Composite depressant, flotation agent and method for reverse flotation dephosphorization of phosphorus-containing lithium ore
By using composite inhibitors in spodumene and apatite, combining EDTA and its salts and alginate, selective separation of spodumene and apatite is achieved, and the problem of excessive phosphorus content in lithium concentrate is solved. It reduces the cost of lithium extraction and environmental pollution risks, and meets the industry standard lithium recycling requirements.
Patent Information
- Application Number
- CN202210998204.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-08-19
AI Technical Summary
During the flotation separation process of spodumene and apatite, the existing inhibitors are poorly selective and cannot effectively separate spodumene and apatite, resulting in the phosphorus content in lithium concentrate exceeding the standard, increasing the cost of lithium extraction and environmental pollution risks.
A complex inhibitor is used, including component A and component B, which is a compound with a specific structure, such as EDTA and its salt, and component B is alginic acid and its salt, which selectively inhibits lithium radiance through synergistic action. Stone basically does not inhibit apatite, thereby achieving selective separation of spodumene and apatite.
It significantly reduces the P2O5 content in lithium concentrate, improves lithium recovery rate, reduces the loss rate of lithium in apatite tailings, meets the non-ferrous metal industry standards, and has a simple, safe and suitable for industrial applications.
Smart Images

Figure CN115430526B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of mineral flotation, and in particular relates to the technical field of flotation separation of spodumene and apatite. Background Art
[0002] Lithium is a silvery white, soft, rare metal of the new century. It has strong electrochemical activity and is widely used in various fields. With the rapid development of the world's industry and the rising demand for new energy, the development and utilization of lithium mineral resources has also attracted much attention. Lithium is mainly separated and extracted from various lithium-containing minerals. Common lithium-containing minerals include spodumene [LiAl(SiO3)2], lithium mica [KLi 1.5 Al 1.5 (AlSi3O 10 )], lithium aluminum phosphate [LiAl(PO4)(OHF)], etc., usually coexist with gangue minerals such as feldspar, quartz, mica, and apatite.
[0003] In industry, spodumene is the main raw material for extracting lithium. As one of the main lithium-containing mineral resources, for low-grade spodumene mines, a large amount of harmful impurities will accumulate during the flotation enrichment of concentrates, such as excessive phosphorus and other impurities, which is extremely unfavorable for the subsequent smelting and lithium extraction process. It will not only reduce the recovery rate of lithium, but also add impurity removal procedures, which will increase the cost of lithium extraction sharply. And according to the latest non-ferrous metal industry standards, the P2O5 content of all spodumene concentrates must be less than 1.0%. If it is greater than this value, the price of spodumene concentrate will be greatly discounted. At the same time, the less phosphorus content in the spodumene concentrate, the better the quality and the higher the price. As lithium-containing mines at home and abroad are gradually becoming low-grade and high-impurity, it is not uncommon for the phosphorus content of lithium concentrates enriched by flotation to exceed the standard. Conventional high-phosphorus lithium concentrate dephosphorization methods include strong acid leaching to dissolve phosphorus-containing minerals and strong acid reverse flotation dephosphorization, which have the disadvantages of serious environmental damage and large equipment investment. Therefore, it is urgent to develop an efficient and simple dephosphorization method. Considering that the main minerals in the high-phosphorus lithium concentrate activated by metal ions are spodumene and apatite, both of which have good floatability, and the floatability of apatite is better than that of spodumene, the phosphorus-containing minerals in the lithium concentrate can be removed by inhibiting the reverse flotation of spodumene and apatite in a suitable slurry environment. At the same time, there are few studies on spodumene inhibitors. The conventional spodumene inhibitor sodium sulfide is easily oxidized, the selectivity is not obvious enough and the inhibitory property is weak, so it is impossible to separate spodumene and apatite by flotation. Therefore, it is of great significance to study and develop a new type of spodumene composite inhibitor with high selectivity and strong inhibitory property. Summary of the invention
[0004] The object of the present invention is to provide a composite inhibitor for reverse flotation dephosphorization of phosphorus-containing lithium ore, aiming to provide a composite inhibitor for selectively inhibiting spodumene in spodumene-apatite.
[0005] The second object of the present invention is to provide a method for reverse flotation dephosphorization in phosphorus-containing lithium ore, aiming to utilize the composite inhibitor to selectively inhibit spodumene, thereby reverse flotating apatite to obtain spodumene concentrate.
[0006] The third object of the present invention is to provide a composite flotation agent for reverse flotation and dephosphorization of phosphorus-containing lithium ore comprising the composite inhibitor.
[0007] Both spodumene and apatite in phosphorus-containing lithium ore have good floatability, but the selective flotation separation of the two is difficult; the existing inhibitors have poor selectivity for spodumene and apatite, and cannot achieve good flotation separation. To this end, the present invention provides the following technical solutions:
[0008] A composite inhibitor for reverse flotation dephosphorization of phosphorus-containing lithium ore, comprising component A and component B;
[0009] The component A is at least one of the compounds having the structure of Formula 1:
[0010]
[0011] The A1 to A4 are independently carboxylate or phosphate;
[0012] The X and Y are independently C1-C6 alkylene;
[0013] The component B comprises at least one of alginic acid and its salts, and malic acid and its salts.
[0014] The present invention finds that combining components A and B can achieve synergy and can selectively inhibit spodumene in spodumene-apatite while substantially not inhibiting apatite, thereby enabling inhibition of spodumene and reverse flotation of apatite, thereby improving the reverse flotation separation selectivity of spodumene and apatite.
[0015] In the present invention, the combination of component A and component B is the key to synergistically improving the spodumene-apatite inhibition selectivity. The present invention also found that further control of the component structure is helpful to further improve the synergistic effect of the combined components.
[0016] In the present invention, the ionic state of Formula 1 can be provided by the acid of the structure and its water-soluble salt (such as sodium salt, potassium salt, ammonium salt, etc.).
[0017] Preferably, the component A is a compound having the structural formula 1-A or 1-B;
[0018]
[0019] Preferably, the formula 1-A comprises at least one of EDTA and EDTA salts; preferably comprises at least one of EDTA, disodium EDTA, tetrasodium EDTA, dipotassium EDTA and tetrapotassium EDTA.
[0020]
[0021] The n is 1, 2 or 3.
[0022] In Formula 1-B, at least one of EDTMP, EDTMP salt, HMDTMP, and HMDTMP salt is included; more preferably, at least one of EDTMP, tetrasodium EDTMP, tetrapotassium EDTMP, HMDTMP, tetrasodium HMDTMP, and tetrapotassium HMDTMP is included.
[0023] Preferably, the component A comprises formula 1-A and formula 1-B. The present invention has found that the combination of formula 1-A and formula 1-B can achieve a better combined synergistic effect with component B, which helps to further improve the inhibition effect of spodumene in phosphorus-containing lithium minerals and further weaken the inhibition of apatite, so that the reverse flotation removal effect of apatite can be further improved and the loss of spodumene can be reduced.
[0024] Preferably, the molar ratio of Formula 1-A to Formula 1-B is 1 to 5:1; more preferably 3 to 5:1.
[0025] In the present invention, the component control of the component B is the key to achieving the selective inhibition of spodumene in combination with the component A.
[0026] In the present invention, in the component B, the alginate is a water-soluble salt of alginic acid, preferably at least one of sodium alginate, potassium alginate and ammonium alginate;
[0027] Preferably, the malate is a water-soluble salt of malic acid, preferably at least one of sodium malate, potassium malate and ammonium malate.
[0028] Preferably, the molar proportion of component A in the composite inhibitor is 60 to 90 parts, and the molar proportion of component B is not higher than 40 parts. More preferably, the molar proportion of component A is 70 to 90 parts, and the molar proportion of component B is 5 to 30 parts. Even more preferably, the molar proportion of component A is 75 to 85 parts, and the molar proportion of component B is 15 to 25 parts.
[0029] The present invention also provides a method for reverse flotation dephosphorization in phosphorus-containing lithium ore, wherein the phosphorus-containing lithium ore is subjected to reverse flotation using a flotation agent containing the composite depressant to suppress spodumene therein, and reverse flotation of apatite therein to obtain spodumene concentrate and apatite tailings.
[0030] The present invention also found that, with the innovative use of the composite inhibitor, combined with the dosage of the composite inhibitor in the reverse flotation stage, pH and the temperature of the reverse flotation, further synergy can be achieved, further improving the inhibition selectivity of spodumene in phosphorus-containing lithium ore, improving the separation selectivity of spodumene and apatite, and further reducing the P2O5 content in the spodumene concentrate to ensure that the non-ferrous metal industry standards are fully met, while significantly reducing the loss rate of lithium in the apatite tailings.
[0031] In the present invention, in the reverse flotation stage, the amount of the composite depressant is greater than or equal to 5×10 -5 mol / L; preferably 2×10 -4 mol / L-8×10 -4 mol / L, more preferably 4 to 8×10 -4 mol / L, the most preferred is 5 to 6×10 -4 mol / L;
[0032] Preferably, in the reverse flotation stage, the pH of the pulp is 4 to 10, preferably 5 to 9, and more preferably 6 to 7;
[0033] Preferably, in the reverse flotation stage, the temperature of the slurry is 5 to 50°C, preferably 10 to 40°C; more preferably 20 to 40°C;
[0034] In the present invention, the flotation reagent also includes a collector;
[0035] The collector of the present invention may be a collector known in the industry for apatite flotation, for example, the collector includes at least one of sodium oleate, oxidized paraffin soap, cyclopentane acid soap, and tall oil soap;
[0036] The amount of collector can be adjusted as needed. For example, the amount of collector is preferably 5×10 -5 mol / L~3×10 -4 mol / L.
[0037] In the present invention, the phosphorus-containing lithium ore is a mineral containing spodumene and apatite.
[0038] In the present invention, the phosphorus-containing lithium ore can be a phosphorus-containing lithium concentrate obtained by positive flotation. For example, the lithium ore is subjected to flotation by a metal ion activator and a fatty acid collector to obtain the phosphorus-containing lithium concentrate to be treated. The metal ion activator is a commonly used agent with activation performance in the industry, such as calcium chloride, magnesium chloride, ferric chloride, copper sulfate, etc. The fatty acid collector is a commonly used agent with collection performance in the industry, such as sodium oleate, oxidized paraffin soap, cyclopentane acid soap, etc.
[0039] The present invention also provides a composite flotation agent for reverse flotation dephosphorization of phosphorus-containing lithium ore, comprising a collector and the composite depressant;
[0040] Preferably, the collector comprises at least one of sodium oleate, oxidized paraffin soap, cyclopentane acid soap and tall oil soap.
[0041] Beneficial Effects
[0042] 1. In the present invention, component A and component B are combined to achieve synergy, can selectively inhibit spodumene in spodumene-apatite, and basically do not affect the flotation of apatite. In this way, apatite can be removed based on the reverse flotation method, and the loss rate of lithium in the apatite tailings can be significantly reduced.
[0043] 2. In the present invention, the combination of Formula 1-A, Formula 1-B and component B can further synergistically enhance the inhibition of spodumene and further reduce the impact on apatite flotation, which helps to further achieve high-selective reverse flotation separation of spodumene-apatite.
[0044] 3. In the present invention, under the composite inhibitor, the combination of the inhibitor dosage, pH and temperature in the reverse flotation stage is further coordinated to further achieve synergy and further improve the reverse flotation separation selectivity of spodumene-apatite. In addition, the processing conditions of the present invention are mild, which is conducive to industrial production and application.
[0045] 4. The medicament of the present invention has a wide source, is simple to prepare, is reasonably priced, is non-toxic and harmless, has strong adaptability, and has great promotion value and application prospects in actual production.
[0046] 5. The composite inhibitor of the present invention has a synergistic effect, which can significantly reduce the P2O5 content in spodumene concentrate, which can not only ensure the selling price of spodumene concentrate, but also reduce the impurity removal process in the subsequent smelting and lithium extraction process, thereby improving the recovery rate of lithium metal and reducing the cost of lithium extraction. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 Flotation flow chart used for the examples and comparative examples; DETAILED DESCRIPTION
[0048] The effect of the present invention is illustrated by taking the high-phosphorus lithium concentrate flotated in Henan as an example. In the following cases, unless otherwise stated, the composition of the minerals used is as shown in Table 1:
[0049] Table 1 Original grade and origin of high phosphorus lithium concentrate
[0050]
[0051] Example 1
[0052] use Figure 1 The process shown in the figure is to implement the inhibitor 1 in different # ~8 # 、Comparison inhibitor 1 # ~13 # Lithium ore B was subjected to reverse flotation dephosphorization. The flotation process parameters of each group of cases were the same, and the only difference was the inhibitor, so as to explore the selectivity and inhibitory effect of the composite inhibitor in this case. (Note: The ratios in the following combined reagents refer to molar ratios)
[0053] Example Inhibitors:
[0054] Implementation of inhibitor 1 # : Composite inhibitor component (disodium EDTA: EDTMP: sodium alginate = 6:2:2).
[0055] Implementation of Inhibitor 2 # : Composite inhibitor component (disodium EDTA: EDTMP: sodium alginate = 8:1:1).
[0056] Implementation of Inhibitor 3 # : Composite inhibitor component (disodium EDTA: EDTMP: sodium alginate = 4:3:3).
[0057] Implementation of Inhibitor 4 # : Composite inhibitor component (tetrasodium EDTA: EDTMP: sodium alginate = 6:2:2).
[0058] Implementation of inhibitor 5 # : Composite inhibitor component (disodium EDTA: tetrasodium EDTMP: sodium alginate = 6:2:2).
[0059] Implementation of inhibitor 6 # : Composite inhibitor component (disodium EDTA: EDTMP: sodium malate = 6:2:2).
[0060] Implementation of inhibitor 7 # : Composite inhibitor component (disodium EDTA: sodium alginate = 4:1).
[0061] Implementation of inhibitor 8 # : Composite inhibitor component (EDTMP: sodium alginate = 4:1).
[0062] Comparative ratio inhibitor:
[0063] Comparison inhibitor 1 # : Conventional inhibitor sodium sulfide.
[0064] Comparison inhibitor 2 # : Single inhibitor component A (disodium EDTA).
[0065] Comparison inhibitor 3 # : Single inhibitor component A (tetrasodium EDTA).
[0066] Comparison inhibitor 4 # : Single inhibitor component A (EDTMP).
[0067] Comparison inhibitor 5 # : Single inhibitor component A (tetrasodium EDTMP).
[0068] Comparison inhibitor 6 # : Single inhibitor component B (sodium alginate).
[0069] Comparison inhibitor 7 # : Single inhibitor component B (sodium malate).
[0070] Comparison inhibitor 8 # : Similar to the inhibitor component (nitrilotriacetic acid) in formula 1-A.
[0071] Comparison inhibitor 9 # : Similar to the inhibitor component in formula 1-B (aminotrimethylenephosphonic acid).
[0072] Comparison inhibitor 10 # : Similar to inhibitor component B (sodium citrate).
[0073] Comparison of inhibitors 11 # : Similar composite inhibitor component (nitrotriacetic acid: sodium alginate = 4:1).
[0074] Comparison inhibitor 12 # : Similar composite inhibitor component (amino trimethylene phosphonic acid: sodium alginate = 4:1).
[0075] Comparison inhibitor 13 # : Similar composite inhibitor component (disodium EDTA: sodium citrate = 4:1).
[0076] The specific operation is as follows: a certain amount of lithium ore b is weighed and added to the flotation tank, and water is added to ensure that the pulp concentration is 20%; the reverse flotation of lithium ore b adopts a one-roughing-one-sweeping-one-fine process, and the pulp temperature is maintained at 20°C; the roughing is followed by adding 1.5×10 -3 mol / L to adjust the slurry pH to 6, different inhibitors and dosages 6×10 -4 mol / L, sodium oleate 1×10 -4 mol / L, stirring for 3min, 5min, 3min respectively, scraping for 3min; scanning and adding half amount of inhibitor 3×10 -4 mol / L, sodium oleate 5×10 -5mol / L, stirring time was 3min and 2min respectively, scraping foam was 3min; only one-fourth of the inhibitor was added 1.5×10 -4 mol / L, stirring time is 2min, scraping foam is 3min, the intermediate ore is returned in sequence, and a closed-loop circulation is carried out. After reaching equilibrium, the apatite tailings are scraped to the tailings basin along with the final foam, and the spodumene concentrate remains in the flotation tank. The concentrate and tailings are filtered and dried, and then weighed separately. The concentrate and tailings are chemically analyzed for P2O5 and Li2O grades and the recovery rate is calculated.
[0077] Table 2 shows the separation effect of lithium ore b under different types of inhibitors. (Based on the change under roughing conditions, the pH of the reverse flotation slurry is 6; the temperature of the reverse flotation slurry is 20°C; the amount of inhibitor is 6×10 -4 mol / L; the amount of collector sodium oleate is 1×10 -4 mol / L).
[0078] Table 2 Separation effect of lithium ore b under different inhibitor types
[0079]
[0080]
[0081]
[0082] As can be seen from Table 2, the implementation inhibitor 1 comprising three components # ~6 # The dephosphorization effect of 1 # The best result is that the P2O5 content in lithium concentrate can be reduced from 4.54% to 0.44%, the phosphorus removal rate is as high as 91.95%, and the lithium loss rate in apatite tailings is only 9.32%. In addition, compared with the implementation of inhibitor 1 # , changing the ratio between the three components of the implementation of inhibitor 2 # and 3 # The P2O5 content in the spodumene concentrate is high and the lithium loss rate in the apatite tailings is also high, indicating that the inhibitor components can only play the best synergistic role under the appropriate formula and ratio of the composite inhibitor; compared with adding only the conventional inhibitor sodium sulfide, that is, the comparative inhibitor 1 # When inhibitor A or inhibitor B is added alone, i.e., inhibitor 2 # ~7 #The P2O5 content in spodumene concentrate can be reduced to about 0.9%, and the phosphorus removal rate is about 85%. However, the loss rate of lithium in apatite tailings is as high as 20%, indicating that single inhibitor A or inhibitor B has a certain inhibitory effect on spodumene, and has little effect on the reverse flotation of apatite, but the separation effect of the two needs to be improved; when the implementation inhibitor 1 comprising three components # When the two components in the present invention are used in combination, the inhibitor 7 is implemented. # , 8 # The lithium extraction and dephosphorization effect is improved, the P2O5 content in the spodumene concentrate is less than 0.7%, and the lithium loss rate in the apatite tailings is reduced to about 18%; the use of a single and composite component of the composite inhibitor similar to the present invention is compared with the inhibitor 8 # ~13 # The lithium extraction and dephosphorization effect is obviously not as good as the implementation of inhibitor 1 # ~8 # , indicating that only by using the composite inhibitor can a better lithium extraction and dephosphorization effect be achieved; considering the synergy of the composite inhibitor of the present invention, the composite inhibitor (disodium EDTA: EDTMP: sodium alginate = 6:2:2) was selected as the preferred composite inhibitor formula and ratio for subsequent experiments and tests.
[0083] Example 2
[0084] In order to verify the dephosphorization effect of different dosages of composite inhibitor (Disodium EDTA: EDTMP: Sodium Alginate = 6:2:2) in this case, we used the flotation lithium ore b in Henan Province. Figure 1 The process shown in the figure uses different inhibitor dosages of 0 mol / L, 2×10 -4 mol / L、4×10 -4 mol / L、6×10 -4 mol / L、8×10 -4 mol / L was used for reverse flotation dephosphorization of lithium ore b. The flotation process parameters of each group of cases were the same, and the only difference was the dosage of composite depressant, so as to explore the selectivity and inhibition effect of different dosages of composite depressants in this case.
[0085] The specific operation is the same as that of Example 1. # The difference between the two experiments was that only the dosage of the composite inhibitor was changed.
[0086] Table 3 shows the separation effect of lithium ore b under different inhibitor dosages. (Based on the changes under roughing conditions, the pH of the reverse flotation slurry is 6; the reverse flotation slurry temperature is 20°C; the amount of collector sodium oleate is 1×10 -4 mol / L).
[0087] Table 3 Separation effect of lithium ore b at different inhibitor dosages
[0088]
[0089] It can be seen from Table 3 that when no composite depressant is added, although a small amount of lithium is enriched in the positive flotation concentrate, phosphorus is also further enriched, and the P2O5 content is 5.37%, far exceeding the non-ferrous metal industry standard. The lithium loss rate in the positive flotation tailings is as high as 23.68%, indicating that it is difficult to separate spodumene and apatite in the high-phosphorus lithium concentrate without adding depressants. Within the tested composite depressant dosage range, the composite depressant has a strong selective inhibition ability on spodumene, but almost no inhibition on apatite. The P2O5 content in the spodumene concentrate meets the non-ferrous metal industry standard, and the P2O5 removal rate is about 90%. The lithium loss rate in the apatite tailings is only about 10%, which means that the composite depressant described in this case 2 can efficiently separate spodumene and apatite. As the composite depressant dosage increases from 2×10 -4 mol / L increased to 8×10 -4 mol / L, the recovery rate of Li2O of the composite inhibitor of the present invention gradually increases and then decreases, and the removal effect of apatite also increases sharply at first and then weakens. The weakening of the dephosphorization effect is due to the fact that the composite inhibitor of the present invention has a certain inhibitory effect on both spodumene and apatite when used in high dosage. Therefore, it is necessary to control the dosage of the composite inhibitor to exert its best synergistic separation. When the dosage of the composite inhibitor is 6×10 -4 mol / L, the separation effect of spodumene and apatite in high-phosphorus lithium concentrate is the best. At this time, the composite inhibitor of the present invention reduces the P2O5 content of lithium concentrate from 4.54% to 0.44%, and the phosphorus removal rate is as high as 91.95%. At the same time, the Li2O grade of lithium concentrate is increased from 4.43% to 4.83%, and the loss rate of lithium in apatite tailings is only 9.32%. Considering the synergy of the composite inhibitor of the present invention, 6×10 -4 mol / L was selected as the optimal dosage of composite inhibitor for subsequent experiments and tests.
[0090] Example 3
[0091] In order to verify the dephosphorization effect of the composite inhibitor (Disodium EDTA: EDTMP: Sodium Alginate = 6:2:2) under different pulp pH, we used the flotation lithium ore b in Henan Province. Figure 1 In the process shown, lithium ore b was subjected to reverse flotation dephosphorization at different slurry pH values of 4, 5, 6, 7, 8, and 9. The flotation process parameters of each group of cases were the same, and the only difference was the slurry pH value, so as to explore the selectivity and inhibitory effect of the composite depressant at different slurry pH values in this case.
[0092] The specific operation is the same as that of Example 1. #The difference in the experiment is that only the pH of the slurry is adjusted.
[0093] Table 4 shows the separation effect of lithium ore b under different pulp pH. (Based on the change under roughing conditions, the collector sodium oleate is 1×10 -4 mol / L; the dosage of the composite inhibitor is 6×10 -4 mol / L; reverse flotation slurry temperature is 20℃).
[0094] Table 4 Separation effect of lithium ore b at different pulp pH
[0095]
[0096]
[0097] It can be seen from Table 4 that when the pH is between 4 and 10, the composite inhibitor has a good inhibitory performance on spodumene. In this pH range, the lithium loss rate in apatite tailings is less than 20%, the P2O5 removal rate is greater than 65%, and the lithium recovery rate in spodumene concentrate is higher than 80%, and the P2O5 content is lower than 1.8%. When the pH is 5 to 9, the P2O5 removal rate of the composite inhibitor of the present invention is above 84%, and the P2O5 content in spodumene concentrate is less than 1%, especially when the pH is 6, the P2O5 removal rate in lithium concentrate is as high as 91.95%, and the lithium loss rate in apatite tailings is only 9.32%. It shows that the composite inhibitor described in this case 3 can efficiently separate spodumene and apatite in high-phosphorus lithium concentrate in a wide acid-base range (pH between 5 and 9), and the slurry pH has little effect on its inhibitory ability and has good stability. When the pH is 4 or 10, the dephosphorization effect is significantly weakened. This is because the composite inhibitor of the present invention has a good inhibitory effect on spodumene in a strong acid environment, but also affects the floatability of apatite. In a strong alkaline environment, it has a certain inhibitory effect on both spodumene and apatite. Therefore, the slurry pH needs to be adjusted to exert its best synergistic sorting. Considering the synergy of the composite inhibitor of the present invention, the slurry pH of 6 was selected as the preferred one for subsequent experiments and tests.
[0098] Example 4
[0099] In order to verify the dephosphorization effect of the composite inhibitor (Disodium EDTA: EDTMP: Sodium Alginate = 6:2:2) at different slurry temperatures, we used the flotation lithium ore b in Henan Province. Figure 1 In the process shown, lithium ore b was subjected to reverse flotation dephosphorization at different slurry temperatures of 10°C, 20°C, 30°C and 40°C. The flotation process parameters of each group of cases were the same, and the only difference was the slurry temperature, so as to explore the selectivity and inhibitory effect of the composite depressant at different slurry temperatures in this case.
[0100] The specific operation is the same as that of Example 1. # The difference between the two experiments is that only the slurry temperature is adjusted.
[0101] Table 5 shows the separation effect of lithium ore b at different pulp temperatures. (Based on the change under roughing conditions, the pH of the reverse flotation pulp is 6; the amount of collector sodium oleate is 1×10 -4 mol / L; the dosage of the composite inhibitor is 6×10 -4 mol / L).
[0102] Table 5 Separation effect of lithium ore b at different slurry temperatures
[0103]
[0104] It can be seen from Table 5 that low temperature has little effect on the separation effect of the composite inhibitor of the present invention. When the slurry temperature is greater than 20°C, the P2O5 removal rate in the lithium concentrate only slightly increases, and the lithium loss rate in the apatite tailings also decreases slightly. This shows that the composite inhibitor described in this case 4 can efficiently separate spodumene and apatite in high-phosphorus lithium concentrate within a wide temperature range (between 10 and 40°C), and the slurry temperature has little effect on its inhibitory ability and has good stability. Taking into account the comprehensive consideration, the slurry temperature of the composite inhibitor of the present invention is 20°C, which is selected as the preferred one for subsequent experiments and tests.
[0105] Example 5
[0106] In order to verify the dephosphorization effect of different dosages of composite inhibitor (Disodium EDTA: EDTMP: Sodium Alginate = 6:2:2) under the condition of low phosphorus content in lithium concentrate, we used flotation lithium ore a in Henan Province. Figure 1 The process shown in the figure is to use different inhibitor dosages of 2×10 -4 mol / L、4×10 -4 mol / L、6×10 -4 mol / L、8×10 -4 mol / L was used for reverse flotation dephosphorization of lithium ore a. The flotation process parameters of each group of cases were the same, and the only difference was the dosage of composite depressant, so as to explore the selectivity and inhibition effect of different dosages of composite depressants in this case.
[0107] The specific operation is the same as that of Example 1. # The difference between the two experiments was that only the dosage of the composite inhibitor was changed.
[0108] Table 6 shows the separation effect of lithium ore a under different inhibitor dosages. (Based on the changes under roughing conditions, the pH of the reverse flotation slurry is 6; the reverse flotation slurry temperature is 20°C; the amount of collector sodium oleate is 1×10 -4 mol / L).
[0109] Table 6 Separation effect of lithium ore a at different inhibitor dosages
[0110]
[0111] It can be seen from Table 6 that different amounts of the composite inhibitor of the present invention have little effect on the separation of spodumene and apatite in high-phosphorus lithium concentrate with low phosphorus content; -4 mol / L of the composite inhibitor, the separation effect is optimal. At this time, the composite inhibitor of the present invention reduces the P2O5 content of the lithium concentrate from 2.07% to 0.38%, and the phosphorus removal rate is as high as 83.52%. At the same time, the Li2O grade of the lithium concentrate is increased from 4.75% to 4.87%, and the lithium loss rate in the apatite tailings is only 7.98%. This shows that the composite inhibitor of the present invention is also suitable for the reverse flotation dephosphorization method of phosphorus-containing lithium ore with a low phosphorus content.
[0112] Example 6
[0113] In order to verify the dephosphorization effect of different dosages of composite inhibitor (Disodium EDTA: EDTMP: Sodium Alginate = 6:2:2) under the condition of high phosphorus content in lithium concentrate, we used the flotation lithium ore c in Henan Province. Figure 1 The process shown in the figure is to use different inhibitor dosages of 2×10 -4 mol / L、4×10 -4 mol / L、6×10 -4 mol / L、8×10 -4 mol / L was used for reverse flotation dephosphorization of lithium ore c. The flotation process parameters of each group of cases were the same, and the only difference was the dosage of composite depressant, so as to explore the selectivity and inhibition effect of different dosages of composite depressants in this case.
[0114] The specific operation is the same as that of Example 1. # The difference between the two experiments was that only the dosage of the composite inhibitor was changed.
[0115] Table 7 shows the separation effect of lithium ore c under different inhibitor dosages. (Based on the changes under roughing conditions, the pH of the reverse flotation slurry is 7; the reverse flotation slurry temperature is 20°C; the amount of collector sodium oleate is 1×10 -4 mol / L).
[0116] Table 6 Separation effect of lithium ore c at different inhibitor dosages
[0117]
[0118] It can be seen from Table 7 that different amounts of the composite inhibitor of the present invention have a greater influence on the separation effect of spodumene and apatite in high-phosphorus lithium concentrate with a very high phosphorus content; -4When the composite inhibitor dosage is 1.5 mol / L, the separation effect is the best. At this time, the composite inhibitor of the present invention reduces the P2O5 content of lithium concentrate from 8.79% to 0.49%, and the phosphorus removal rate is as high as 95.92%. At the same time, the Li2O grade of lithium concentrate is increased from 4.07% to 4.48%, and the lithium loss rate in apatite tailings is 19.51%. It shows that the composite inhibitor of the present invention is also suitable for the reverse flotation dephosphorization method of phosphorus-containing lithium ore with a high phosphorus content.
[0119] In summary, the composite inhibitor comprising three components described in the present invention can exert the best synergistic effect by adopting appropriate ratios and formulas, has a good reverse flotation dephosphorization effect on different types of high-phosphorus lithium concentrates, can achieve selective separation of spodumene and apatite, and make the P2O5 content in spodumene concentrate reach the non-ferrous metal industry standard, thereby reducing the loss rate of lithium in apatite tailings.
Claims
1. A composite depressant for reverse flotation dephosphorization of phosphorus-containing lithium ore, characterized in that: Comprising component A and component B; The component A is a compound having the structural formula of formula 1-A and formula 1-B; Formula 1-A Formula 1-B The n is 1, 2 or 3; The component B comprises at least one of alginic acid and its salts, and malic acid and its salts.
2. The composite inhibitor for reverse flotation dephosphorization of phosphorus-containing lithium ore according to claim 1, characterized in that: The formula 1-A comprises at least one of EDTA and EDTA salt.
3. The composite inhibitor for reverse flotation dephosphorization of phosphorus-containing lithium ore according to claim 2, characterized in that: The formula 1-A comprises at least one of EDTA, disodium EDTA, tetrasodium EDTA, dipotassium EDTA and tetrapotassium EDTA.
4. The composite inhibitor for reverse flotation dephosphorization of phosphorus-containing lithium ore according to claim 2, characterized in that: In Formula 1-B, at least one of EDTMP, EDTMP salt, HMDTMP and HMDTMP salt is included.
5. The composite inhibitor for reverse flotation dephosphorization of phosphorus-containing lithium ore according to claim 4, characterized in that: In Formula 1-B, at least one of EDTMP, tetrasodium EDTMP, tetrapotassium EDTMP, HMDTMP, tetrasodium HMDTMP, and tetrapotassium HMDTMP is included.
6. The composite inhibitor for reverse flotation dephosphorization of phosphorus-containing lithium ore according to claim 1, characterized in that: In the component A, the molar ratio of formula 1-A to formula 1-B is 1-5:
1.
7. The composite depressor for reverse flotation dephosphorization of phosphorus-containing lithium ore according to claim 6, characterized in that: In the component A, the molar ratio of formula 1-A to formula 1-B is 3 to 5:
1.
8. The composite depressant for reverse flotation dephosphorization of phosphorus-containing lithium ore according to claim 1, characterized in that: In the component B, the alginate is a water-soluble salt of alginic acid.
9. The composite inhibitor for reverse flotation dephosphorization of phosphorus-containing lithium ore according to claim 8, characterized in that: In the component B, the alginate is at least one of sodium alginate, potassium alginate and ammonium alginate.
10. The composite inhibitor for reverse flotation dephosphorization of phosphorus-containing lithium ore according to claim 1, characterized in that: In the component B, the malate is a water-soluble salt of malic acid.
11. The composite depressant for reverse flotation dephosphorization of phosphorus-containing lithium ore according to claim 10, characterized in that: In the component B, the malate is at least one of sodium malate, potassium malate and ammonium malate.
12. The composite inhibitor for reverse flotation dephosphorization of phosphorus-containing lithium ore according to any one of claims 1 to 11, characterized in that: The molar proportion of component A is 60 to 90 parts; the molar proportion of component B is not higher than 40 parts.
13. The composite depressant for reverse flotation dephosphorization of phosphorus-containing lithium ore according to claim 12, characterized in that: The molar proportion of component A is 70 to 90 parts; the molar proportion of component B is 5 to 30 parts.
14. The composite depressant for reverse flotation dephosphorization of phosphorus-containing lithium ore according to claim 12, characterized in that: The molar proportion of component A is 75 to 85 parts; the molar proportion of component B is 15 to 25 parts.
15. A method for dephosphorization by reverse flotation in phosphorus-containing lithium ore, characterized in that: The phosphorus-containing lithium ore is reversely floated using a flotation agent comprising the composite depressant according to any one of claims 1 to 14 to suppress the spodumene therein, and reversely float the apatite therein to obtain the spodumene concentrate and the apatite tailings.
16. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 15, characterized in that: In the reverse flotation stage, the dosage of composite depressant is greater than or equal to 5×10 -5 mol / L.
17. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 16, characterized in that: In the reverse flotation stage, the dosage of the composite depressant is 2×10 -4 mol / L~8×10 -4 mol / L.
18. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 17, characterized in that: In the reverse flotation stage, the dosage of composite depressant is 4~8×10 -4 mol / L.
19. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 18, characterized in that: In the reverse flotation stage, the dosage of composite depressant is 5~6×10 -4 mol / L.
20. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 15, characterized in that: During the reverse flotation stage, the pH of the slurry is 4~10.
21. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 20, characterized in that: During the reverse flotation stage, the pH of the slurry is 5~9.
22. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 21, characterized in that: During the reverse flotation stage, the pH of the slurry is 6~7.
23. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 15, characterized in that: During the reverse flotation stage, the temperature of the slurry is 5~50℃.
24. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 23, characterized in that: During the reverse flotation stage, the temperature of the slurry is 10~40℃.
25. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 24, characterized in that: During the reverse flotation stage, the temperature of the slurry is 20~40℃.
26. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 15, characterized in that: The phosphorus-containing lithium ore is a mineral containing spodumene and apatite.
27. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to any one of claims 15 to 26, characterized in that: The flotation reagent also contains a collector.
28. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 27, characterized in that: The collector comprises at least one of sodium oleate, oxidized paraffin soap, cyclopentane acid soap and tall oil soap.
29. The reverse flotation dephosphorization method in phosphorus-containing lithium ore according to claim 28, characterized in that: The amount of the collector is 5×10 -5 mol / L ~3×10 -4 mol / L.
30. A composite flotation agent for reverse flotation and dephosphorization of phosphorus-containing lithium ore, characterized in that: The invention comprises a collector and the composite inhibitor according to any one of claims 1 to 14.
31. The composite flotation agent for reverse flotation and dephosphorization of phosphorus-containing lithium ore according to claim 30, characterized in that: The collector comprises at least one of sodium oleate, oxidized paraffin soap, cyclopentane acid soap and tall oil soap.