A method for preparing titanium dioxide nanotube arrays on spherical titanium particles

By preparing titanium dioxide nanotube arrays on spherical titanium particles, the problems of low mass transfer efficiency and high energy consumption in traditional electrochemical oxidation technology are solved, and efficient electrochemical oxidation reactions and improved stability of electrode materials are achieved.

CN115433986BActive Publication Date: 2024-11-12YANCHENG INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211251830.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-13
Publication Date
2024-11-12
Estimated Expiration
2042-10-13

AI Technical Summary

Technical Problem

In traditional electrochemical oxidation technology, the mass transfer efficiency of plate electrodes is low and energy consumption is high, making it difficult to achieve industrial application. The external pressure and the microporous electrodes are micron-level, which increases the energy consumption of the pump.

Method used

The titanium dioxide nanotube array was prepared on spherical titanium particles, and the titanium dioxide nanotubes were uniformly formed in the rotation mode by anodizing method to improve the specific surface area and stability, and as the electrode support material, the filter electrolysis and the loading of the catalytic layer was realized.

Benefits of technology

The efficiency of electrochemical oxidation reaction and the life of the electrode are improved, energy consumption is reduced, and electrode materials with large specific surface area and strong stability are realized, which simplifies the process and improves operability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115433986B_ABST
    Figure CN115433986B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a titanium dioxide nanotube array on a spherical titanium particle, comprising taking the spherical titanium particle as an anode, wrapping a hollow ball as a cathode, and placing the spherical titanium particle in an electrolyte solution; controlling the spherical titanium particle to rotate at a preset speed in the hollow ball, and adopting an anodic oxidation method to prepare titanium dioxide nanotubes on the outer surface of the spherical titanium particle, and the spherical titanium particle can form a filter layer by stacking to realize filtering electrolysis, wherein the titanium dioxide nanotubes improve the specific surface area and stability of the particle, enhance the efficiency during reaction and the service life during application, the process is simple, the operability is strong, and the titanium dioxide nanotubes can be used as a carrier of electrode materials, and have the advantages of large specific surface area, strong stability, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrode carrier material preparation, in particular to a method for preparing a titanium dioxide nanotube array on spherical titanium particles. Background Art

[0002] Electrochemical oxidation technology is an environmentally friendly technology with the characteristics of fast removal rate, simple operation, easy automation, small footprint and easy large-scale use. It has attracted much attention from researchers in recent years. Traditional electrochemical oxidation technology is mainly based on plate electrodes. Two electrode plates are inserted into the wastewater, and the electrochemical reaction on the electrode plates is used to generate hydroxyl radicals (·OH) to complete the degradation of pollutants. However, this method has low mass transfer efficiency of pollutants and low contact probability with the electrode plates, so the energy consumption is high and it is difficult to achieve industrial application. Therefore, the key to promoting the development of electrochemical oxidation technology lies in the development of anode materials. At present, the most popular anode materials are microporous electrodes or electrocatalytic membrane electrodes. The porous titanium matrix is ​​used as the material to replace the original closed titanium plate material. The porous structure allows pollutants to pass through the electrode under power drive (such as a pump), thereby forming a directional flow, thereby improving the mass transfer of pollutants and thus improving the degradation efficiency. However, this electrode requires external pressure to achieve directional mass transfer of pollutants, and the pores of the microporous electrode are at the micron level, which increases the energy consumption of the pump.

[0003] In wastewater treatment, adding fillers to form filtration treatment is one of the common means to improve treatment efficiency. Therefore, we can break through the traditional thinking and change the electrode shape from plate to small spheres. Several small spheres form a filler layer. When water flows through, an electrochemical oxidation reaction occurs, which can improve the treatment effect. The water can flow naturally without increasing the consumption of pump energy. Compared with the common three-dimensional electrodes, it can improve the mass transfer of pollutants and reduce the input of intermediate fillers. However, in order to ensure the treatment effect, a certain specific surface area needs to be guaranteed. Titanium dioxide nanotubes can greatly increase the specific surface area. Therefore, using spherical titanium particles as the matrix and preparing titanium dioxide nanotubes on their surface can realize the preparation of spherical electrochemical oxidation electrode carriers with large specific surface area. Summary of the invention

[0004] The invention provides a method for preparing a titanium dioxide nanotube array on a spherical titanium particle, which is used to solve the problem of insufficient performance of existing electrode materials.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing a titanium dioxide nanotube array on a spherical titanium particle, comprising the following steps:

[0006] S1, pretreatment, cleaning the spherical titanium particles;

[0007] S2, using spherical titanium particles as anodes, wrapping hollow balls as cathodes, and placing them in electrolyte solutions;

[0008] S3. Control the spherical titanium particles to rotate at a preset speed in the hollow sphere, and prepare titanium dioxide nanotubes on the outer surface of the spherical titanium particles by an anodic oxidation method.

[0009] Preferably, in step S1, the spherical titanium particles are first rinsed with ultrapure water for 2 minutes, then ultrasonically cleaned with isopropanol for 20 minutes, then ultrasonically cleaned with NaOH for 15 minutes, and finally ultrasonically cleaned with ultrapure water for 30 minutes.

[0010] Preferably, in step S2, the spherical titanium particle is located at the center of the hollow sphere, and the distance between the surface of the spherical titanium particle and the inner wall of the hollow sphere is 1 cm.

[0011] Preferably, the diameter of the spherical titanium particles is 2-5 cm, and the diameter of the hollow spheres is 4-7 cm.

[0012] Preferably, in step S2, the electrolyte solution comprises ethylene glycol, deionized water and ammonium fluoride, wherein the mass ratio of ethylene glycol to deionized water is 2-40:1, and the amount of ammonium fluoride accounts for 0.05-0.6% of the mass of the mixed solution.

[0013] Preferably, in step S3, the spherical titanium particles are controlled to rotate in the hollow sphere at a speed of 2-6 s / cycle.

[0014] Preferably, the spherical titanium particles are connected to a titanium rod, one end of which extends out of a hollow ball and is connected to an output shaft of a motor, and the titanium rod and the motor are insulated, and the motor drives the titanium rod to rotate, thereby controlling the rotation of the spherical titanium particles.

[0015] Preferably, in step S3, electrolysis is maintained at a voltage of 20V-80V for 0.5-3h, and then calcined in a muffle furnace at 400-700°C for 2-8h, with a heating rate of 0.5-4°C / min.

[0016] Compared with the prior art, the present invention has the following beneficial effects: the present invention uses spherical titanium particles as a matrix, and adopts an anodic oxidation method to uniformly prepare titanium dioxide nanotubes on their outer surface in a rotating mode. The spherical titanium particles can form a filter layer by accumulation to achieve filtering electrolysis, and can be used as a carrier material. The catalytic layer can be loaded by means of reduction treatment or deposition, brushing, etc. to serve as an electrode for electrochemical oxidation technology. Among them, the titanium dioxide nanotubes increase the specific surface area and stability of the particles, enhance the efficiency during the reaction and the lifespan during application. The present invention has a simple process and strong operability, can be used as a carrier of electrode materials, and has the advantages of large specific surface area and strong stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention.

[0018] In the attached picture:

[0019] Figure 1 It is a schematic diagram of the structure of the spherical titanium particles and the hollow spheres assembled in the present invention;

[0020] Figure 2 is a SEM image of a titanium dioxide nanotube array prepared on a spherical titanium particle of the present invention;

[0021] Figure 3 is an EDS image of a titanium dioxide nanotube array prepared on a spherical titanium particle of the present invention;

[0022] Figure 4 It is a data comparison diagram of the present invention with and without titanium dioxide nanotubes. DETAILED DESCRIPTION

[0023] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0024] refer to Figure 1 As shown in FIG. 1 , it is a schematic diagram of the assembly of spherical titanium particles and hollow spheres, wherein the spherical titanium particles are used as anodes, and the hollow spheres wrapped outside are used as cathodes. The spherical titanium particles are placed in an electrolyte solution, and the spherical titanium particles are controlled to rotate at a preset speed in the hollow spheres, such as Figure 1 As shown, a titanium rod can be connected to the spherical titanium particles, one end of the titanium rod extends out of the hollow ball and is connected to the output shaft of the motor, and the titanium rod and the motor are insulated. The motor drives the titanium rod to rotate, thereby controlling the rotation of the spherical titanium particles, wherein the rotation speed range is 2-6s / cycle.

[0025] The spherical titanium particle is located at the center of the hollow sphere, and the distance between the surface of the spherical titanium particle and the inner wall of the hollow sphere is 1 cm.

[0026] The electrolyte solution includes ethylene glycol, deionized water and ammonium fluoride, wherein the mass ratio of ethylene glycol to deionized water is 2-40:1, and the amount of ammonium fluoride accounts for 0.05-0.6% of the mass of the mixed solution;

[0027] The electrolysis environment is: electrolysis is maintained at a voltage of 20V-80V for 0.5-3h, and after electrolysis, calcination is performed in a muffle furnace at 400-700°C for 2-8h, with a heating rate of 0.5-4°C / min.

[0028] Example 1: A method for preparing a titanium dioxide nanotube array on a spherical titanium particle, comprising the following steps:

[0029] S1, spherical titanium particles with a diameter of 2 cm were first rinsed with ultrapure water for 2 min, then ultrasonically cleaned with isopropanol for 20 min, then ultrasonically cleaned with NaOH for 15 min, and finally ultrasonically cleaned with ultrapure water for 30 min;

[0030] S2, prepare an electrolyte solution of ethylene glycol, deionized water and ammonium fluoride, wherein the mass ratio of ethylene glycol to deionized water is 2:1, and the mass concentration of ammonium fluoride is 0.3%, and place spherical titanium particles into the electrolyte solution for anodization, wherein the voltage of anodization is 60 V, the time is 3 h, and the motor speed is 2 s / week;

[0031] S3. The anodized spherical titanium particles are heated to 600° C. at a heating rate of 2° C. / min, and calcined at 600° C. for 2 h.

[0032] Example 2: A method for preparing a titanium dioxide nanotube array on a spherical titanium particle, comprising the following steps:

[0033] S1, spherical titanium particles with a diameter of 5 cm were first rinsed with ultrapure water for 2 min, then ultrasonically cleaned with isopropanol for 20 min, then ultrasonically cleaned with NaOH for 15 min, and finally ultrasonically cleaned with ultrapure water for 30 min;

[0034] S2, prepare an electrolyte solution of ethylene glycol, deionized water and ammonium fluoride, wherein the mass ratio of ethylene glycol to deionized water is 20:1, and the mass concentration of ammonium fluoride is 0.05%, and place spherical titanium particles into the electrolyte solution for anodization, wherein the anodization voltage is 40 V, the time is 1 h, and the motor speed is 3 s / cycle;

[0035] S3. The anodized spherical titanium particles were heated to 700°C at a heating rate of 3°C / min and calcined at 700°C for 2h.

[0036] Example 3: A method for preparing a titanium dioxide nanotube array on a spherical titanium particle, comprising the following steps:

[0037] S1, spherical titanium particles with a diameter of 2 cm were first rinsed with ultrapure water for 2 min, then ultrasonically cleaned with isopropanol for 20 min, then ultrasonically cleaned with NaOH for 15 min, and finally ultrasonically cleaned with ultrapure water for 30 min;

[0038] S2, prepare an electrolyte solution of ethylene glycol, deionized water and ammonium fluoride, wherein the mass ratio of ethylene glycol to deionized water is 10:1, and the mass concentration of ammonium fluoride is 0.05%, and place spherical titanium particles into the electrolyte solution for anodization, wherein the anodization voltage is 80 V, the time is 0.5 h, and the motor speed is 3 s / cycle;

[0039] S3. The anodized spherical titanium particles are heated to 500° C. at a heating rate of 5° C. / min, and calcined at 500° C. for 2 h.

[0040] Example 4: A method for preparing a titanium dioxide nanotube array on a spherical titanium particle, comprising the following steps:

[0041] S1, spherical titanium particles with a diameter of 3 cm were first rinsed with ultrapure water for 2 min, then ultrasonically cleaned with isopropanol for 20 min, then ultrasonically cleaned with NaOH for 15 min, and finally ultrasonically cleaned with ultrapure water for 30 min;

[0042] S2, prepare an electrolyte solution of ethylene glycol, deionized water and ammonium fluoride, wherein the mass ratio of ethylene glycol to deionized water is 8:1, and the mass concentration of ammonium fluoride is 0.6%, and place spherical titanium particles into the electrolyte solution for anodization, wherein the anodization voltage is 40 V, the time is 2 h, and the motor speed is 6 s / cycle;

[0043] S3. The anodized spherical titanium particles were heated to 550° C. at a heating rate of 0.5° C. / min, and calcined at 550° C. for 2 h.

[0044] Example 5: A method for preparing a titanium dioxide nanotube array on a spherical titanium particle, comprising the following steps:

[0045] S1, spherical titanium particles with a diameter of 2 cm were first rinsed with ultrapure water for 2 min, then ultrasonically cleaned with isopropanol for 20 min, then ultrasonically cleaned with NaOH for 15 min, and finally ultrasonically cleaned with ultrapure water for 30 min;

[0046] S2, prepare an electrolyte solution of ethylene glycol, deionized water and ammonium fluoride, wherein the mass ratio of ethylene glycol to deionized water is 20:1, and the mass concentration of ammonium fluoride is 0.3%, and place spherical titanium particles into the electrolyte solution for anodization, wherein the anodization voltage is 55 V, the time is 2 h, and the motor speed is 5 s / cycle;

[0047] S3. The anodized spherical titanium particles were heated to 550° C. at a heating rate of 5° C. / min, and calcined at 550° C. for 2 h.

[0048] refer to Figure 2 The SEM image of the titanium dioxide nanotube array prepared on the spherical titanium particles prepared in Example 5 is shown in FIG. Figure 2 It can be seen that the titanium dioxide nanotube array has been successfully prepared on the spherical titanium particles, and the overall structure is compact without collapse.

[0049] refer to Figure 3 As shown, this is the EDS image of the titanium dioxide nanotube array prepared on the spherical titanium particles obtained in Example 5. Figure 3 It can be seen that the constituent elements of the titanium dioxide nanotube array are Ti and O.

[0050] refer to Figure 4 Shown is a comparison of the adsorption and desorption data of solid titanium spheres and titanium dioxide nanotubes.

[0051] Finally, it should be noted that the above description is only a preferred example of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a titanium dioxide nanotube array on spherical titanium particles, characterized in that: The steps include: S1, pretreatment, cleaning the spherical titanium particles; S2, using spherical titanium particles as anodes, wrapping hollow balls as cathodes, and placing them in electrolyte solutions; S3. Control the spherical titanium particles to rotate at a preset speed in the hollow sphere, and prepare titanium dioxide nanotubes on the outer surface of the spherical titanium particles by an anodic oxidation method.

2. The method for preparing a titanium dioxide nanotube array on spherical titanium particles according to claim 1, characterized in that: In step S1, the spherical titanium particles are first rinsed with ultrapure water for 2 minutes, then ultrasonically cleaned with isopropanol for 20 minutes, then ultrasonically cleaned with NaOH for 15 minutes, and finally ultrasonically cleaned with ultrapure water for 30 minutes.

3. The method for preparing a titanium dioxide nanotube array on spherical titanium particles according to claim 1, characterized in that: In step S2, the spherical titanium particle is located at the center of the hollow sphere, and the distance between the surface of the spherical titanium particle and the inner wall of the hollow sphere is 1 cm.

4. The method for preparing a titanium dioxide nanotube array on spherical titanium particles according to claim 3, characterized in that: The diameter of the spherical titanium particles is 2-5 cm, and the diameter of the hollow spheres is 4-7 cm.

5. The method for preparing titanium dioxide nanotube arrays on spherical titanium particles according to claim 1, characterized in that: In step S2, the electrolyte solution includes ethylene glycol, deionized water and ammonium fluoride, wherein the mass ratio of ethylene glycol to deionized water is 2-40:1, and the amount of ammonium fluoride accounts for 0.05-0.6% of the mass of the mixed solution.

6. The method for preparing titanium dioxide nanotube arrays on spherical titanium particles according to claim 1, characterized in that: In step S3, the spherical titanium particles are controlled to rotate in the hollow sphere at a rotation speed of 2-6 s / cycle.

7. A method for preparing titanium dioxide nanotube arrays on spherical titanium particles according to claim 1 or 6, characterized in that: The spherical titanium particles are connected to a titanium rod, one end of which extends out of a hollow ball and is connected to an output shaft of a motor. The titanium rod and the motor are insulated, and the motor drives the titanium rod to rotate, thereby controlling the spherical titanium particles to rotate.

8. The method for preparing titanium dioxide nanotube arrays on spherical titanium particles according to claim 1, characterized in that: In step S3, electrolysis is maintained at a voltage of 20V-80V for 0.5-3h, and then calcined in a muffle furnace at 400-700°C for 2-8h with a heating rate of 0.5-4°C / min.