Heteroatom-containing metallocene catalyst system and method for catalyzing the polymerization of alpha-olefins

By using a metallocene catalyst system containing a heteroatom ligand structure in α-olefin oligomerization, the problems of high toxicity and low economic benefits in the existing technology are solved, and a lubricating oil base with high activity, low cost and excellent performance is achieved. Oil production.

CN115400797BActive Publication Date: 2024-09-27INST OF COAL CHEM CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211001347.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-19
Publication Date
2024-09-27
Estimated Expiration
2042-08-19

AI Technical Summary

Technical Problem

The existing technology has the problems of highly toxic catalysts, sewage generation and low economic benefits in the α-olefin oligomerization process. Especially in the polymerization of long-chain α-olefins, the application of heteroatom metallocene catalysts is relatively limited.

Method used

Using a metallocene catalyst system containing a heteroatom ligand structure, through the combination of main catalyst and cocatalyst, non-bridged or bridged metallocene compounds and alkyl aluminum/borides are used as cocatalysts to carry out the oligomerization of α-olefins reaction, reducing dependence on solvents and maintaining high activity at low promoter/main catalyst molar ratios.

Benefits of technology

The catalytic effect of α-olefin oligomerization with high activity, good selectivity, high viscosity index and low pour point is achieved, the cost is reduced, and a lubricating oil base oil with excellent performance is obtained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115400797B
    Figure CN115400797B
Patent Text Reader

Abstract

The invention discloses a metallocene catalyst system containing heteroatoms and a method for catalyzing the polymerization of alpha-olefins, and belongs to the technical field of preparing medium and high viscosity lubricating oils by polymerization of alpha-olefins. The catalyst system is composed of a metallocene compound as a main catalyst and a mixture of one or more of alkyl aluminum / methylaluminoxane, modified methylaluminoxane, ethylaluminoxane or isobutylaluminoxane in any proportion or an alkyl aluminum / boron compound as a cocatalyst. In the catalytic process of the present invention, except for a small amount of solvent required to dissolve the boride, the rest of the process does not involve the use of solvent, and is a green method for the polymerization of alpha-olefins; the catalytic system used has high catalytic activity and high single-pass conversion rate; the alpha-olefin oligomer obtained has a high viscosity index, a low pour point, and low dimer selectivity, and is an excellent method for catalyzing the polymerization of alpha-olefins.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a metallocene catalyst system containing a heteroatom ligand structure and a method for catalyzing the polymerization of alpha-olefins. The system can catalyze the polymerization of alpha-olefins such as 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, etc. to generate polyalpha-olefin (PAO) lubricant base oil, belonging to the technical field of preparing medium- and high-viscosity lubricants by polymerization of alpha-olefins. Background Art

[0002] Polyalphaolefin (PAO) is a synthetic base oil with excellent performance, which is obtained by polymerization or copolymerization of alpha-olefins under the action of catalysts and hydrogenation saturation. Compared with traditional mineral base oils, it has a wider operating temperature range, higher viscosity index, lower pour point, better thermal stability, higher oxidation stability, and better reaction to antioxidants, flash point and autoignition point. Therefore, it has a longer oil change cycle, slows down the corrosion and damage of parts, and thus increases the service life of equipment. It is often used in the fields of automobiles, military industry, aerospace, etc.

[0003] Common routes for the polymerization of α-olefins include Zeigler–Natta catalysis, Lewis acid catalysts, i.e., boron trifluoride and aluminum trichloride, chromium compound systems, and metallocene catalyst systems. However, due to the high toxicity of chromium compounds and BF3 gas, and the large amount of wastewater generated in the process, which causes environmental damage, they are gradually being eliminated. The mPAO produced by the metallocene catalyst has a single active center and has a special comb-like structure, which gives it a high structural regularity and no upright side chains, so it has a higher viscosity index, ensuring that it has good lubrication properties at high temperatures, better shear stability helps to extend the oil change cycle, and a lower pour point gives it sufficient lubrication properties at low temperatures, so it has attracted more and more attention.

[0004] In recent years, metallocene catalysts have developed rapidly, and their types have evolved from the initial non-bridged to bridged, di-cyclopentadienyl to mono-cyclopentadienyl, carbon bridge to silicon bridge and even to the introduction of heteroatoms, all of which reflect the diversity and novelty of metallocene catalysts. For heterocyclopentadienyl compounds, heteroatoms directly affect the stereoselectivity of olefin polymerization due to their electronic effects.

[0005] US Patent No. US20050010004 introduces a supported catalyst containing an indole ligand, which has a good effect on the activity and molecular weight of catalytic olefins.

[0006] US Patent No. 09 / 461,858 describes a large number of metallocene compound ligands containing heteroatoms and various substituents on the cyclopentadienyl group, which have good catalytic activity in polymerizing propylene.

[0007] CN108250252A discloses a metallocene bridged catalyst containing S and O heteroatoms, which has good effects in homopolymerization and copolymerization of α-olefins, especially long-chain α-olefins. However, the amount of co-catalyst used is too high, and the economic benefits are not high.

[0008] US Patent No. 20070135623 discloses a metallocene catalyst containing a monocyclic or polycyclic ligand, and the ligand contains one or more cyclic heteroatoms, which has good activity in the polymerization of ethylene or propylene.

[0009] US Patent No. 6,548,724 discloses a non-bridged metallocene catalyst for preparing low-viscosity poly-α-olefin from 1-decene. The resulting synthetic base oil has good viscosity-temperature properties, but the dimer selectivity is as high as 49%.

[0010] The application of heteroatom metallocene catalysts is still in its infancy. The few reports that exist are mostly for the polymerization of ethylene and propylene. No reports on the polymerization of long-chain α-olefins have been found in literature searches. Since the introduction of heteroatoms greatly changes the stereostructure and electronic effects of metallocene compounds, this has a great impact on the product distribution of its polymerization products. This type of catalyst has good activity and selectivity in catalyzing the polymerization of α-olefins and has good viscosity-temperature properties. It also has high activity when the molar ratio of the additive to the main catalyst is very low, and is very suitable for making high-grade lubricant base oils. Summary of the invention

[0011] The purpose of the present invention is to provide a metallocene catalyst system containing a heteroatom ligand structure and a method for catalyzing the polymerization of α-olefins. This type of catalyst has good catalytic activity and selectivity for the polymerization of α-olefins and has good viscosity-temperature properties. It also has high activity when the molar ratio of the auxiliary agent to the main catalyst is very low.

[0012] In order to achieve the above object, the present invention provides a metallocene catalyst system containing heteroatoms, wherein the catalyst system is composed of a main catalyst and a co-catalyst, wherein the main catalyst is a metallocene compound containing heteroatoms, and its structural formula is as follows:

[0013]

[0014] Wherein the cyclopentadienyl is a monosubstituted or polysubstituted cyclopentadienyl group, M is a transition metal such as titanium, zirconium or hafnium, and M is a halogen or an alkyl group; R1 is a substituent on the indole group, R2 and R3 are substituents on the cyclopentadienyl group, R1, R2 and R3 are alkyl groups, aryl groups or hydrogen atoms, and are the same or different from each other; Y is a bridging substituent group, and Y is dimethylsilyl or vinylidene;

[0015] Furthermore, the co-catalyst is one or a mixture of any proportion of alkyl aluminum / methyl aluminumoxane, modified methyl aluminumoxane, ethyl aluminumoxane or isobutyl aluminumoxane, or an alkyl aluminum / boron compound.

[0016] Furthermore, the alkyl aluminum is one of trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, and diethyl aluminum chloride, or a mixture of two or more of them in any proportion; the boron compound is one of B(C6F5)3, Ph3CB(C6F5), PhNMe2HB(C6F5)4, or Ph3CB[(CF3)2C6H3]4.

[0017] The cocatalyst is preferably triisobutylaluminum and methylaluminoxane or modified methylaluminoxane or Ph3CB(C6F5) toluene solution.

[0018] Furthermore, the molar ratio of the alkyl aluminum to methylaluminoxane, modified methylaluminoxane, ethylaluminoxane or isobutylaluminoxane to the main catalyst is 10-200:10-500:1; the molar ratio of the alkyl aluminum to the boride to the main catalyst is 10-200:1-2:1.

[0019] Furthermore, the main catalyst is a non-bridged metallocene compound containing heterocyclic atoms or a bridged metallocene compound containing heterocyclic atoms.

[0020] Furthermore, the heteroatom-containing non-bridged metallocene compound is:

[0021] Complex 1: bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)zirconium dichloride;

[0022] Complex 2: bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)titanium dichloride;

[0023] Complex 3: bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)hafnium dichloride;

[0024] Complex 4: bis(2,4-dimethylcyclopentadienyl[b]indolyl)zirconium dichloride;

[0025] Complex 5: bis(2,4-dimethylcyclopentadienyl[b]indolyl)titanium dichloride;

[0026] Complex 6: bis(2,4-dimethylcyclopentadienyl[b]indolyl)hafnium dichloride;

[0027] Complex 7: bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)zirconium dimethyl;

[0028] Complex 8: bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)dimethyltitanium;

[0029] Complex 9: bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)hafnium dimethyl;

[0030] Complex 10: bis(2,4-dimethylcyclopentadienyl[b]indolyl)zirconium dimethyl;

[0031] Complex 11: bis(2,4-dimethylcyclopentadienyl[b]indolyl)dimethyltitanium;

[0032] Complex 12: bis(2,4-dimethylcyclopentadienyl[b]indolyl)hafnium dimethyl;

[0033] Complex 13: bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)zirconium dichloride;

[0034] Complex 14: bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)titanium dichloride;

[0035] Complex 15: bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)hafnium dichloride;

[0036] Complex 16: bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)zirconium dichloride;

[0037] Complex 17: bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)titanium dichloride;

[0038] Complex 18: bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)hafnium dichloride;

[0039] Complex 19: bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)zirconium dimethyl;

[0040] Complex 20: bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)dimethyltitanium;

[0041] Complex 21: bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)hafnium dimethyl;

[0042] Complex 22: bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)zirconium dimethyl;

[0043] Complex 23: bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)dimethyltitanium;

[0044] Complex 24: bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)hafnium dimethyl.

[0045] Furthermore, the heteroatom-containing bridged metallocene compound is:

[0046] Complex 1: dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]zirconium dichloride;

[0047] Complex 2: dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]titanium dichloride;

[0048] Complex 3: dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]hafnium dichloride;

[0049] Complex 4: dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]zirconium dichloride;

[0050] Complex 5: dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]titanium dichloride;

[0051] Complex 6: dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]hafnium dichloride;

[0052] Complex 7: dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]zirconium dimethyl;

[0053] Complex 8: dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]dimethyltitanium;

[0054] Complex 9: dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]dimethylhafnium;

[0055] Complex 10: dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]zirconium dimethyl;

[0056] Complex 11: dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]dimethyltitanium;

[0057] Complex 12: dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]dimethylhafnium;

[0058] Complex 13: dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]zirconium dichloride;

[0059] Complex 14: dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]titanium dichloride;

[0060] Complex 15: dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]hafnium dichloride;

[0061] Complex 16: dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]zirconium dichloride;

[0062] Complex 17: dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]titanium dichloride;

[0063] Complex 18: dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]hafnium dichloride;

[0064] Complex 19: dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]zirconium dimethyl;

[0065] Complex 20: dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]dimethyltitanium;

[0066] Complex 21: dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]dimethylhafnium;

[0067] Complex 22: dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]zirconium dimethyl;

[0068] Complex 23: dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]dimethyltitanium;

[0069] Complex 24: dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]hafnium dimethyl.

[0070] The main catalyst metallocene compound is preferably bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)zirconium dichloride.

[0071] The invention discloses a method for catalyzing the polymerization of alpha-olefins by a metallocene catalyst system containing heteroatoms, wherein a metallocene compound, purified alpha-olefins and a co-catalyst are stirred in an oil bath pot at 40 to 110°C for 5 to 20 minutes, the co-catalyst is added again for reaction for 30 to 480 minutes, a hydrochloric acid ethanol solution is added to the reaction mixture for stirring, an organic layer is separated, dried and filtered, and unreacted raw materials are removed by reduced pressure distillation to obtain an alpha-olefin polymerization product, wherein the molar ratio of the main catalyst to the alpha-olefin is 1:1×10 -5 ~8×10 -4 .

[0072] The time for adding the co-catalyst again to react is preferably 240 minutes. In the present invention, except for using a small amount of toluene solvent when the boride is used as the co-catalyst, the rest of the process does not involve the use of solvents.

[0073] Furthermore, the α-olefin is a C6-C20 straight-chain α-olefin, and the preferred α-olefin is 1-hexene, 1-octene, 1-decene, 1-dodecene, and 1-tetradecene.

[0074] Furthermore, the oligomerization product is a mixture of dimers, trimers, tetramers, pentamers and higher polymers of α-olefin monomers, and isomers exist in the product, which is polymerized in a head-to-head, head-to-tail, and tail-to-tail insertion manner.

[0075] Compared with the prior art, the present invention has the following advantages:

[0076] No solvent is required for the polymerization of α-olefins. Only when the boride is used as a co-catalyst, a small amount of toluene solvent is used to dissolve the boride. Even when the molar ratio of the co-catalyst to the main catalyst is very low, it will have high activity and high selectivity for trimers, tetramers and pentamers. The catalytic system used has high catalytic activity and high single-pass conversion rate; the α-olefin oligomers obtained have a high viscosity index, a low pour point, and low dimer selectivity, which is an excellent method for catalyzing the polymerization of α-olefins. A preferred example of the present invention uses a non-bridged metallocene catalyst to prepare a medium-low viscosity oligomer of 1-decene, with a kinematic viscosity of 14.98 mm at 100°C. 2 / s. BRIEF DESCRIPTION OF THE DRAWINGS

[0077] Figure 1 is the structural formula of a heteroatom-containing metallocene compound;

[0078] Figure 2 This is the H`NMR diagram of the oligomer of Example 3 of the present invention;

[0079] Figure 3 This is the C'NMR diagram of the oligomer of Example 3 of the present invention. DETAILED DESCRIPTION

[0080] The present invention is illustrated by the following examples, but the present invention is not limited thereto.

[0081] Example 1

[0082] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)zirconium dichloride was placed. The flask was taken out and argon was replaced three times on a Schlenk apparatus. 30 mL of 1-decene was added and stirred for 5 minutes. 50 μmol of triisobutylaluminum (10 eq.) was added and stirred at 70° C. for 10 minutes. Then, 50 μmol (10 eq.) of methylaluminoxane was added and the reaction was completed for 60 minutes. A 5% ethanol solution of hydrochloric acid was added and stirred to separate the liquids. The mixture was dried and the unreacted raw materials were removed by distillation under reduced pressure to obtain 15.27 g of the product with a conversion rate of 68.63%.

[0083] Example 2

[0084] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of bis(2,4-dimethylcyclopentadienyl[b]indolyl)titanium dichloride was placed in it; the flask was taken out and argon was replaced three times on a Schlenk apparatus; 10 mL of 1-decene was added and stirred for 5 minutes; 500 μmol of triisobutylaluminum (100 eq.) was added and stirred at 90° C. for 20 minutes; then 250 μmol of modified methylaluminoxane (50 eq.) was added and the reaction was completed for 180 minutes; 5% ethanolic hydrochloric acid solution was added and stirred to separate the liquids; the mixture was dried and the unreacted raw materials were removed by distillation under reduced pressure to obtain 4.52 g of the product with a conversion rate of 60.2%.

[0085] Example 3

[0086] A clean 100 mL three-necked flask was placed in a glove box with 5 μmol of bis(2,4-dimethylcyclopentadienyl[b]indolyl)zirconium dichloride; the mixture was taken out and replaced with argon three times on a Schlenk apparatus, 20 mL of 1-octene was added and stirred for 5 minutes, 100 μmol (20 eq.) of triisobutylaluminum was added and stirred at 80°C for 20 minutes, and then 250 μmol of methylaluminoxane (50 eq.) was added and the reaction was completed for 240 minutes, 5% hydrochloric acid ethanol solution was added and stirred for separation, and the mixture was dried and unreacted raw materials were removed by distillation under reduced pressure to obtain 12.93 g of product with a conversion rate of 90.4% (such as Figure 1 , Figure 2 shown).

[0087] Example 4

[0088] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)zirconium dichloride was placed. The flask was taken out and argon was replaced three times on a Schlenk apparatus. 20 mL of 1-decene was added and stirred for 5 minutes. 1000 μmol (20 eq.) of triisobutylaluminum was added and stirred at 70° C. for 10 minutes. After that, 50 μmol of methylaluminoxane (10 eq.) was added and the reaction was completed for 60 minutes. A 5% ethanol solution of hydrochloric acid was added and stirred for separation. The mixture was dried and unreacted raw materials were removed by distillation under reduced pressure to obtain 10.91 g of product with a conversion rate of 73.6%.

[0089] Example 5

[0090] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)zirconium dichloride was placed; the flask was taken out and argon was replaced three times on a Schlenk apparatus; 30 mL of 1-decene and 400 μmol of trimethylaluminum (80 eq.) were added, and the mixture was stirred at 60° C. for 20 minutes, followed by addition of 2.5 mL of Ph3CB(C6F5) toluene solution (concentration 2.4 μmol / mL) and the reaction was completed for 120 minutes; 5% ethanolic hydrochloric acid solution was added, stirred, separated, dried, and unreacted raw materials were removed by distillation under reduced pressure to obtain 12.37 g of product with a conversion rate of 55.64%.

[0091] Example 6

[0092] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of bis(2,4-dimethylcyclopentadienyl[b]indolyl)titanium dichloride was placed in it; the flask was taken out and argon was replaced three times on a Schlenk apparatus; 10 mL of 1-decene and 500 μmol of triisobutylaluminum (100 eq.) were added, and the mixture was stirred at 60°C for 10 minutes, followed by addition of 2.5 mL of Ph3CB(C6F5) toluene solution (concentration 2.4 μmol / ml) and the reaction was completed for 120 minutes; 5% ethanolic hydrochloric acid solution was added, stirred, separated, dried, and unreacted raw materials were removed by distillation under reduced pressure to obtain 4.24 g of product with a conversion rate of 57.26%.

[0093] Example 7

[0094] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of bis(2,4-dimethylcyclopentadienyl[b]indolyl)zirconium dichloride was placed. The flask was taken out and argon was replaced three times on a Schlenk apparatus. 20 mL of 1-hexene and 100 μmol of triisobutylaluminum (20 eq.) were added, and the mixture was stirred at 80°C for 20 minutes. Then, 2.5 mL of Ph3CB(C6F5) toluene solution (concentration 2.4 μmol / mL) was added and the reaction was completed for 480 minutes. A 5% ethanolic hydrochloric acid solution was added, and the mixture was stirred and separated. The mixture was dried and the unreacted raw materials were removed by distillation under reduced pressure to obtain 10.67 g of the product with a conversion rate of 77.79%.

[0095] Example 8

[0096] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of bis(2,4-dimethylcyclopentadienyl[b]indolyl)titanium dichloride was placed in it; the flask was taken out and argon was replaced three times on a Schlenk apparatus; 20 mL of 1-decene and 100 μmol of triethylaluminum (20 eq.) were added, and the mixture was stirred at 80°C for 20 minutes, followed by addition of 2.5 mL of Ph3CB(C6F5) toluene solution (concentration 2.4 μmol / mL) and the reaction was completed for 120 minutes; 5% ethanolic hydrochloric acid solution was added, stirred, separated, dried, and unreacted raw materials were removed by distillation under reduced pressure to obtain 10.14 g of product with a conversion rate of 68.41%.

[0097] Table 1 shows the product distribution and properties of α-olefin oligomers catalyzed by different non-bridged metallocenes

[0098]

[0099] From the data in Table 1, it can be seen that the selectivity of mPAO obtained by different catalysts for dimers is controlled at 20-30%, and the viscosity index is large, indicating that the viscosity-temperature property is very good.

[0100] Example 9

[0101] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]hafnium dichloride was placed in the flask; the flask was taken out and argon was replaced three times on a Schlenk apparatus, 20 mL of 1-decene was added and stirred for 5 minutes, 200 μmol of trimethylaluminum (40 eq.) was added and stirred at 50° C. for 20 minutes, and then 50 μmol (10 eq.) of methylaluminoxane was added and the reaction was completed for 180 minutes, 5% ethanolic hydrochloric acid solution was added and stirred to separate the liquids, and the mixture was dried and unreacted raw materials were removed by distillation under reduced pressure to obtain 9.76 g of product with a conversion rate of 65.89%.

[0102] Example 10

[0103] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]zirconium dimethyl was placed in the flask. The flask was taken out and argon was replaced three times on a Schlenk apparatus. 10 ml of 1-octene was added and stirred for 5 minutes. 100 μmol of triisobutylaluminum (20 eq.) was added and stirred at 80° C. for 20 minutes. 500 μmol (100 eq.) of modified methylaluminoxane was added and the reaction was completed after 240 minutes. A 5% ethanol solution of hydrochloric acid was added and stirred to separate the liquids. The mixture was dried and the unreacted raw materials were removed by distillation under reduced pressure to obtain 6.18 g of the product with a conversion rate of 85.89%.

[0104] Embodiment 11

[0105] A clean 100 mL three-necked flask was used to place 5 μmol of dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]titanium dichloride in a glove box; the flask was taken out and argon was replaced three times on a Schlenk apparatus, 30 mL of 1-hexene was added and stirred for 5 minutes, 50 μmol of triisobutylaluminum (10 eq.) was added and stirred at 40° C. for 20 minutes, and then 250 μmol (50 eq.) of methylaluminoxane was added and the reaction was completed for 180 minutes, 5% hydrochloric acid ethanol solution was added and stirred for separation, and the mixture was dried and unreacted raw materials were removed by distillation under reduced pressure to obtain 16.68 g of product with a conversion rate of 81.03%.

[0106] Example 12

[0107] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]dimethylhafnium was placed in the flask. The flask was taken out and argon was replaced three times on a Schlenk apparatus. 20 ml of 1-dodecene was added and stirred for 5 minutes. 200 μmol of triisobutylaluminum (40 eq.) was added and stirred at 60° C. for 10 minutes. 250 μmol (50 eq.) of modified methylaluminoxane was added and the reaction lasted for 240 minutes. A 5% ethanol solution of hydrochloric acid was added and stirred to separate the liquids. The mixture was dried and the unreacted raw materials were removed by distillation under reduced pressure to obtain 8.09 g of the product with a conversion rate of 53.24%.

[0108] Example 13

[0109] A clean 100 mL three-necked flask was used to charge 5 μmol of dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]zirconium dichloride in a glove box; the flask was taken out and argon was replaced three times on a Schlenk apparatus; 20 ml of 1-decene and 250 μmol of triethylaluminum (50 eq.) were added, and the mixture was stirred at 50° C. for 20 minutes, followed by addition of 2.3 mL of Ph3CB(C6F5) toluene solution (concentration 2.4 μmol / mL) and the reaction was completed for 360 minutes; 5% ethanolic hydrochloric acid solution was added, stirred, separated, dried, and unreacted raw materials were removed by distillation under reduced pressure to obtain 11 g of product with a conversion rate of 74.29%.

[0110] Embodiment 14

[0111] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]titanium dichloride was placed in it; the flask was taken out and argon was replaced three times on a Schlenk apparatus; 20 mL of 1-tetradecene and 1000 μmol of triisobutylaluminum (200 eq.) were added, and the mixture was stirred at 70°C for 20 minutes, followed by addition of 2.3 mL of Ph3CB(C6F5) toluene solution (concentration 2.4 μmol / mL) and the reaction was completed for 240 minutes; 5% ethanolic hydrochloric acid solution was added, stirred, separated, dried, and unreacted raw materials were removed by distillation under reduced pressure to obtain 9.86 g of product with a conversion rate of 64.05%.

[0112] Embodiment 15

[0113] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]hafnium dichloride was placed in the flask; the flask was taken out and argon was replaced three times on a Schlenk apparatus; 10 ml of 1-tetradecene and 200 μmol of trimethylaluminum (40 eq.) were added, and the mixture was stirred at 70° C. for 20 minutes, followed by addition of 2.3 mL of Ph3CB(C6F5) toluene solution (concentration 2.4 μmol / mL) and the reaction was completed for 180 minutes; 5% ethanolic hydrochloric acid solution was added, stirred, separated, dried, and unreacted raw materials were removed by distillation under reduced pressure to obtain 12.03 g of product with a conversion rate of 78.09%.

[0114] Example 16

[0115] Use a clean 100mL three-necked flask to charge 5μmol of dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]dimethyltitanium in a glove box; take it out and replace argon on a Schlenk apparatus three times, add 20mL of 1-octene, 100μmol of triethylaluminum (40eq.), stir at 80°C for 5 minutes, then add 2.3mL of Ph3CB(C6F5) toluene solution (concentration 2.4μmol / mL) and react for 60 minutes. Add 5% hydrochloric acid ethanol solution, stir and separate the liquids, dry, and remove the unreacted raw materials by distillation under reduced pressure to obtain 10.81g of product with a conversion rate of 75.6%.

[0116] Table 2 shows the performance of α-olefin oligomers catalyzed by different bridged metallocenes

[0117]

[0118] It can be seen from the data in Table 1 and Table 2 that both medium-low viscosity and high-viscosity base synthetic oils have very high viscosity index and low pour point, and are a type of lubricant base oil with excellent performance.

[0119] Comparative Example 1

[0120] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of bis-indenyl zirconium dichloride was placed. The flask was taken out and argon was replaced three times on a Schlenk apparatus. 20 mL of 1-decene was added and stirred for 5 minutes. 100 μmol (20 eq.) of triisobutylaluminum was added and stirred at 70° C. for 20 minutes. After that, 50 μmol of methylaluminoxane (10 eq.) was added and the reaction was completed for 60 minutes. A 5% ethanol solution of hydrochloric acid was added and stirred for separation. The mixture was dried and unreacted raw materials were removed by distillation under reduced pressure to obtain 0.646 g of product with a conversion rate of 4.36%.

[0121] Comparative Example 2

[0122] A clean 100 mL three-necked flask was placed in a glove box and 5 μmol of bis(2-methylindenyl)zirconium dichloride was placed. The flask was taken out and argon was replaced three times on a Schlenk apparatus. 20 mL of 1-decene was added and stirred for 5 minutes. 100 μmol (20 eq.) of triisobutylaluminum was added and stirred at 70° C. for 20 minutes. After that, 50 μmol of methylaluminoxane (10 eq.) was added and the reaction was completed for 60 minutes. A 5% ethanol solution of hydrochloric acid was added and stirred for separation. The mixture was dried and the unreacted raw materials were removed by distillation under reduced pressure to obtain 3.27 g of product with a conversion rate of 22.06%.

[0123] Table 3 shows the performance of different catalysts at low Al MAO Performance and activity under Zr

[0124]

[0125] It can be seen from the data in Table 3 that when the co-catalyst / main catalyst molar ratio is low, the catalyst has a higher activity than the traditional metallocene catalyst, greatly reduces the cost, and has a higher viscosity index.

[0126] The above embodiments are only illustrative of the principles and feasibility of the present invention and are not limited to the contents in the embodiments. Any technicians in this field shall not violate the spirit and scope of the present invention. Various changes and modifications may be made within the conceptual scope of the technical solution of the present invention. Any changes and modifications made are within the protection scope of the present invention.

Claims

1. A method for the oligomerization of alpha-olefins catalyzed by a metallocene catalyst system containing heteroatoms, characterized in that: The metallocene compound, the purified α-olefin and the co-catalyst are stirred in an oil bath at 40-70°C for 5-20 minutes, the co-catalyst is added again and reacted for 30-480 minutes, the hydrochloric acid ethanol solution is added to the reaction mixture and stirred, the organic layer is separated, dried and filtered, and then the unreacted raw materials are removed by reduced pressure distillation to obtain an α-olefin oligomerization product, and the molar ratio of the main catalyst to the α-olefin is 1:1×10 -5 ~8×10 -4 ; The metallocene catalyst system containing heteroatoms is a catalyst system composed of a main catalyst and a co-catalyst. The main catalyst is a metallocene compound containing heteroatoms, and its structural formula is as follows: The cyclopentadienyl is a monosubstituted or polysubstituted cyclopentadienyl group, M is a transition metal such as titanium, zirconium or hafnium, and M is a halogen or an alkyl group; R1 is a substituent on the indole group, R2 and R3 are substituents on the cyclopentadienyl group, R1, R2 and R3 are alkyl groups, aryl groups or hydrogen atoms, and are the same or different from each other; Y is a bridging substituent group, and Y is dimethylsilyl or vinylidene; and the α-olefin is a C6-C20 straight-chain α-olefin.

2. The method for catalyzing the oligomerization of α-olefins by a metallocene catalyst system containing heteroatoms according to claim 1, characterized in that: The oligomerization product is a mixture of dimers, trimers, tetramers, pentamers and higher polymers of α-olefin monomers.

3. The method for catalyzing the oligomerization of α-olefins by a metallocene catalyst system containing heteroatoms according to claim 1, characterized in that: The co-catalyst is one or a mixture of two or more of alkyl aluminum / methyl aluminumoxane, modified methyl aluminumoxane, ethyl aluminumoxane or isobutyl aluminumoxane in any proportion, or an alkyl aluminum / boron compound.

4. The method for catalyzing the oligomerization of α-olefins by a metallocene catalyst system containing heteroatoms according to claim 3, characterized in that: The alkyl aluminum is one of trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, and diethyl aluminum chloride, or a mixture of two or more of them in any proportion; the boron compound is one of B(C6F5)3, Ph3CB(C6F5), PhNMe2HB(C6F5)4, or Ph3CB[(CF3)2C6H3]4.

5. The method for catalyzing the oligomerization of α-olefins by a metallocene catalyst system containing heteroatoms according to claim 4, characterized in that: The molar ratio of the alkyl aluminum to methylaluminoxane, modified methylaluminoxane, ethylaluminoxane or isobutylaluminoxane and the main catalyst is 10-200:10-500:1; the molar ratio of the alkyl aluminum to the boride and the main catalyst is 10-200:1-2:

1.

6. The method for catalyzing the oligomerization of α-olefins by a metallocene catalyst system containing heteroatoms according to claim 1, characterized in that: The main catalyst is a non-bridged metallocene compound containing heterocyclic atoms or a bridged metallocene compound containing heterocyclic atoms.

7. The method for catalyzing the oligomerization of α-olefins by a metallocene catalyst system containing heteroatoms according to claim 6, characterized in that: The heteroatom-containing non-bridged metallocene compound is: Complex 1: bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)zirconium dichloride; Complex 2: bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)titanium dichloride; Complex 3: bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)hafnium dichloride; Complex 4: bis(2,4-dimethylcyclopentadienyl[b]indolyl)zirconium dichloride; Complex 5: bis(2,4-dimethylcyclopentadienyl[b]indolyl)titanium dichloride; Complex 6: bis(2,4-dimethylcyclopentadienyl[b]indolyl)hafnium dichloride; Complex 7: bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)zirconium dimethyl; Complex 8: bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)dimethyltitanium; Complex 9: bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)hafnium dimethyl; Complex 10: bis(2,4-dimethylcyclopentadienyl[b]indolyl)zirconium dimethyl; Complex 11: bis(2,4-dimethylcyclopentadienyl[b]indolyl)dimethyltitanium; Complex 12: bis(2,4-dimethylcyclopentadienyl[b]indolyl)hafnium dimethyl; Complex 13: bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)zirconium dichloride; Complex 14: bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)titanium dichloride; Complex 15: bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)hafnium dichloride; Complex 16: bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)zirconium dichloride; Complex 17: bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)titanium dichloride; Complex 18: bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)hafnium dichloride; Complex 19: bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)zirconium dimethyl; Complex 20: bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)dimethyltitanium; Complex 21: bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)hafnium dimethyl; Complex 22: bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)zirconium dimethyl; Complex 23: bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)dimethyltitanium; Complex 24: bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)hafnium dimethyl.

8. The method for catalyzing the oligomerization of α-olefins by a metallocene catalyst system containing heteroatoms according to claim 6, characterized in that: The heteroatom-containing bridged metallocene compound is: Complex 1: dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]zirconium dichloride; Complex 2: dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]titanium dichloride; Complex 3: dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]hafnium dichloride; Complex 4: dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]zirconium dichloride; Complex 5: dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]titanium dichloride; Complex 6: dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]hafnium dichloride; Complex 7: dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]zirconium dimethyl; Complex 8: dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]dimethyltitanium; Complex 9: dimethylsilyl[bis(2-methyl-4-phenylcyclopentadienyl[b]indolyl)]dimethylhafnium; Complex 10: dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]zirconium dimethyl; Complex 11: dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]dimethyltitanium; Complex 12: dimethylsilyl[bis(2,4-dimethylcyclopentadienyl[b]indolyl)]dimethylhafnium; Complex 13: dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]zirconium dichloride; Complex 14: dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]titanium dichloride; Complex 15: dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]hafnium dichloride; Complex 16: dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]zirconium dichloride; Complex 17: dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]titanium dichloride; Complex 18: dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]hafnium dichloride; Complex 19: dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]zirconium dimethyl; Complex 20: dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]dimethyltitanium; Complex 21: dimethylsilyl[bis(2,3-dimethyl-4-phenylcyclopentadienyl[b]indolyl)]dimethylhafnium; Complex 22: dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]zirconium dimethyl; Complex 23: dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]dimethyltitanium; Complex 24: dimethylsilyl[bis(2,3,4-trimethylcyclopentadienyl[b]indolyl)]hafnium dimethyl.