mn 0.3 )(OH)2, LiOH and (CH3COO)3Al are mixed in a molar ratio of 0.98:1.07:0.02, and ground for 0.5h at a relative humidity of 10% and a temperature of 45°C to obtain a mixed powder, which is loosely spread into crucible No. 1, and Al2(SO4)3 powder accounting for 20% of the amount of the precursor material is weighed and put into crucible No. 2, and then the two crucibles are placed in a muffle furnace and first heated to 500°C for pre-calcination for 5h, and then heated to 850°C for calcination for 12h, with a heating rate of 5°C / min, and the atmosphere is air, and finally cooled at a rate of 2°C / min to obtain a Li2SO4-coated and Al-doped composite layered positive electrode material, denoted as Al 0.02 -Li(Ni 0.7 Mn 0.3 )O2@Li2SO4.
[0052] The XRD test result of the composite layered positive electrode material shows that the layered structure of the composite layered positive electrode material is not changed compared with the bulk positive electrode material of Comparative Example 1.
[0053] The EDS test results of the composite layered positive electrode material show that Al and S elements are distributed in the composite material. Combined with the reaction process, it can be determined that the S element is coated on the surface of the layered positive electrode material in the form of Li2SO4. By calculation, the amount of the Li2SO4 coating layer is 3% of the layered positive electrode material body.
[0054] After 200 cycles, the assembled battery still has a specific capacity of 169.5 mAh / g, and the capacity retention rate is 88.6%.
[0055] Example 5
[0056] The precursor (Ni 0.9 Co 0.05 Mn 0.05 )(OH)2, LiOH and Al2(SO4)3 are mixed in a molar ratio of 0.99:1.07:0.005, and anhydrous ethanol is added to grind for 1 hour under the conditions of relative humidity of 5% and temperature of 45°C to obtain a mixed powder, and the mixed powder is loosely spread into crucible No. 1, and CuSO4 powder accounting for 50% of the amount of the precursor material is weighed and put into crucible No. 2, and then the two crucibles are put into a tubular furnace in the order of crucible No. 2 close to the air inlet end, first heated to 480°C for pre-burning for 5h, and then heated to 750°C for calcination for 15h, the heating rate is 2°C / min, the atmosphere is oxygen, the gas flow rate is 150cfm, and finally cooled at a rate of 2°C / min to obtain a Li2SO4-coated and Al-doped composite layered positive electrode material, recorded as Al 0.01 -Li(Ni 0.9 Co 0.05 Mn 0.05 )O2@Li2SO4.
[0057] The XRD test result of the composite layered positive electrode material shows that the layered structure of the composite layered positive electrode material is not changed compared with the bulk positive electrode material of Comparative Example 1.
[0058] The EDS test results of the composite layered positive electrode material show that Al and S elements are distributed in the composite material. Combined with the reaction process, it can be determined that the S element is coated on the surface of the layered positive electrode material in the form of Li2SO4. By calculation, the amount of the Li2SO4 coating layer is 5% of the layered positive electrode material body.
[0059] After 200 cycles, the assembled battery still has a specific capacity of 155.3 mAh / g, and the capacity retention rate is 79.5%.
[0060] Example 6
[0061] The precursor (Ni 0.9 Fe 0.05 Mn 0.05 )(OH)2, LiOH and aluminum oxalate (C6Al2O 12 ·xH2O) in a molar ratio of 0.96:1.07:0.02, anhydrous ethanol was added and ground for 1 hour under the conditions of relative humidity of 10% and temperature of 45°C to obtain a mixed powder, the mixed powder was loosely spread into crucible No. 1, CuSO4 powder accounting for 50% of the amount of the precursor material was weighed and put into crucible No. 2, and then the two crucibles were put into a tube furnace in the order of crucible No. 2 close to the air inlet end, first heated to 480°C for pre-calcination for 5h, then heated to 800°C for calcination for 12h, the heating rate was 5°C / min, the atmosphere was oxygen, the gas flow rate was 200cfm, and finally cooled at a rate of 2°C / min to obtain a Li2SO4-coated and Al-doped composite layered positive electrode material, recorded as Al 0.04 -Li(Ni 0.9 Fe 0.05 Mn 0.05 )O2@Li2SO4.
[0062] The XRD test result of the composite layered positive electrode material shows that the layered structure of the composite layered positive electrode material is not changed compared with the bulk positive electrode material of Comparative Example 1.
[0063] The EDS test results of the composite layered positive electrode material show that Al and S elements are distributed in the composite material. Combined with the reaction process, it can be determined that the S element is coated on the surface of the layered positive electrode material in the form of Li2SO4. By calculation, the amount of the Li2SO4 coating layer is 3% of the layered positive electrode material body.
[0064] After 200 cycles, the assembled battery still has a specific capacity of 177.9 mAh / g, and the capacity retention rate is 93.7%.
[0065] Comparative Example 1
[0066] The precursor (Ni 0.9 Fe 0.05 Mn 0.05)(OH)2 and LiOH were mixed in a molar ratio of 1.00:1.07, and anhydrous ethanol was added to grind for 0.5 h under the conditions of relative humidity of 10% and temperature of 45°C to obtain a mixed powder, and the mixed powder was loosely spread in a crucible, and the crucible was placed in a tubular furnace and heated to 500°C for pre-calcination for 5 h, and then heated to 750°C for calcination for 12 h, with a heating rate of 5°C / min, an oxygen atmosphere, and a gas flow rate of 200 cfm, and finally cooled at a rate of 2°C / min to obtain a layered positive electrode material, denoted as Li(Ni 0.9 Co 0.05 Mn 0.05 )O2.
[0067] The XRD test result of the layered positive electrode material shows that the material has a layered structure.
[0068] After 200 cycles, the assembled battery has a specific capacity of only 115.4 mAh / g, and the capacity retention rate is 67.1%.
[0069] Comparative Example 2
[0070] The precursor (Ni 0.9 Fe 0.05 Mn 0.05 )(OH)2, LiOH and (CH3COO)3Al are mixed in a molar ratio of 0.90:1.07:0.10, and anhydrous ethanol is added and ground for 0.5h under the conditions of relative humidity of 10% and temperature of 45°C to obtain a mixed powder, which is loosely spread into crucible No. 1, and CuSO4 powder accounting for 30% of the amount of the precursor material is weighed and put into crucible No. 2, and then the two crucibles are put into a tubular furnace in the order of crucible No. 2 close to the air inlet end, and the temperature is first raised to 500°C for pre-calcination for 5h, and then raised to 750°C for calcination for 12h, the heating rate is 5°C / min, the atmosphere is oxygen, the gas flow rate is 200cfm, and finally the temperature is lowered at a rate of 2°C / min to obtain a Li2SO4-coated and Al-doped composite material, recorded as Al 0.11 -Li(Ni 0.9 Co 0.05 Mn 0.05 )O2@Li2SO4.
[0071] The XRD test results of the composite material are as follows: Figure 4 As shown, the results show that the layered structure of the composite material has changed compared to the bulk positive electrode material of Comparative Example 1. Due to the change in the layered structure, it is no longer suitable for use as a positive electrode material.
[0072] The EDS test results of the composite material show that Al and S elements are distributed in the composite material. Combined with the reaction process, it can be determined that the S element is coated on the surface of the layered positive electrode material in the form of Li2SO4. By calculation, the amount of the Li2SO4 coating layer is 3% of the layered positive electrode material body.
[0073] Comparative Example 3
[0074] The precursor (Ni 0.9 Fe 0.05 Mn 0.05 )(OH)2, LiOH and Al2(SO4)3 were mixed in a molar ratio of 0.98:1.07:0.01, and anhydrous ethanol was added to grind for 0.5h under the conditions of relative humidity of 10% and temperature of 45°C to obtain a mixed powder, and the mixed powder was loosely spread in a crucible, and then the crucible was placed in a tubular furnace and heated to 500°C for pre-burning for 5h, and then heated to 750°C for calcination for 12h, with a heating rate of 5°C / min, an oxygen atmosphere, a gas flow rate of 200cfm, and finally cooled at a rate of 2°C / min to obtain a Li2SO4-coated and Al-doped composite layered positive electrode material, denoted as Al 0.02 -Li(Ni 0.9 Co 0.05 Mn 0.05 )O2@Li2SO4.
[0075] The XRD test result of the composite layered positive electrode material shows that the layered structure of the composite layered positive electrode material is not changed compared with the bulk positive electrode material of Comparative Example 1.
[0076] The EDS test results of the composite layered positive electrode material show that Al and S elements are distributed in the composite material. Combined with the reaction process, it can be determined that the S element is coated on the surface of the layered positive electrode material in the form of Li2SO4. By calculation, the amount of the Li2SO4 coating layer is 0.5% of the layered positive electrode material body.
[0077] After 200 cycles, the assembled battery has a specific capacity of only 120.6 mAh / g, and the capacity retention rate is 66.2%.
[0078] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.
Claims
1. A Li2SO4 coated and Al-doped composite layered positive electrode material, characterized in that: The material is prepared by the following method, and the method steps are as follows: (1) Grinding and mixing layered cathode material precursor powder, lithium source and aluminum source in anhydrous ethanol to obtain a mixed powder; (2) placing the mixed powder into crucible I, placing sulfate into crucible II, placing the two crucibles into a tube furnace, first heating to 480°C-520°C for pre-burning for 4h-6h under an oxygen atmosphere, then heating to 600°C-900°C for calcining for 10h-12h, cooling after calcination, and obtaining a Li2SO4-coated and Al-doped composite layered positive electrode material in crucible I; The molar ratio of the layered cathode material precursor powder to the lithium source is 1:1.05-1.2, the amount of the aluminum source is 0.5%-10% of the amount of the layered cathode material precursor powder; the amount of the sulfate in the sulfate is 20%-50% of the amount of the layered cathode material precursor powder; The sulfate is a sulfate that decomposes at 520-900°C to produce sulfur trioxide gas; In step (1), the layered cathode material precursor powder is (Ni x A y M 1-x-y )(OH)2、(Ni x A y M 1-x-y )CO3 or (Ni x A y M 1-x-y )C2O4, wherein A is Co or Fe, M is Mn, Al or W, 0 <x<1,0≤y<1,0≤1-x-y<1; In step (2), crucible II is placed at the air inlet end of the tube furnace; In step (1), the nickel content in the layered positive electrode material precursor powder is greater than 0.8, and in step (2), the gas flow rate is 50CFM~300CFM.
2. A Li2SO4 coated and Al-doped composite layered positive electrode material as claimed in claim 1, characterized in that: In step (1), the lithium source is lithium hydroxide, lithium carbonate or lithium oxalate; the aluminum source is aluminum acetate, aluminum oxalate, aluminum carbonate, aluminum hydroxide or aluminum sulfate; in step (2), the sulfate is copper sulfate or aluminum sulfate.
3. The Li2SO4 coated and Al-doped composite layered positive electrode material according to claim 1, characterized in that: In step (1), during grinding, the relative humidity is 5% to 20%, the temperature is 30° C. to 60° C., and the grinding time is 0.5 h to 2 h.
4. The Li2SO4 coated and Al-doped composite layered positive electrode material according to claim 1, characterized in that: In step (2), the heating rate is 2°C / min to 15°C / min, and the cooling rate is 1°C / min to 10°C / min.
5. The Li2SO4 coated and Al-doped composite layered positive electrode material according to claim 1, characterized in that: The particle diameter of the Li2SO4 coated and Al-doped composite layered positive electrode material is 1 μm to 15 μm, the coating amount of Li2SO4 is 1% to 5% of the amount of the layered positive electrode material, and the doping amount of Al element is 0.5% to 10% of the amount of the layered positive electrode material.
6. A Li2SO4 coated and Al-doped composite layered positive electrode material as claimed in claim 5, characterized in that: The coating amount of Li2SO4 is 2-3% of the amount of the layered positive electrode material, and the doping amount of the Al element is 1-3% of the amount of the layered positive electrode material.
7. A lithium ion battery, characterized in that: The positive electrode material of the battery adopts a Li2SO4-coated and Al-doped composite layered positive electrode material as described in any one of claims 1 to 6.
Citation Information
Patent Citations
Aluminum-doped and modified cathode material for high-capacity lithium ion batteries
CN106654255A
Positive electrode material surface modification method and positive electrode material prepared by method
CN110635131A
Lithium ion battery positive electrode active material and preparation method thereof
CN113972352A