Preparation method of composite hydroxide and composite hydroxide

By adding aqueous metal solutions of nickel (Ni) and cobalt (Co) respectively during the manufacturing process of the composite hydroxide, and controlling the reaction conditions, the problems of production cost and reactivity uniformity are solved, and efficient battery characteristics are improved.

CN115362133BInactive Publication Date: 2024-10-25TANAKA CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180025913.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-02
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing technology has shortcomings in reducing the production cost of composite hydroxides containing nickel (Ni) and cobalt (Co) and appropriately controlling the BET specific surface area, and it is difficult to uniformize the reactivity of composite hydroxides and lithium compounds.

Method used

By adding the first metal-containing aqueous solution and the second metal-containing aqueous solution containing nickel (Ni) and cobalt (Co) to the reaction tank respectively, the reaction temperature and ammonium ion concentration are controlled to ensure uniformity of the BET specific surface area of ​​the composite hydroxide. , and suppress the changes in BET specific surface area caused by different particle sizes.

Benefits of technology

It is possible to reduce the production cost of the composite hydroxide without compromising the tap density, and to uniformize the reactivity between the composite hydroxide and the lithium compound, thereby improving the battery characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115362133B_ABST
    Figure CN115362133B_ABST
Patent Text Reader

Abstract

The present invention provides a method for manufacturing a composite hydroxide containing nickel (Ni) and cobalt (Co), which can appropriately control the BET specific surface area without impairing the tap density and can reduce the production cost. The present invention relates to a method for manufacturing a composite hydroxide, which is a method for manufacturing a composite hydroxide containing at least nickel (Ni) and cobalt (Co). Among them, a first metal-containing aqueous solution containing A mol% of nickel (Ni) and B mol% of cobalt (Co), a second metal-containing aqueous solution containing C mol% of nickel (Ni) and D mol% of cobalt (Co) (wherein, A > C, B < D, A + B = 100, C + D = 100), an alkali metal aqueous solution and an aqueous solution containing an ammonium ion donor are independently supplied to a reaction tank, and the pH value of the solution in the reaction tank is maintained in the range of 10.0 or more and 13.0 or less based on a liquid temperature of 25 °C, and the ammonium ion concentration is maintained in the range of 1.0 g / L or more and 10.0 g / L or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a composite hydroxide, which is a method for producing a composite hydroxide containing nickel (Ni) and cobalt (Co), and can appropriately control the BET specific surface area while reducing the production cost of the composite hydroxide. In addition, the present invention relates to a composite hydroxide, which is a composite hydroxide containing nickel (Ni) and cobalt (Co), and the reactivity of the composite hydroxide with a lithium compound is uniformed by suppressing the change in the BET specific surface area caused by the difference in particle size. Background Art

[0002] In recent years, from the viewpoint of reducing environmental load, secondary batteries have been used in a wide range of fields such as power sources for portable device power supplies, electric vehicles, etc., which are used or used in combination. As secondary batteries, for example, there are secondary batteries using non-aqueous electrolytes such as lithium ion secondary batteries. Secondary batteries using non-aqueous electrolytes such as lithium ion secondary batteries are suitable for miniaturization and light weight, and have battery characteristics such as high utilization rate, high cycle characteristics, and large charge and discharge capacity.

[0003] The positive electrode active material of non-aqueous electrolyte secondary batteries such as lithium ion secondary batteries uses a composite hydroxide as its precursor. As the composite hydroxide of the precursor of the positive electrode active material, a composite hydroxide containing nickel (Ni) and cobalt (Co) is sometimes used.

[0004] In addition, along with the high functionality of equipment equipped with secondary batteries, further improvement of battery characteristics such as further high capacity is required. Therefore, a method for manufacturing a composite hydroxide containing nickel (Ni) and cobalt (Co) is studied to obtain a positive electrode active material that can impart better battery characteristics. In the method for manufacturing the above-mentioned composite hydroxide, it is studied to impart excellent battery characteristics by designing a method for adding a raw material solution. As a method for manufacturing the above-mentioned composite hydroxide related to a method for adding a raw material solution, for example, an aqueous solution of a metal compound containing Ni and at least one element selected from Co or Mn, an aqueous solution of sodium aluminate, an aqueous solution of sodium hydroxide, and an aqueous solution containing an ammonium ion donor are proposed to be independently and simultaneously supplied to the same reaction tank for reaction (patent document 1).

[0005] In Patent Document 1, the particles of the composite hydroxide containing nickel (Ni) and cobalt (Co) are spherical in shape, and the positive electrode active material obtained from the composite hydroxide can be loaded on the positive electrode at a high density, thereby obtaining a high-capacity positive electrode material with good safety such as thermal stability and charge-discharge cycle characteristics.

[0006] On the other hand, due to the use of secondary batteries in a wide range of fields, it is also required to reduce the production cost of the composite hydroxide containing nickel (Ni) and cobalt (Co). In addition, in the case of using the composite hydroxide containing nickel (Ni) and cobalt (Co) as the precursor of the positive electrode active material of lithium ion secondary battery, the composite hydroxide as the precursor is based on its use conditions, etc., in order to give excellent cycle characteristics, high capacity and other battery characteristics, sometimes it is necessary to properly control the reactivity with lithium. For the composite hydroxide as a precursor, by properly controlling the BET specific surface area, the reactivity with lithium can be properly controlled. In addition, by making the BET specific surface area uniform regardless of the particle size of the composite hydroxide as a precursor, the reactivity of the composite hydroxide and lithium is uniformized, so that the composite hydroxide can give excellent cycle characteristics, high capacity and other battery characteristics.

[0007] However, there is room for improvement in reducing the production cost of the composite hydroxide and in appropriately controlling the BET specific surface area in Patent Document 1. In addition, there is room for improvement in making the BET specific surface area uniform regardless of the particle size of the composite hydroxide in Patent Document 1.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2006-089364 Summary of the invention

[0011] Problems to be solved by the invention

[0012] In view of the above situation, the object of the present invention is to provide a method for manufacturing a composite hydroxide containing nickel (Ni) and cobalt (Co) and a composite hydroxide, wherein the manufacturing method can appropriately control the BET specific surface area without damaging the tap density and can reduce production costs, and the composite hydroxide can suppress the change in the BET specific surface area caused by the difference in particle size, thereby making the reactivity of the composite hydroxide with the metal compound uniform and improving the battery characteristics.

[0013] Means of solving the problem

[0014] In the present invention, as a raw material solution of a composite hydroxide containing nickel (Ni) and cobalt (Co), a first raw material solution mainly containing nickel (Ni) and a second raw material solution mainly containing cobalt (Co) are prepared, and the first raw material solution and the second raw material solution are respectively added to a reaction tank to manufacture a composite hydroxide containing nickel (Ni) and cobalt (Co).

[0015] The gist of the present invention is as follows.

[0016] [1] A method for manufacturing a composite hydroxide, which is a method for manufacturing a composite hydroxide containing at least nickel (Ni) and cobalt (Co), wherein a first metal-containing aqueous solution containing A mol% of nickel (Ni) and B mol% of cobalt (Co), a second metal-containing aqueous solution containing C mol% of nickel (Ni) and D mol% of cobalt (Co) (where A > C, B < D, A + B = 100, C + D = 100), an alkali metal aqueous solution, and an aqueous solution containing an ammonium ion donor are independently supplied to a reaction tank, and the pH value of the solution in the reaction tank is maintained in the range of 10.0 or more and 13.0 or less based on a liquid temperature of 25 °C, and the ammonium ion concentration is maintained in the range of 1.0 g / L or more and 10.0 g / L or less.

[0017] [2] The method for manufacturing a composite hydroxide according to [1], wherein the ratio of A to C is 5 or more, and the ratio of D to B is 5 or more.

[0018] [3] The method for manufacturing a composite hydroxide according to [1] or [2], wherein the first metal-containing aqueous solution does not contain cobalt (Co), and the second metal-containing aqueous solution does not contain nickel (Ni).

[0019] [4] The method for manufacturing a composite hydroxide according to any one of [1] to [3], wherein the first metal-containing aqueous solution and the second metal-containing aqueous solution are simultaneously supplied to the reaction tank.

[0020] [5] The method for manufacturing a composite hydroxide according to any one of [1] to [4], wherein the composite hydroxide is represented by Ni 1-x-y Co x M y O z (OH) 2-α (0 < x ≤ 0.3, 0 ≤ y ≤ 0.3, 0 ≤ z ≤ 3.00, -0.50 ≤ α < 2.00, M represents one or more additive metal elements selected from the group consisting of Mn, Mg, Zr, Al, Ca, Ti, Nb, V, Cr, Mo, and W).

[0021] [6] The method for manufacturing a composite hydroxide according to any one of [1] to [5], wherein the first metal-containing aqueous solution is supplied to the reaction tank from a first raw material liquid supply section, and the second metal-containing aqueous solution is supplied to the reaction tank from a second raw material liquid supply section different from the first raw material liquid supply section.

[0022] [7] The method for manufacturing a composite hydroxide according to any one of [1] to [6], wherein the reaction tank is a continuous reaction tank that overflows the generated composite hydroxide.

[0023] [8] The manufacturing method of the composite hydroxide according to any one of [1] to [7], wherein the ammonium ion concentration in the reaction tank is maintained in the range of 1.0 g / L or more and 5.0 g / L or less.

[0024] [9] The manufacturing method of the composite hydroxide according to any one of [1] to [8], wherein the reaction temperature in the reaction tank is 20°C or more and 80°C or less.

[0025]

[10] The manufacturing method of the composite hydroxide according to any one of [1] to [9], wherein the composite hydroxide is a precursor of a positive electrode active material of a secondary battery.

[0026]

[11] A composite hydroxide which is a composite hydroxide containing at least nickel (Ni) and cobalt (Co), wherein the composite hydroxide has a first particle with a secondary particle size (D10) in the range of ±1.0 μm of 10% by volume in volume percentage, a second particle with a secondary particle size (D50) in the range of ±1.0 μm of 50% by volume in volume percentage, and a third particle with a secondary particle size (D90) in the range of ±1.0 μm of 90% by volume in volume percentage.

[0027] The absolute value of the change ratio is calculated by the BET specific surface area of the first particle and the secondary particle size (D50) with a volume percentage of 50% by volume and the BET specific surface area of the third particle and the secondary particle size (D50) with a volume percentage of 50% by volume using the following formula (1). The product of the absolute value of the change ratio and the molar percentage of cobalt (Co) contained in the composite hydroxide relative to the metal elements contained in the composite hydroxide (where the metal elements are Ni, Co, Mn, Mg, Zr, Al, Ca, Ti, Nb, V, Cr, Mo, and W) is 0 or more and 0.015 or less.

[0028] |(BET specific surface area of the third particle - BET specific surface area of the first particle) / (D50 of the third particle - D50 of the first particle)| = absolute value of the change ratio ··· Formula (1)

[0029]

[12] The composite hydroxide according to

[11] , wherein the composite hydroxide is represented by Ni 1-x-y Co x M y O z (OH) 2-α (0 < x + y < 0.20, 0 ≤ z ≤ 3.00, -0.50 ≤ α < 2.00, M represents one or more additive metal elements selected from the group consisting of Mn, Mg, Zr, Al, Ca, Ti, Nb, V, Cr, Mo, and W).

[0030]

[13] The composite hydroxide as described in

[12] , wherein in the Ni 1-x-y Co x M y O z (OH) 2-α , 0.02 < x < 0.20.

[0031]

[14] The composite hydroxide according to any one of

[11] to

[13] , wherein the value of (D90 of the composite hydroxide - D10 of the composite hydroxide) / D50 of the composite hydroxide is 0.50 or more and 1.40 or less.

[0032] Advantages of the Invention

[0033] According to the method for manufacturing a composite hydroxide of the present invention, by independently supplying a first metal-containing aqueous solution containing A mol% of nickel (Ni) and B mol% of cobalt (Co) and a second metal-containing aqueous solution containing C mol% of nickel (Ni) and D mol% of cobalt (Co) (where A > C, B > D, A + B = 100, C + D = 100) to a reaction tank, a composite hydroxide with a BET specific surface area appropriately controlled without impairing the tap density can be manufactured while suppressing the reaction temperature and / or the ammonium ion concentration. Thus, according to the method of the present invention, when manufacturing a composite hydroxide with an appropriately controlled BET specific surface area, the reaction temperature and / or the ammonium ion concentration can be suppressed, and therefore the production cost of the composite hydroxide can be reduced.

[0034] According to the method for manufacturing a composite hydroxide of the present invention, by making the ratio of the nickel (Ni) content of the first metal-containing aqueous solution to the nickel (Ni) content of the second metal-containing aqueous solution 5 or more and the ratio of the cobalt (Co) content of the second metal-containing aqueous solution to the cobalt (Co) content of the first metal-containing aqueous solution 5 or more, a composite hydroxide with a BET specific surface area more appropriately controlled without impairing the tap density can be manufactured even if the reaction temperature and / or the ammonium ion concentration are further suppressed.

[0035] According to the method for manufacturing a composite hydroxide of the present invention, by making the first metal-containing aqueous solution free of cobalt (Co) and the second metal-containing aqueous solution free of nickel (Ni), a composite hydroxide with a BET specific surface area more reliably and appropriately controlled without impairing the tap density can be manufactured even if the reaction temperature and / or the ammonium ion concentration are further suppressed.

[0036] According to the method for manufacturing a composite hydroxide of the present invention, the composite hydroxide is represented by Ni 1-x- y Co x M y Oz (OH) 2-α (0 < x ≤ 0.3, 0 ≤ y ≤ 0.3, 0 ≤ z ≤ 3.00, -0.50 ≤ α < 2.00, where M represents one or more additive metal elements selected from the group consisting of Mn, Mg, Zr, Al, Ca, Ti, Nb, V, Cr, Mo, and W), which can help endow a secondary battery using the obtained composite hydroxide as a cathode active material precursor with high-capacity battery characteristics.

[0037] According to the method for manufacturing the composite hydroxide of the present invention, the reaction tank is a continuous reaction tank that overflows the generated composite hydroxide, thereby improving the production efficiency of the composite hydroxide.

[0038] According to the composite hydroxide of the present invention, the composite hydroxide has a first particle with a secondary particle size (D10) in the range of ±1.0 μm of 10% by volume in volume percentage, a second particle with a secondary particle size (D50) in the range of ±1.0 μm of 50% by volume in volume percentage, and a third particle with a secondary particle size (D90) in the range of ±1.0 μm of 90% by volume in volume percentage. The absolute value of the change ratio is calculated from the BET specific surface area in the first particle and the secondary particle size (D50) of 50% by volume in volume percentage, and the BET specific surface area in the third particle and the secondary particle size (D50) of 50% by volume in volume percentage using the above formula (1). The product of the absolute value of the change ratio and the molar percentage of cobalt (Co) relative to the metal elements contained in the above composite hydroxide (where the metal elements are Ni, Co, Mn, Mg, Zr, Al, Ca, Ti, Nb, V, Cr, Mo, and W) is 0 or more and 0.015 or less, thereby suppressing the change in the BET specific surface area caused by different particle sizes, making the reactivity of the composite hydroxide with metal compounds such as lithium compounds uniform, and improving battery characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a side cross-sectional view showing an outline of an example of a reaction apparatus used in the method for manufacturing the composite hydroxide of the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0040] The manufacturing method of the composite hydroxide of the present invention will be described in detail below. In the manufacturing method of the composite hydroxide of the present invention, a first metal-containing aqueous solution containing A mol% of nickel (Ni) and B mol% of cobalt (Co), a second metal-containing aqueous solution containing C mol% of nickel (Ni) and D mol% of cobalt (Co) (where A > C, B > D, A + B = 100, C + D = 100), an alkali metal aqueous solution, and an aqueous solution containing an ammonium ion donor are independently supplied to a reaction tank, and the pH value of the solution in the reaction tank is maintained in the range of 10.0 or more and 13.0 or less based on a liquid temperature of 25 °C, and the ammonium ion concentration is maintained in the range of 1.0 g / L or more and 10.0 g / L or less. By the present invention, a composite hydroxide containing nickel (Ni) and cobalt (Co) is manufactured.

[0041] In the present invention, a first metal-containing aqueous solution as a first raw material solution mainly containing nickel (Ni) among nickel (Ni) and cobalt (Co), and a second metal-containing aqueous solution as a second raw material solution mainly containing cobalt (Co) are separately prepared, and the first metal-containing aqueous solution and the second metal-containing aqueous solution are added into the reaction tank through respective paths. When adding the first metal-containing aqueous solution and the second metal-containing aqueous solution into the reaction tank, the pH value of the solution in the reaction tank is maintained in the range of 10.0 or more and 13.0 or less based on a liquid temperature of 25 °C, and the ammonium ion concentration is maintained in the range of 1.0 g / L or more and 10.0 g / L or less.

[0042] For manufacturing a composite hydroxide with a BET specific surface area appropriately controlled, it is necessary to increase the reaction temperature and the ammonium ion concentration to promote the particle growth of the composite hydroxide. On the other hand, in the present invention, by adding the first metal-containing aqueous solution and the second metal-containing aqueous solution into the reaction tank separately, a composite hydroxide with a BET specific surface area appropriately controlled without impairing the tapped density can be manufactured while suppressing the reaction temperature and / or the ammonium ion concentration. Thus, when manufacturing a composite hydroxide with a BET specific surface area appropriately controlled, the reaction temperature and / or the ammonium ion concentration can be suppressed, that is, the energy consumption can be reduced, and the usage amount of ammonium ions can be suppressed, so that the production cost of the composite hydroxide can be reduced.

[0043] <The first metal-containing aqueous solution and the second metal-containing aqueous solution>

[0044] In the present invention, as raw material solutions, a plurality of raw material solutions with different compositions are prepared, namely, a first metal-containing aqueous solution and a second metal-containing aqueous solution.

[0045] The first metal-containing aqueous solution is a metal-containing aqueous solution mainly containing nickel (Ni) among nickel (Ni) and cobalt (Co). The second metal-containing aqueous solution is a metal-containing aqueous solution mainly containing cobalt (Co) among nickel (Ni) and cobalt (Co). Therefore, the molar concentration of nickel (Ni) (A mol%) and the molar concentration of cobalt (Co) (B mol%) in the first metal-containing aqueous solution are different from the molar concentration of nickel (Ni) (C mol%) and the molar concentration of cobalt (Co) (D mol%) in the second metal-containing aqueous solution. Additionally, the molar concentration of nickel (Ni) has a relationship of A > C, and the molar concentration of cobalt (Co) has a relationship of B < D. Furthermore, there is a relationship of A + B = 100 and C + D = 100. Therefore, nickel (Ni) and cobalt (Co) are mainly supplied to the reaction tank as different raw material liquids.

[0046] Regarding the molar concentration of nickel (Ni), as long as the relationship of A > C is satisfied, the ratio of the molar concentration of nickel (Ni) in the first metal-containing aqueous solution to the molar concentration of nickel (Ni) in the second metal-containing aqueous solution is not particularly limited. From the perspective that even if the reaction temperature and / or the ammonium ion concentration are further suppressed, a composite hydroxide can be produced that does not damage the tapped density and more appropriately controls the BET specific surface area, the ratio of the molar concentration of nickel (Ni) in the first metal-containing aqueous solution to the molar concentration of nickel (Ni) in the second metal-containing aqueous solution is preferably 5 or more, more preferably 10 or more, and further preferably 20 or more. From the perspective that even if the reaction temperature and / or the ammonium ion concentration are further suppressed, a composite hydroxide can be produced that does not damage the tapped density and more reliably and appropriately controls the BET specific surface area, it is particularly preferred that the second metal-containing aqueous solution does not contain nickel (Ni). That is, the lower the molar concentration of nickel (Ni) in the second metal-containing aqueous solution, the more preferred.

[0047] Regarding the molar concentration of cobalt (Co), as long as the relationship of B < D is satisfied, the ratio of the molar concentration of cobalt (Co) in the first metal-containing aqueous solution to the molar concentration of cobalt (Co) in the second metal-containing aqueous solution is not particularly limited. From the perspective that even if the reaction temperature and / or the ammonium ion concentration are further suppressed, a composite hydroxide can be produced that more appropriately controls the BET specific surface area without damaging the tapped density, the ratio of the molar concentration of cobalt (Co) in the second metal-containing aqueous solution to the molar concentration of cobalt (Co) in the first metal-containing aqueous solution is preferably 5 or more, more preferably 10 or more, and further preferably 20 or more. From the perspective that even if the reaction temperature and / or the ammonium ion concentration are further suppressed, a composite hydroxide can be produced that more reliably and appropriately controls the BET specific surface area without damaging the tapped density, it is particularly preferred that the first metal-containing aqueous solution does not contain cobalt (Co). That is, the lower the molar concentration of cobalt (Co) in the first metal-containing aqueous solution, the more preferred.

[0048] As described above, the composite hydroxide containing nickel (Ni) and cobalt (Co) produced by the method of the present invention is particularly preferably such that nickel (Ni) and cobalt (Co) are derived from different raw material solutions.

[0049] The first metal-containing aqueous solution and the second metal-containing aqueous solution are, for example, simultaneously and independently supplied to the reaction tank. Therefore, the supply of the first metal-containing aqueous solution to the reaction tank and the supply of the second metal-containing aqueous solution to the reaction tank are carried out in parallel, and thus the supply of nickel (Ni) and cobalt (Co) to the reaction tank is carried out in parallel. Depending on the composition of nickel (Ni) and cobalt (Co) in the composite hydroxide and the residence time in the reaction tank, the molar concentration of nickel (Ni) in the first metal-containing aqueous solution, the molar concentration of cobalt (Co) in the second metal-containing aqueous solution, and the flow rates of the first metal-containing aqueous solution and the second metal-containing aqueous solution are appropriately adjusted.

[0050] The supply amount of nickel (Ni) supplied to the reaction tank per unit time relative to the supply amount of cobalt (Co) is not particularly limited and can be appropriately selected according to the desired composition ratio of nickel (Ni) and cobalt (Co) in the composite hydroxide. For example, from the viewpoint of imparting high-capacity battery characteristics to a secondary battery using the obtained composite hydroxide as a precursor of a positive electrode active material, the supply amount of nickel (Ni) supplied to the reaction tank per unit time relative to the supply amount of cobalt (Co) is preferably in the range of 2.5 or more and 50.0 or less, and particularly preferably in the range of 6.0 or more and 30.0 or less.

[0051] The composite hydroxide containing nickel (Ni) and cobalt (Co) may further contain an additional metal element M other than nickel (Ni) and cobalt (Co) as needed. Examples of the additional metal element M include manganese (Mn), magnesium (Mg), aluminum (Al), calcium (Ca), titanium (Ti), vanadium (V), chromium (Cr), zirconium (Zr), niobium (Nb), molybdenum (Mo), and tungsten (W). These additional metal elements M can be used singly or in combination of two or more.

[0052] Examples of the composite hydroxide containing nickel (Ni) and cobalt (Co) include those represented by the general formula Ni 1-x-y Co x M y O z (OH) 2-α (0 < x ≤ 0.3, 0 ≤ y ≤ 0.3, 0 ≤ z ≤ 3.00, -0.50 ≤ α < 2.00, where M represents one or more additional metal elements selected from the group consisting of Mn, Mg, Zr, Al, Ca, Ti, Nb, V, Cr, Mo, and W).

[0053] In addition, the additional metal element M may be contained only in the first metal-containing aqueous solution, may be contained only in the second metal-containing aqueous solution, or may be contained in both the first metal-containing aqueous solution and the second metal-containing aqueous solution. Therefore, the additional metal element M may be supplied to the reaction tank in a state of being contained only in the raw material solution containing nickel (Ni), may be supplied to the reaction tank in a state of being contained only in the raw material solution containing cobalt (Co), or may be supplied to the reaction tank in a state of being contained in both the raw material solution containing nickel (Ni) and the raw material solution containing cobalt (Co).

[0054] In the method for producing a composite hydroxide of the present invention, a first metal-containing aqueous solution containing a salt of nickel (Ni) (e.g., sulfate), a second metal-containing aqueous solution containing a salt of cobalt (Co) (e.g., sulfate), an aqueous solution containing an ammonium ion donor, and an alkali metal aqueous solution are independently added to a reaction tank by a coprecipitation method, thereby performing a neutralization reaction in the reaction tank to produce particles of a composite hydroxide containing nickel (Ni) and cobalt (Co), thereby obtaining a slurry-like suspension containing a composite hydroxide containing nickel (Ni) and cobalt (Co).

[0055] <Alkali Metal Aqueous Solution>

[0056] The alkali metal aqueous solution is a pH adjusting agent. As the alkali metal aqueous solution, sodium hydroxide, potassium hydroxide, etc. can be cited. In the method for producing the composite hydroxide of the present invention, the pH value of the mother solution in the reaction tank at a liquid temperature of 25°C is adjusted to a range of 10.0 to 13.0. The pH value of the mother solution in the reaction tank at a liquid temperature of 25°C is not particularly limited as long as it is in the range of 10.0 to 13.0, and is preferably in the range of 10.5 to 12.0.

[0057] <Ammonium ion donor>

[0058] The ammonium ion donor is a complexing agent. Ammonium ions can form complexes with nickel (Ni) ions, cobalt (Co) ions, and ions of the added metal element M. As ammonium ion donors, for example, ammonia, ammonium sulfate, ammonium chloride, ammonium carbonate, ammonium fluoride, etc. can be cited. In the manufacturing method of the composite hydroxide of the present invention, even if the usage amount of the ammonium ion concentration of the mother liquor in the reaction tank is suppressed, the composite hydroxide with the BET specific surface area properly controlled can be manufactured. Specifically, the ammonium ion concentration of the mother liquor in the reaction tank is adjusted to a range of more than 1.0g / L and less than 10.0g / L. In the manufacturing method of the composite hydroxide of the present invention, since the usage amount of the ammonium ion donor can be suppressed, the production cost can be reduced. As mentioned above, it is preferred that the ammonium ion concentration of the mother liquor in the reaction tank is adjusted to a range of more than 1.0g / L and less than 5.0g / L.

[0059] In addition, in the method for producing a composite hydroxide of the present invention, even if the reaction temperature of the mother liquor in the reaction tank is suppressed, a composite hydroxide with a properly controlled BET specific surface area can be produced. Specifically, even if the reaction temperature is controlled to be above 20°C and below 80°C, a composite hydroxide with a properly controlled BET specific surface area can be produced.

[0060] Next, an example of a reaction apparatus used in the method for producing the composite hydroxide of the present invention will be described. Figure 1 This is a side cross-sectional view schematically illustrating an example of a reaction apparatus used in the method for producing a composite hydroxide of the present invention.

[0061] like Figure 1 As shown, the reaction device 1 used in the method for producing a composite hydroxide of the present invention comprises a reaction tank 10 for storing a mother liquor 20, a first raw liquid supply unit 11 for supplying a first metal-containing aqueous solution 21 to the mother liquor 20 in the reaction tank 10, a second raw liquid supply unit 12 for supplying a second metal-containing aqueous solution 22 to the mother liquor 20 in the reaction tank 10, an alkali metal supply unit 13 for supplying an alkali metal aqueous solution 23 to the reaction tank 10, and an ammonium ion supply unit 14 for supplying an aqueous solution 24 containing an ammonium ion donor to the mother liquor 20 in the reaction tank 10.

[0062] The first raw material liquid supply part 11 is a tubular body having one end connected to the reaction tank 10 and the other end connected to a storage tank (not shown) storing the first metal-containing aqueous solution 21. The second raw material liquid supply part 12 is a tubular body having one end connected to the reaction tank 10 and the other end connected to a storage tank (not shown) storing the second metal-containing aqueous solution 22. The alkali metal supply part 13 is a tubular body having one end connected to the reaction tank 10 and the other end connected to a storage tank (not shown) storing the alkali metal aqueous solution 23. The ammonium ion supply part 14 is a tubular body having one end connected to the reaction tank 10 and the other end connected to a storage tank (not shown) storing the aqueous solution 24 containing an ammonium ion donor.

[0063] In the reaction apparatus 1, the first raw material solution supply unit 11 is arranged at a different position from the second raw material solution supply unit 12. In addition, the storage tank storing the first metal-containing aqueous solution 21 is a storage tank different from the storage tank storing the second metal-containing aqueous solution 22. Therefore, the first metal-containing aqueous solution 21 and the second metal-containing aqueous solution 22 are added to the reaction tank 10 through different paths.

[0064] In addition, a stirrer 17 is provided inside the reaction tank 10. The stirrer 17 mixes the first metal-containing aqueous solution 21 and the second metal-containing aqueous solution 22 contained in the mother liquor 20 stored in the reaction tank 10, the alkali metal aqueous solution 23 supplied from the alkali metal supply unit 13, and the aqueous solution 24 containing an ammonium ion donor supplied from the ammonium ion supply unit 14, thereby making the raw material concentration of the entire mother liquor 20 stored in the reaction tank 10 uniform.

[0065] As the agitator 17, for example, a stirring device having a stirring blade having a plurality of propeller blades at the front end of the stirring shaft can be cited. In addition, the stirring speed of the agitator 17 can be appropriately selected according to the volume of the reaction tank 10, the type of the stirring blade, and the residence time. For example, when the coprecipitation reaction is carried out using three propeller blades and the residence time is 10 to 25 hours, the stirring power is preferably 0.3 kW / m 3 Above and 4.0kW / m 3 Below, particularly preferably 1.8 kW / m 3 Above and 2.6kW / m 3 the following.

[0066] A slurry containing a composite hydroxide (composite hydroxide containing nickel (Ni) and cobalt (Co)) 25 is obtained from a reaction tank 10 in which a mother liquor 20 containing metal components from a first metal-containing aqueous solution 21 and a second metal-containing aqueous solution 22 having a uniform raw material concentration is stored. The composite hydroxide is a reaction product obtained by generation-growth. An overflow pipe 18 connected to the inside of the reaction tank 10 is provided on the side surface of the top side of the reaction tank 10, and the slurry 25 containing the target composite hydroxide is taken out from the reaction tank 10 to the outside through the overflow pipe 18.

[0067] As described above, the reaction device 1 is a reaction device having a continuous reaction tank 10, and the slurry 25 containing the target composite hydroxide is overflowed and recovered. Since the reaction tank 10 is a continuous type that overflows the slurry 25 containing the generated composite hydroxide, the production efficiency of the slurry 25 containing the composite hydroxide can be improved.

[0068] It should be noted that Figure 1 The reaction apparatus 1 shown in the figure is an overview of an example of a continuous reaction apparatus. The reaction apparatus used in the method for producing a composite hydroxide of the present invention is not limited to Figure 1 The reaction apparatus 1 shown in the figure only needs to have a structure in which the first metal-containing aqueous solution and the second metal-containing aqueous solution are added independently to the reaction tank. In addition, the reaction apparatus used in the method for producing the composite hydroxide of the present invention only needs to have a structure in which the first metal-containing aqueous solution and the second metal-containing aqueous solution are added independently to the reaction tank, and a batch reaction tank that is not discharged outside the system before the reaction in the reaction tank is completed can be substituted for the continuous reaction tank.

[0069] The composite hydroxide manufactured by the manufacturing method of the present invention can be used as a precursor of the positive electrode active material of a secondary battery. Next, the manufacturing method of the positive electrode active material using the composite hydroxide manufactured by the manufacturing method of the present invention as a precursor is described. For example, in the manufacturing method of the positive electrode active material using the composite hydroxide manufactured by the manufacturing method of the present invention as a precursor, first, a lithium compound is added to the composite hydroxide manufactured by the manufacturing method of the present invention to prepare a mixture of the composite hydroxide and the lithium compound. As a lithium compound, as long as it is a compound having lithium, it is not particularly limited, for example, lithium carbonate, lithium hydroxide, etc. can be cited.

[0070] Next, by firing the mixture obtained by the above operation, a positive electrode active material can be manufactured. As firing conditions, for example, a firing temperature of 700°C or more and 1000°C or less, a heating rate of 50°C / hour or more and 300°C / hour or less, and a firing time of 5 hours or more and 20 hours or less can be cited. There is no particular limitation on the firing atmosphere, for example, air, oxygen, etc. can be cited. In addition, as a firing furnace for firing, there is no particular limitation, for example, a stationary box furnace, a roller bottom continuous furnace, etc. can be cited.

[0071] Examples of secondary batteries using the composite hydroxide produced by the production method of the present invention include lithium ion secondary batteries.

[0072] Next, the composite hydroxide manufactured by the manufacturing method of the present invention is described in detail. The composite hydroxide of the present invention is a composite hydroxide containing at least nickel (Ni) and cobalt (Co), and the composite hydroxide has a first particle with a secondary particle size (D10) ±1.0 μm range of 10 volume % cumulative percentage, a second particle with a secondary particle size (D50) ±1.0 μm range of 50 volume % cumulative percentage, and a third particle with a secondary particle size (D90) ±1.0 μm range of 90 volume % cumulative percentage, and the BET specific surface area and volume cumulative percentage of the first particle are obtained. The absolute value of the change ratio of the secondary particle size (D50) of 50 volume % and the BET specific surface area and volume cumulative percentage of the secondary particle size (D50) of 50 volume % in the above-mentioned third particles is calculated using the following formula (1), and the product of the absolute value of the change ratio and the molar percentage of cobalt (Co) relative to the metal element contained in the above-mentioned composite hydroxide (wherein the metal element is Ni, Co, Mn, Mg, Zr, Al, Ca, Ti, Nb, V, Cr, Mo and W) is greater than 0 and less than 0.015.

[0073] |(BET specific surface area of ​​the third particle - BET specific surface area of ​​the first particle) / (D50 of the third particle - D50 of the first particle)| = absolute value of the change ratio ···Formula (1)

[0074] In the composite hydroxide with the previous particle size distribution, the BET specific surface area of ​​the small particle size is large compared with the large particle size. When the composite hydroxide and the lithium compound are fired, the contact area of ​​the composite hydroxide of the small particle size and the lithium compound per unit volume increases, and the reaction with the lithium compound is promoted compared with the composite hydroxide of the large particle size. Therefore, in the previous composite hydroxide, the composite hydroxide of the large particle size and the composite hydroxide of the small particle size have a great difference in the reactivity with the lithium compound, and as the composite hydroxide as a whole, the reaction with the lithium compound becomes uneven. If the reaction as the composite hydroxide as a whole with the lithium compound is uneven, it is possible to hinder battery characteristics or battery life.

[0075] In contrast, the composite hydroxide of the present invention, by having the above-mentioned structure, can suppress the change in BET specific surface area caused by the difference in particle size, that is, it can reduce the difference between the BET specific surface area of ​​the first particle, the BET specific surface area of ​​the second particle and the BET specific surface area of ​​the third particle, thereby making the reactivity of the composite hydroxide as a whole with metal compounds such as lithium compounds uniform, and improving battery characteristics.

[0076] When the composite hydroxide of the present invention is classified into small particles, i.e., first particles, having a secondary particle size in the range of D10±1.0μm, medium particles, i.e., second particles, having a secondary particle size in the range of D50±1.0μm, and large particles, i.e., third particles, having a secondary particle size in the range of D90±1.0μm, the absolute value of the ratio of the difference between the BET specific surface area of ​​the third particle and the BET specific surface area of ​​the first particle relative to the difference between the D50 of the third particle and the D50 of the first particle (hereinafter, the absolute value is sometimes referred to as the BET slope) is reduced, and as a result, the product of the BET slope and the molar percentage of cobalt (Co) relative to the metal elements (wherein the metal elements are Ni, Co, Mn, Mg, Zr, Al, Ca, Ti, Nb, V, Cr, Mo and W) contained in the composite hydroxide (hereinafter, sometimes referred to as the cobalt molar percentage) is suppressed to below 0.015. Since the composition of the composite hydroxide also has an influence on the BET specific surface area and battery characteristics of the composite hydroxide, the composition of the BET slope and the cobalt mole percentage is used as the characteristic of the composite hydroxide of the present invention. In addition, as a method for classifying the composite hydroxide of the present invention into the first particle, the second particle and the third particle, air flow classification can be cited.

[0077] The value of the product of the BET slope and the cobalt mole percentage is not particularly limited as long as it is 0 or more and 0.015 or less. From the viewpoint of further homogenizing the reactivity of the composite hydroxide as a whole with the lithium compound and further improving the battery characteristics, it is preferably 0.013 or less, and particularly preferably 0.011 or less.

[0078] Examples of the composite hydroxide of the present invention include those represented by the general formula Ni 1-x-y Co x M y O z (OH) 2-α (0 < x + y < 0.20, 0 ≤ z ≤ 3.00, -0.50 ≤ α < 2.00, where M represents one or more additive metal elements selected from the group consisting of Mn, Mg, Zr, Al, Ca, Ti, Nb, V, Cr, Mo, and W). In the composite hydroxide of the above general formula, the content of nickel (Ni) is more than 80 mol% relative to the total of nickel (Ni), cobalt (Co), and the additive metal element (M).

[0079] In addition, in the composite hydroxide represented by the general formula Ni 1-x-y Co x M y O z (OH) 2-α it is preferable that 0.02 < x < 0.20, that is, cobalt (Co) is contained in a range of more than 2 mol% and less than 20 mol% relative to the total of nickel (Ni), cobalt (Co), and the additive metal element (M).

[0080] The composite hydroxide of the present invention has a predetermined particle size distribution interval, for example, the value of (D90 of the composite hydroxide - D10 of the composite hydroxide) / D50 of the composite hydroxide, which is an index of particle size distribution, is in the range of 0.50 or more and 1.40 or less. By making the value of (D90 of the composite hydroxide - D10 of the composite hydroxide) / D50 of the composite hydroxide 0.50 or more and 1.40 or less, the loading density of the positive electrode active material using the composite hydroxide of the present invention as a precursor on the positive electrode can be increased, and more excellent battery characteristics can be exerted. The value of (D90 of the composite hydroxide - D10 of the composite hydroxide) / D50 of the composite hydroxide is not particularly limited. From the viewpoint of increasing the loading density of the positive electrode, the lower limit of the value of (D90 of the composite hydroxide - D10 of the composite hydroxide) / D50 of the composite hydroxide is preferably 0.65 or more, and particularly preferably 0.80 or more. In addition, the BET specific surface area of ​​the composite hydroxide of the present invention is not particularly limited. From the viewpoint of controlling the reactivity with metal compounds such as lithium compounds, its upper limit is preferably 50.0 or less, more preferably 25.0 or less, and particularly preferably 15.0 or less. In addition, the lower limit of the BET specific surface area is preferably 3.0 or more, more preferably 4.5 or more, and particularly preferably 6.0 or more.

[0081] Example

[0082] Next, a method for producing the composite hydroxide of the present invention and examples of the composite hydroxide of the present invention will be described, but the present invention is not limited to these examples unless the gist of the present invention is exceeded.

[0083] Preparation of Composite Hydroxides in Examples and Comparative Examples

[0084] Preparation of the composite hydroxide of Example 1

[0085] The composition of the composite hydroxide is shown in Table 1 below. Aqueous solution containing cobalt (corresponding to the first metal-containing aqueous solution), a cobalt sulfate aqueous solution containing no nickel (corresponding to the second metal-containing aqueous solution), an aqueous solution of ammonium sulfate (corresponding to an aqueous solution containing an ammonium ion donor), and an aqueous solution of sodium hydroxide (corresponding to an alkali metal aqueous solution) are mixed in a specified amount. The pH of the mixed solution in the reaction tank is maintained at 11.7 at a liquid temperature of 25°C, and the ammonia concentration is maintained at 4.4 g / L, while stirring continuously with a stirrer. In addition, the liquid temperature (reaction temperature) of the mixed solution in the reaction tank is maintained at 70°C. The slurry containing the generated composite hydroxide particles is overflowed from the overflow pipe of the reaction tank and taken out. The slurry of the composite hydroxide particles collected after more than 41.7 hours from the start of the reaction is washed with an alkali aqueous solution and water in turn, and dehydrated and dried to obtain a composite hydroxide. The composition and manufacturing conditions of the composite hydroxide of Example 1 above are shown in Table 1 below.

[0086] Preparation of the composite hydroxide of Example 2

[0087] The composition of the composite hydroxide is shown in Table 1 below. A cobalt sulfate aqueous solution, a manganese sulfate aqueous solution and a magnesium sulfate aqueous solution are mixed in a specified amount and an aqueous solution that does not contain nickel (corresponding to the second metal-containing aqueous solution), a cobalt-free nickel sulfate aqueous solution (corresponding to the first metal-containing aqueous solution), an ammonium sulfate aqueous solution (corresponding to an aqueous solution containing an ammonium ion donor), and a sodium hydroxide aqueous solution (corresponding to an alkali metal aqueous solution) are added dropwise to the reaction tank independently and simultaneously, while the pH of the mixed solution in the reaction tank is maintained at 11.2 at a liquid temperature of 25°C, and the ammonia concentration is maintained at 3.7g / L, while stirring continuously with a stirrer. In addition, the liquid temperature (reaction temperature) of the mixed solution in the reaction tank is maintained at 70°C. The slurry containing the generated composite hydroxide particles is overflowed from the overflow pipe of the reaction tank and taken out. The slurry of the composite hydroxide particles collected after more than 42.0 hours from the start of the reaction is washed with an alkali aqueous solution and water in turn, and each treatment of dehydration and drying is implemented to obtain a composite hydroxide. The composition and manufacturing conditions of the composite hydroxide of Example 2 above are shown in Table 1 below.

[0088] Preparation of composite hydroxide of Comparative Example 1

[0089] The composition of the composite hydroxide is shown in Table 1 below. A metal salt aqueous solution, an ammonium sulfate aqueous solution (ammonium ion donor) and a sodium hydroxide aqueous solution mixed with a specified amount of nickel sulfate aqueous solution, a cobalt sulfate aqueous solution, a manganese sulfate aqueous solution and a magnesium sulfate aqueous solution are added dropwise to the reaction tank independently and simultaneously, while the pH of the mixed solution in the reaction tank is maintained at 11.5 at a liquid temperature of 25°C, and the ammonia concentration is maintained at 3.7g / L, while stirring continuously with a stirrer. In addition, the liquid temperature of the mixed solution in the reaction tank is maintained at 70°C. The slurry containing the generated composite hydroxide particles is overflowed from the overflow pipe of the reaction tank and taken out. The slurry of the composite hydroxide particles collected after more than 41.7 hours from the start of the reaction is washed with an alkaline aqueous solution and water in turn, and each treatment of dehydration and drying is implemented to obtain a composite hydroxide. The composition and manufacturing conditions of the composite hydroxide of the above-mentioned Comparative Example 1 are shown in Table 1 below.

[0090] Preparation of composite hydroxide of Comparative Example 2

[0091] A composite hydroxide was obtained in the same manner as in Comparative Example 1 except that the pH was 11.9 at a liquid temperature of 25° C. and the ammonia concentration was 6.0 g / L. The composition and production conditions of the composite hydroxide of Comparative Example 2 are shown in Table 1 below.

[0092] Preparation of the composite hydroxide of Example 3

[0093] The composition of the composite hydroxide is shown in Table 2 below. A cobalt-free aqueous solution (corresponding to the first metal-containing aqueous solution) containing a mixture of a nickel sulfate aqueous solution and a manganese sulfate aqueous solution, a nickel-free cobalt sulfate aqueous solution (corresponding to the second metal-containing aqueous solution), an ammonium sulfate aqueous solution (ammonium ion donor) and a sodium hydroxide aqueous solution are added dropwise to the reaction tank independently and simultaneously, while the pH of the mixed solution in the reaction tank is maintained at 10.9 at a liquid temperature of 25°C, and the ammonia concentration is maintained at 4.7 g / L, while stirring continuously with a stirrer. In addition, the liquid temperature of the mixed solution in the reaction tank is maintained at 70°C. The slurry containing the generated composite hydroxide particles is taken out by overflowing from the overflow pipe of the reaction tank. The slurry of the composite hydroxide particles collected after more than 41.7 hours from the start of the reaction is washed with an alkaline aqueous solution and water in turn, and dehydrated and dried to obtain a composite hydroxide. The composition and manufacturing conditions of the composite hydroxide of Example 3 above are shown in Table 2 below.

[0094] Preparation of composite hydroxide of Comparative Example 3

[0095] The composition of the composite hydroxide is shown in Table 2 below. A metal salt aqueous solution, an ammonium sulfate aqueous solution (ammonium ion donor) and a sodium hydroxide aqueous solution mixed with a specified amount of nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution are added dropwise to the reaction tank independently and simultaneously, while the pH of the mixed solution in the reaction tank is maintained at 11.4 at a liquid temperature of 25°C, and the ammonia concentration is maintained at 4.4g / L, while stirring continuously with a stirrer. In addition, the liquid temperature of the mixed solution in the reaction tank is maintained at 50°C. The slurry containing the generated composite hydroxide particles is taken out by overflowing from the overflow pipe of the reaction tank. The slurry of the composite hydroxide particles collected after more than 41.7 hours from the start of the reaction is washed with an alkaline aqueous solution and water in turn, and each treatment of dehydration and drying is implemented to obtain a composite hydroxide. The composition and manufacturing conditions of the composite hydroxide of the above-mentioned Comparative Example 3 are shown in Table 2 below.

[0096] Preparation of composite hydroxide of Comparative Example 4

[0097] A composite hydroxide was obtained in the same manner as in Comparative Example 3 except that the pH was maintained at 11.1 at a liquid temperature of 25°C, the ammonia concentration was maintained at 4.7 g / L, and the liquid temperature of the mixed liquid in the reaction tank was maintained at 70°C. The composition and production conditions of the composite hydroxide of Comparative Example 4 are shown in Table 2 below.

[0098] Preparation of the composite hydroxide of Example 4

[0099] The composition of the composite hydroxide is shown in Table 3 below. A cobalt-free aqueous solution (corresponding to the first metal-containing aqueous solution) and a nickel-free cobalt sulfate aqueous solution (corresponding to the second metal-containing aqueous solution) are used to dissolve a nickel sulfate aqueous solution and a manganese sulfate aqueous solution in a specified amount, and the pH is maintained at 11.4 at a liquid temperature of 25°C, the ammonia concentration is maintained at 2.1 g / L, the liquid temperature of the mixed solution in the reaction tank is maintained at 71°C, and the slurry of the composite hydroxide particles collected after more than 51.0 hours from the start of the reaction is washed with an alkaline aqueous solution and water in sequence, and each treatment of dehydration and drying is performed to obtain a composite hydroxide. The composite hydroxide is obtained in the same manner as in Example 3 except that the above-mentioned composition and manufacturing conditions of the composite hydroxide of Example 4 are shown in Table 3 below.

[0100] Preparation of the composite hydroxide of Example 5

[0101] The composition of the composite hydroxide is shown in Table 3 below. A cobalt sulfate aqueous solution and a manganese sulfate aqueous solution are dissolved in a predetermined amount and an aqueous solution containing no nickel (corresponding to the second metal-containing aqueous solution) and a cobalt-free nickel sulfate aqueous solution (corresponding to the first metal-containing aqueous solution) are used, the pH is maintained at 11.0 at a liquid temperature of 25°C, the ammonia concentration is maintained at 2.3 g / L, and the slurry of the composite hydroxide particles collected after more than 48.6 hours from the start of the reaction is washed with an alkaline aqueous solution and water in sequence, and each treatment of dehydration and drying is performed to obtain a composite hydroxide. The composite hydroxide is obtained in the same manner as in Example 4. The composition and manufacturing conditions of the composite hydroxide of Example 5 are shown in Table 3 below.

[0102] Preparation of composite hydroxide of Comparative Example 5

[0103] A metal salt aqueous solution mixed with a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution was used instead of the first metal-containing aqueous solution and the second metal-containing aqueous solution, the liquid temperature of the mixed solution in the reaction tank was set to 60°C, the pH was set to 11.7 at a liquid temperature of 25°C, the ammonia concentration was 2.0 g / L, and the slurry of the composite hydroxide particles collected after more than 49.2 hours from the start of the reaction was washed in the order of an alkaline aqueous solution and water, and each treatment of dehydration and drying was performed to obtain a composite hydroxide. A composite hydroxide was obtained in the same manner as in Example 4. The composition and production conditions of the composite hydroxide of the above-mentioned Comparative Example 5 are shown in Table 3 below.

[0104] Preparation of Composite Hydroxide of Comparative Example 6

[0105] A metal salt aqueous solution mixed with a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution was used instead of the first metal-containing aqueous solution and the second metal-containing aqueous solution, the pH was set to 11.0 at a liquid temperature of 25°C, the ammonia concentration was set to 1.7 g / L, and the slurry of composite hydroxide particles collected after more than 50.1 hours from the start of the reaction was washed in the order of an alkaline aqueous solution and water, and dehydrated and dried to obtain a composite hydroxide. The composite hydroxide was obtained in the same manner as in Example 4. The composition and production conditions of the composite hydroxide of Comparative Example 6 are shown in Table 3 below.

[0106] Preparation of the composite hydroxide of Example 6

[0107] The composition of the composite hydroxide is shown in Table 4 below. A cobalt-free aqueous solution (corresponding to the first metal-containing aqueous solution) and a nickel-free cobalt sulfate aqueous solution (corresponding to the second metal-containing aqueous solution) are mixed in a predetermined amount, and the pH is maintained at 11.3 at a liquid temperature of 25°C, and the ammonia concentration is maintained at 3.1 g / L. The liquid temperature of the mixed solution in the reaction tank is maintained at 75°C, and the slurry of the composite hydroxide particles collected after more than 32.7 hours from the start of the reaction is washed with an alkaline aqueous solution and water in sequence, and each treatment of dehydration and drying is performed to obtain a composite hydroxide. The composite hydroxide is obtained in the same manner as in Example 3 except that the above-mentioned composition and manufacturing conditions of the composite hydroxide of Example 6 are shown in Table 4 below.

[0108] Preparation of Composite Hydroxide of Comparative Example 7

[0109] A composite hydroxide was obtained in the same manner as in Example 6 except that a metal salt aqueous solution in which a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution were mixed was used instead of the first metal-containing aqueous solution and the second metal-containing aqueous solution, the pH was maintained at 11.0 at a liquid temperature of 25° C., the ammonia concentration was maintained at 2.6 g / L, and the liquid temperature of the mixed liquid in the reaction tank was maintained at 70° C. The composition and production conditions of the composite hydroxide of Comparative Example 7 are shown in Table 4 below.

[0110] Preparation of Composite Hydroxide of Comparative Example 8

[0111] A composite hydroxide was obtained in the same manner as in Example 6 except that a metal salt aqueous solution obtained by mixing a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution was used instead of the first metal-containing aqueous solution and the second metal-containing aqueous solution, the ammonia concentration was maintained at 3.7 g / L, and the liquid temperature of the mixed solution in the reaction tank was maintained at 80° C. The composition and production conditions of the composite hydroxide of Comparative Example 8 are shown in Table 4 below.

[0112] Evaluation of the produced composite hydroxide

[0113] (1) Secondary particle size at 50% cumulative volume percentage (D50)

[0114] The obtained composite hydroxide was measured using a particle size distribution measuring device (MT3300EX II manufactured by Nikkiso Co., Ltd. in Examples 1, 2, 4 to 6 and Comparative Examples 1, 2, 5 to 8, and LA-950 manufactured by Horiba Ltd. in Example 3 and Comparative Examples 3 and 4) (the principle of any device is the laser diffraction scattering method). In addition, the measuring conditions of the particle size distribution measuring device are as follows. Solvent: water, solvent refractive index: 1.33, particle refractive index: 1.55, transmittance 80±5%, dispersion medium: 10.0 mass% sodium hexametaphosphate aqueous solution.

[0115] (2) Tap density (TD)

[0116] The obtained composite hydroxide was measured for tap density by constant volume measurement using a tap density meter (manufactured by Seishin Enterprise Co., Ltd., KYT-4000). In addition, the measurement conditions of TD are as follows. Battery capacity: 20 cc, stroke length: 10 mm, number of taps: 200 times (500 times in Example 3 and Comparative Examples 3 and 4).

[0117] (3) BET specific surface area

[0118] 0.3 g of the obtained composite hydroxide was dried at 105° C. for 30 minutes in a nitrogen atmosphere, and then measured by a single-point BET method using a specific surface area measuring apparatus (Macsorb, manufactured by Mountech Co., Ltd.).

[0119] The evaluation results of the physical properties of the composite hydroxides of Examples and Comparative Examples are shown in Tables 1 to 4 below.

[0120] Table 1

[0121]

[0122] Table 2

[0123]

[0124] Table 3

[0125]

[0126] Table 4

[0127]

[0128] As can be seen from Table 1, in the composite hydroxides of Examples 1 and 2, in which the first metal-containing aqueous solution containing nickel (Ni) but not cobalt (Co) and the second metal-containing aqueous solution containing cobalt (Co) but not nickel (Ni) are independently and simultaneously added to the reaction tank, the ammonia concentrations are 4.4 g / L and 3.7 g / L, respectively, and by adding a small amount, the BET specific surface area can be suppressed to 15.1 m 2 / g, 10.7m 2 / g. In addition, the tap density was 2.11 g / ml and 2.01 g / ml, respectively, and excellent tap density was obtained. The composition of the composite hydroxide of Examples 1 and 2 was Ni:Co:Mn:Mg=94.8:4.7:0.26:0.26, and D50 was 11.2 μm and 10.6 μm, respectively.

[0129] As can be seen from Table 1, for the composite hydroxide of Ni:Co:Mn:Mg=94.8:4.7:0.26:0.26, although the reaction conditions are the same as those in Examples 1 and 2 and the D50 is the same, in Comparative Example 1 in which nickel (Ni) and cobalt (Co) are added to the same raw material solution, the BET specific surface area is 24.8 m 2 / g, the BET specific surface area cannot be suppressed. In addition, although D50 is the same as that of Examples 1 and 2, in Comparative Example 2 in which nickel (Ni) and cobalt (Co) are added using the same raw material solution, the BET specific surface area can be suppressed to some extent by setting the ammonia concentration to 6.0 g / L. Therefore, in Comparative Example 2, the amount of ammonium ion donor used is increased, and the production cost of the composite hydroxide cannot be reduced.

[0130] As can be seen from Table 2, in Example 3 in which the first metal-containing aqueous solution containing nickel (Ni) but not containing cobalt (Co) and the second metal-containing aqueous solution containing cobalt (Co) but not containing nickel (Ni) are independently and simultaneously added to the reaction tank, the ammonia concentration is 4.7 g / L, and the BET specific surface area can be suppressed to 5.1 m by adding a small amount of ammonia. 2 / g. Moreover, the tap density was 2.26 g / ml, which was an excellent tap density. The composition of the composite hydroxide of Example 3 was Ni:Co:Mn=55:20:25, and D50 was 12.5 μm.

[0131] As shown in Table 2, for the composite hydroxide of Ni:Co:Mn=55:20:25, the BET specific surface area increased to 9.4 m2 in Comparative Example 3 in which the reaction temperature was as low as 50°C and nickel (Ni) and cobalt (Co) were added to the same raw material solution. 2 / g, the BET specific surface area cannot be suppressed. In addition, in Comparative Example 4, in which the reaction conditions were set to be the same as those in Example 3 and the D50 was the same, but nickel (Ni) and cobalt (Co) were added to the same raw material solution, the BET specific surface area was 6.2 m 2 / g, it still cannot suppress the BET specific surface area.

[0132] As can be seen from Table 3, in the composite hydroxides of Examples 4 and 5 in which the first metal-containing aqueous solution containing nickel (Ni) but not cobalt (Co) and the second metal-containing aqueous solution containing cobalt (Co) but not nickel (Ni) are independently and simultaneously added to the reaction tank, the ammonia concentrations are 2.1 g / L and 2.3 g / L, respectively, and by adding a small amount, the BET specific surface area can be suppressed to 6.6 m 2 / g, 6.0m 2 / g. Moreover, the tap density was 2.04 g / ml and 2.00 g / ml, respectively, and excellent tap density was obtained. The composition of the composite hydroxide of Examples 4 and 5 was Ni:Co:Mn=83.1:12.1:4.9, and D50 was 10.4 μm and 10.1 μm, respectively.

[0133] As shown in Table 3, for the composite hydroxide of Ni:Co:Mn=83.1:12.1:4.9, when the reaction temperature is as low as 60°C and nickel (Ni) and cobalt (Co) are added to the same raw material solution, the BET specific surface area increases to 11.1 m 2 / g, the BET specific surface area cannot be suppressed. In addition, in Comparative Example 6, in which the reaction conditions were set to be the same as those of Examples 4 and 5 and the D50 was the same, but nickel (Ni) and cobalt (Co) were added to the same raw material solution, the BET specific surface area was 10.8 m 2 / g, it still cannot suppress the BET specific surface area.

[0134] As can be seen from Table 4, in Example 6 in which the first metal-containing aqueous solution containing nickel (Ni) but not containing cobalt (Co) and the second metal-containing aqueous solution containing cobalt (Co) but not containing nickel (Ni) are independently and simultaneously added to the reaction tank, the BET specific surface area can be suppressed to 8.4 m by suppressing the reaction temperature to 75°C, the ammonia concentration to 3.1 g / L and adding a small amount. 2 / g. Moreover, the tap density was 2.05 g / ml, which was an excellent tap density. The composition of the composite hydroxide of Example 6 was Ni:Co:Mn=83.1:12.1:4.9, and D50 was 10.8 μm.

[0135] In contrast, as shown in Table 4 above, for the composite hydroxide of Ni:Co:Mn=83.1:12.1:4.9, in Comparative Example 7 in which the reaction temperature is 70°C, the ammonia concentration is 2.6 g / L, the reaction temperature and the ammonia concentration are both low, and nickel (Ni) and cobalt (Co) are added to the same raw material solution, the BET specific surface area increases to 14.2 m 2 / g, the BET specific surface area cannot be suppressed. In addition, in Comparative Example 8 in which the reaction temperature is 80°C, the ammonia concentration is 3.7 g / L, the reaction temperature and the ammonia concentration are increased compared with Example 6, and nickel (Ni) and cobalt (Co) are added using the same raw material solution, the BET specific surface area can be suppressed to be equivalent to that of Example 6. Therefore, in Comparative Example 8, it is impossible to reduce energy consumption, and it is impossible to suppress the amount of ammonium ions used, and thus it is impossible to suppress the production cost of the composite hydroxide.

[0136] In addition, among the composite hydroxides of Examples 1 to 6 and Comparative Examples 1 to 8, for the composite hydroxides of Examples 1, 2, 4 to 6 and Comparative Examples 1, 2, 6 and 7, the secondary particle diameter (D10) at a volume cumulative percentage of 10% and the secondary particle diameter (D90) at a volume cumulative percentage of 90% were measured in the same manner as the evaluation method for the secondary particle diameter (D50) at a volume cumulative percentage of 50%. The value of (D90-D10) / D50 as a particle size distribution index was calculated from D10, D50 and D90 of the composite hydroxide.

[0137] Furthermore, for the composite hydroxides of Examples 1, 2, 4 to 6 and the composite hydroxides of Comparative Examples 1, 2, 6 and 7, the composite hydroxides are classified by airflow classification into the first particle whose secondary particle size D50 after classification is in the range of D10±1.0μm of the composite hydroxide, the second particle whose secondary particle size D50 after classification is in the range of D50±1.0μm of the composite hydroxide, and the third particle whose secondary particle size D50 after classification is in the range of D90±1.0μm of the composite hydroxide. For the first particle and the third particle obtained by classifying the composite hydroxide, the secondary particle size (D50) with a volume cumulative percentage of 50 volume% is measured in the same manner as the evaluation method of the secondary particle size (D50) with a volume cumulative percentage of 50 volume%. In addition, for the first particle and the third particle, the BET specific surface area is measured in the same manner as the evaluation method of the BET specific surface area. The BET slope was calculated from the D50 and BET specific surface area of ​​the first and third particles, and the product of the BET slope and the molar percentage of cobalt was calculated from the calculated BET slope and the composition.

[0138] The results of each of the above items are shown in Table 5 below.

[0139] [Table 5]

[0140]

[0141] (4) Thermogravimetric measurement (TG measurement)

[0142] In the composite hydroxides of Examples 1, 2, 4 to 6 and the composite hydroxides of Comparative Examples 1, 2, 6 and 7, the first and third particles of the composite hydroxides of Examples 1, 2, 6 and Comparative Examples 1, 2, 7 were respectively mixed with lithium hydroxide monohydrate and lithium hydroxide at a molar ratio of lithium / total metal elements = 1.05, and TG measurement was performed under the conditions of a heating rate of 10°C / min, an oxygen supply of 200ml / min, and a sampling frequency of 1 time / 1 second. In addition, DTG was calculated by differentiating the TG data. From the relationship between DTG and temperature, the peak top temperature of the first particle and the third particle, which is believed to be derived from the reaction of the composite hydroxide with lithium, was obtained, and then the difference between the above-mentioned peak top temperature of the first particle and the above-mentioned peak top temperature of the third particle was obtained.

[0143] The evaluation results of the TG measurement are shown in Table 6 below.

[0144] Table 6

[0145]

[0146] As shown in Tables 5 and 6 above, in Examples 1, 2, and 6 where the product of the BET slope and the molar percentage of cobalt is less than 0.015, the difference between the first particle and the third particle is reduced to less than 11.3°C for the peak temperature of about 300°C, which is believed to be derived from the reaction of the composite hydroxide with lithium. Therefore, it can be seen that, including Examples 1, 2, and 6, in Examples 1 to 6 where the product of the BET slope and the molar percentage of cobalt is less than 0.015, the reactivity of the composite hydroxide as a whole with the lithium compound is uniformized, and the battery characteristics such as cycle characteristics can be improved. In addition, the values ​​of (D90-D10) / D50 of the composite hydroxides of Examples 1, 2, 4 to 6 are in the range of 1.07 to 1.15, and have a particle size distribution range of the same degree as that of conventional composite hydroxides.

[0147] On the other hand, in Comparative Examples 1, 2, and 7 where the product of the BET slope and the cobalt mole percentage exceeds 0.015, the difference between the first particle and the third particle at the peak top temperature near 300° C. is 14.8° C. or more. Therefore, it can be seen that in Comparative Examples 1 to 8 where the product of the BET slope and the cobalt mole percentage exceeds 0.015, including Comparative Examples 1, 2, and 7, the reactivity of the composite hydroxide as a whole with the lithium compound is not uniform, and the battery characteristics such as the cycle characteristics cannot be sufficiently improved.

[0148] Industrial Applicability

[0149] The manufacturing method of the composite hydroxide containing nickel (Ni) and cobalt (Co) of the present invention can appropriately control the BET specific surface area without damaging the tap density, thereby appropriately adjusting the reactivity with lithium, and in addition, since the production cost can be reduced, the utilization value is high in the field of the positive active material of the lithium ion secondary battery. In addition, the composite hydroxide containing nickel (Ni) and cobalt (Co) of the present invention can improve battery characteristics such as cycle characteristics due to the homogenization of the reactivity with lithium regardless of the size of the particle size, and thus the utilization value is high in the field of the positive active material of the lithium ion secondary battery.

[0150] Explanation of symbols

[0151] 1. Reaction apparatus

[0152] 10 Reaction tank

[0153] 21. The first metal-containing aqueous solution

[0154] 22. The second metal-containing aqueous solution

Claims

1. A method for producing a composite hydroxide, comprising: a method for producing a composite hydroxide containing nickel (Ni), cobalt (Co) and one or more metal elements M selected from the group consisting of manganese (Mn), magnesium (Mg), aluminum (Al), calcium (Ca), titanium (Ti), vanadium (V), chromium (Cr), zirconium (Zr), niobium (Nb), molybdenum (Mo) and tungsten (W), wherein: The following solutions are independently and simultaneously supplied to the reaction tank in the following manner, that is, a first metal-containing aqueous solution containing A mol % of nickel (Ni) and B mol % of cobalt (Co) is supplied to the reaction tank by a first raw material solution supply part having one end connected to the reaction tank; a second metal-containing aqueous solution containing C mol % of nickel (Ni) and D mol % of cobalt (Co) is supplied to the reaction tank by a second raw material solution supply part having one end connected to the reaction tank and arranged at a position different from the first raw material solution supply part; an alkali metal aqueous solution is supplied to the reaction tank by an alkali metal supply part having one end connected to the reaction tank into a reaction tank; an aqueous solution containing an ammonium ion donor is supplied to the reaction tank by an ammonium ion supply unit having one end connected to the reaction tank, wherein the added metal element M is contained only in the first metal-containing aqueous solution, or only in the second metal-containing aqueous solution, or in both the first metal-containing aqueous solution and the second metal-containing aqueous solution, and the pH value of the solution in the reaction tank is maintained at a range of 10.0 to 13.0 at a liquid temperature of 25° C., and the ammonium ion concentration is maintained at a range of 1.0 g / L to 10.0 g / L, wherein A>C, B <D、A+B=100、C+D=100。 2. The method for producing a composite hydroxide according to claim 1, wherein The ratio of A to C is 5 or more, and the ratio of D to B is 5 or more.

3. The method for producing a composite hydroxide according to claim 1, wherein The first metal-containing aqueous solution does not contain cobalt (Co), and the second metal-containing aqueous solution does not contain nickel (Ni).

4. The method for producing a composite hydroxide according to any one of claims 1 to 3, wherein The nickel of the composite hydroxide 1-x-y Co x M y O z (OH) 2-α is represented by 0 < x ≤ 0.3, 0 ≤ y ≤ 0.3, 0 ≤ z ≤ 3.00, -0.50 ≤ α < 2.00, where M represents one or more additive metal elements selected from the group consisting of Mn, Mg, Zr, Al, Ca, Ti, Nb, V, Cr, Mo, and W.

5. The method for producing a composite hydroxide according to any one of claims 1 to 3, wherein The reaction tank is a continuous reaction tank that allows the generated composite hydroxide to overflow.

6. The method for producing a composite hydroxide according to claim 4, wherein The reaction tank is a continuous reaction tank that allows the generated composite hydroxide to overflow.

7. The method for producing a composite hydroxide according to any one of claims 1 to 3, wherein The ammonium ion concentration in the reaction tank is maintained in a range of 1.0 g / L or more and 5.0 g / L or less.

8. The method for producing a composite hydroxide according to claim 4, wherein The ammonium ion concentration in the reaction tank is maintained in a range of 1.0 g / L or more and 5.0 g / L or less.

9. The method for producing a composite hydroxide according to claim 5, wherein: The ammonium ion concentration in the reaction tank is maintained in a range of 1.0 g / L or more and 5.0 g / L or less.

10. The method for producing a composite hydroxide according to claim 6, wherein: The ammonium ion concentration in the reaction tank is maintained in a range of 1.0 g / L or more and 5.0 g / L or less.

11. The method for producing a composite hydroxide according to any one of claims 1 to 3, 6, and 8 to 10, wherein: The reaction temperature in the reaction tank is 20° C. or higher and 80° C. or lower.

12. The method for producing a composite hydroxide according to claim 4, wherein: The reaction temperature in the reaction tank is 20° C. or higher and 80° C. or lower.

13. The method for producing a composite hydroxide according to claim 5, wherein: The reaction temperature in the reaction tank is 20° C. or higher and 80° C. or lower.

14. The method for producing a composite hydroxide according to claim 7, wherein: The reaction temperature in the reaction tank is 20° C. or higher and 80° C. or lower.

15. A composite hydroxide, which is a composite hydroxide containing at least nickel (Ni) and cobalt (Co), and is obtained by the method for producing a composite hydroxide according to any one of claims 1 to 14, in, Determine the secondary particle size D10 of the composite hydroxide with a volume cumulative percentage of 10 volume%, the secondary particle size D50 with a volume cumulative percentage of 50 volume%, and the secondary particle size D90 with a volume cumulative percentage of 90 volume%, and classify the composite hydroxide into: a first particle with a secondary particle size D50 of the composite hydroxide within a range of D10±1.0 μm after classification, a second particle with a secondary particle size D50 of the composite hydroxide within a range of D50±1.0 μm after classification, and a third particle with a secondary particle size D50 of the composite hydroxide within a range of D90±1.0 μm after classification, and measure the BET specific surface area and the secondary particle size D50 with a volume cumulative percentage of 50 volume% for the first particle and the third particle, The absolute value of the change ratio is calculated using the following formula (1) from the BET specific surface area of ​​the first particle and the secondary particle size D50 with a volume cumulative percentage of 50 volume % and the BET specific surface area of ​​the third particle and the secondary particle size D50 with a volume cumulative percentage of 50 volume %, and the product of the absolute value of the change ratio and the molar percentage of cobalt (Co) contained in the composite hydroxide relative to the metal element contained in the composite hydroxide is greater than 0 and less than 0.015, wherein the metal element is nickel (Ni), cobalt (Co) and one or more additional metal elements M selected from the group consisting of manganese (Mn), magnesium (Mg), aluminum (Al), calcium (Ca), titanium (Ti), vanadium (V), chromium (Cr), zirconium (Zr), niobium (Nb), molybdenum (Mo) and tungsten (W), |(BET specific surface area of ​​the third particle−BET specific surface area of ​​the first particle) / (D50 of the third particle−D50 of the first particle)|=absolute value of the change ratio···Formula (1).

16. The composite hydroxide according to claim 15, wherein The nickel of the composite hydroxide 1-x-y Co x M y O z (OH) 2-α is represented by 0 < x + y < 0.20, 0 ≤ z ≤ 3.00, -0.50 ≤ α < 2.00, and M represents one or more additive metal elements selected from the group consisting of Mn, Mg, Zr, Al, Ca, Ti, Nb, V, Cr, Mo, and W.

17. The composite hydroxide according to claim 16, wherein In the Ni 1-x-y Co x M y O z (OH) 2-α Medium, 0.02 <x<0.20。 18. The composite hydroxide according to any one of claims 15 to 17, wherein The value of (D90 of the composite hydroxide - D10 of the composite hydroxide) / D50 of the composite hydroxide is 0.50 or more and 1.40 or less.

19. Use of the composite hydroxide according to any one of claims 15 to 18 as a precursor of a positive electrode active material for a secondary battery.