Method for electrodeposition of nanocrystalline pure copper based on copper methanesulfonate electrolyte system
Through the electrodeposition method based on the copper methane sulfonate electrolyte system, the problems of low deposition efficiency and uneven grain size of nanocrystalline pure copper are solved, and efficient and low-cost preparation of nanocrystalline pure copper is achieved, which significantly improves the deposition rate. Rate and density uniformity.
Patent Information
- Application Number
- CN202110544896.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-19
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-05-19
AI Technical Summary
The existing technology has problems such as low deposition efficiency, uneven grain size, high residual stress and high cost when preparing nanocrystalline pure copper. Especially when depositing a thicker pure copper coating is required, the Cu2+ concentration of the copper sulfate system is limited, resulting in a slower deposition rate.
Adopt an electrolyte system based on copper methane sulfonate, by formulating an electrolyte containing copper methane sulfonate, diaminoethylene tetraacetate, nitrilotriacetic acid, ammonium nitrate and cetyltrimethylammonium bromide, combined with appropriate The electrical parameters and pretreatment steps achieve efficient electrodeposition of nanocrystalline pure copper.
It increases the copper ion concentration and conductivity, increases the nucleation rate and deposition rate, prepares nanocrystalline pure copper with high density, low porosity and uniform grain size, and reduces electroplating time and cost.
Smart Images

Figure CN115369458B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano material preparation, and relates to a method for electrodepositing nanocrystalline pure copper based on a copper methanesulfonate electrolyte system. Background Art
[0002] Copper materials are widely used due to their excellent properties such as high thermal conductivity, electrical conductivity, and ductility. Nanocrystalline copper has a small grain size and a significant structural feature of containing a large number of internal interfaces. Therefore, it has surface and interface effects, small size effects, quantum size effects, and macroscopic quantum tunneling effects that are different from traditional solid materials, and exhibits special physical and mechanical properties. Compared with ordinary coarse-grained copper, the tiny tensile specimens of nanocrystalline copper exhibit higher yield strength, and high-density nano-twinned pure copper also exhibits better plasticity.
[0003] At present, the methods for preparing nanocrystalline metal materials include metal evaporation condensation-in-situ cold pressing, mechanical grinding, amorphous crystallization, severe plastic deformation, electrolytic deposition, etc. These preparation methods can be divided into three categories according to the process of their interface formation: external pressure synthesis, deposition synthesis, and phase change interface formation. Solid nanocrystalline materials prepared by inert gas condensation method inevitably have a large number of defects, such as impurities, pores, etc., and their density is only 75% to 90% of that of coarse-crystalline materials, and the output is relatively low; the problem with mechanical grinding method is that the powder is easily contaminated and oxidized during the ball milling process, and it is difficult to obtain a pure crystal interface. The compacted bulk nanosamples often have defects such as micropores, and grain coarsening is easy to occur during the compaction process; the amorphous crystallization method uses amorphous solids as precursor materials, and controls the crystallization kinetics of amorphous solids to make the crystallization products nano-sized grains. It usually consists of two processes: obtaining and crystallizing amorphous solids, which are almost impossible to obtain from large pieces of amorphous pure copper; the nanocrystalline profiles prepared by severe plastic deformation method have large residual stress and contain substructures composed of high-density dislocations. At the same time, the grain size is uneven, and its distribution varies from tens of nanometers to micrometers. Compared with the above methods, the process of preparing nanocrystalline pure copper by electrodeposition is relatively simple and is rarely restricted by grain size and shape. The deposited pure copper has high density, low porosity and residual stress, and is low in cost and high in efficiency, making it of great industrial value.
[0004] In the research field of preparing nanocrystalline pure copper by electrodeposition, the current reports focus on the copper sulfate system electrolyte. In order to improve the deposition efficiency, it is necessary to increase the Cu content in the electrolyte. 2+ However, since the copper sulfate solution needs to add sulfuric acid, the solubility of copper sulfate is low. 2+ The concentration increase is extremely limited. For pure copper plating with a larger thickness, the deposition rate is limited and a longer electroplating time is required. Summary of the invention
[0005] The object of the present invention is to provide a method for electrodepositing nanocrystalline pure copper based on a copper methanesulfonate electrolyte system.
[0006] The technical solution for achieving the purpose of the present invention is as follows:
[0007] The method for electrodepositing nanocrystalline pure copper based on a copper methanesulfonate electrolyte system comprises the following steps:
[0008] (1) preparing an electrolyte, wherein the electrolyte comprises: 300 g / L copper methanesulfonate (C2H6CuO6S2), 40-80 g / L of a primary chelating agent diaminoethylene tetraacetate, 10-20 g / L of a secondary chelating agent nitrilotriacetic acid, 15 g / L of a conductive salt ammonium nitrate, 2 g / L of a surfactant hexadecyltrimethylammonium bromide, and the remainder is deionized water, and the pH value is adjusted to 8-9 with ammonia water;
[0009] (2) Degreasing and cleaning the cathode, placing the anode and the pretreated cathode into the electrolyte in the electrolytic cell, placing the electrolytic cell in a constant temperature water bath, and passing current to perform electrolysis under stirring.
[0010] Preferably, in step (1), the composition of the electrolyte is: 300 g / L copper methanesulfonate, 60 g / L diaminoethylene tetraacetate, 20 g / L nitrilotriacetic acid, 15 g / L ammonium nitrate, 2 g / L hexadecyltrimethylammonium bromide, and the balance is deionized water, and the pH value is adjusted to 8.3 with ammonia water.
[0011] Preferably, in step (2), the temperature of the electrolyte is 35°C.
[0012] Preferably, in step (2), the electrolysis time is 5 h.
[0013] In step (2), the anode used is an anode material conventionally applicable in the art, such as an electrolytic copper plate; the cathode used is a cathode material conventionally applicable in the art, such as a pure copper plate.
[0014] Preferably, in step (2), nanocrystalline pure copper is deposited by pulse electrodeposition at a current density of 6A / dm 2 , the frequency is 1kHz and the duty cycle is 25%.
[0015] Compared with the prior art, the present invention has the following advantages:
[0016] (1) The main salt used in the present invention is copper methanesulfonate. The copper ion concentration in the electrolyte is not limited by the sulfuric acid concentration. Therefore, a high copper ion concentration can be used to improve the deposition efficiency. At the same time, due to its high conductivity, the pure copper nucleation rate in the electrodeposition process can be improved. The electrolyte uses tetraacetic acid diaminoethylene (EDTA) as the main complexing agent, and adds an auxiliary complexing agent nitrilotriacetic acid (N(CH2COOH)3) to improve the dispersion ability of the electrolyte and promote the dissolution of the anode. The conductive salt ammonium nitrate (NH4NO3) is added to increase the current working density and the electrodeposition nucleation rate. An appropriate amount of surfactant hexadecyltrimethylammonium bromide is added to increase the wetting ability of the plating solution on the cathode surface and reduce the surface tension of the interface between the plating solution and the substrate. 4+ It forms a stable complex with copper to improve the conductivity. From the perspective of electrolyte composition, it has the thermodynamic and kinetic basis for preparing nanocrystalline pure copper. With appropriate electrical parameters, nanocrystalline pure copper can be prepared.
[0017] (2) The present invention controls the size of the deposited pure copper grains to 30 to 200 nm by adjusting the concentrations of tetraacetic acid diaminoethylene and nitrilotriacetic acid. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the TEM image of the nanocrystalline copper prepared in Example 1.
[0019] Figure 2 This is the TEM image of the nanocrystalline copper prepared in Example 2.
[0020] Figure 3 This is the TEM image of the nanocrystalline copper prepared in Example 3.
[0021] Figure 4 This is the TEM image of the nanocrystalline copper prepared in Example 4.
[0022] Figure 5 This is the TEM image of the nanocrystalline copper prepared in Example 5.
[0023] Figure 6 TEM image of nanocrystalline copper prepared in comparative example.
[0024] Figure 7 This is the XRD pattern of nanocrystalline copper prepared in Example 5. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below in conjunction with the embodiments and drawings.
[0026] Example 1
[0027] The method for electrodepositing nanocrystalline pure copper based on a copper methanesulfonate electrolyte system comprises the following steps:
[0028] (1) Preparation of electrolyte: Weigh each plating solution component according to the following formula, dissolve the following plating solution components with water, mix the plating solution components evenly and pour them into a beaker, then add ammonia water to adjust the pH to 8.3;
[0029] The plating solution contains 300 g / L of main salt, i.e. copper methanesulfonate, 40 g / L of primary chelating agent, i.e. diaminoethylene tetraacetate, 15 g / L of secondary chelating agent, 15 g / L of nitrilotriacetic acid, 15 g / L of conductive salt, i.e. ammonium nitrate, and 2 g / L of surfactant, i.e. hexadecyltrimethylammonium bromide.
[0030] (2) A copper plate is used as a cathode and electrolytic copper is used as an anode. The cathode is pretreated by conventional degreasing, pickling, alkali washing and activation. The anode and the pretreated cathode are placed in an electrolyte in an electrolytic cell. The electrolytic cell is placed in a constant temperature water bath. An electric stirrer is installed in the electrolytic cell. The stirring rod of the electric stirrer is inserted into the electrolyte. The water bath temperature is adjusted to 35° C., and current is passed through the stirring state for electrolysis. The current density of the cathode is 6 A / dm 2 , the electrolysis time is 5h.
[0031] Example 2
[0032] The method for electrodepositing nanocrystalline pure copper based on a copper methanesulfonate electrolyte system comprises the following steps:
[0033] (1) Preparation of electrolyte: Weigh each plating solution component according to the following formula, dissolve the following plating solution components with water, mix the plating solution components evenly and pour them into a beaker, then add ammonia water to adjust the pH to 8.3;
[0034] The plating solution contains 300 g / L of main salt, i.e. copper methanesulfonate, 60 g / L of primary chelating agent, i.e. diaminoethylene tetraacetate, 15 g / L of secondary chelating agent, 15 g / L of nitrilotriacetic acid, 15 g / L of conductive salt, i.e. ammonium nitrate, and 2 g / L of surfactant, i.e. hexadecyltrimethylammonium bromide.
[0035] (2) A copper plate is used as a cathode and electrolytic copper is used as an anode. The cathode is pretreated by conventional degreasing, pickling, alkali washing and activation. The anode and the pretreated cathode are placed in an electrolyte in an electrolytic cell. The electrolytic cell is placed in a constant temperature water bath. An electric stirrer is installed in the electrolytic cell. The stirring rod of the electric stirrer is inserted into the electrolyte. The water bath temperature is adjusted to 35° C., and current is passed through the stirring state for electrolysis. The current density of the cathode is 6 A / dm 2 , the electrolysis time is 5h.
[0036] Example 3
[0037] The method for electrodepositing nanocrystalline pure copper based on a copper methanesulfonate electrolyte system comprises the following steps:
[0038] (1) Preparation of electrolyte: Weigh each plating solution component according to the following formula, dissolve the following plating solution components with water, mix the plating solution components evenly and pour them into a beaker, then add ammonia water to adjust the pH to 8.3;
[0039] The plating solution contains 300 g / L of main salt, i.e. copper methanesulfonate, 80 g / L of primary chelating agent, i.e. diaminoethylene tetraacetate, 15 g / L of secondary chelating agent, 15 g / L of nitrilotriacetic acid, 15 g / L of conductive salt, and 2 g / L of surfactant, i.e. hexadecyltrimethylammonium bromide.
[0040] (2) A copper plate is used as a cathode and electrolytic copper is used as an anode. The cathode is pretreated by conventional degreasing, pickling, alkali washing and activation. The anode and the pretreated cathode are placed in an electrolyte in an electrolytic cell. The electrolytic cell is placed in a constant temperature water bath. An electric stirrer is installed in the electrolytic cell. The stirring rod of the electric stirrer is inserted into the electrolyte. The water bath temperature is adjusted to 35° C., and current is passed through the stirring state for electrolysis. The current density of the cathode is 6 A / dm 2 , the electrolysis time is 5h.
[0041] Example 4
[0042] The method for electrodepositing nanocrystalline pure copper based on a copper methanesulfonate electrolyte system comprises the following steps:
[0043] (1) Preparation of electrolyte: Weigh each plating solution component according to the following formula, dissolve the following plating solution components with water, mix the plating solution components evenly and pour them into a beaker, then add ammonia water to adjust the pH to 8.3;
[0044] The plating solution contains 300 g / L of main salt, i.e. copper methanesulfonate, 60 g / L of primary chelating agent, i.e. diaminoethylene tetraacetate, 10 g / L of secondary chelating agent, 15 g / L of conductive salt, i.e. ammonium nitrate, and 2 g / L of surfactant, i.e. hexadecyltrimethylammonium bromide.
[0045] (2) A copper plate is used as a cathode and electrolytic copper is used as an anode. The cathode is pretreated by conventional degreasing, pickling, alkali washing and activation. The anode and the pretreated cathode are placed in an electrolyte in an electrolytic cell. The electrolytic cell is placed in a constant temperature water bath. An electric stirrer is installed in the electrolytic cell. The stirring rod of the electric stirrer is inserted into the electrolyte. The water bath temperature is adjusted to 35° C., and current is passed through the stirring state for electrolysis. The current density of the cathode is 6 A / dm 2 , the electrolysis time is 5h.
[0046] Example 5
[0047] The method for electrodepositing nanocrystalline pure copper based on a copper methanesulfonate electrolyte system comprises the following steps:
[0048] (1) Preparation of electrolyte: Weigh each plating solution component according to the following formula, dissolve the following plating solution components with water, mix the plating solution components evenly and pour them into a beaker, then add ammonia water to adjust the pH to 8.3;
[0049] The plating solution contains 300 g / L of main salt, i.e. copper methanesulfonate, 60 g / L of primary chelating agent, i.e. diaminoethylene tetraacetate, 20 g / L of secondary chelating agent, 15 g / L of conductive salt, i.e. ammonium nitrate, and 2 g / L of surfactant, i.e. hexadecyltrimethylammonium bromide.
[0050] (2) A copper plate is used as a cathode and electrolytic copper is used as an anode. The cathode is pretreated by conventional degreasing, pickling, alkali washing and activation. The anode and the pretreated cathode are placed in an electrolyte in an electrolytic cell. The electrolytic cell is placed in a constant temperature water bath. An electric stirrer is installed in the electrolytic cell. The stirring rod of the electric stirrer is inserted into the electrolyte. The water bath temperature is adjusted to 35° C., and current is passed through the stirring state for electrolysis. The current density of the cathode is 6 A / dm 2 , the electrolysis time is 5h.
[0051] Comparative Example
[0052] The method for electrodepositing nanocrystalline pure copper based on a copper sulfate electrolyte system comprises the following steps:
[0053] (1) Preparation of electrolyte: Weigh each plating solution component according to the following formula, dissolve the following plating solution components with water, mix the plating solution components evenly and pour them into a beaker, then add ammonia water to adjust the pH to 8.3;
[0054] The plating solution contains 100 g / L of main salt copper sulfate pentahydrate, 60 g / L of primary chelating agent diaminoethylene tetraacetate, 20 g / L of secondary chelating agent nitrilotriacetic acid, 15 g / L of conductive salt ammonium nitrate, and 2 g / L of surfactant hexadecyltrimethylammonium bromide.
[0055] (2) A copper plate is used as a cathode and electrolytic copper is used as an anode. The cathode is pretreated by conventional degreasing, pickling, alkali washing and activation. The anode and the pretreated cathode are placed in an electrolyte in an electrolytic cell. The electrolytic cell is placed in a constant temperature water bath. An electric stirrer is installed in the electrolytic cell. The stirring rod of the electric stirrer is inserted into the electrolyte. The water bath temperature is adjusted to 35° C., and current is passed through the stirring state for electrolysis. The current density of the cathode is 6 A / dm 2 , the electrolysis time is 5h.
[0056] Figure 1 The average grain size of Example 1 is 200 nm, and the grain distribution is not very uniform. Figure 2 The average grain size of Example 2 is 42 nm. Figure 3The average grain size of Example 3 is 89 nm. Figure 4 The average grain size of Example 4 is 51 nm. Figure 5 The optimal embodiment 5 has an average crystal grain size of 27 nm. The crystal grain size first decreases and then increases with the increase of the content of the primary complexing agent, namely, tetraacetic acid diaminoethylene, and decreases with the increase of the content of the secondary complexing agent, namely, nitrilotriacetic acid. Figure 6 For comparative example: the grain size seen in the field of view is greater than 500nm. The grain size of nanocrystalline pure copper electrodeposited based on the copper methanesulfonate electrolyte system is smaller than the grain size of nanocrystalline pure copper electrodeposited based on the copper sulfate system under the same conditions.
Claims
1. A method for electrodepositing nanocrystalline pure copper based on a copper methanesulfonate electrolyte system, characterized in that: The following steps are involved: (1) preparing an electrolyte, wherein the electrolyte comprises: 300 g / L copper methanesulfonate, 40-80 g / L primary chelating agent diaminoethylene tetraacetate, 10-20 g / L secondary chelating agent nitrilotriacetic acid, 15 g / L conductive salt ammonium nitrate, 2 g / L surfactant hexadecyltrimethylammonium bromide, the remainder being deionized water, and the pH value is adjusted to 8-9 by using ammonia water; (2) Degreasing and cleaning the cathode, placing the anode and the pretreated cathode into the electrolyte in the electrolytic cell, placing the electrolytic cell in a constant temperature water bath, and passing current to perform electrolysis under stirring.
2. The method according to claim 1, characterized in that: In step (1), the composition of the electrolyte is: 300 g / L copper methanesulfonate, 60 g / L diaminoethylene tetraacetate, 20 g / L nitrilotriacetic acid, 15 g / L ammonium nitrate, 2 g / L hexadecyltrimethylammonium bromide, and the balance is deionized water, and the pH value is adjusted to 8.3 with ammonia water.
3. The method according to claim 1, characterized in that In step (2), the temperature of the electrolyte is 35°C.
4. The method according to claim 1, characterized in that: In step (2), the electrolysis time is 5 h.
5. The method according to claim 1, characterized in that In step (2), the anode used is an electrolytic copper plate; the cathode used is a pure copper plate.
6. The method according to claim 1, characterized in that In step (2), nanocrystalline pure copper is deposited by pulse electrodeposition at a current density of 6A / dm 2 , the frequency is 1kHz and the duty cycle is 25%.
Citation Information
Patent Citations
Method for preparing micro-nano needle conical structure for copper interconnection by electrochemical deposition
CN103603020A
Electroplating method of adding Fe<2+> and Fe<3+> in copper-interconnection copper methane sulfonate plating solution