A method for improving the weld quality of 2xxx aluminum alloy sheets

Through two-stage solid solution treatment, deep cold rolling, warm rolling and underwater friction stir welding, the problem of large loss of material performance during traditional welding is solved, and the mechanical properties of 2xxx aluminum alloy joints are significantly improved. It is suitable for aviation Lightweight demands in the aerospace industry.

CN115415321BActive Publication Date: 2024-11-12CENT SOUTH UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210905071.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-29
Publication Date
2024-11-12
Estimated Expiration
2042-07-29

AI Technical Summary

Technical Problem

The temperature of the traditional air-cooled friction stir welding to the 2xxx aluminum alloy is high during welding, resulting in large loss of material performance, generally insufficient joint strength, and generally only 370-380MPa, which is difficult to meet the lightweight needs of the aerospace industry.

Method used

Underwater friction stir welding is carried out after two-stage solid solution treatment, deep cold rolling, warm rolling and aging treatment. The peak temperature and high temperature duration of the welding area are reduced through liquid nitrogen cooling and water cooling, and grain coarsening and precipitation are reduced. The dissolution of the phase improves the mechanical properties of the joint.

Benefits of technology

It significantly improves the yield strength and tensile strength of the 2xxx aluminum alloy joint, enhances the mechanical properties of the welding area, and achieves higher mechanical properties and thermal stability. It is suitable for the connection of high-strength aluminum alloys and has industrial application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115415321B_ABST
    Figure CN115415321B_ABST
Patent Text Reader

Abstract

A method for improving the weld quality of 2xxx aluminum alloy thin plates, wherein the 2xxx aluminum alloy plates are subjected to two-stage solid solution treatment at 755-760K for 10-20min and 765-770K for 30-60min, then quenched at room temperature and cooled to room temperature, then cooled in liquid nitrogen, and deep cold rolled, with a total reduction rate of 45%-55%; then heated at 390-400K for 4-5min, and warm rolled, with a total reduction rate of 60-70%; finally, an aging treatment at 395-405K for 10-13h is performed, and the plates after the aging treatment can be subjected to underwater friction stir welding. The present invention can improve the specific strength of the entire 2xxx aluminum alloy workpiece, thereby reducing the thickness to achieve lightweight, and ultimately improve the mechanical properties of the 2xxx aluminum alloy joint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal material rolling and welding, and in particular relates to a method for improving the quality of welds of 2xxx aluminum alloy sheets. Background Art

[0002] 2××× series aluminum alloy is an Al-Cu alloy, which is an important heat-treatable strengthened aluminum alloy. It has high strength, good heat resistance and processing properties, but is not easy to weld. This series of alloys are widely used in the fields of aviation and aerospace to manufacture aircraft structures (skins, frames, bulkheads, etc.), missile components and various other structural parts. When used in the aerospace industry, in order to achieve lightweight, it is difficult to avoid welding processes, and the joints are generally the weakest areas of the entire component. Therefore, improving the strength of the welded joints of 2××× aluminum alloys plays an important role in promoting the development of the aerospace industry.

[0003] The strength of the base material of the commonly used aluminum alloy is not high, and performance loss is inevitable during the welding process. The main welding method for heat-treatable and strengthened aluminum alloys is stir friction welding. The joint is divided into the weld nugget zone (abbreviated as NZ), thermally affected zone (abbreviated as TMAZ), heat affected zone (abbreviated as HAZ) and base material (abbreviated as BM) from the welding center to the outside according to the different stirring and thermal effects. However, the temperature of traditional air-cooled stir friction welding is relatively high, which causes a large loss of material performance. Therefore, the joint strength performance is generally poor, and the yield strength is generally only 370-380MPa. Summary of the invention

[0004] In order to overcome the shortcomings of the above-mentioned prior art, the object of the present invention is to provide a method for improving the quality of welds of 2xxx aluminum alloy thin plates, so as to improve the overall specific strength of 2xxx aluminum alloy workpieces, thereby reducing the thickness to achieve lightweight, and ultimately improving the mechanical properties of 2xxx aluminum alloy joints.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for improving the weld quality of 2xxx aluminum alloy thin plates comprises the following steps:

[0007] In the first step, the 2xxx aluminum alloy plate is subjected to a two-stage solution treatment, the first stage solution treatment temperature is 755-760K, the time is 10-20min; the second stage solution treatment temperature is 765-770K, the time is 30-60min;

[0008] In the second step, the plate after the two-stage solution treatment is quenched in water at room temperature and cooled to room temperature;

[0009] The third step is to immerse the plate cooled to room temperature in liquid nitrogen to cool it down to 77-87K;

[0010] The fourth step is to immediately roll the cooled sheet;

[0011] Step 5, repeating steps 3 and 4 until the total reduction rate reaches 45% to 55%. The rolling reduction rate can be adjusted appropriately according to the thickness of the 2xxx-T6 plate to be welded;

[0012] Step 6, heating the plate after rolling in step 5 at 390-400K for 4-5min;

[0013] Step 7, rolling the heated sheet immediately;

[0014] Step 8, repeating steps 6 and 7 until the total reduction rate reaches 60-70%;

[0015] The ninth step is to perform aging treatment on the plate after rolling in the eighth step, with the treatment temperature being 395-405K and the time being between 10 and 13 hours, so as to achieve simultaneous improvement of material strength and elongation;

[0016] The tenth step is to perform underwater friction stir welding on the plates after aging treatment.

[0017] In one embodiment, in the first step, the thickness of the 2xxx aluminum alloy plate is 0.8 mm to 4 mm.

[0018] In one embodiment, in the fourth step, the rolling speed is 3-4 m / min, and the single-pass reduction rate is 7%-8%.

[0019] In one embodiment, in the sixth step, the plate is placed in a forced air drying furnace for heating.

[0020] In one embodiment, in the seventh step, the rolling speed is 3-4 m / min, and the single-pass reduction rate is 4%-5%.

[0021] In one embodiment, in the tenth step, the welding speed is 50-300 mm / min, the rotation speed is 500-5000 rpm, and the water flow rate is 5-10 L / min.

[0022] The main principles of the present invention are:

[0023] After deep cold rolling and warm rolling, the 2xxx aluminum alloy treated by solid solution has a large number of fine precipitates compared to ordinary T4 state materials, with higher strength and thermal stability, leaving room for performance degradation during welding of the joint. At the same time, through underwater friction stir welding, running water cooling reduces the peak temperature and high temperature duration of the welding area, reduces the coarsening of grains and the dissolution or coarsening of precipitates, greatly improves the strength of the soft zone, and improves the mechanical properties of the joint to a greater extent.

[0024] The method of the present invention is suitable for connecting high-strength 2xxx aluminum alloy strips, and the thickness of the strip products ranges from 0.25mm to 1.2mm. The aluminum alloy strips connected using this technology have excellent mechanical properties and have industrial application prospects in industries such as circuit boards, batteries, new energy vehicles, and aerospace. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Shown is the process flow chart of CWR and underwater friction stir welding of 2xxx aluminum alloy.

[0026] Figure 2 Schematic diagram of the friction stir welding weld surface, where (a) is CWR / T4; (b) is T4 / T4; and (c) is CWR / CWR.

[0027] Figure 3 Optical micrographs of CWR / T4 joints, where (a) is the complete joint, (b) is the HAZ / TMAZ on AS, (c) is the TMAZ / HAZ on RS, (d) is the NZ on AS, (e) is the NZ on RS, (f) is the optical micrograph of the black strip, and (g) is the enlarged image of the area within the dashed box in (f).

[0028] Figure 4 Optical micrographs of T4 / T4 joints, where (a) is the complete joint, (b) is the HAZ / TMAZ on RS, (c) is the NZ, and (d) is the TMAZ / HAZ on AS.

[0029] Figure 5 Optical micrographs of CWR / CWR joints, where (a) is the complete joint, (b) is the HAZ / TMAZ on RS, (c) is the NZ, and (d) is the TMAZ / HAZ on AS.

[0030] Figure 6 It is a schematic diagram comparing the tensile curves of a conventional friction stir welded 2024 aluminum alloy joint and the joint of the present invention.

[0031] Figure 7 It is a schematic diagram comparing the mechanical properties of a conventional friction stir welded 2024 aluminum alloy joint and the joint of the present invention. DETAILED DESCRIPTION

[0032] The embodiments of the present invention are described in detail below with reference to the accompanying drawings and examples.

[0033] like Figure 1 As shown, the present invention is a method for improving the quality of the weld of a 2xxx aluminum alloy sheet, comprising the following steps:

[0034] In the first step, the 2xxx aluminum alloy sheet is subjected to a two-stage solution treatment.

[0035] In the present invention, the thickness of the 2xxx aluminum alloy sheet is 0.8 mm to 4 mm, which meets the definition of "thin sheet". Here, through the two-stage solution treatment, it is possible to prevent the sheet from being overburned due to the temperature surge during the solution treatment, and it is also beneficial for the sheet to be fully dissolved, which is convenient for subsequent plastic processing.

[0036] For example, in this embodiment, the first-stage solid solution treatment temperature may be 758K, and the time may be 10 to 20 minutes; the second-stage solid solution treatment temperature may be 768K, and the time may be 30 to 60 minutes.

[0037] The second step is to quench the plate after the two-stage solid solution treatment in water at room temperature and cool it to room temperature. This step can form a supersaturated solid solution through rapid cooling, so that finer precipitation phases can be formed through artificial aging after plastic deformation, thereby improving the performance of the plate.

[0038] In the third step, the plate 2 cooled to room temperature is immersed in a cryogenic box 1 cooled by liquid nitrogen to cool the plate 2 to a temperature of 77-80K.

[0039] The fourth step is to immediately roll the cooled plate, that is, to make the plate 4 deep-cooled by liquid nitrogen pass through the roller 3 to achieve rolling. For example, the rolling speed is 3-4 m / min, and the single-pass reduction rate is 7%-8%.

[0040] Step 5: Repeat steps 3 and 4 until the total reduction rate reaches 48% to 52%.

[0041] Through the deep cold rolling from the third step to the fifth step, a large number of dislocations and subgrains can be formed inside the 2xxx aluminum alloy, which in turn promotes the production of a large number of dynamically recrystallized grains and the formation of a certain number of precipitates during the subsequent hot rolling process.

[0042] In the sixth step, the plate after rolling in the fifth step is heated at 390-398 K for 4-5 min. For example, the plate can be placed in a blast drying furnace 5 during heating.

[0043] The seventh step is to immediately roll the heated plate 6. For example, the rolling speed is 3-4 m / min and the single-pass reduction rate is 4%-5%.

[0044] Step 8: Repeat steps 6 and 7 until the total reduction rate reaches 60-70%.

[0045] The warm rolling process from the sixth step to the eighth step can promote the precipitation of solute atoms or clusters into finer precipitation strengthening phases, thereby improving the strength and thermal stability of the material.

[0046] Therefore, after deep cold rolling + warm rolling process (abbreviated as CWR in the full text), a base material with higher strength can be produced.

[0047] The ninth step is to perform aging treatment on the plate 7 after rolling in the eighth step. For example, the treatment temperature is 400-405K and the time is between 10 and 13 hours to achieve simultaneous improvement of material strength and elongation. Through the aging treatment in this step, on the one hand, a large number of defects generated by the material during plastic processing can be eliminated through low-temperature recovery, and at the same time, a large number of solute atoms or clusters can exist in the form of a more stable precipitation phase, thereby improving its thermal stability and avoiding a sharp deterioration of performance in the subsequent welding process. On the other hand, it can reduce the residual stress of the plate, which is beneficial to the subsequent clamping of the welding equipment.

[0048] The tenth step is to perform underwater friction stir welding on the aging treated plate to obtain a high-performance joint. For example, the welding speed is 50-300 mm / min, the rotation speed is 500-5000 rpm, and the water flow rate is 5-10 L / min. Figure 1 In the figure, the device relied on by underwater friction stir welding includes a water tank 13 with a water inlet 15 and a water outlet 8, the water tank 13 has a built-in stirring head 12 and a pad 9, two welding base materials 11 are fixed by a clamping device 10, and the weld 14 can be clearly seen along the welding direction.

[0049] The traditional air-cooled friction stir welding has a high temperature, which will dissolve or coarsen the precipitation strengthening phase in the heat-treated aluminum alloy, coarsen the grains in the heat-affected zone, thereby softening the joint and seriously reducing its mechanical properties. In order to solve these problems, the present invention uses water cooling to reduce the peak temperature and high temperature duration of the welding area, reduce grain coarsening and precipitation phase dissolution, and is conducive to maintaining the excellent performance of the parent material.

[0050] In a specific embodiment of the present invention, a 1 mm thick 2024 aluminum alloy high-performance joint is prepared by welding. The original material used is a 3 mm thick 2024 aluminum alloy plate, the first stage solution treatment temperature is 758K, the time is 10 min; the second stage solution treatment temperature is 768K, the time is 30 min. Its deep cooling temperature in liquid nitrogen is 77K, the speed of deep cold rolling is 3m / min, the single pass reduction rate is 8%, and it is repeated until the total reduction rate reaches 50%. Subsequently, it is heated at 393K in a blast drying furnace for 5 minutes, the rolling speed of warm rolling is 3m / min, the single pass reduction rate is 5%, and it is repeated until the total reduction rate reaches 66% (that is, the final thickness is 1mm), and a 2024 aluminum alloy strip without crack defects and relatively straight is prepared.

[0051] The aging treatment temperature is 403K, the time is between 12h, and the yield strength of the base material reaches 554MPa, the tensile strength is 615MPa, and the uniform elongation is 4.5%. Finally, underwater friction stir welding is performed, the stirring shoulder diameter is 10mm, the stirring needle diameter is 3.5mm, the stirring needle length is 0.7mm, the pressing depth is 0.2mm, there is no inclination, the pitch is 0.5mm, the welding speed is 50mm / min, the rotation speed is 2500rpm, and the water flow rate is 5L / min.

[0052] like Figure 2 As shown in (a), (b) and (c), it can be seen that the surface quality of the joint is good without obvious defects. Figures 3 to 5 This is a metallographic photograph of the joint. It can be seen that the BM area is composed of fine equiaxed crystals with a diameter of about 2μm. The main difference is that the grains in the TMAZ and HAZ areas of the CWR material are finer, so the strength is higher. The yield strength of the T4 / T4 joint is 259MPa, the tensile strength is 355MPa, and the uniform elongation is 5.8%. In contrast, the yield strength of the CWR / T4 joint is 309MPa, the tensile strength is 414MPa, and the uniform elongation reaches 6.9%. The yield strength of the CWR / CWR joint is 299MPa, the tensile strength is 420MPa, and the uniform elongation reaches 7.8%. The mechanical properties of the strip prepared by CWR after welding are shown in Figure 2. Figure 6 and Figure 7 As shown, the performance of the joint is greatly improved compared with that of the traditional joint, indicating that the present invention has obvious advancement.

Claims

1. A method for improving the weld quality of 2024 aluminum alloy sheet, characterized in that: The steps include: In the first step, the 2024 aluminum alloy plate is subjected to a two-stage solution treatment. The first stage solution treatment temperature is 755-760K, and the time is 10-20min; the second stage solution treatment temperature is 765-770K, and the time is 30-60min. In the second step, the plate after the two-stage solution treatment is quenched in water at room temperature and cooled to room temperature; The third step is to immerse the plate cooled to room temperature in liquid nitrogen to cool it down to 77-87K; The fourth step is to immediately roll the cooled sheet; Step 5: Repeat steps 3 and 4 until the total reduction rate reaches 45% to 55%; Step 6, heating the plate after rolling in step 5 at 390-400K for 4-5min; Step 7, rolling the heated sheet immediately; Step 8, repeating steps 6 and 7 until the total reduction rate reaches 60-70%; The ninth step is to perform aging treatment on the plate after rolling in the eighth step, with the treatment temperature being 395-405K and the time being between 10 and 13 hours, so as to achieve simultaneous improvement of material strength and elongation; The tenth step is to perform underwater friction stir welding on the plates after aging treatment.

2. The method for improving the weld quality of 2024 aluminum alloy sheet according to claim 1, characterized in that: In the first step, the thickness of the 2024 aluminum alloy plate is 0.8 to 4 mm.

3. The method for improving the weld quality of 2024 aluminum alloy sheet according to claim 1, characterized in that: In the fourth step, the rolling speed is 3-4 m / min, and the single-pass reduction rate is 7-8%.

4. The method for improving the weld quality of 2024 aluminum alloy sheet according to claim 1, characterized in that: The sixth step is to place the plate in a blast drying furnace for heating.

5. The method for improving the weld quality of 2024 aluminum alloy sheet according to claim 1, characterized in that: In the seventh step, the rolling speed is 3-4 m / min, and the single-pass reduction rate is 4%-5%.

6. The method for improving the weld quality of 2024 aluminum alloy sheet according to claim 1, characterized in that: In the tenth step, the welding speed is 50-300 mm / min, the rotation speed is 500-5000 rpm, and the water flow rate is 5-10 L / min.

Citation Information

Patent Citations

  • Friction stir welding method in underwater environment

    CN101439439A

  • Method for improving plasticity of underwater stir friction welding joint

    CN101934426A

  • Ausforming method capable of improving mechanical property of aluminum alloy rolled plate

    CN108018509A

  • Underwater friction stir welding and postweld heat treatment combined process method

    CN112108755A

  • Welding device and method for underwater friction stir welding

    CN113146022A