A modified polysiloxane-polycarbonate composition and its preparation method and application

The modified polysiloxane-polycarbonate composition was prepared by a batch one-step polymerization method, which solved the problems of insufficient flowability and toughness in the prior art, realized the preparation of polycarbonate materials with high flowability and high toughness, and reduced the preparation cost.

CN115403912BActive Publication Date: 2024-11-15NINGBO GANGZHI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210872480.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-20
Publication Date
2024-11-15
Estimated Expiration
2042-07-20

AI Technical Summary

Technical Problem

Existing technologies struggle to produce polycarbonate materials with better flowability and stronger toughness, and the preparation methods and raw material costs are not very favorable.

Method used

A batch one-step polymerization method is adopted, in which silicone oil and castor oil are introduced to react with components such as bisphenol A to form a modified polysiloxane-polycarbonate composition. Phosgenesis and polycondensation reactions are carried out simultaneously, and the reaction pH and component content are controlled to achieve high mechanical properties.

Benefits of technology

A polysiloxane-polycarbonate material with high fluidity and toughness was prepared, simplifying the preparation process and reducing raw material and time costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115403912B_ABST
    Figure CN115403912B_ABST
Patent Text Reader

Abstract

The present invention provides a modified polysiloxane-polycarbonate composition and its preparation method and application, and relates to the technical field of polymer materials. Specifically, the modified polysiloxane-polycarbonate composition includes the following components by mass: 80-120 parts of bisphenol A, 70-90 parts of silicone oil, 15-25 parts of castor oil, 10-30 parts of sebacic acid, 90-110 parts of phosgene, 3-5 parts of triethylamine, 3-7 parts of additives and several solvents. By adopting a one-step intermittent synthesis route, the pH and the molecular weight of sodium carbonate in the aqueous phase or the polycarbonate in the oil phase are monitored in real time and a reaction composition is finally obtained. The modified polysiloxane-polycarbonate composition has high-quality mechanical strength such as high mobile phase and strong toughness, and the preparation method is simple and easy, low cost, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a modified polysiloxane-polycarbonate composition and a preparation method and application thereof. Background Art

[0002] Polycarbonate (PC) is a high molecular polymer containing carbonate groups in the molecular chain. Due to its structural particularity, it has become the fastest growing general engineering plastic among the five major engineering plastics. It is widely used in many fields such as building materials, automobiles, medical devices, aerospace, electronics and optics. Polycarbonate is mainly prepared by the polycondensation reaction of aromatic diols such as bisphenol A and carbonate precursors such as phosgene. It has excellent impact strength, dimensional stability, heat resistance and transparency. In order to further expand the application field of polycarbonate, polycarbonate products with other characteristics need to be prepared.

[0003] For example, in the invention patent with application number TW20170135612, by introducing a polysiloxane structure into the main chain of polycarbonate and a decanedioyl structure at the same time, it is possible to ensure that polycarbonate has good fluidity while having properties such as chemical corrosion resistance and low-temperature impact strength. Another example is in the invention patent with application number CN201610079183.X, by adding isocyanate-terminated polydimethylsiloxane or epoxy-terminated polydimethylsiloxane, it reacts with the hydroxyl groups on the PC molecular chain to form a block copolymer, thereby obtaining a modified polycarbonate with high fluidity and low-temperature toughness. However, there are still other technical means to achieve carbonate polymers with better fluidity and stronger toughness, which are more friendly to the preparation method and raw material cost while taking into account the performance.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The first object of the present invention is to provide a modified polysiloxane-polycarbonate composition, which can realize a polysiloxane-polycarbonate material with high mobile phase and strong toughness by introducing two components, silicone oil and castor oil.

[0006] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0007] A modified polysiloxane-polycarbonate composition is prepared by including the following components in parts by mass:

[0008] 80-120 parts of bisphenol A, 70-90 parts of silicone oil, 15-25 parts of castor oil, 10-30 parts of sebacic acid, 90-110 parts of phosgene, 3-5 parts of triethylamine, 3-7 parts of additives, and some solvents.

[0009] Preferably, the additive comprises at least one of p-cumylphenol, p-isopropylphenol and p-tert-butylphenol;

[0010] More preferably, the additive is p-cumylphenol.

[0011] Preferably, the solvent includes an organic solvent and an inorganic solvent;

[0012] Wherein, the organic solvent is selected from dichloromethane, and the inorganic solvent comprises an aqueous solution of alkaline hydroxide;

[0013] More preferably, the alkaline hydroxide includes at least one of sodium hydroxide, potassium hydroxide, ammonia monohydrate and lithium hydroxide;

[0014] More preferably, the mass content of the aqueous solution of the alkaline hydroxide is 30% to 40%.

[0015] Preferably, the mass fraction of the solvent is 1800 to 2500 parts;

[0016] Wherein, the mass ratio of the organic solvent to the inorganic solvent is (14-16):(5-7).

[0017] Preferably, the molecular weight of the silicone oil is 2.3×10 4 ~2.5×10 4 .

[0018] The second object of the present invention is to provide a method for preparing the modified polysiloxane-polycarbonate composition; the modified polysiloxane-polycarbonate composition has high mechanical properties while simplifying the preparation process, which is more friendly to raw materials and time costs.

[0019] The preparation method of the modified polysiloxane-polycarbonate composition adopts intermittent one-step polymerization, and the phosgenation reaction and the polycondensation reaction are carried out simultaneously, and specifically comprises the following steps:

[0020] After fully mixing all the components except phosgene, phosgene is introduced to synthesize the modified polysiloxane-polycarbonate composition by a one-step method; the content of sodium carbonate in the water phase and / or the molecular weight of the polycarbonate in the oil phase are monitored in real time to determine the reaction endpoint;

[0021] As phosgene is introduced into the reaction vessel until the reaction of bisphenol A reaches 90%, the side reaction will gradually become obvious: NaOH+COCl2==Na2CO3+NaCl+H2O.

[0022] Preferably, when the content of sodium carbonate in the aqueous phase is 16 g / kg to 18 g / kg, the introduction of phosgene is stopped and the reaction is terminated;

[0023] Preferably, when the molecular weight of the polycarbonate in the oil phase is 2700-3100, the introduction of phosgene is stopped and the reaction is terminated.

[0024] Preferably, before the reaction starts, the pH of the reaction system is 8.8 to 9.5; after the reaction ends, the pH of the reaction system is 10.5 to 11.3.

[0025] Preferably, an aqueous solution of alkaline hydroxide is continuously added during the reaction to control the pH of the reaction system to be maintained within the range of 8.8 to 11.3.

[0026] More preferably, before the reaction starts, the pH of the reaction system is 9.2; after the reaction ends, the pH of the reaction system is 10.8;

[0027] More preferably, at the midpoint of the reaction, the pH of the reaction system is 10.3, and the acceptable pH fluctuation range is 10.5 to 11.3.

[0028] Preferably, the preparation method may specifically include the following steps:

[0029] (1) mixing bisphenol A, triethylamine, additives and an inorganic solvent to obtain a first mixed phase; mixing sebacic acid, silicone oil, castor oil and an organic solvent to obtain a second mixed phase;

[0030] (2) adding the second mixed phase dropwise to the first mixed phase, while introducing phosgene into the closed reaction system; and continuing the reaction for 2 to 5 hours;

[0031] (3) subjecting the mixed phase obtained by the reaction to separation and purification treatments in sequence;

[0032] More preferably, in step (2), the temperature of the reaction system is 15°C to 60°C.

[0033] Preferably, the organic solvent in the present invention can be recycled and reused; however, it should be noted that the content of triethylamine in the organic solvent should be detected before recycling, and the amount of fresh triethylamine added should be reduced according to the residual triethylamine content, similarly to the inorganic solvent.

[0034] The third object of the present invention is to provide the use of the modified polysiloxane-polycarbonate composition in polymer materials; specifically, the use of the modified polysiloxane-polycarbonate composition in polymer materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the specific implementation scheme of the present invention, the drawings required for use in the specific implementation scheme or background technology description will be briefly introduced below. Obviously, the drawings in the following description are some implementation schemes of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 The graph is a variation curve of the phosgene intake, the sodium carbonate content in the water phase, and the molecular weight of the polycarbonate in the oil phase in the embodiment of the present invention. DETAILED DESCRIPTION

[0037] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0038] A modified polysiloxane-polycarbonate composition is prepared by including the following components in parts by mass:

[0039] 80-120 parts of bisphenol A, 70-90 parts of silicone oil, 15-25 parts of castor oil, 10-30 parts of sebacic acid, 90-110 parts of phosgene, 3-5 parts of triethylamine, 3-7 parts of additives, and 1800-2500 parts of solvent.

[0040] As a preferred embodiment, the weight proportions of bisphenol A include but are not limited to 80 parts, 82 parts, 84 parts, 86 parts, 88 parts, 90 parts, 92 parts, 94 parts, 96 parts, 98 parts, 100 parts, 102 parts, 104 parts, 106 parts, 108 parts, 110 parts, 112 parts, 114 parts, 116 parts, 118 parts, 120 parts; the weight proportions of silicone oil include but are not limited to 70 parts, 72 parts, 74 parts, 76 parts, 78 parts, 80 parts, 82 parts, 84 parts, 86 parts, 88 parts, 90 parts; the weight proportions of castor oil include but are not limited to 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts 3 parts, 24 parts, 25 parts; the weight parts of the sebacic acid include but are not limited to 10 parts, 15 parts, 20 parts, 25 parts, 30 parts; the weight parts of the phosgene include but are not limited to 90 parts, 92 parts, 94 parts, 96 parts, 98 parts, 100 parts, 102 parts, 104 parts, 106 parts, 108 parts, 110 parts; the weight parts of the triethylamine include but are not limited to 3 parts, 4 parts, 5 parts; the weight parts of the additive include but are not limited to 3 parts, 4 parts, 5 parts, 6 parts, 7 parts; the weight parts of the solvent include but are not limited to 1800 parts, 1900 parts, 2000 parts, 2100 parts, 2200 parts, 2300 parts, 2400 parts, 2500 parts.

[0041] As a preferred embodiment, the solvent includes an organic solvent and an inorganic solvent; the mass ratio of the organic solvent to the inorganic solvent includes but is not limited to 14:5, 14:6, 14:7, 15:5, 15:6, 15:7, 16:5, 16:6, 16:7.

[0042] The preparation method of the modified polysiloxane-polycarbonate composition mainly comprises the following steps: after fully mixing all components except phosgene, introducing phosgene, and synthesizing the modified polysiloxane-polycarbonate composition by a one-step method; real-time monitoring of the content of sodium carbonate in the water phase, and / or real-time monitoring of the molecular weight of polycarbonate in the oil phase to determine the reaction endpoint;

[0043] As a preferred embodiment, when the content of sodium carbonate in the aqueous phase includes but is not limited to 16 g / kg, 17 g / kg, 18 g / kg, and / or when the molecular weight of the polycarbonate in the oil phase includes but is not limited to 2700, 2800, 2900, 3000, 3100, the introduction of phosgene is stopped and the reaction is terminated.

[0044] As a preferred embodiment, the pH of the reaction system at the beginning of the reaction includes but is not limited to 8.8, 8.9, 9.0, 9.1, 9.2, 9.3, 9.4, 9.5; the pH of the reaction system at the end of the reaction includes but is not limited to 10.5, 10.6, 10.7, 10.8, 10.9, 11.0, 11.1, 11.2, 11.3.

[0045] Example

[0046] (1) Raw materials weighing: 100 g bisphenol A, 80 g silicone oil (molecular weight 24k), 20 g castor oil, 20 g sebacic acid, 4.9 g p-cumylphenol, 266 g 33% sodium hydroxide solution, 4.2 g triethylamine, 1489 g dichloromethane, and 352 g deionized water;

[0047] (2) bisphenol A, triethylamine, p-cumylphenol, sodium hydroxide solution and deionized water are mixed to obtain a first mixed phase; sebacic acid, silicone oil, castor oil and dichloromethane are mixed to obtain a second mixed phase; after each mixed phase is stirred independently until uniform, the first mixed phase is transferred to a three-necked flask, and the reaction temperature is heated and maintained at 45° C.; the second mixed phase is added dropwise to the three-necked flask, and phosgene is introduced at the same time to start the reaction;

[0048] (3) Real-time monitoring of the pH of the reaction system to see if it is between 8.8 and 11.3; if the pH value is too high, it means that the phosgene flow rate is too high, and the pH value can be controlled to be within the above range by adding additional sodium hydroxide aqueous solution;

[0049] (4) Real-time monitoring of the content of sodium carbonate in the water phase and the molecular weight of polycarbonate in the oil phase, and drawing of a real-time curve graph by computer, such as Figure 1 As shown; among them, Figure 1 The horizontal axis is the phosgene input (unit: pounds), Figure 1 The vertical axis (left) is the sodium carbonate content. Figure 1 The ordinate (right) is the molecular weight of polycarbonate. In this embodiment, when the total mass of phosgene introduced reaches 4300 pounds, the reaction is stopped.

[0050] (5) The emulsion after the reaction is centrifuged and then eluted with dichloromethane to obtain a modified polysiloxane-polycarbonate composition.

[0051] Table 1 is a summary of the test results of the strength performance indicators of the products prepared in this embodiment.

[0052] Table 1

[0053] Performance Indicators parameter unit Test Standards Tensile stress, yld, Type Ⅰ, 50mm / min 61 MPa ASTM D 638 Tensile stress, brk, Type Ⅰ, 50mm / min 58 MPa ASTM D 638 Tensile modulus, 5mm / min 2250 MPa ASTM D 638 Bending stress, yld, 1.3mm / min, 50mm span 98 MPa ASTM D 790 Flexural modulus, 1.3mm / min, 50mm span 2265 MPa ASTM D 790 Hardness, Rockwell hardness R 136 / ASTM D 785 Tensile stress, yld, 50mm / min 65 MPa ISO 527 Tensile stress, brk, 50mm / min 62 MPa ISO 527 Tensile modulus, 1mm / min 2237 MPa ISO 527

[0054] Table 2 is a summary of the test results of the mechanical properties of the products prepared in this example.

[0055] Table 2

[0056]

[0057]

[0058] Table 3 is a summary of the test results of thermal performance indicators of the products prepared in this embodiment.

[0059] Table 3

[0060] Performance Indicators parameter unit Test Standards Vicat softening temperature, Rate B / 50 138 ℃ ASTM D 1525 HDT, 0.45MPa, 3.2mm (before annealing) 123 ℃ ASTM D 648 HDT, 1.82MPa, 3.2mm (before annealing) 117 ℃ ASTM D 648

[0061] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A modified polysiloxane-polycarbonate composition, characterized in that: The modified polysiloxane-polycarbonate composition is prepared from the following components in parts by mass: 80-120 parts of bisphenol A; Silicone oil 70-90 parts; 15-25 parts of castor oil; 10-30 parts of sebacic acid; Phosgene 90-110 parts; 3-5 parts of triethylamine; 3-7 parts of additives; 1800-2500 parts of solvent; The molecular weight of the silicone oil is 2.3×10 4 ~2.5×10 4 .

2. The modified polysiloxane-polycarbonate composition according to claim 1, characterized in that: The additive includes at least one of p-cumylphenol, p-isopropylphenol and p-tert-butylphenol.

3. The modified polysiloxane-polycarbonate composition according to claim 1, characterized in that: The solvent includes organic solvent and inorganic solvent; wherein, The organic solvent is dichloromethane; The inorganic solvent includes an aqueous solution of an alkaline hydroxide.

4. The modified polysiloxane-polycarbonate composition according to claim 3, characterized in that: The alkaline hydroxide includes at least one of sodium hydroxide, potassium hydroxide, ammonia monohydrate and lithium hydroxide.

5. The modified polysiloxane-polycarbonate composition according to claim 3, characterized in that: The mass content of the aqueous solution of the alkaline hydroxide is 30% to 40%.

6. The modified polysiloxane-polycarbonate composition according to claim 3, characterized in that: The mass ratio of the organic solvent to the inorganic solvent is (14-16):(5-7).

7. The method for preparing the modified polysiloxane-polycarbonate composition according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: After fully mixing all components except phosgene, phosgene is introduced to synthesize the modified polysiloxane-polycarbonate composition by a one-step method; The sodium carbonate content in the water phase is monitored in real time, and / or the molecular weight of the polycarbonate in the oil phase is monitored in real time to determine the reaction endpoint.

8. The method for preparing the modified polysiloxane-polycarbonate composition according to claim 7, characterized in that: When the content of sodium carbonate in the aqueous phase is 16 g / kg to 18 g / kg, the introduction of phosgene is stopped and the reaction is terminated; When the molecular weight of the polycarbonate in the oil phase is 2700-3100, the introduction of phosgene is stopped and the reaction is terminated.

9. The method for preparing the modified polysiloxane-polycarbonate composition according to claim 7, characterized in that: Before the reaction begins, the pH of the reaction system is 8.8 to 9.5; after the reaction ends, the pH of the reaction system is 10.5 to 11.

3.

10. The method for preparing the modified polysiloxane-polycarbonate composition according to claim 7, characterized in that: During the reaction, an aqueous solution of alkaline hydroxide is continuously added to control the pH of the reaction system to be maintained within a range of 8.8 to 11.

3.

11. The method for preparing the modified polysiloxane-polycarbonate composition according to claim 7, characterized in that: The preparation method comprises the following steps: (1) mixing bisphenol A, triethylamine, additives and an inorganic solvent to obtain a first mixed phase; mixing sebacic acid, silicone oil, castor oil and an organic solvent to obtain a second mixed phase; (2) adding the second mixed phase dropwise to the first mixed phase, while introducing phosgene into the closed reaction system; and continuing the reaction for 2 to 5 hours; (3) The mixed phase obtained by the reaction is subjected to separation and purification treatments in sequence.

12. The method for preparing the modified polysiloxane-polycarbonate composition according to claim 11, characterized in that: In step (2), the temperature of the reaction system is 15°C to 60°C.

13. Use of the modified polysiloxane-polycarbonate composition according to any one of claims 1 to 6 in polymer materials.