Catalyst, method for producing isobutylaldehyde and methacrolein, method for producing methacrylic acid, and method for producing methacrylic acid ester
By using a catalyst with an average electronegativity of 2.1 to 2.8 and a catalyst containing a metal oxide, the problems of low isobutyraldehyde selectivity and complex hydrogen reduction treatment in the isobutanol dehydrogenation reaction are solved, and efficient and safe isobutyric acid is achieved. Manufacture of butyraldehyde and methacrolein.
Patent Information
- Application Number
- CN202180023785.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-08
- Filing Date
- 2021-03-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-03-31
AI Technical Summary
In the existing isobutanol dehydrogenation reaction, it is difficult to produce isobutyraldehyde with high selectivity, and hydrogen reduction treatment is required, which poses safety risks and operational complexity.
Use a catalyst with an average electronegativity of 2.1 to 2.8, including metal oxides such as Al, Si, Zn, Ag, Ce, La and Mg oxides, for the dehydrogenation reaction of isobutanol to avoid hydrogen reduction treatment and inhibit Oxidation and dimerization of isobutyraldehyde.
It achieves the production of isobutyraldehyde and methacrolein with high selectivity, simplifies the process flow, and avoids the safety risks and operational complexity of hydrogen reduction.
Smart Images

Figure BDA0003861065220000201 
Figure BDA0003861065220000221 
Figure BDA0003861065220000241
Abstract
Description
Technical Field
[0001] The present invention relates to a catalyst, a method for producing isobutylaldehyde and methacrolein, a method for producing methacrylic acid and a method for producing methacrylate.
[0002] This application claims priority based on Japanese Patent Application No. 2020-65205 filed in Japan on March 31, 2020 and Japanese Patent Application No. 2020-150757 filed in Japan on September 8, 2020, the contents of which are incorporated herein by reference. Background Art
[0003] Isobutyraldehyde can be derived into methacrolein and methacrylic acid by an oxidation reaction using a heteropolyacid, and is a useful intermediate of methacrylate (Non-Patent Documents 1 and 2).
[0004] As an industrial production method of isobutylaldehyde, there is a hydroformylation reaction of propylene and carbon monoxide. However, in this method, isobutylaldehyde is produced as a by-product when producing normal butyraldehyde, so it is impossible to selectively produce isobutylaldehyde in an arbitrary amount.
[0005] As a method for producing isobutylaldehyde, there is also a known method of converting isobutyl alcohol (hereinafter also referred to as "isobutanol") into isobutylaldehyde through a dehydrogenation reaction. Non-patent document 3 describes that isobutylaldehyde can be synthesized by dehydrogenating isobutyl alcohol using Zn / swelling soil as a catalyst. In addition, isobutyl alcohol as a raw material can also be produced from biomass (patent document 1), and it is also expected that methacrylate can be synthesized from renewable raw materials.
[0006] In addition, Patent Documents 2 and 3 propose the use of a copper catalyst or a copper-magnesium catalyst as a dehydrogenation catalyst. However, these catalysts need to be reduced with hydrogen before the reaction begins. It is also known that hydrogen has a wide explosive range (4 to 75% by volume), which further embrittles metals such as stainless steel, making it difficult to operate and requiring an explosion-proof structure, concentration management of hydrogen-containing gas, and safety mechanisms in case of abnormalities.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application No. 2011-505490
[0010] Patent Document 2: Japanese Patent Application Publication No. 2010-104938
[0011] Patent Document 3: Japanese Patent Application Publication No. 2016-79143
[0012] Non-patent literature
[0013] Non-patent document 1: Journal of Catalysis 195 (2000) 360-375
[0014] Non-patent document 2: Journal of Molecular Catalysis A: Chemical 152 (2000) 141-155
[0015] Non-patent document 3: Journal of the Serbian Chemical Society 73, 997-1009 (2008) Summary of the invention
[0016] However, there are few studies on methods for synthesizing isobutylaldehyde by dehydrogenation of isobutyl alcohol, and the selectivity for isobutylaldehyde is not sufficient. In addition, complicated treatments such as reduction treatment with hydrogen are required.
[0017] An object of the present invention is to provide a dehydrogenation catalyst which can produce isobutylaldehyde and methacrolein with high selectivity from isobutyl alcohol without requiring reduction treatment with hydrogen while suppressing oxidation and bimolecularization of isobutylaldehyde, and a method for producing a dehydrogenated compound using the dehydrogenation catalyst.
[0018] The present invention has the following configurations.
[0019] [1] A catalyst with an average electronegativity of 2.1 to 2.8.
[0020] [2] The catalyst according to [1], comprising a metal oxide having an average electronegativity of 2.1 to 2.8.
[0021] [3] The catalyst according to [2], wherein the metal oxide comprises oxides of one or more metals selected from the group consisting of Al, Si, Zn, Ag, Ce, La and Mg.
[0022] [4] The catalyst according to [2], wherein the metal oxide comprises an oxide of one or more metals selected from the group consisting of Zn, Al, Fe, Si, Zr and Ti.
[0023] [5] The catalyst according to any one of [1] to [4], comprising one or more alkali metals.
[0024] [6] The catalyst according to any one of [1] to [5], wherein the amount of acid is 0.3 mmol / g or less based on 1 g of the catalyst.
[0025] [7] The catalyst according to any one of [1] to [6], which is a catalyst for producing at least one dehydrogenated compound selected from isobutylaldehyde and methacrolein from isobutyl alcohol.
[0026] [8] The catalyst according to any one of [1] to [7], wherein the average electronegativity of the catalyst is preferably 2.10 to 2.75, more preferably 2.10 to 2.70, further preferably 2.10 to 2.65, particularly preferably 2.10 to 2.60, particularly preferably 2.10 to 2.55, and most preferably 2.10 to 2.50.
[0027] [9] The catalyst according to any one of [1] to [8], wherein the catalyst contains a metal oxide, and the content of the metal oxide is preferably 80% to 100% by mass, more preferably 85% to 100% by mass, further preferably 90% to 100% by mass, particularly preferably 95% to 100% by mass, particularly preferably 97.5% to 100% by mass, and most preferably 99% to 100% by mass, relative to the total mass of the catalyst.
[0028]
[10] A catalyst according to any one of [1] to [9], wherein the catalyst comprises a metal oxide and an alkali metal, and the content of the alkali metal relative to the total mass of the metal in the catalyst is preferably 1.0 mol% to 9.0 mol%, more preferably 2.0 mol% to 8.5 mol%, further preferably 3.0 mol% to 8.0 mol%, particularly preferably 4.0 mol% to 7.5 mol%, and most preferably 5.0 mol% to 7.0 mol%.
[0029]
[11] The catalyst according to any one of [1] to
[10] , wherein the acid amount of the catalyst is preferably 0 mmol / g to 0.25 mmol / g, more preferably 0 mmol / g to 0.20 mmol / g, further preferably 0 mmol / g to 0.15 mmol / g, particularly preferably 0 mmol / g to 0.10 mmol / g, and most preferably 0 mmol / g to 0.08 mmol / g.
[0030]
[12] The catalyst according to any one of [1] to
[11] , wherein the base amount of the catalyst is preferably 0 mmol / g to 4.0 mmol / g, more preferably 0.001 mmol / g to 3.0 mmol / g, further preferably 0.01 mmol / g to 2.0 mmol / g, particularly preferably 0.1 mmol / g to 1.0 mmol / g, and most preferably 0.15 mmol / g to 0.5 mmol / g.
[0031]
[13] The catalyst according to any one of [1] to
[12] , wherein the BET specific surface area of the catalyst is preferably 3 m 2 / g~230m 2 / g, more preferably 5m 2 / g~200m 2 / g, more preferably 10m 2 / g~180m 2 / g, particularly preferably 30m 2 / g~170m 2 / g.
[0032]
[14] A method for producing the catalyst according to any one of [1] to
[13] , comprising calcining a metal oxide.
[0033]
[15] The method for producing a catalyst according to
[14] , wherein the calcination temperature is preferably 200°C to 1000°C, more preferably 250°C to 950°C, further preferably 300°C to 900°C, particularly preferably 350°C to 850°C, particularly preferably 400°C to 800°C, and most preferably 450°C to 750°C.
[0034]
[16] A method for producing a dehydrogenated compound from isobutanol, comprising using the catalyst described in any one of [1] to
[13] to produce at least one dehydrogenated compound selected from isobutyraldehyde and methacrolein from isobutanol.
[0035]
[17] The method for producing a dehydrogenated compound according to
[16] , wherein the production of the dehydrogenated compound is carried out in a liquid phase or a gas phase.
[0036]
[18] The method for producing a dehydrogenated compound according to
[16] or
[17] , wherein the production of the dehydrogenated compound is carried out in a gas phase, comprising gasifying a raw material gas containing isobutanol at a temperature of 108°C to 600°C and a pressure of 0.05 MPa to 1 MPa.
[0037]
[19] The method for producing a dehydrogenated compound according to
[17] , wherein the concentration of isobutanol in the raw gas is preferably 0.1% to 100% by volume, more preferably 1% to 50% by volume, and even more preferably 10% to 30% by volume relative to the total volume of the raw gas.
[0038]
[20] A method for producing a dehydrogenated compound according to
[18] or
[19] , wherein the raw gas contains water vapor, and the concentration of the water vapor in the raw gas is preferably 2.5% to 80.0% by volume, more preferably 5.0% to 75.0% by volume, further preferably 10.0% to 70.0% by volume, particularly preferably 15.0% to 65.0% by volume, and most preferably 20.0% to 60.0% by volume relative to the total volume of the raw gas.
[0039]
[21] The method for producing a dehydrogenated compound according to any one of
[16] to
[20] , wherein in the production of the dehydrogenated compound, the reaction temperature is preferably 320°C to 600°C, more preferably 340°C to 580°C, further preferably 360°C to 560°C, and particularly preferably 380°C to 540°C.
[0040]
[22] A method for producing a dehydrogenated compound according to any one of
[16] to
[21] , wherein W / F calculated by the amount of isobutanol supplied to the reactor (unit: g / h) ÷ the mass of the catalyst filled in the reaction tube (unit: g) is preferably 0.30 to 8.0, more preferably 0.50 to 4.5, further preferably 0.6 to 4.5, particularly preferably 0.65 to 2.0, and most preferably 0.68 to 1.0.
[0041]
[23] A method for producing methacrylic acid, comprising producing methacrylic acid from at least one selected from isobutylaldehyde and methacrolein obtained by the method for producing a dehydrogenated compound according to any one of
[16] to
[22] .
[0042]
[24] The method for producing methacrylic acid according to
[23] , wherein the production of the methacrylic acid is carried out in a gas phase.
[0043]
[25] A method for producing a methacrylic acid ester, comprising producing methacrylic acid by the method for producing methacrylic acid according to
[23] , and producing a methacrylic acid ester from the obtained methacrylic acid and an alcohol having 1 to 20 carbon atoms.
[0044]
[26] The method for producing methacrylate according to
[25] , wherein the alcohol having 1 to 20 carbon atoms is at least one selected from aliphatic alcohols and aromatic alcohols.
[0045]
[27] The method for producing methacrylate according to
[26] , wherein the alcohol having 1 to 20 carbon atoms is an aliphatic alcohol, and the aliphatic alcohol is at least one selected from methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol and eicosanol.
[0046]
[28] The method for producing a methacrylate according to any one of
[25] to
[27] , wherein the production of the methacrylate is carried out in the presence of a catalyst, and the catalyst is sulfuric acid or an ion exchange resin.
[0047]
[29] The method for producing methacrylate according to
[28] , wherein the catalyst is an ion exchange resin, and the flow rate of methacrylic acid and the alcohol having 1 to 20 carbon atoms is preferably 0.10 to 10.0 times, more preferably 0.20 to 5.0 times, in terms of the mass ratio relative to the amount of the ion exchange resin.
[0048]
[30] The method for producing a methacrylate according to any one of
[25] to
[29] , wherein the reaction temperature in producing the methacrylate is 40°C to 130°C.
[0049] According to the present invention, there can be provided a dehydrogenation catalyst capable of producing isobutylaldehyde and methacrolein with high selectivity from isobutyl alcohol without requiring reduction treatment with hydrogen while suppressing oxidation and bimolecularization of isobutylaldehyde, and a method for producing a dehydrogenated compound using the dehydrogenation catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 1 to 3.
[0051] Figure 2 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 5 to 7.
[0052] Figure 3 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 8 to 10.
[0053] Figure 4 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 11 to 13.
[0054] Figure 5 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 14 to 16.
[0055] Figure 6It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 8 and 17 to 19.
[0056] Figure 7 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 20 to 24.
[0057] Fig. 8A It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 25 to 31 and Comparative Example 1.
[0058] Figure 8B This is a graph showing the selectivity and average electronegativity of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 25 to 31 and Comparative Example 1.
[0059] Figure 8C It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 25 to 31 and Comparative Example 1.
[0060] Fig. 9 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 33 to 36.
[0061] Fig.10 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 37 to 40.
[0062] Fig.11 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 25, 41 and 42.
[0063] Fig.12 The graphs show the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 1, 43 and 44.
[0064] Fig.13 The graphs show the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 3, 13 and 45.
[0065] Fig.14It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 46 to 50.
[0066] Fig.15 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) in Examples 51 to 53 and 28, and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL).
[0067] Fig.16 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 5, 54 to 56 and 8.
[0068] Fig.17 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) in Examples 57 and 2, and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL).
[0069] Fig.18 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 58, 22 and 59.
[0070] Fig.19 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 61 to 63.
[0071] Fig. 20 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 53 and 64.
[0072] Fig.21 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 52 and 65 to 67.
[0073] Fig. 22 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 67 to 71, 52 and 79.
[0074] Fig.23 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 72 to 76.
[0075] Fig.24It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 77, 74 and 69.
[0076] Fig.25 It is a graph showing the conversion rate of isobutyl alcohol (iBuOH) and the selectivity and yield of isobutylaldehyde (iBAld) and methacrolein (MAL) in Examples 75 and 78. DETAILED DESCRIPTION
[0077] [First embodiment]
[0078] (catalyst)
[0079] The catalyst of the first embodiment (hereinafter also referred to as "catalyst (A)") is a catalyst capable of producing isobutylaldehyde and / or methacrolein by a dehydrogenation reaction of isobutyl alcohol (iso-Butanol), and is a catalyst that does not require reduction with hydrogen.
[0080] The average electronegativity of the catalyst (A) is 2.10 to 2.80. The average electronegativity of the catalyst is preferably 2.10 to 2.75, more preferably 2.10 to 2.70, further preferably 2.10 to 2.65, particularly preferably 2.10 to 2.60, particularly preferably 2.10 to 2.55, and most preferably 2.10 to 2.50. When the average electronegativity is within the above range, a catalyst can be obtained that effectively produces isobutyraldehyde while suppressing the dehydration reaction of isobutanol and the dimerization of the generated isobutyraldehyde. In the present invention, compound P p Q q R r The average electronegativity of is defined by the following Sanderson formula. Average electronegativity = (S P p ·S Q q ·S R r ) 1 / (p+q+r)
[0081] S P :Pauling electronegativity of element P
[0082] S Q :Pauling electronegativity of element Q
[0083] S R : Pauling electronegativity of element R
[0084] p : The number of elements in element P
[0085] q: The number of elements in element Q
[0086] r : The number of elements of element R
[0087] As the constituent element of the catalyst (A), from the viewpoint of improving the selectivity of isobutylaldehyde, a catalyst containing one or more metal oxides selected from the group consisting of Al, Si, Zn, Ti, Ag, Ce, La and Mg is preferred, a catalyst containing one or more metal oxides selected from the group consisting of Al, Zn, Ti, Ag, Ce, La and Mg is more preferred, a catalyst containing one or more metal oxides selected from the group consisting of Al, Zn, Ti, Ag, Ce and Mg is further preferred, a catalyst containing one or more metal oxides selected from the group consisting of Al, Zn, Ag, Ce and Mg is particularly preferred, a catalyst containing one or more metal oxides selected from the group consisting of Al, Zn, Ag and Mg is particularly preferred, and a catalyst containing one or more metal oxides selected from the group consisting of Al, Zn and Ag is most preferred. It should be noted that the above metals may be used alone or in combination of two or more.
[0088] In addition, from the viewpoint of improving the selectivity of isobutylaldehyde, the content of the metal oxide contained in the catalyst is preferably 80% by mass or more, more preferably 85% by mass or more, further preferably 90% by mass or more, particularly preferably 95% by mass or more, particularly preferably 97.5% by mass or more, and most preferably 99% by mass or more, relative to the sum of the masses of all metal oxides contained in the catalyst. By using the catalyst (A), it is possible to produce isobutylaldehyde and methacrolein from isobutyl alcohol with high selectivity while suppressing dehydration reaction and oxidation and dimerization of isobutylaldehyde without reducing with hydrogen.
[0089] The catalyst (A) is not particularly limited as long as it contains one or more metal oxides selected from Al, Si, Zn, Ag, Ce, La and Mg, and a known method can be used. For example, the catalyst (A) can be easily produced by a coprecipitation method, a vapor deposition method, an impregnation method, a mixing method or a method using these methods in combination. The raw material of the catalyst (A) is not particularly limited, and examples thereof include hydroxides, nitrates, acetates and sulfates.
[0090] The catalyst (A) may be calcined before use. From the viewpoint of increasing the selectivity of isobutylaldehyde and / or methacrolein, the calcination temperature is preferably 200°C to 1000°C, more preferably 250°C to 950°C, further preferably 300°C to 900°C, particularly preferably 350°C to 850°C, particularly preferably 400°C to 800°C, and most preferably 450°C to 750°C. When calcining, from the viewpoint of removing sulfate ions, acetate ions, etc. in the catalyst, it is preferably under air or oxygen. In order to suppress the heat generation of the catalyst during calcination, the air or oxygen may be diluted with an inert gas. Examples of the inert gas include helium, neon, krypton, xenon, and radon.
[0091] [Second embodiment]
[0092] (catalyst)
[0093] The catalyst of the second embodiment (hereinafter also referred to as "catalyst (B)") is a catalyst for producing isobutylaldehyde and / or methacrolein by dehydrogenation reaction of isobutyl alcohol (isobutanol), and is a catalyst that does not require reduction with hydrogen.
[0094] The average electronegativity of the catalyst (B) is 2.10 to 2.80.
[0095] The catalyst (B) is a catalyst containing an oxide of one or more metals selected from the group consisting of Al, Si, Fe, Zr and Ti and one or more alkali metals. By using the catalyst (B), it is possible to produce isobutyraldehyde and methacrolein from isobutanol with high selectivity while suppressing dehydration reaction and oxidation and dimerization of isobutyraldehyde without the need for reduction with hydrogen.
[0096] Examples of the alkali metal include Na, K, Rb, and Cs.
[0097] The lower limit of the content of the alkali metal in the catalyst (B) is preferably 1.0 mol% or more, more preferably 2.0 mol% or more, further preferably 3.0 mol% or more, particularly preferably 4.0 mol% or more, and most preferably 5.0 mol% or more, relative to the total amount of metal atoms in the catalyst. If the content of the alkali metal is above the above lower limit, the dehydration reaction can be suppressed. In addition, the upper limit of the content of the alkali metal in the catalyst (B) is preferably 9.0 mol% or less, more preferably 8.5 mol% or less, further preferably 8.0 mol% or less, particularly preferably 7.5 mol% or less, and most preferably 7.0 mol% or less, relative to the total amount of metal atoms in the catalyst. If the content of the alkali metal is below the above upper limit, the oxidation and dimerization of isobutyraldehyde can be suppressed.
[0098] When the catalyst contains a metal oxide and an alkali metal, the alkali metal is preferably supported on the metal oxide.
[0099] The mass ratio represented by [mass of alkali metal] / [mass of metal oxide] is preferably 1 to 10, more preferably 2 to 9, and even more preferably 2.3 to 8.
[0100] From the viewpoint of improving the selectivity of isobutylaldehyde and methacrolein, the acid amount of the catalyst (B) is preferably 0.25 mmol / g or less, more preferably 0.20 mmol / g or less, further preferably 0.15 mmol / g or less, particularly preferably 0.10 mmol / g or less, and most preferably 0.08 mmol / g or less. 3 The measurement was performed using the temperature-dependent desorption spectroscopy (TPD) method using a probe molecule.
[0101] In addition, the amount of base in the dehydrogenation catalyst (2) is preferably 4.0 mmol / g or less, more preferably 3.0 mmol / g or less, further preferably 2.0 mmol / g or less, particularly preferably 1.0 mmol / g or less, and most preferably 0.5 mmol / g or less, from the viewpoint of improving the selectivity of isobutylaldehyde and methacrolein. 2 The measurement was performed using the temperature-dependent desorption spectroscopy (TPD) method using a probe molecule.
[0102] As a method for reducing the acid content of the catalyst (B), for example, there is a method of supporting an alkali metal on a metal oxide. The acid content tends to decrease by increasing the supported amount of the alkali metal.
[0103] In addition, as a method for reducing the amount of alkali in the catalyst (B), for example, a method of reducing the amount of alkali metal supported on a metal oxide can be cited. By reducing the amount of alkali metal supported, the amount of alkali tends to decrease. It should be noted that the alkali metal can be used alone or in combination of two or more.
[0104] The method for producing the catalyst (B) is not particularly limited as long as the metal oxide containing one or more metals selected from Al, Si, Fe, Zr, and Ti contains at least one or more metals selected from alkali metals, and a known method can be used. For example, the catalyst (B) can be easily produced by a coprecipitation method, a vapor deposition method, an impregnation method, a mixing method, or a method using these methods in combination. The raw material of the catalyst (B) is not particularly limited, and examples thereof include hydroxides, nitrates, acetates, and sulfates.
[0105] The catalyst (B) may be calcined before use. From the viewpoint of increasing the selectivity of isobutylaldehyde and / or methacrolein, the calcination temperature is preferably 200°C to 1000°C, more preferably 250°C to 950°C, further preferably 300°C to 900°C, particularly preferably 350°C to 850°C, particularly preferably 400°C to 800°C, and most preferably 450°C to 750°C. When calcining, from the viewpoint of removing sulfate ions, acetate ions, etc. in the catalyst, it is preferably under air or oxygen. In order to suppress the heat generation of the catalyst during calcination, the air or oxygen is diluted with an inert gas. Examples of the inert gas include helium, neon, krypton, xenon, and radon.
[0106] (Shape of Catalyst)
[0107] Catalysts (A) and (B) can be shaped as needed. For example, in the case of a gas phase fixed bed reaction, the shapes of catalysts (A) and (B) are preferably determined by considering the pressure loss in the reactor and the diffusion of the gas. Furthermore, in any reaction of a gas phase fluidized bed reaction and a liquid phase reaction, the shapes of catalysts (A) and (B) are preferably determined by considering the reaction conditions and the movement of substances.
[0108] Examples of a method for molding the catalysts (A) and (B) include a method using a powder molding machine such as a tablet molding machine, an extrusion molding machine, and a tumbling granulator.
[0109] The catalysts (A) and (B) may be molded into any shape such as a spherical shape, a ring shape, a cylindrical shape, or a star shape.
[0110] The molded catalysts (A) and (B) may be ground and used in the form of powders. If necessary, additives may be mixed with the catalysts (A) and (B) during molding.
[0111] (Method for producing isobutylaldehyde and / or methacrolein)
[0112] The method for producing isobutylaldehyde and / or methacrolein of the third embodiment is a method for producing isobutylaldehyde and / or methacrolein by subjecting isobutyl alcohol to a dehydrogenation reaction, wherein isobutyl alcohol is subjected to a dehydrogenation reaction in the presence of one or both of catalysts (A) and (B) to produce isobutylaldehyde and / or methacrolein. In the method for producing isobutylaldehyde and / or methacrolein of the third embodiment, the target product may be both isobutylaldehyde and methacrolein, may be only isobutylaldehyde, or may be only methacrolein. Among them, the method for producing isobutylaldehyde and / or methacrolein of the third embodiment is preferably a method for producing isobutylaldehyde and methacrolein with a total selectivity of 5% or more during stable operation after the start of the reaction, and more preferably a method for producing isobutylaldehyde and methacrolein with a total selectivity of 10% or more. In addition, in the method for producing a dehydrogenated compound of the sixth embodiment, it is preferred that the generation of isobutylene is small, so the selectivity of isobutylene in the method for producing a dehydrogenated compound of the sixth embodiment during stable operation is preferably 60% or less, and more preferably 50% or less.
[0113] The isobutanol used as the starting material is not particularly limited, but isobutanol derived from biomass is preferred from the viewpoint of environmental protection. The isobutanol used as the starting material may be a mixture of isobutanol derived from fossils and isobutanol derived from biomass.
[0114] "Isobutanol from biomass" refers to isobutanol obtained by purifying organic compounds obtained through a fermentation process using fermentable sugars from biomass, or isobutanol obtained by a process including catalytic chemical conversion and thermochemical conversion of biomass. Biomass can be roughly divided into biomass from resource crops and biomass from waste. Examples of biomass from resource crops include edible crops, wood, and flowers, and unused portions of these crops may also be used. Examples of biomass from waste include food waste and sewage sludge, livestock feces, and waste paper.
[0115] The dehydrogenation reaction of isobutanol can be carried out in a liquid phase or in a gas phase. When the reaction is carried out in a gas phase, a fixed bed or a fluidized bed can be used. The following describes the case where the reaction is carried out in a gas phase, but the present invention is not limited thereto.
[0116] For example, by using an evaporator to evaporate the raw material, it can be supplied to the reactor as raw material gas. As an evaporator, there is no particular limitation, and examples thereof include a sleeve type, a natural circulation horizontal tube type, a natural circulation immersed tube type, a natural circulation vertical short tube type, a vertical long tube ascending film type, a horizontal tube descending film type, a forced circulation horizontal tube type, a forced circulation vertical tube type, and a coil type. In addition, the following method can also be used: only a heating coil is wound around the raw material supply piping, and the raw material moving in the raw material supply piping is evaporated in the raw material supply piping before being placed in the reactor, and is supplied to the reactor in a gaseous state. The evaporator is also not particularly limited in the case of evaporating components other than the raw material such as a dilution gas and supplying them to the reactor.
[0117] The conditions for gasifying the raw material are not particularly limited. For example, the temperature may be 108° C. to 600° C., and the pressure may be 0.05 MPa to 1 MPa in terms of absolute pressure.
[0118] The isobutyl alcohol concentration can be adjusted by diluting the isobutyl alcohol in the raw material gas with the diluent gas. The raw material gas may be a gas consisting only of isobutyl alcohol.
[0119] As diluent gas, as long as the dehydrogenation reaction of isobutanol is not affected, for example, air, nitrogen, helium, neon, krypton, xenon, radon, argon, methane, ethane, propane, butane, isobutane, carbon monoxide, carbon dioxide, nitrogen monoxide, nitrogen dioxide, nitrous oxide, nitrogen trioxide, nitrogen tetroxide, nitrogen pentoxide and water vapor etc. can be enumerated. If it is the scope that does not promote side reaction, then hydrogen can also be used as diluent gas. The diluent gas included in the raw gas can be 1 kind, can also be 2 or more kinds. Water can also be included in the raw gas.
[0120] The lower limit of the isobutyl alcohol concentration in the raw material gas is not particularly limited, but is preferably 0.1% by volume or more relative to the total volume of the raw material gas. The upper limit is not particularly limited, but is 100% by volume or less.
[0121] When water vapor is supplied to the reactor, the lower limit of the water vapor concentration in the raw material gas is preferably 2.5% by volume or more, more preferably 5.0% by volume or more, further preferably 10.0% by volume or more, particularly preferably 15.0% by volume or more, and most preferably 20.0% by volume or more, relative to the total volume of the raw material gas. The upper limit of the water vapor concentration in the raw material gas is preferably 80.0% by volume or less, more preferably 75.0% by volume or less, further preferably 70.0% by volume or less, particularly preferably 65.0% by volume or less, and most preferably 60.0% by volume or less.
[0122] The lower limit of the reaction temperature (temperature of the catalyst layer during the reaction) for the dehydrogenation reaction of isobutyl alcohol is preferably 320°C or more, more preferably 340°C or more, further preferably 360°C or more, and particularly preferably 380°C or more. The upper limit of the reaction temperature is preferably 600°C or less, more preferably 580°C or less, further preferably 560°C or less, particularly preferably 540°C or less, particularly preferably 520°C or less, and most preferably 500°C or less. If the reaction temperature is moderately high, the successive dehydrogenation reaction from isobutylaldehyde to methacrolein can be promoted. In addition, there is no need to increase the amount of catalyst or reduce the supply rate of the raw material gas, which is also advantageous from the viewpoint of cost and productivity.
[0123] The reaction temperature is the lowest temperature among the temperatures of the catalyst layer in the reactor that can be confirmed after the reaction becomes a stable state. Therefore, when the catalyst layer has a temperature distribution, it is preferred to increase the measurement points, or to continuously measure the temperature in the catalyst filling direction. The control method of the reaction temperature is not particularly limited, and a known method can be used.
[0124] The reaction pressure of the dehydrogenation reaction of isobutanol is not particularly limited, but is preferably 0.050 MPa or more in absolute pressure.
[0125] The upper limit of the reaction pressure is not particularly limited, but is preferably 10.0 MPa or less.
[0126] The reaction pressure refers to a value measured by a pressure sensor installed at a position where the influence of pressure loss with respect to the pressure at the inlet of the reactor is negligible.
[0127] [Method for producing methacrylic acid from isobutylaldehyde and / or methacrolein]
[0128] The method for producing methacrylic acid of the present invention is a method for producing methacrylic acid using isobutylaldehyde produced by the above-mentioned method for producing isobutylaldehyde, and can produce methacrylic acid from isobutylaldehyde with a high selectivity.
[0129] As the catalyst used for producing methacrylic acid from isobutylaldehyde and / or methacrolein, a known catalyst can be used, and examples thereof include a catalyst containing a heteropoly acid composed of molybdenum and phosphorus, and iron phosphate.
[0130] In the reactor for producing methacrylic acid, a fixed bed can be used. The catalyst layer for the second stage oxidation reaction is not particularly limited, and may be a non-dilution layer containing only the catalyst for the second stage oxidation reaction, or may be a dilution layer containing no inert carrier. In addition, the catalyst layer for the second stage oxidation reaction may be a single layer or a mixed layer consisting of a plurality of layers.
[0131] It is economical to use air as a molecular oxygen source used in the reaction of producing methacrylic acid from isobutylaldehyde and / or methacrolein, but air enriched with pure oxygen may be used as necessary.
[0132] Water (water vapor) may be added to the reaction gas in the reaction of producing methacrylic acid from isobutylaldehyde and / or methacrolein in addition to isobutylaldehyde and / or methacrolein and molecular oxygen.
[0133] The reaction gas in the reaction of producing methacrylic acid from isobutylaldehyde and / or methacrolein may contain a small amount of impurities such as lower saturated aldehydes, but the amount is preferably as small as possible. In addition, the reaction gas in the reaction of producing methacrylic acid from isobutylaldehyde and / or methacrolein may contain inert gases such as nitrogen and carbon dioxide.
[0134] [Method for producing methacrylate]
[0135] The method for producing methacrylic acid ester of the present invention is a method for producing methacrylic acid ester using methacrylic acid produced by the above-mentioned method for producing methacrylic acid.
[0136] The method for producing methacrylic acid ester of the present invention comprises a step of producing methacrylic acid by the above-mentioned method for producing methacrylic acid and a step of producing methacrylic acid ester by esterification reaction of methacrylic acid with an alcohol having 1 to 20 carbon atoms. According to this method, methacrylic acid ester can be produced from isobutylaldehyde and / or methacrolein with high selectivity.
[0137] For example, methacrylic acid produced by the above-mentioned production method is recovered by extraction, distillation operation or the like, and then subjected to an esterification reaction with methanol in the presence of an acid catalyst.
[0138] Examples of the alcohol having 1 to 20 carbon atoms include aliphatic alcohols such as methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol and eicosanol; and aromatic alcohols such as benzyl alcohol.
[0139] The esterification reaction preferably uses a catalyst. As the catalyst used, an acid catalyst is preferably used, and sulfuric acid and ion exchange resins can be used. As the ion exchange resin, a strongly acidic cation exchange resin is preferably used. As specific examples of strongly acidic cation exchange resins, for example, Diaion (registered trademark), PK216, RCP12H (Mitsubishi Chemical Corporation), Lewatit (registered trademark), K2431 (Bayer Corporation), Amberlyst (registered trademark) 15WET (Rohm and Haas Japan Corporation) and the like can be cited. These can be used alone or in combination of two or more.
[0140] The flow direction of the reaction fluid in the esterification reaction may be either vertically upward or vertically downward, and may be appropriately selected. When the swelling of the ion exchange resin used as the acid catalyst for the esterification reaction is large, the flow direction of the reaction fluid is preferably vertically upward. When the reaction fluid forms a heterogeneous phase, the flow direction of the reaction fluid is preferably vertically downward.
[0141] When the esterification reaction is carried out by filling the fixed bed type reactor with an ion exchange resin, the flow rate of the raw material containing methacrylic acid and the alcohol having 1 to 20 carbon atoms is preferably 0.10 times or more, more preferably 0.20 times or more, in terms of the mass ratio relative to the amount of the ion exchange resin. In addition, the flow rate of the raw material is preferably 10.0 times or less, more preferably 5.0 times or less, in terms of the mass ratio relative to the amount of the ion exchange resin.
[0142] When a strongly acidic cation exchange resin is used as an acid catalyst, the reaction temperature of the esterification reaction is preferably 40° C. to 130° C. The higher the reaction temperature, the faster the reaction rate, and the more effectively the reaction can be carried out. The lower the reaction temperature, the slower the deterioration rate of the ion exchange resin, and the longer the esterification reaction can be continuously carried out. From the viewpoint of chemical equilibrium, the reaction temperature of the esterification reaction can be appropriately determined to be the optimal temperature.
[0143] From the viewpoint of chemical balance, the raw material composition can be simplified by increasing the concentration of either methacrylic acid or the alcohol having 1 to 20 carbon atoms to increase the conversion rate of the raw material with the lower concentration, thereby simplifying the recovery and purification process.
[0144] As described above, the present invention uses catalysts (A) and (B) to efficiently produce isobutylaldehyde and methacrolein from isobutyl alcohol while suppressing oxidation and bimolecularization of isobutylaldehyde without requiring reduction treatment with hydrogen.
[0145] Example
[0146] Hereinafter, the present invention will be specifically described using examples, but the present invention is not limited to the following description.
[0147] [Conversion rate and opt-in rate]
[0148] The raw material gas and the product were analyzed using gas chromatography. The conversion rate of isobutanol and the selectivity of each product were defined as follows.
[0149] Conversion rate of isobutanol (%) = (b / a) × 100
[0150] W / F = the amount of isobutanol supplied to the reactor (unit: g / h) ÷ the mass of the catalyst filled in the reaction tube (unit: g)
[0151] Isobutyraldehyde selectivity (%) = (c / b) × 100
[0152] Methacrolein selectivity (%) = (d / b) × 100
[0153] Selectivity of isobutyric acid (%) = (e / b) × 100
[0154] Selectivity of C4 butenes (%) = (f / b) × 100
[0155] Propylene selectivity (%) = (g / b) × 100
[0156] Selectivity of propionaldehyde (%) = (h / b) × 100
[0157] Ketone selectivity (%) = [(i / b) + (j / b)] × 100
[0158] Selectivity of cyclic compound (%) = [(k / b) + (l / b) + (m / b)] × 100
[0159] COx (CO and CO 2 ) selection rate (%) = (n / b) × 100
[0160] Coke selectivity (%) = (o / b) × 100
[0161] Selectivity of unknown substances (%) = 100 - selectivity of isobutyraldehyde - selectivity of methacrolein - selectivity of isobutyric acid - selectivity of C4 butenes - selectivity of propylene - selectivity of propionaldehyde - selectivity of ketones - selectivity of cyclic compounds - selectivity of COx - selectivity of coke
[0162] In addition, the symbols in the above formula have the following meanings.
[0163] a: Number of moles of isobutanol supplied / 4
[0164] b: Number of moles of isobutanol reacted / 4
[0165] c: Number of moles of isobutyraldehyde generated / 4
[0166] d: Number of moles of methacrolein generated / 4
[0167] e: number of moles of isobutyric acid generated / 4
[0168] f: Number of moles of C4 butenes (isobutylene, 1-butene, trans-2-butene and cis-2-butene) produced / 4
[0169] g: number of moles of propylene produced / 3
[0170] h: number of moles of propionaldehyde generated / 3
[0171] i: (the number of moles of 2-methyl-3-pentanone produced / 6 + the number of moles of 3-methyl-2-butanone produced / 5
[0172] j: Number of moles of ketone 2(3-pentanone) generated / 5
[0173] k: Number of moles of generated cyclic compound 1 (methylcyclopentenone) / 6
[0174] l: Number of moles of generated cyclic compound type 2 (dimethylcyclopentanone and dimethylcyclopentenone) / 7
[0175] m: Number of moles of generated cyclic compound 3 (trimethylcyclopentanone and trimethylcyclopentenone) / 8
[0176] n: Number of moles of carbon monoxide and carbon dioxide produced / 1
[0177] o: Number of moles of coke produced / 1
[0178] Isobutyraldehyde + methacrolein yield = (isobutyraldehyde selectivity + methacrolein selectivity) × isobutanol conversion rate ÷ 100
[0179] [Analysis method of acid amount of catalyst]
[0180] The acid amount of the catalyst was measured using BELCAT (manufactured by Microtrac BEL).
[0181] After the catalyst was placed in a measuring cell, it was pre-treated at 550°C for 1 hour while He was flowing at 50 cc / min. After the pre-treatment, the cell was cooled to 100°C and 1.0 vol% NH 3 A mixed gas of NH and 99.0 volume % He was circulated at 50 cc / min for 1 hour to make NH 3 Then, while He as a carrier was flowing at 30 cc / min and stabilizing, the temperature was raised to 800°C at 10°C / min, and NH 3 The amount of acid released was calculated from the following formula.
[0182] Acid amount on catalyst (mmol / g) = NH 3 The amount of desorption (mmol) ÷ the weight of the catalyst placed in the measuring cell (g)
[0183] [Analysis method of the amount of base in the catalyst]
[0184] The alkali content of the catalyst was measured using BELCATII (manufactured by Microtrac BEL). After the catalyst was placed in the measuring cell, it was pre-treated at 550°C for 1 hour while He was flowing at 50 cc / min. After the pre-treatment, the cell was cooled to 50°C and 2.9% by volume of CO was added. 2 A mixed gas of 97.1% by volume of Ar was flowed at 50 cc / min for 1 hour to make CO 2 Then, while He as a carrier was flowing at 30 cc / min, the temperature was raised to 800°C at 10°C / min, and CO was measured. 2 The amount of alkali removed was calculated by the following formula.
[0185] Base amount on catalyst (mmol / g) = CO 2 The amount of desorption (mmol) ÷ the weight of the catalyst placed in the measuring cell (g)
[0186] [Analysis method of BET specific surface area of catalyst]
[0187] The catalyst placed in the measuring cell was heated in vacuum at 300°C overnight, and then the nitrogen adsorption isotherm at liquid nitrogen temperature (77K) was measured using BELSORP-mini (manufactured by Microtrac BEL). The nitrogen adsorption isotherm obtained was analyzed using the BET method to calculate the BET specific surface area (m 2 / g).
[0188] [Evaluation method of coke deposition amount after reaction evaluation]
[0189] The catalyst after the reaction was extracted from the reaction tube and pulverized into uniform fine powder. The powder was placed in a measuring cell and the carbon deposition amount was measured using an organic trace element analyzer (Micro corder JM10 manufactured by J-SCIENCE). The coke deposition amount was calculated from the following formula.
[0190] Coke precipitation amount (C-mol) = catalyst filling amount × carbon concentration obtained by analysis (mass %) ÷ 100 ÷ 12.01 (g / mol)
[0191] [Example 1]
[0192] (Preparation of Dehydrogenation Catalyst)
[0193] 1.9 g of zirconium oxynitrate dihydrate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was added to 70 mL of distilled water (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.), and stirred until completely dissolved to prepare Liquid A.
[0194] 45 g of iron (III) nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to 600 mL of distilled water and stirred until completely dissolved to obtain liquid B. 60 mL of distilled water was added to 40 mL of ammonia water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) to obtain liquid C.
[0195] Liquid A was added to liquid B and stirred for 30 minutes. Then, liquid C was added dropwise until the pH reached about 7 and stirred for 1 hour. The obtained precipitate was separated by suction filtration for 24 hours and dried at 110°C overnight. The obtained solid was crushed in a mortar and calcined at 500°C in air for 2 hours.
[0196] After calcination, the mixture was further finely pulverized in a mortar to obtain ZrO 2 (7) -FeOx. The numbers in parentheses represent the content (mol%) of each component. The content of FeOx is 93 mol%.
[0197] 0.60 g of potassium nitrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 3.0 mL of distilled water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) to prepare a potassium nitrate aqueous solution. 2 (7)-FeOx is evenly dripped with potassium nitrate aqueous solution and stirred for 15 minutes. After drying at 25°C for 24 hours, it is dried in a vacuum dryer at 40°C for 2 hours, dried at 60°C for 2 hours, and dried in a dryer at 110°C for 24 hours. After drying, it is ground in a mortar and calcined in a calcining furnace at 550°C in air for 12 hours. After calcination, it is ground again in a mortar and pressed into a tablet forming machine at 2.0 tons for 15 minutes to form a sheet. A sieve is used to obtain K(5) / ZrO with a particle size of 300 to 850 μm. 2 (6.7)-FeOx(88.3)(catalyst (abbreviation): B-1, average electronegativity: 2.55).
[0198] The numbers in parentheses represent the content (mol%) of each component. In addition, the acid content of catalyst B-1 is 0.004 mmol / g, the base content is 0.187 mmol / g, and the BET specific surface area is 30 m 2 / g.
[0199] (Catalyst Performance Evaluation)
[0200] 1.1 g of catalyst B-1 was filled into a vertical tubular reaction tube to form a catalyst layer. In the reactor, the temperature of the catalyst layer was adjusted using an electric furnace so that the temperature of the catalyst layer reached a specified temperature. Isobutanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., specific gravity 0.80 g / mL) and pure water were adjusted to 1.9 mL / hour and 2.0 mL / hour, respectively, using a cylinder pump, and supplied to an evaporator set at 150°C for evaporation. Nitrogen as a dilution gas was supplied to the evaporator at a flow rate of 1140 mL (standard state) / hour using a mass flow meter, and supplied to the reactor together with the evaporated isobutanol. The isobutanol concentration in the raw gas supplied to the catalyst layer was 11.4% by volume, and W / F was 0.70 h / h. -1 The temperature of the catalyst layer during the reaction (reaction temperature) was 450° C. A pressure gauge for measuring the reaction pressure was installed between the evaporator and the reactor inlet. The reaction pressure was atmospheric pressure.
[0201] After the reaction reached a steady state, the gas at the reactor outlet was collected and analyzed using a gas chromatograph (GC-8A, Shimadzu Corporation) for propylene, isobutylene, 1-butene, cis-2-butene, trans-2-butene, CO and CO 2 In addition, the reaction gas discharged from the reactor outlet side was passed into an ice-cold trap for collection, and isobutanol, isobutyraldehyde, isobutyric acid, 2,4-dimethyl-3-pentanone, methacrolein, propionaldehyde, 2-methyl-3-pentanone, 3-methyl-2-butanone, 3-pentanone, dimethylcyclopentanone, dimethylcyclopentenone, methylcyclopentenone, trimethylcyclopentanone, and trimethylcyclopentane were quantitatively determined using a gas chromatograph (manufactured by Shimadzu Corporation, GC-2014, internal standard: isopropanol).
[0202] [Example 2]
[0203] 4.9 g of aluminum nitrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to 170 mL of distilled water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and stirred until completely dissolved. The obtained solution was referred to as liquid A. Al as a composite oxide was obtained in the same manner as in Example 1. 2 O 3 (7)-FeOx. In addition to using Al 2 O 3 (7)-FeOx, K(5) / Al was obtained in the same manner as in Example 1 2 O 3 (6.7)-FeOx(88.3)(catalyst (abbreviation): B-2, average electronegativity: 2.56). The numbers in parentheses represent the content (mol%) of each component. In addition, the acid content of catalyst B-2 is 0.000 mmol / g, and the base content is 0.268 mmol / g.
[0204] The catalyst performance was evaluated in the same manner as in Example 1 except that 1.1 g of the catalyst B-2 was used instead of the catalyst B-1.
[0205] [Example 3]
[0206] γ-alumina (manufactured by Strem Chemicals Inc.) was calcined in air at 550°C for 12 hours using an electric furnace as a pretreatment. 0.60 g of potassium nitrate (manufactured by Fujifilm Wako Pure Chemicals Co., Ltd.) was dissolved in 4.0 mL of distilled water (manufactured by Fujifilm Wako Pure Chemicals Co., Ltd.) to prepare an aqueous potassium nitrate solution. The aqueous potassium nitrate solution was evenly dropped onto 4.0 g of the pretreated alumina that was taken out into a mortar, and stirred for 15 minutes. After drying at 25°C for 24 hours, it was dried at 40°C for 2 hours using a vacuum dryer, dried at 60°C for 2 hours, and dried at 110°C for 24 hours using a dryer. After the drying treatment, it was ground in a mortar and calcined in air at 550°C for 12 hours using a calcining furnace. After calcination, it was ground again in a mortar and pressed into a sheet shape using a tablet forming machine at 2 tons for 15 minutes, and a particle size of 300 to 850 μm of K(5) / Al was prepared using a sieve. 2 O 3 (Catalyst (abbreviation): B-3, average electronegativity: 2.48). The numbers in brackets represent the ratio of the supported metal element in the catalyst to the atomic weight of Al (mol%). In addition, the acid content of catalyst B-3 is 0.079 mmol / g, the base content is 0.439 mmol / g, and the BET specific surface area is 173 m 2 / g.Al 2 O 3 The content rate is 95 mol%.
[0207] The catalyst performance was evaluated in the same manner as in Example 1 except that 1.1 g of Catalyst B-3 was used instead of Catalyst B-1.
[0208] The reaction conditions and evaluation results of Examples 1 to 3 are shown in Table 1. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 1. Figure 1 .
[0209] [Table 1]
[0210]
[0211] As shown in Table 1 and Figure 1 As shown, the catalysts having an average electronegativity falling within the range of 2.1 to 2.8 produced isobutylaldehyde and methacrolein without undergoing hydrogen reduction.
[0212] [Example 5]
[0213] The catalyst performance was evaluated in the same manner as in Example 1 except as shown below. 1.1 g of catalyst B-3 was used instead of catalyst B-1. No water was supplied to the reactor, the flow rate of isobutanol supplied to the reactor was adjusted to 1.9 mL / hour, and the reaction temperature was set to 500°C. The flow rate of nitrogen was set to 3660 mL (standard state) / hour. The isobutanol concentration in the raw gas supplied to the catalyst layer was 11.4% by volume, and the W / F was 0.70 h / h. -1 The temperature of the catalyst layer during the reaction (reaction temperature) was 500°C.
[0214] [Example 6]
[0215] 6.0 g of titanium oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of ZrO 2 (7)-FeOx, except that potassium was loaded in the same manner as in Example 1 to prepare K(5) / TiO 2 (Catalyst (abbreviation): B-4, average electronegativity: 2.59). The numbers in brackets represent the ratio of the supported metal element in the catalyst to the atomic weight of Ti (mol%). In addition, the acid content of catalyst B-4 is 0.002 mmol / g, the base content is 0.022 mmol / g, and the BET specific surface area is 13 m 2 / g.TiO 2 The content rate is 95 mol%.
[0216] The catalyst performance was evaluated in the same manner as in Example 5 except that 1.1 g of Catalyst B-4 was used instead of Catalyst B-3.
[0217] [Example 7]
[0218] BEA type zeolite (manufactured by Tosoh Corporation, SiO 2 / Al 2 O 3 =500, HSZ-980HOA) was calcined in air at 550°C in an electric furnace for 12 hours as a pretreatment. 6.1 g of potassium nitrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 100 mL of distilled water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) to prepare an aqueous potassium nitrate solution. The pretreated BEA-type zeolite was added thereto, stirred at 70°C for 3 hours using a stirrer, and the solid component was recovered by centrifugal separation. This operation was repeated 3 times. Next, the recovered solid component was washed with distilled water, and the solid component was recovered by centrifugal separation. This washing operation was repeated 2 times. Furthermore, the solid component was washed with 2-propanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and the solid component was recovered by centrifugal separation.
[0219] The recovered solid component was calcined in air at 550° C. for 12 hours using an electric furnace to prepare K-BEA in which potassium was supported on zeolite.
[0220] Dissolve 0.65 g of potassium nitrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) in 3.0 mL of distilled water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) to prepare an aqueous potassium nitrate solution. Add the aqueous potassium nitrate solution evenly to 5.0 g of K-BEA taken out in a mortar and stir for 15 minutes. Dry at 25°C for 24 hours, dry at 40°C for 2 hours using a vacuum dryer, dry at 60°C for 2 hours, and dry at 110°C for 24 hours using a dryer. Repeat this operation twice. Then, grind it in a mortar and calcine it in a calcining furnace at 550°C in air for 12 hours. After calcination, grind it again in a mortar, press it at 2 tons for 15 minutes using a tablet forming machine to form a sheet, and use a sieve to prepare K(10) / K-BEA (catalyst (abbreviation): B-5, average electronegativity: 2.78) with a particle size of 300 to 850 μm. The numbers in parentheses represent the ratio (mol%) of the supported metal element in the catalyst to the Si atomic weight. In addition, the acid content of catalyst B-5 was 0.000 mmol / g, and the base content was 0.005 mmol / g.
[0221] The catalyst performance was evaluated in the same manner as in Example 5 except that 1.1 g of catalyst B-5 was used instead of catalyst B-3.
[0222] The reaction conditions and evaluation results of Examples 5 to 7 are shown in Table 2. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 2. Figure 2 .
[0223] [Table 2]
[0224]
[0225] As shown in Table 2 and Figure 2 As shown, in Examples 5 to 7 using Catalysts B-3 to 5 in which an alkali metal is supported on alumina, titania or zeolite, the selectivity for isobutylaldehyde and methacrolein is high.
[0226] [Example 8]
[0227] The catalyst performance was evaluated in the same manner as in Example 1 except as shown below. 1.1 g of catalyst B-3 was used instead of catalyst B-1. The flow rates of isobutanol and water supplied to the reactor were 1.9 mL / hour and 1.0 mL / hour, respectively, the flow rate of nitrogen was 2400 mL (standard state) / hour, and the reaction temperature was 500°C. The isobutanol concentration in the raw gas supplied to the catalyst layer was 11.4% by volume, the water concentration was 29.6% by volume, and the W / F was 0.70 h / min.-1 The temperature of the catalyst layer during the reaction (reaction temperature) was 500°C.
[0228] [Example 9]
[0229] Catalyst A-1 was calcined at 700° C. for 12 hours in an electric furnace, and then loaded with potassium in the same manner as in Example 1 to prepare K(5) / Al as a dehydrogenation catalyst. 2 O 3 -700°C (catalyst (abbreviation): B-6, average electronegativity: 2.48). The numbers in parentheses represent the ratio (mol%) of the supported metal element in the catalyst to the atomic weight of Al. 2 O 3 The content rate is 95 mol%.
[0230] The catalyst performance was evaluated in the same manner as in Example 7 except that 1.1 g of catalyst B-6 was used instead of catalyst B-3.
[0231] [Example 10]
[0232] K(5) / SA63158 (catalyst (abbreviation): B-7, average electronegativity: 2.48) was prepared as a dehydrogenation catalyst by using γ-alumina (Saint-Gobain SA63158) in the same manner as in Example 1 except that potassium was supported. The numbers in parentheses represent the ratio (mol%) of the supported metal element in the catalyst relative to the atomic weight of Al. The content of γ-alumina was 95 mol%.
[0233] The catalyst performance was evaluated in the same manner as in Example 7 except that 1.0 g of Catalyst B-7 was used instead of Catalyst B-3.
[0234] The reaction conditions and evaluation results of Examples 8 to 10 are shown in Table 3. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 3. Figure 3 .
[0235] [Table 3]
[0236]
[0237] As shown in Table 3 and Figure 3 As shown, in Examples 8 to 10 using Catalysts B-3 and 6 to 7 in which an alkali metal is supported on various aluminas, the selectivity of isobutylaldehyde and methacrolein is high.
[0238] [Example 11]
[0239] As an alumina carrier, a reference catalyst of the Catalyst Society (JRC-ALO5) was used. In addition, potassium was loaded in the same manner as in Example 1 to prepare K(5) / AL05 (catalyst (abbreviation): B-8, average electronegativity: 2.48) as a dehydrogenation catalyst. The numbers in brackets represent the ratio of the loaded metal element in the catalyst to the atomic weight of Al (mol%). The BET specific surface area is 197 m 2 / g. The content of JRC-ALO5 was 95 mol%.
[0240] The catalyst performance was evaluated in the same manner as in Example 1 except that 1.0 g of Catalyst B-8 was used instead of Catalyst B-1 and the reaction temperature was set to 500°C.
[0241] [Example 12]
[0242] As an alumina carrier, a reference catalyst of the Catalyst Society (JRC-ALO8) was used. In addition, potassium was loaded in the same manner as in Example 1 to prepare K(5) / AL08 (catalyst (abbreviation): B-9, average electronegativity: 2.48) as a dehydrogenation catalyst. The numbers in brackets represent the ratio of the loaded metal element in the catalyst to the atomic weight of Al (mol%). The BET specific surface area is 158 m 2 / g. The content of JRC-ALO8 was 95 mol%.
[0243] The catalyst performance was evaluated in the same manner as in Example 1 except that 1.0 g of catalyst B-9 was used instead of catalyst B-1.
[0244] [Example 13]
[0245] The catalyst performance was evaluated in the same manner as in Example 11 except that 1.1 g of Catalyst B-3 was used instead of Catalyst B-9.
[0246] The reaction conditions and evaluation results of Examples 11 to 13 are shown in Table 4. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 4. Figure 4 .
[0247] [Table 4]
[0248]
[0249] As shown in Table 4 and Figure 4 As shown, in Examples 11 to 13 using Catalysts B-3 and 8 to 9 in which an alkali metal is supported on various aluminas, the selectivity of isobutylaldehyde and methacrolein is high.
[0250] [Example 14]
[0251] γ-alumina (manufactured by Strem Chemicals Inc.) was calcined in air at 550°C for 12 hours using an electric furnace as a pretreatment. 0.89 g of potassium nitrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 4.0 mL of distilled water to prepare an aqueous potassium nitrate solution. The aqueous potassium nitrate solution was evenly dropped onto 6.0 g of the pretreated alumina taken out into a mortar and stirred for 15 minutes. After drying at 25°C for 24 hours, it was dried at 40°C for 2 hours using a vacuum dryer, dried at 60°C for 2 hours, and dried at 110°C for 24 hours using a dryer. After the drying treatment, it was ground in a mortar and calcined in air at 550°C for 12 hours using a calcining furnace. After calcination, it was ground again in a mortar and pressed into sheets using a tablet former at 2 tons for 15 minutes, and a K(7.5) / Al with a particle size of 300 to 850 μm was prepared using a sieve. 2 O 3 (Catalyst B-10). The numbers in parentheses represent the ratio of the supported metal element in the catalyst to the atomic weight of Al (mol%). In addition, the acid content of Catalyst L is 0.040 mmol / g, the base content is 0.590 mmol / g, and the BET specific surface area is 159 m 2 / g.Al 2 O 3 The content rate is 92.5 mol%.
[0252] 1.1 g of catalyst B-10 was used instead of catalyst B-3, the flow rate of isobutyl alcohol supplied to the reactor was adjusted to 1.9 mL / hour, and the reaction temperature was set to 500°C. The flow rate of nitrogen was set to 1140 mL (standard state) / hour, and the isobutyl alcohol concentration in the raw gas supplied to the catalyst layer was set to 28.8% by volume, and the W / F was set to 0.70 h -1 The catalyst performance was evaluated in the same manner as in Example 1 except for the above.
[0253] [Example 15]
[0254] γ-alumina (manufactured by Strem Chemicals Inc.) was calcined in air at 550°C for 12 hours using an electric furnace as a pretreatment. 0.89 g of potassium nitrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 4.0 mL of distilled water to prepare an aqueous potassium nitrate solution. The aqueous potassium nitrate solution was evenly dropped onto 6.0 g of the pretreated alumina taken out into a mortar and stirred for 15 minutes. After drying at 25°C for 24 hours, it was dried at 40°C for 2 hours using a vacuum dryer, dried at 60°C for 2 hours, and dried at 110°C for 24 hours using a dryer. After the drying treatment, it was ground in a mortar and calcined in air at 850°C for 12 hours using a calcining furnace. After calcination, it was ground again in a mortar and formed into sheets using a tablet former at 2 tons for 15 minutes, and a K(7.5) / Al with a particle size of 300 to 850μm was prepared using a sieve. 2 O 3 -850°C (Catalyst B-11). The numbers in parentheses represent the ratio (mol%) of the supported metal element to the atomic weight of Al in the catalyst. 2 O 3 The content rate is 92.5 mol%.
[0255] The catalyst performance was evaluated in the same manner as in Example 14 except that 1.1 g of catalyst B-11 was used instead of catalyst B-10.
[0256] [Example 16]
[0257] K(7.5) / Al was prepared by the same method as in Example 14 except that 0.58 g of potassium acetate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used as the potassium raw material. 2 O 3 (Catalyst B-12) was used as a dehydrogenation catalyst. The numbers in parentheses represent the ratio of the supported metal element in the catalyst to the atomic weight of Al (mol%). In addition, the acid content of Catalyst N was 0.030 mmol / g, the base content was 0.650 mmol / g, and the BET specific surface area was 177 m 2 / g.Al 2 O 3 The content rate is 92.5 mol%.
[0258] The catalyst performance was evaluated in the same manner as in Example 14 except that 1.1 g of catalyst B-12 was used instead of catalyst B-10.
[0259] The reaction conditions and evaluation results of Examples 14 to 16 are shown in Table 5. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 5. Figure 5 .
[0260] [Table 5]
[0261]
[0262] As shown in Table 5 and Figure 5 As shown, in Examples 14 to 16 in which calcination was performed after potassium loading or the potassium precursor was changed in catalyst preparation, the selectivity of isobutyraldehyde and methacrolein was high.
[0263] [Example 17]
[0264] Na(5) / Al was prepared in the same manner as in Example 3 except that 0.50 g of sodium nitrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the raw material of the alkali metal. 2 O 3 (catalyst (abbreviation): B-13, average electronegativity: 2.49) as a dehydrogenation catalyst. The numbers in brackets represent the ratio of the supported metal element in the catalyst to the atomic weight of Al (mol%). In addition, the acid content of catalyst B-13 is 0.111 mmol / g, and the base content is 0.373 mmol / g. The BET specific surface area is 170 m 2 / g.Al 2 O 3 The content rate is 95 mol%.
[0265] The catalyst performance was evaluated in the same manner as in Example 8 except that 1.1 g of catalyst B-13 was used instead of catalyst B-3.
[0266] [Example 18]
[0267] Rb(5) / Al was prepared in the same manner as in Example 3 except that 0.89 g of rubidium nitrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the raw material of the alkali metal. 2 O 3 (catalyst (abbreviation): B-14, average electronegativity: 2.48) as a dehydrogenation catalyst. The numbers in brackets represent the ratio of the supported metal element in the catalyst to the atomic weight of Al (mol%). In addition, the acid content of catalyst B-14 is 0.056 mmol / g, and the base content is 0.431 mmol / g. The BET specific surface area is 162 m 2 / g.Al 2 O 3 The content rate is 95 mol%.
[0268] The catalyst performance was evaluated in the same manner as in Example 8 except that 1.1 g of catalyst B-14 was used instead of catalyst B-3.
[0269] [Example 19]
[0270] Cs(5) / Al was prepared in the same manner as in Example 7 except that 1.1 g of cesium nitrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the raw material of the alkali metal. 2 O 3 (catalyst (abbreviation): B-15, average electronegativity: 2.48) as a dehydrogenation catalyst. The numbers in brackets represent the ratio of the supported metal element in the catalyst to the atomic weight of Al (mol%). In addition, the acid content of catalyst B-15 is 0.046 mmol / g, and the base content is 0.437 mmol / g. The BET specific surface area is 157 m 2 / g.Al 2 O 3 The content rate is 95 mol%.
[0271] The catalyst performance was evaluated in the same manner as in Example 8 except that 1.1 g of Catalyst B-15 was used instead of Catalyst B-3.
[0272] The reaction conditions and evaluation results of Examples 8 and 17 to 19 are shown in Table 6. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 6. Figure 6 .
[0273] [Table 6]
[0274]
[0275] As shown in Table 6 and Figure 6 As shown, in Examples 8 and 17 to 19 using Catalysts B-3 and 13 to 15 supporting an alkali metal other than potassium, the selectivity of isobutylaldehyde and methacrolein was high.
[0276] [Example 20]
[0277] 1.1 g of magnesium oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., acid content: 0.000 mmol / g, base content: 0.030 mmol / g, BET specific surface area: 8.0 m 2 / g, average electronegativity: 2.12) was used as catalyst (abbreviated as A-2), and the catalyst performance was evaluated in the same manner as in Example 5 except for the above.
[0278] [Example 21]
[0279] 0.5 g of catalyst B-13 (acid amount: 0.111 mmol / g, base amount: 0.373 mmol / g, BET specific surface area: 170 m 2 / g, average electronegativity: 2.49), the catalyst performance was evaluated in the same manner as in Example 5 except that the flow rate of isobutanol supplied to the reactor was 0.95 mL / hour and the flow rate of nitrogen was 1800 mL (standard state) / hour.
[0280] [Example 22]
[0281] 1.1 g of catalyst B-3 (acid amount: 0.079 mmol / g, base amount: 0.439 mmol / g, BET specific surface area: 173 m 2 / g, average electronegativity: 2.48), and the catalyst performance was evaluated in the same manner as in Example 5, except for the above.
[0282] [Example 23]
[0283] 1.1 g of catalyst B-14 (acid amount: 0.056 mmol / g, base amount: 0.431 mmol / g, BET specific surface area: 162 m 2 / g, average electronegativity: 2.48), and the catalyst performance was evaluated in the same manner as in Example 5, except for the above.
[0284] [Example 24]
[0285] 1.1 g of catalyst B-15 (acid content: 0.046 mmol / g, base content: 0.437 mmol / g, BET specific surface area: 157 m 2 / g, average electronegativity: 2.48), and the catalyst performance was evaluated in the same manner as in Example 5, except for the above.
[0286] The reaction conditions and evaluation results of Examples 20 to 24 are shown in Tables 7A and 7B. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Tables 7A and 7B. Figure 7 .
[0287] [Table 7A]
[0288]
[0289] [Table 7B]
[0290]
[0291] As shown in Table 7A, Table 7B and Figure 7 As shown, when catalysts A-2, B-3, and 14 to 15 having an average electronegativity falling within the range of 2.1 to 2.8 are used, the catalysts are not subjected to hydrogen reduction, and the selectivity for isobutylaldehyde and methacrolein is high.
[0292] [Example 25]
[0293] The catalyst performance was evaluated in the same manner as in Example 1 except for the following. The reaction tube was filled with catalyst A-2 (acid amount: 0.000 mmol / g, base amount: 0.030 mmol / g, BET specific surface area: 8.0 m 2 / g, average electronegativity: 2.12) 1.1g, to form a catalyst layer. No water is supplied to the reaction tube, and the flow rate of isobutyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., specific gravity 0.80g / mL) is 1.9mL / hour, and it is supplied to an evaporator set at 150°C to evaporate. The flow rate of nitrogen is 1080mL (standard state) / hour. The isobutyl alcohol concentration in the raw material gas supplied to the catalyst layer is 29.6% by volume, and the temperature of the catalyst layer during the reaction (reaction temperature) is 500°C.
[0294] [Example 26]
[0295] 1.1 g of cerium oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., acid content: 0.004 mmol / g, base content: 0.004 mmol / g, BET specific surface area: 5.0 m 2 / g, average electronegativity: 2.37) as Catalyst A-3, the catalytic performance was evaluated in the same manner as in Example 25 except for the above.
[0296] [Example 27]
[0297] The catalyst performance was evaluated in the same manner as in Example 25 except that 1.1 g of catalyst B-3 (acid amount: 0.079 mmol / g, base amount: 0.439 mmol / g, average electronegativity: 2.48) was used.
[0298] [Example 28]
[0299] 1.1 g of zinc oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., acid content: 0.004 mmol / g, base content: 0.003 mmol / g, BET specific surface area: 7.0 m 2 / g, average electronegativity: 2.38) as Catalyst A-4, the catalytic performance was evaluated in the same manner as in Example 25 except for the above.
[0300] [Example 29]
[0301] The catalyst performance was evaluated in the same manner as in Example 25 except that 1.1 g of silver oxide (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., average electronegativity: 2.34) was used as Catalyst A-5.
[0302] [Example 30]
[0303] 1.1 g of hydrotalcite (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., acid content: 0.242 mmol / g, base content: 0.172 mmol / g, BET specific surface area: 197 m 2 / g, average electronegativity: 2.49) as Catalyst A-6, the catalytic performance was evaluated in the same manner as in Example 25 except for the above.
[0304] [Example 31]
[0305] The catalyst performance was evaluated in the same manner as in Example 25 except that 1.1 g of lanthanum oxide (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., acid amount: 0.000 mmol / g, base amount: 0.006 mmol / g, average electronegativity: 2.18) was used as Catalyst A-7.
[0306] [Comparative Example 1]
[0307] The catalyst performance was evaluated in the same manner as in Example 25 except that 1.1 g of silicon oxide (manufactured by Fuji Silysia Co., Ltd., trade name: CARiACT Q-10, acid content: 0.008 mmol / g, average electronegativity: 2.82) was used.
[0308] Tables 8A to 8C show the reaction conditions and evaluation results of Examples 25 to 31 and Comparative Example 1. In addition, FIG8 shows the conversion rate of isobutyl alcohol based on the catalyst, and the selectivity and yield of isobutylaldehyde and methacrolein (MAL) in each example.
[0309] [Table 8A]
[0310]
[0311] [Table 8B]
[0312]
[0313] [Table 8C]
[0314]
[0315] As shown in Tables 8A to 8C and FIG. 8 , in Examples 25 to 31 using catalysts having an average electronegativity in the range of 2.1 to 2.8, the selectivity for isobutylaldehyde and methacrolein was higher than that for catalysts outside the above range.
[0316] [Examples 33 to 36]
[0317] The catalyst performance was evaluated in the same manner as in Example 8 except that the reaction temperature was changed as shown in Table 9 and the catalyst B-1 was used.
[0318] The reaction conditions and evaluation results of Examples 33 to 36 are shown in Table 9. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 9. Fig. 9 .
[0319] [Table 9]
[0320]
[0321] As shown in Table 9 and Fig. 9 As shown, in Examples 33 to 36 using Catalyst B-1, the selectivities of isobutylaldehyde and methacrolein were high at any reaction temperature.
[0322] [Examples 37 to 39]
[0323] The catalyst performance was evaluated in the same manner as in Example 8 except that the amount of catalyst B-3 used was changed as shown in Table 10.
[0324] [Example 40]
[0325] Using 3.2 g of catalyst B-3, the flow rates of isobutanol and water were set to 0.55 mL / hour and 0.30 mL / hour, respectively, and supplied to an evaporator set at 150°C for evaporation. The flow rate of nitrogen was set to 720 mL (standard state) / hour. The isobutanol concentration and water concentration in the raw gas supplied to the catalyst layer were 10.9 volume % and 30.4 volume %, respectively. Except for this, the catalyst performance was evaluated in the same manner as in Example 37.
[0326] The reaction conditions and evaluation results of Examples 37 to 40 are shown in Table 10. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 10. Fig.10 .
[0327] [Table 10]
[0328]
[0329] As shown in Table 10 and Fig.10 As shown, in Examples 37 to 40 using Catalyst B-3, the selectivities of isobutylaldehyde and methacrolein were high under any W / F conditions.
[0330] [Example 41]
[0331] The catalyst performance was evaluated in the same manner as in Example 25 except that 2.2 g of catalyst A-2 was used.
[0332] [Example 42]
[0333] The catalyst performance was evaluated in the same manner as in Example 1 except as shown below. 3.3 g of catalyst A-2 was filled in the reaction tube to form a catalyst layer. No water was supplied to the reaction tube, and the flow rate of isobutanol was 0.92 mL / hour, and it was supplied to an evaporator set at 150°C to evaporate it. The flow rate of nitrogen was 540 mL (standard state) / hour. The isobutanol concentration in the raw gas supplied to the catalyst layer was 29.6% by volume, and the temperature of the catalyst layer during the reaction (reaction temperature) was 500°C.
[0334] The reaction conditions and evaluation results of Examples 25, 41 and 42 are shown in Table 11. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 11. Fig.11 .
[0335] [Table 11]
[0336]
[0337] As shown in Table 11 and Fig.11 As shown, in Examples 25, 41 and 42 using Catalyst A-2, the selectivities of isobutylaldehyde and methacrolein were high under any W / F conditions.
[0338] [Examples 43-44]
[0339] The catalyst performance was evaluated in the same manner as in Example 1 except that the reaction temperature was changed as shown in Table 12.
[0340] The reaction conditions and evaluation results of Examples 1, 43 and 44 are shown in Table 12. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 12. Fig.12 .
[0341] [Table 12]
[0342]
[0343] As shown in Table 12 and Fig.12 As shown, in Examples 1, 43 and 44 using Catalyst B-1, the selectivities of isobutylaldehyde and methacrolein were high at any reaction temperature.
[0344] [Example 45]
[0345] The catalyst performance was evaluated in the same manner as in Example 3 except that the reaction temperature was changed as shown in Table 13.
[0346] The reaction conditions and evaluation results of Examples 3, 13 and 45 are shown in Table 13. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 13. Fig.13 .
[0347] [Table 13]
[0348]
[0349] As shown in Table 13 and Fig.13 As shown, in Examples 3, 13 and 45 using Catalyst C, the selectivities to isobutylaldehyde and methacrolein were high at any reaction temperature.
[0350] [Examples 46 to 50]
[0351] The catalyst performance was evaluated in the same manner as in Example 25 except that 1.1 g of catalyst B-10 was used instead of catalyst A-2 and the reaction temperature was changed as shown in Table 14.
[0352] The reaction conditions and evaluation results of Examples 46 to 50 are shown in Tables 14A and 14B. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Tables 14A and 14B. Fig.14 .
[0353] [Table 14A]
[0354]
[0355] [Table 14B]
[0356]
[0357] As shown in Tables 14A, 14B and Fig.14 As shown, in Examples 46 to 50 using Catalyst N, the selectivities to isobutylaldehyde and methacrolein were high at any reaction temperature.
[0358] [Examples 51 to 53]
[0359] The catalyst performance was evaluated in the same manner as in Example 28, except that the reaction temperature was changed as shown in Table 15.
[0360] The reaction conditions and evaluation results of Examples 28 and 51 to 53 are shown in Table 15. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 15. Fig.15 .
[0361] [Table 15]
[0362]
[0363] As shown in Table 15 and Fig.15 As shown, in Examples 28 and 51 to 53 using Catalyst A-4, the selectivities of isobutylaldehyde and methacrolein were high at any reaction temperature.
[0364] [Example 54]
[0365] The catalyst performance was evaluated in the same manner as in Example 5 except as shown below. 1.1 g of catalyst B-3 was filled in the reaction tube to form a catalyst layer. The flow rates of isobutanol and water were set to 1.9 mL / hour and 0.50 mL / hour, respectively, and supplied to an evaporator set at 150°C for evaporation. The flow rate of nitrogen was 3000 mL (standard state) / hour. The concentrations of isobutanol and water in the raw gas supplied to the catalyst layer were 11.4% by volume and 14.8% by volume, respectively, and the temperature of the catalyst layer during the reaction (reaction temperature) was 500°C.
[0366] [Example 55]
[0367] The catalyst performance was evaluated in the same manner as in Example 8 except as shown below. 1.1 g of catalyst B-3 was filled in the reaction tube to form a catalyst layer. The flow rates of isobutanol and water were set to 1.9 mL / hour and 2.0 mL / hour, respectively, and supplied to an evaporator set at 150°C for evaporation. The flow rate of nitrogen was set to 1140 mL (standard state) / hour. The concentrations of isobutanol and water in the raw gas supplied to the catalyst layer were 11.4% by volume and 60.2% by volume, and the temperature of the catalyst layer during the reaction (reaction temperature) was 500°C.
[0368] [Example 56]
[0369] The catalyst performance was evaluated in the same manner as in Example 8 except as shown below. 1.1 g of catalyst B-3 was filled in the reaction tube to form a catalyst layer. The flow rates of isobutanol and water were 1.9 mL / hour and 2.6 mL / hour, respectively, and supplied to an evaporator set at 150°C for evaporation. The flow rate of nitrogen was 540 mL (standard state) / hour. The concentrations of isobutanol and water in the raw gas supplied to the catalyst layer were 10.9% by volume and 76.4% by volume, and the temperature of the catalyst layer during the reaction (reaction temperature) was 500°C.
[0370] The reaction conditions and evaluation results of Examples 5, 8, and 54 to 56 are shown in Tables 16A and 16B. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Tables 16A and 16B. Fig.16 .
[0371] [Table 16A]
[0372]
[0373] [Table 16B]
[0374]
[0375] As shown in Table 16, Table 16B and Fig.16 As shown, in Examples 5, 8, and 54 to 56 using Catalyst B-3, the selectivities of isobutylaldehyde and methacrolein were high at any water concentration.
[0376] [Example 57]
[0377] The catalyst performance was evaluated in the same manner as in Example 2 except as shown below. 1.1 g of catalyst B-2 was filled in the reaction tube to form a catalyst layer. The flow rate of isobutanol was set to 1.9 mL / hour and supplied to an evaporator set at 150°C to evaporate it. The flow rate of nitrogen was set to 3660 mL (standard state) / hour. In addition, the reaction temperature was set to 450°C. The concentration of isobutanol in the raw gas supplied to the catalyst layer was 11.4% by volume.
[0378] The reaction conditions and evaluation results of Examples 2 and 57 are shown in Table 17. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 17. Fig.17 .
[0379] [Table 17]
[0380]
[0381] As shown in Table 17 and Fig.17 As shown, in Examples 2 and 57 using Catalyst B-2, the selectivities of isobutylaldehyde and methacrolein were high at any water concentration.
[0382] [Example 58]
[0383] γ-alumina (manufactured by Strem Chemicals Inc.) was calcined in air at 550°C for 12 hours using an electric furnace as a pretreatment. 0.30 g of potassium nitrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 4.0 mL of distilled water to prepare an aqueous potassium nitrate solution. The aqueous potassium nitrate solution was evenly dripped onto 6.0 g of the pretreated alumina taken out into a mortar and stirred for 15 minutes. After drying at 25°C for 24 hours, it was dried at 40°C for 2 hours using a vacuum dryer, dried at 60°C for 2 hours, and dried at 110°C for 24 hours using a dryer. After the drying treatment, it was ground in a mortar and calcined in air at 550°C for 12 hours using a calcining furnace. After calcination, it was ground again in a mortar and pressed into sheets using a tablet former at 2 tons for 15 minutes. A K(2.5) / Al with a particle size of 300 to 850 μm was prepared using a sieve. 2 O 3 (Catalyst (abbreviation): B-16, acid content: 0.167mmol / g, base content: 0.230mmol / g, BET specific surface area: 183m 2 / g, average electronegativity: 2.51).
[0384] Catalyst B-16 (acid amount: 0.167 mmol / g, base amount: 0.230 mmol / g, BET specific surface area: 183 m 2 / g) 0.5 g, isobutyl alcohol was supplied to an evaporator set at 150°C for evaporation at 0.89 mL / hour, and the catalyst performance was evaluated in the same manner as in Example 5 except that the flow rate of nitrogen was 1740 mL (standard state) / hour.
[0385] [Example 59]
[0386] The catalyst performance was evaluated in the same manner as in Example 58 except that 0.5 g of Catalyst B-10 (acid amount: 0.037 mmol / g, base amount: 0.638 mmol / g) was used.
[0387] The reaction conditions and evaluation results of Examples 22, 58 and 59 are shown in Table 18. In addition, the conversion rate of isobutyl alcohol based on the catalyst, the selectivity and yield of isobutylaldehyde and methacrolein (MAL) of each example are shown in Table 18. Fig.18 .
[0388] [Table 18]
[0389]
[0390] As shown in Table 18 and Fig.18 As shown, even when various catalysts having different acid and base amounts were used, the selectivity between isobutylaldehyde and methacrolein was high.
[0391] [Example 61]
[0392] The catalyst performance was evaluated in the same manner as in Example 1 except as shown below. 1.1 g of catalyst B-1 was filled in the reaction tube to form a catalyst layer. The flow rates of isobutyl alcohol and water were 1.9 mL / hour and 0.50 mL / hour, respectively, and supplied to an evaporator set at 150° C. to evaporate. The flow rate of nitrogen was 1620 mL (standard state) / hour. In addition, the reaction temperature was 450° C.
[0393] The concentrations of isobutanol and water in the raw material gas supplied to the catalyst layer were 17.0% by volume and 23.0% by volume.
[0394] [Example 62]
[0395] The catalyst performance was evaluated in the same manner as in Example 1 except as shown below. 1.1 g of catalyst B-1 was filled in the reaction tube to form a catalyst layer. The flow rates of isobutanol and water were 1.9 mL / hour and 0.50 mL / hour, respectively, and supplied to an evaporator set at 150°C for evaporation. Air and nitrogen were used as diluent gases, and their flow rates were 900 mL (standard state) / hour and 780 mL (standard state) / hour, respectively, supplied to the evaporator, and supplied to the reactor together with the evaporated isobutanol. In addition, the reaction temperature was 450°C. The concentrations of isobutanol, water, and oxygen in the raw gas supplied to the catalyst layer were 16.7% by volume, 22.6% by volume, and 6.8% by volume.
[0396] [Example 63]
[0397] 1.1 g of catalyst B-1 was filled in the reaction tube to form a catalyst layer. The flow rates of isobutanol and water were set to 1.9 mL / hour and 0.50 mL / hour, respectively, and supplied to an evaporator set at 150°C for evaporation. Air was used as a diluent gas, and the flow rate was 1680 mL (standard state) / hour, supplied to the evaporator, and supplied to the reactor together with the evaporated isobutanol. In addition, the reaction temperature was set to 450°C. The concentrations of isobutanol, water, and oxygen in the raw gas supplied to the catalyst layer were 16.8% by volume, 22.7% by volume, and 12.8% by volume.
[0398] Table 19 shows the reaction conditions and evaluation results of Examples 61 to 63.
[0399] [Table 19]
[0400]
[0401] As shown in Table 19, in Examples 61 to 63 using Catalyst B-1, the selectivity of isobutylaldehyde and methacrolein was high even when air was used as the diluent gas for the raw material gas.
[0402] [Example 64]
[0403] The catalyst performance was evaluated in the same manner as in Example 53 except as shown below. 1.1 g of catalyst A-4 was filled in the reaction tube to form a catalyst layer. The flow rates of isobutanol and water were set to 1.9 mL / hour and 0.50 mL / hour, respectively, and supplied to an evaporator set at 150°C for evaporation. Nitrogen was used as a diluent gas, and their flow rate was set to 480 mL (standard state) / hour, supplied to the evaporator, and supplied to the reactor together with the evaporated isobutanol. In addition, the reaction temperature was set to 450°C. The concentrations of isobutanol and water in the raw gas supplied to the catalyst layer were 29.5% by volume and 40.0% by volume.
[0404] As shown in Table 20, in Examples 53 and 64 using Catalyst A-4, the selectivity of isobutylaldehyde and methacrolein was high even when water was used as the diluent gas for the raw material gas.
[0405] [Table 20]
[0406]
[0407] [Example 65]
[0408] To 5.8 g of tetraethoxysilane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 19.7 g of ethanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and a few drops of 0.1 mol / l hydrochloric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added, and the tetraethoxysilane was hydrolyzed while stirring at 75°C for 2 hours. 6.5 g of zinc nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added thereto, and after stirring for 1 hour, a few drops of aqueous ammonia (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added, and stirring was continued for 3 hours while heating at 75°C to obtain a gel. The obtained gel was dried in a dryer at 110°C for 12 hours, and then calcined at 500°C for 12 hours. After calcination, the mixture was crushed in a mortar, pressed at 2.0 tons for 15 minutes using a tablet forming machine to form a sheet, and a ZnO(75)-SiO having a particle size of 300 to 850 μm was obtained using a sieve. 2 (25) (catalyst (abbreviation): A-8, average electronegativity: 2.48, acid content: 0.094 mmol / g, base content: 0.002 mmol / g) The numbers in parentheses represent the content of the metal element (mol %).
[0409] The catalyst performance was evaluated in the same manner as in Example 52 except that 1.1 g of catalyst A-8 was used.
[0410] [Example 66]
[0411] 13.31 g of titanium sulfate and 14.85 g of zinc nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to 170 g of distilled water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and dissolved at 25° C. (the element concentration of titanium and aluminum oxide was adjusted to 0.4 mol / l). After stirring the liquid for 1 hour, aqueous ammonia (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added dropwise until the pH became 8.0, and the mixture was further stirred at 25° C. for 2 hours.
[0412] The obtained precipitate was separated and recovered by a centrifugal separator. Distilled water was added to the recovered precipitate to form a slurry, which was separated by a centrifugal separator. This operation was repeated twice.
[0413] The precipitate was recovered and dried in a dryer at 110°C for 12 hours. The obtained solid was calcined in air at 550°C for 8 hours. After calcination, it was ground in a mortar and pressed in a tablet forming machine at 2.0 tons for 15 minutes to form a sheet. A sieve was used to obtain ZnO(75)-TiO with a particle size of 300 to 850 μm. 2 (25) (Catalyst (abbreviation): A-9, average electronegativity: 2.44, acid content: 0.097 mmol / g, base content: 0.000 mmol / g, BET specific surface area: 18 m 2 / g). The numbers in parentheses represent the content (mol%) of the metal elements.
[0414] The catalyst performance was evaluated in the same manner as in Example 52 except that 1.1 g of catalyst A-9 was used.
[0415] [Example 67]
[0416] 12.5 g of aluminum nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 29.7 g of zinc nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to 330 g of distilled water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and dissolved at 25°C. After stirring the liquid for 1 hour, aqueous ammonia (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added dropwise until the pH reached 8.0, and the mixture was further stirred at 25°C for 2 hours. The obtained precipitate was separated using a centrifuge and washed with distilled water. This operation was repeated twice. The precipitate was dried at 110°C for 12 hours using a dryer. The obtained solid was calcined in air at 550°C for 8 hours. After calcination, the solid was crushed using a mortar and pressed into a sheet using a tablet former at 2.0 tons for 15 minutes. A sieve was used to obtain ZnO(75)-Al with a particle size of 300 to 850 μm.2 O 3 (25) (Catalyst (abbreviation): A-10, average electronegativity: 2.41, acid content: 0.04 mmol / g, base content: 0.004 mmol / g, BET specific surface area: 32 m 2 / g). The numbers in parentheses represent the content (mol %) of each component.
[0417] The catalyst performance was evaluated in the same manner as in Example 52 except that 1.1 g of catalyst A-10 was used.
[0418] [Table 21]
[0419]
[0420] As shown in Table 21, in Examples 52 and 65 to 67 using Catalysts A-4 and 8 to 10, the selectivities of isobutylaldehyde and methacrolein were high.
[0421] [Example 68]
[0422] 28.09 g of aluminum nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 7.43 g of zinc nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to 250 g of distilled water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and dissolved at 25°C. After stirring the liquid for 1 hour, aqueous ammonia (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added dropwise until the pH reached 8.0, and the mixture was further stirred at 25°C for 2 hours. The obtained precipitate was separated using a centrifuge and washed with distilled water. This operation was repeated twice. The precipitate was dried at 110°C for 12 hours using a dryer. The obtained solid was calcined in air at 550°C for 8 hours. After calcination, the solid was crushed using a mortar and pressed into sheets using a tablet former at 2.0 tons for 15 minutes. A sieve was used to obtain ZnO(25)-Al with a particle size of 300 to 850 μm. 2 O 3 (75) (catalyst (abbreviation): A-11, average electronegativity: 2.51, acid content: 0.284 mmol / g, base content: 0.119 mmol / g) The numbers in parentheses represent the content (mol %) of each component.
[0423] The catalyst performance was evaluated in the same manner as in Example 52 except that 1.1 g of catalyst A-11 was used.
[0424] [Example 69]
[0425] 37.83 g of aluminum nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 30.0 g of zinc nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to 630 g of distilled water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and dissolved at 25°C. After stirring the liquid for 1 hour, aqueous ammonia (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added dropwise until the pH reached 8.0, and the mixture was further stirred at 25°C for 2 hours. The obtained precipitate was separated using a centrifuge and washed with distilled water. This operation was repeated twice. The precipitate was dried at 110°C for 12 hours using a desiccant. The obtained solid was calcined in air at 550°C for 8 hours. After calcination, the solid was crushed using a mortar and pressed into a sheet using a tablet former at 2.0 tons for 15 minutes. A sieve was used to obtain ZnO(40)-Al with a particle size of 300 to 850 μm. 2 O 3 (60) (catalyst (abbreviation): A-12, average electronegativity: 2.48, acid content: 0.131 mmol / g, base content: 0.187 mmol / g) The numbers in parentheses represent the content (mol %) of each component.
[0426] The catalyst performance was evaluated in the same manner as in Example 52 except that 1.1 g of catalyst A-12 was used.
[0427] [Example 70]
[0428] 56.74 g of aluminum nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 30.0 g of zinc nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to 500 g of distilled water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and dissolved at 25°C. After stirring the liquid for 1 hour, aqueous ammonia (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added dropwise until the pH reached 8.0, and the mixture was further stirred at 25°C for 2 hours. The obtained precipitate was separated using a centrifuge and washed with distilled water. This operation was repeated twice. The precipitate was dried at 110°C for 12 hours using a dryer. The obtained solid was calcined in air at 550°C for 8 hours. After calcination, the solid was crushed using a mortar and pressed into sheets using a tablet former at 2.0 tons for 15 minutes. A sieve was used to obtain ZnO(50)-Al with a particle size of 300 to 850 μm. 2 O 3 (50) (Catalyst (abbreviation): A-13, average electronegativity: 2.48, acid content: 0.103 mmol / g, base content: 0.107 mmol / g, BET specific surface area: 53 m 2 / g). The numbers in parentheses represent the content (mol %) of each component.
[0429] The catalyst performance was evaluated in the same manner as in Example 52 except that 1.1 g of catalyst A-13 was used.
[0430] [Example 71]
[0431] 12.61 g of aluminum nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 20.0 g of zinc nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to 250 g of distilled water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and dissolved at 25°C. After stirring the liquid for 1 hour, aqueous ammonia (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added dropwise until the pH reached 8.0, and the mixture was further stirred at 25°C for 2 hours. The obtained precipitate was separated using a centrifuge and washed with distilled water. This operation was repeated twice. The precipitate was dried at 110°C for 12 hours using a dryer. The obtained solid was calcined in air at 550°C for 8 hours. After calcination, the solid was crushed using a mortar and pressed into sheets using a tablet former at 2.0 tons for 15 minutes. A sieve was used to obtain ZnO(66)-Al with a particle size of 300 to 850 μm. 2 O 3 (33) (catalyst (abbreviation): A-14, average electronegativity: 2.47, acid content: 0.077 mmol / g, base content: 0.046 mmol / g). The numbers in parentheses represent the content (mol %) of each component.
[0432] The catalyst performance was evaluated in the same manner as in Example 52 except that 1.1 g of catalyst A-14 was used.
[0433] [Example 79]
[0434] 20.0 g of magnesium nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 14.63 g of aluminum nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to 300 g of distilled water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and dissolved at 25°C. After stirring the liquid for 1 hour, aqueous ammonia (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added dropwise until the pH reached 9.0, and the mixture was further stirred at 25°C for 2 hours. The obtained precipitate was separated using a centrifuge and washed with distilled water. This operation was repeated twice. The precipitate was dried at 110°C for 12 hours using a dryer. The obtained solid was calcined in air at 550°C for 8 hours. After calcination, the solid was crushed using a mortar and pressed into a sheet using a tablet former at 2.0 tons for 15 minutes. A sieve was used to obtain MgO(66)-Al with a particle size of 300 to 850 μm. 2 O 3(33) (catalyst (abbreviation): A-18, average electronegativity: 2.27, acid content: 0.12 mmol / g, base content: 0.13 mmol / g) The numbers in parentheses represent the content (mol %) of each component.
[0435] [Table 22A]
[0436]
[0437] [Table 22B]
[0438]
[0439] As shown in Tables 22A and 22B, in Examples 52, 67 to 71, and 79 using Catalysts A-4, 10, 11 to 14, and 18, the selectivities of isobutylaldehyde and methacrolein were high.
[0440] [Examples 72 to 76]
[0441] The catalyst performance was evaluated in the same manner as in Example 52, except that the catalyst and reaction temperature were changed as shown in Tables 23A and 23B.
[0442] [Table 23A]
[0443]
[0444] [Table 23B]
[0445]
[0446] As shown in Tables 23A and 23B, in Examples 72 to 76 using Catalysts A-10 and 11 to 14, the selectivities of isobutylaldehyde and methacrolein were high.
[0447] [Example 77]
[0448] The catalyst performance was evaluated in the same manner as in Example 52 except that Catalyst A-12 was used and the reaction temperature was set to 300°C.
[0449] [Table 24]
[0450]
[0451] As shown in Table 24, using the catalyst A-12, the selectivity of isobutylaldehyde and methacrolein was high even in the cases of Examples 69, 74 and 77 in which the reaction was carried out at a reaction temperature of 300 to 400°C.
[0452] [Example 78]
[0453] 56.74 g of aluminum nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 30.0 g of zinc nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to 500 g of distilled water (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and dissolved at 25°C. After stirring the liquid for 1 hour, aqueous ammonia (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added dropwise until the pH reached 8.0, and the mixture was further stirred at 25°C for 2 hours. The obtained precipitate was separated using a centrifuge and washed with distilled water. This operation was repeated twice. The precipitate was dried at 110°C for 12 hours using a dryer. The obtained solid was calcined at 900°C in air for 8 hours. After calcination, the solid was crushed using a mortar and pressed into a sheet using a tablet former at 2.0 tons for 15 minutes. A sieve was used to obtain ZnO(50)-Al with a particle size of 300 to 850 μm. 2 O 3 (50) (catalyst (abbreviation): A-16, average electronegativity: 2.48, acid content: 0.103 mmol / g, base content: 0.107 mmol / g) The numbers in parentheses represent the content (mol %) of each component.
[0454] The catalyst performance was evaluated in the same manner as in Example 75 except that 1.1 g of catalyst A-16 was used.
[0455] [Table 25]
[0456]
[0457] As shown in Table 25, when the catalyst A-16 was used, the selectivity of isobutylaldehyde and methacrolein was high even when the reaction temperature was changed to 300 to 400°C.
[0458] Industrial Applicability
[0459] According to the present invention, there are provided a dehydrogenation catalyst capable of producing isobutylaldehyde and methacrolein from isobutyl alcohol with high selectivity while suppressing oxidation and bimolecularization of isobutylaldehyde without requiring reduction treatment with hydrogen, and a method for producing a dehydrogenated compound using the dehydrogenation catalyst.
Claims
1. A catalyst having an average electronegativity of 2.10 to 2.65, The catalyst comprises a metal oxide having an average electronegativity of 2.10 to 2.65, The acid amount of the catalyst is 0.25 mmol / g or less, The content of the metal oxide is 80% by mass or more relative to the total mass of the catalyst, The catalyst is a catalyst for producing at least one dehydrogenation compound selected from isobutylaldehyde and methacrolein from isobutyl alcohol.
2. The catalyst according to claim 1, wherein Contains metal oxides having an average electronegativity of 2.10 to 2.
55.
3. The catalyst according to claim 1 or 2, wherein The metal oxide includes oxides of one or more metals selected from the group consisting of Al, Si, Zn, Ag, Ce, La, and Mg.
4. The catalyst according to claim 1 or 2, wherein The metal oxide includes oxides of one or more metals selected from the group consisting of Zn, Al, Fe, Si, Zr, and Ti.
5. The catalyst according to claim 1 or 2, wherein Contains more than one alkali metal.
6. A method for producing a catalyst according to any one of claims 1 to 5, wherein: This involves calcining the metal oxide.
7. A method for producing a dehydrogenated compound, which is a method for producing a dehydrogenated compound from isobutanol. The method comprises using the catalyst according to any one of claims 2 to 5 to produce at least one dehydrogenated compound selected from isobutylaldehyde and methacrolein from isobutyl alcohol.
8. A method for producing methacrylic acid, comprising producing methacrylic acid from at least one of isobutylaldehyde and methacrolein obtained by the method for producing a dehydrogenated compound according to claim 7.
9. A method for producing methacrylic acid ester, comprising producing methacrylic acid by the method for producing methacrylic acid according to claim 8, and producing methacrylic acid ester from the obtained methacrylic acid and an alcohol having 1 to 20 carbon atoms.
10. Use of a catalyst in producing at least one dehydrogenated compound selected from isobutylaldehyde and methacrolein from isobutyl alcohol, producing at least one dehydrogenated compound selected from isobutylaldehyde and methacrolein from isobutyl alcohol, The average electronegativity of the catalyst is 2.10 to 2.65, The catalyst comprises a metal oxide having an average electronegativity of 2.10 to 2.65, The acid amount of the catalyst is 0.25 mmol / g or less, The content of the metal oxide is 80% by mass or more relative to the total mass of the catalyst.