A method for manufacturing a vanadium-aluminum alloy smelting furnace
By using a special induction coil for the suspension furnace and a water-cooled copper crucible in the vanadium-aluminum alloy smelting furnace, combined with the specific formula of the refractory material and the oven process, the problems of high manufacturing cost, long time and high impurity content of the smelting furnace in the existing technology are solved. , realizing efficient and low-cost vanadium-aluminum alloy smelting to meet aerospace-grade purity requirements.
Patent Information
- Application Number
- CN202210994965.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-18
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-08-18
AI Technical Summary
Existing vanadium-aluminum alloy smelting furnaces are expensive and time-consuming to manufacture, and are difficult to meet aerospace-grade purity requirements. There are problems such as excessive impurity elements and low thermal energy utilization.
Using special induction coils for suspension furnaces, special water-cooled copper crucibles for suspension furnaces and refractory materials, including refractory dry vibrating materials, refractory ramming materials and refractory castables, rapid sintering and low-temperature cooling are achieved through specific oven processes and material formulas. Reduce impurity content and production costs.
It effectively reduces the manufacturing cost and time of the vanadium-aluminum alloy smelting furnace, improves the purity of the vanadium-aluminum alloy, meets aerospace grade standards, and extends the service life of the refractory material.
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing a smelting furnace, in particular to a method for manufacturing a vanadium-aluminum alloy smelting furnace. Background Art
[0002] Vanadium aluminum alloy is a vanadium additive used in the production of titanium alloys such as Ti-6Al-4V. It is divided into 3 levels according to the vanadium content: 50%, 65% and 85%, and the balance is aluminum. Because vanadium aluminum alloy is an additive for vacuum smelting, it is often marked with "VQ" (vacuum quality). The gas content of vanadium aluminum alloy is low, and other impurities such as Fe, Si, C, B, etc. must meet the requirements of titanium alloy.
[0003] The smelting furnace currently used for smelting vanadium aluminum alloy has the following problems: 1. The refractory material used for furnace sleeve knotting has high impurity content. The refractory material used for furnace sleeve knotting is fused magnesia sand, magnesia fire clay and magnesium chloride hexahydrate, which easily causes the content of impurity elements such as Si, Fe, Mg in vanadium aluminum alloy to exceed the standard and cannot meet the requirements of aerospace grade vanadium aluminum alloy; 2. The production cost is high. The smelting furnace is mainly made of refractory materials knotted. When the furnace is cooled and dismantled, more than 70% of the refractory materials will be discarded, resulting in excessively high costs for making the smelting furnace; 3. The production cycle is long. The smelting furnace production process includes knotting material preparation- Knotting - curing - baking - cooling, the steps of knotting material preparation and knotting take 3 to 5 hours, curing takes at least 12 to 16 hours, baking takes 24 to 36 hours, and most of the time it cools naturally after baking. It takes at least 6 to 10 hours of cooling to reduce the furnace temperature to below 60°C. The production cycle of the entire smelting furnace exceeds 48 hours, and some even take more than 72 hours; 4. Baking requires an additional special baking furnace, which consumes too much energy and has low thermal energy utilization. The existing baking method often results in incomplete baking inside the furnace jacket and inconsistent baking effects inside and outside the furnace jacket.
[0004] In view of the current problems of vanadium-aluminum alloy smelting furnaces, there is currently no efficient method for manufacturing vanadium-aluminum alloy smelting furnaces. Therefore, it is necessary to study an efficient, simple to manufacture, and economical vanadium-aluminum alloy smelting furnace method, which can not only reduce the manufacturing cost and manufacturing time of the vanadium-aluminum alloy smelting furnace, but also ensure the purity of the vanadium-aluminum alloy during the smelting process. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a method for manufacturing an efficient vanadium-aluminum alloy smelting furnace to reduce the manufacturing cost and manufacturing time of the vanadium-aluminum alloy smelting furnace while ensuring the purity of the vanadium-aluminum alloy during the smelting process.
[0006] The technical solution adopted by the present invention to solve the technical problem is:
[0007] A method for manufacturing a vanadium-aluminum alloy smelting furnace, wherein the vanadium-aluminum alloy smelting furnace is mainly composed of a special induction coil for a suspension furnace, a special water-cooled copper crucible for a suspension furnace, and refractory materials; the refractory materials are divided into refractory dry vibrating materials, refractory ramming materials, and refractory castable materials; the refractory dry vibrating materials and refractory ramming materials are used for a furnace bottom and a furnace wall, and the refractory castable material is used for a furnace mouth.
[0008] The manufacturing method of the vanadium-aluminum alloy smelting furnace is as follows:
[0009] Step 1: prefabricate the refractory castable into a trumpet-shaped furnace mouth, wherein the upper diameter of the furnace mouth is larger than the diameter of the special induction coil for the suspension furnace, and the lower outer diameter of the furnace mouth is equal to the inner diameter of the special water-cooled copper crucible for the suspension furnace. The prefabricated furnace mouth is assembled inside the special water-cooled copper crucible for the suspension furnace, and the lower part of the furnace mouth extends into the special induction coil for the suspension furnace by 4-8 cm;
[0010] Step 2: Assemble the special water-cooled copper crucible for suspension furnace into the special induction coil for suspension furnace, apply insulating putty on the special induction coil for suspension furnace, spread the refractory dry vibration material on the bottom and wall of the special water-cooled copper crucible for suspension furnace, vibrate the refractory dry vibration material layer with a vibration tool, and then scrape the surface of the refractory dry vibration material layer;
[0011] Step 3: Mix the refractory ramming material and the binder, spread them on the dry vibration material layer after scraping, and compact them with a compaction tool to obtain a refractory crucible;
[0012] Step 4: placing the molybdenum crucible mold in the refractory crucible prepared in step 3, starting the power supply of the vanadium-aluminum alloy smelting furnace to start heating, and using the heat of the induction heating of the molybdenum crucible mold to bake the refractory crucible. The baking process is divided into three process stages: low-temperature drying, medium-temperature consolidation, and high-temperature sintering. After the baking process is completed, stop heating and take out the molybdenum crucible mold;
[0013] Step 5: Continue to operate the cooling water system of the vanadium-aluminum alloy smelting furnace, and cool the special coil of the suspension furnace and the special water-cooled copper crucible of the suspension furnace by water until the temperature of the refractory crucible drops below 60°C, and the entire vanadium-aluminum alloy smelting furnace is completed.
[0014] Preferably, in step one, the weight content of the main components of the refractory castable is 75% to 88% aluminum oxide, 4% to 8% titanium oxide, 3% to 4% magnesium oxide, and 3% to 6% water; the refractory castable ingredients are mainly composed of three parts: 70% to 80% aggregate, 10% to 15% binder, and 10% to 20% admixture; the aggregate of the refractory castable contains coarse aggregate and fine aggregate; the particle size range of the coarse aggregate is 8 to 25 mm; the particle size range of the fine aggregate is 0.1 to 8 mm; the binder is alumina cement; the admixture has the same composition as the aggregate, which is aggregate powder after fine grinding of the aggregate, and the particle size range D90 of the aggregate powder is less than 0.06 mm.
[0015] Preferably, 2%-3% of stainless steel fiber can be added according to the weight of the refractory castable during the process of prefabricating the furnace mouth with the refractory castable in step 1.
[0016] Preferably, the weight content of the main components of the refractory dry vibration material in step 2 is 81% to 85% alumina, 3% to 6% magnesium oxide, 3% to 5% silicon carbide, and 1% to 3% silicon dioxide; the refractory dry vibration material is mainly composed of 60% to 70% aggregate, 20% to 30% powder, 4% to 6% sintering agent, and 1% to 4% thermosetting binder; the aggregate of the refractory dry vibration material contains coarse aggregate, medium aggregate and fine aggregate, and the particle size range of the coarse aggregate is 1 to 4 mm; the particle size range of the medium aggregate is 0.3 to 1 mm; The particle size range of fine aggregate is 0.1-0.3mm; the weight ratio of coarse aggregate, medium aggregate and fine aggregate of the refractory dry vibrating material is 3-5:1-3:3-5 (preferably 4:2:4); the powder has the same composition as the aggregate, which is the aggregate powder obtained by finely grinding the aggregate of the refractory dry vibrating material, and the particle size range of the powder is 0.01-0.074mm; the weight ratio of aggregate and powder of the refractory dry vibrating material is (1-5):1, preferably 3:1; the sintering agent is boric anhydride; and the thermosetting binder is phenolic resin.
[0017] Preferably, in step 2, vanadium-aluminum alloy powder equivalent to 4% to 7% of the total weight of the refractory dry vibrating material is mixed into the refractory dry vibrating material, and the particle size of the vanadium-aluminum alloy powder is ≤100 μm.
[0018] Preferably, in step 2, before spreading the refractory dry vibration material on the bottom and crucible wall of the water-cooled copper crucible dedicated to the suspension furnace, a non-magnetic alarm stainless steel mesh (preferably a layer of non-magnetic alarm stainless steel mesh) is first arranged on the bottom and crucible wall of the water-cooled copper crucible dedicated to the suspension furnace.
[0019] Preferably, in step 2, after the surface of the refractory dry vibration material layer is scraped, a non-magnetic alarm stainless steel mesh (preferably a layer of non-magnetic alarm stainless steel mesh) is set on the refractory dry vibration material layer.
[0020] Preferably, in step 3, the weight content of the main components of the refractory ramming material is 70% to 80% alumina, 15% to 20% silicon dioxide, 2% to 8% silicon carbide, and 3% to 5% magnesium oxide; the refractory ramming material is mainly composed of 65% to 70% aggregate and 30% to 35% powder; the aggregate of the refractory ramming material contains coarse aggregate, medium aggregate and fine aggregate, and the particle size range of the coarse aggregate is 2 to 8 mm; the particle size range of the medium aggregate is 0.8 to 2 mm; the particle size range of the fine aggregate is 0.1 to 0.8 mm; the weight ratio of the coarse aggregate, the medium aggregate and the fine aggregate of the refractory ramming material is 1-5:1-3:4-6 (preferably 3:2:5); the powder has the same composition as the aggregate, which is a fine aggregate powder obtained by finely grinding the aggregate of the refractory ramming material, and the particle size range of the powder is 0.03-0.1 mm; the weight ratio of the aggregate and the powder of the refractory ramming material is (1-5):1 (preferably 3:1); the amount of the binder used is 3%-5% of the weight of the refractory ramming material, and the binder is high alumina cement.
[0021] Preferably, vanadium-aluminum alloy powder equivalent to 2% to 4% of the total weight of the refractory ramming material is added to the refractory ramming material in step three, and the particle size of the vanadium-aluminum alloy powder is ≤100 μm.
[0022] Preferably, in step 4, the low-temperature drying process is to heat up from room temperature to 200-300°C at a rate of 30-60°C / h (preferably 50°C / h), and keep warm for 1-2h; the medium-temperature consolidation process is to heat up from the drying temperature to 700-900°C (preferably 800°C) at a rate of 100-150°C / h, keep warm for 1-2h, and then heat up to 1000°C at a rate of 150-200°C / h, and keep warm for 2-3h; the high-temperature sintering is to heat up to 1400-1600°C (preferably 1500°C) at a rate of 200-250°C / h, and keep warm for 2-3h.
[0023] The beneficial effects of the present invention are:
[0024] The vanadium-aluminum alloy smelting furnace described in the present invention is a special melting furnace for smelting vanadium-aluminum alloy. The refractory material used for knotting the furnace jacket has low impurity content and adopts high-aluminum refractory material. Compared with the furnace jacket refractory material of other vanadium-aluminum alloy smelting furnaces, it is not easy to cause the content of impurity elements such as Si, Fe, Mg in the vanadium-aluminum alloy to exceed the standard, and can meet the requirements of aerospace-grade vanadium-aluminum alloy.
[0025] The present invention innovatively adopts a special induction coil for a suspension furnace, a special water-cooled copper crucible for a suspension furnace and refractory materials to manufacture a vanadium-aluminum alloy smelting furnace. The suspension smelting furnace uses the suspension characteristics of the melt during smelting to reduce the erosion of the melt on the refractory materials during vanadium-aluminum alloy smelting, thereby extending the service life of the refractory materials. When the furnace jacket is knotted, the cooling effect of the special water-cooled copper crucible for the suspension furnace can be used to effectively shorten the cooling time of the furnace jacket after high-temperature sintering, thereby reducing the manufacturing time of the furnace jacket. When smelting vanadium-aluminum alloy, due to the water cooling effect of the special water-cooled copper crucible for the suspension furnace, the temperature of the refractory materials can be effectively reduced, further extending the service life of the refractory materials. At the same time, when smelting vanadium-aluminum alloy, due to the low temperature of the refractory materials, a layer of vanadium-aluminum alloy condensate shell will be formed on the surface of the refractory materials, and this layer of condensate shell can effectively reduce the contact of the refractory materials with the vanadium-aluminum alloy melt, thereby facilitating the improvement of the purity of the vanadium-aluminum alloy and meeting the standards of aerospace-grade vanadium-aluminum alloy.
[0026] Most of the existing technologies use a prefabricated method to make the furnace mouth, which also requires maintenance of the furnace mouth, and the maintenance time is generally 24-72 hours. The present invention uses a method of prefabricating the furnace mouth with refractory castables, which can make the furnace mouth in advance for maintenance, saving a lot of on-site construction time and greatly improving the efficiency of furnace jacket production. Mixing stainless steel fibers into the refractory castable can greatly improve the toughness of the furnace mouth. When pouring vanadium-aluminum alloy melt, the furnace mouth is more resistant to erosion and has a longer service life.
[0027] Different parts of the furnace jacket of the present invention are made of different types of refractory materials. The furnace mouth is made by utilizing the anti-scouring property of the refractory castable, and when pouring the vanadium-aluminum alloy after smelting, it can effectively resist the thermal shock of the vanadium-aluminum alloy melt. The furnace bottom and the furnace wall adopt a two-layer refractory material structure, firstly using refractory dry vibrating material for basic construction, and then using refractory ramming material as the melt contact refractory material. First, use refractory dry vibrating material to carry out the first layer of construction, because the special crucibles for suspension furnaces mostly use split crucibles with certain gaps. The use of refractory dry vibrating material can effectively fill the gaps of the special crucibles for suspension furnaces. The dry vibrating material can ensure that under the action of a small vibration force, the particles can move quickly and fill various gaps, thereby obtaining a higher stacking density. As the first layer of basic construction of refractory materials, it can effectively improve the strength of the refractory crucible. Since the chemical reaction between refractory dry vibrating materials under medium and low temperature baking conditions can also obtain high-temperature phase products and ceramic bonding, it is very suitable as a refractory material for direct contact with the special crucible of the suspension furnace, and the surface of the dry vibrating material is scraped before the second layer of refractory ramming material is constructed, which can effectively increase the bonding area of the two refractory materials to improve the bonding strength. For the furnace jacket formed by the crucible made of two layers of two refractory materials, when the inner layer is broken or the production loss reaches a certain level, only the inner layer of refractory material can be replaced, which reduces the production cost of the furnace jacket and reduces the loss of refractory materials.
[0028] Mixing a certain amount of vanadium-aluminum alloy powder in the construction of refractory dry vibrating material and refractory ramming material can greatly improve the sintering efficiency of the refractory dry vibrating material layer and the refractory ramming material, reduce the sintering time, and achieve rapid sintering of the furnace jacket. The present invention sets a double-layer non-magnetic alarm stainless steel mesh structure, which can monitor the damage degree of the furnace jacket in time. When the inner non-magnetic alarm stainless steel mesh detects a furnace leak, the furnace can be stopped in time for maintenance or only the inner refractory material can be replaced, so that the furnace leak will not be serious enough to damage the water-cooled crucible or the induction coil for the suspension furnace.
[0029] The formula of the refractory material of the furnace jacket of the present invention can not only achieve rapid drying and consolidation, greatly reducing the production time of the furnace jacket and improving work efficiency, but also has high strength after consolidation and long service life. In order to make the induction furnace heat up to bake the furnace and then consolidate the furnace jacket, it is generally adopted to add a furnace full of iron blocks or steel mold crucibles for smelting. During smelting, these iron blocks or steel molds must be completely in a molten state, and finally poured out of the smelting furnace, and some iron or steel clots will remain on the refractory material, affecting the purity of the subsequent vanadium aluminum alloy. The furnace consolidation of the present invention adopts induction heating of a molybdenum crucible with a high melting point, and adopts non-molten metal liquid to bake the refractory material. After the refractory crucible is sintered, the molybdenum crucible can be directly taken out without pollution, high furnace drying efficiency, and no material waste. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with specific embodiments.
[0031] Example 1
[0032] The manufacturing method of the vanadium-aluminum alloy smelting furnace of this embodiment is mainly composed of a special induction coil for a suspension furnace, a special water-cooled copper crucible for a suspension furnace and refractory materials; the refractory materials are divided into refractory dry vibrating materials, refractory ramming materials, and refractory castable materials; the refractory dry vibrating materials and refractory ramming materials are used for the furnace bottom and furnace wall, and the refractory castable material is used for the furnace mouth.
[0033] The manufacturing method of the vanadium-aluminum alloy smelting furnace is as follows:
[0034] Step 1: prefabricate the refractory castable into a trumpet-shaped furnace mouth, wherein the upper diameter of the furnace mouth is larger than the diameter of the special induction coil for the suspension furnace, and the lower outer diameter of the furnace mouth is equal to the inner diameter of the special water-cooled copper crucible for the suspension furnace. The prefabricated furnace mouth is assembled inside the special water-cooled copper crucible for the suspension furnace, and the lower part of the furnace mouth extends into the special induction coil for the suspension furnace by 4-8 cm;
[0035] Step 2: assembling the special water-cooled copper crucible for suspension furnace into the special induction coil for suspension furnace, applying insulating putty on the special induction coil for suspension furnace, spreading refractory dry vibration material on the bottom and wall of the special water-cooled copper crucible for suspension furnace, compacting the refractory dry vibration material layer with a compacting tool, and then shaving the surface of the refractory dry vibration material layer;
[0036] Step 3: Mix the refractory ramming material and the binder, spread them on the dry vibration material layer after scraping, and compact them with a compaction tool to obtain a refractory crucible;
[0037] Step 4: placing the molybdenum crucible mold in the refractory crucible prepared in step 3, starting the power supply of the vanadium-aluminum alloy smelting furnace to start heating, and using the heat of the induction heating of the molybdenum crucible mold to bake the refractory crucible. The baking process is divided into three process stages: low-temperature drying, medium-temperature consolidation, and high-temperature sintering. After the baking process is completed, stop heating and take out the molybdenum crucible mold;
[0038] Step 5: Continue to operate the cooling water system of the vanadium-aluminum alloy smelting furnace, and cool the special coil of the suspension furnace and the special water-cooled copper crucible of the suspension furnace by water until the temperature of the refractory crucible drops below 60°C, and the entire vanadium-aluminum alloy smelting furnace is completed.
[0039] Preferably, the weight content of the main components of the refractory castable in step 1 is 75% to 88% aluminum oxide, 4% to 8% titanium oxide, 3% to 4% magnesium oxide, and 3% to 6% water; the refractory castable ingredients are mainly composed of three parts: 70% to 80% aggregate, 10% to 15% binder, and 10% to 20% admixture; the aggregate of the refractory castable contains coarse aggregate and fine aggregate, and the particle size range of the coarse aggregate is 8 to 25 mm; the particle size range of the fine aggregate is 0.1 to 8 mm; the binder is alumina cement; the admixture has the same composition as the aggregate, which is aggregate powder after fine grinding of the refractory aggregate, and the particle size range D90 of the aggregate powder is less than 0.06 mm.
[0040] Preferably, 2%-3% of stainless steel fiber can be added according to the weight of the refractory castable during the process of prefabricating the furnace mouth of the refractory castable in step 1.
[0041] Preferably, the weight content of the main components of the refractory dry vibration material in step 2 is 81% to 85% alumina, 3% to 6% magnesium oxide, 3% to 5% silicon carbide, and 1% to 3% silicon dioxide; the refractory dry vibration material is mainly composed of 60% to 70% aggregate, 20% to 30% powder, 4% to 6% sintering agent, and 1% to 4% thermosetting binder; the aggregate of the refractory dry vibration material contains coarse aggregate, medium aggregate and fine aggregate, and the particle size range of the coarse aggregate is 1 to 4 mm; the particle size range of the medium aggregate is 0.3 to 1 mm; The particle size range of fine aggregate is 0.1-0.3mm; the weight ratio of coarse aggregate, medium aggregate and fine aggregate of the refractory dry vibrating material is 3-5:1-3:3-5 (preferably 4:2:4); the powder has the same composition as the aggregate, which is the aggregate powder obtained by finely grinding the aggregate of the refractory dry vibrating material, and the particle size range of the powder is 0.01-0.074mm; the weight ratio of aggregate and powder of the refractory dry vibrating material is (1-5):1, preferably 3:1; the sintering agent is boric anhydride; and the thermosetting binder is phenolic resin.
[0042] Preferably, 4% to 7% by weight of vanadium-aluminum alloy powder is mixed into the refractory dry vibrating material in step 2, and the particle size of the vanadium-aluminum alloy powder is ≤100 μm.
[0043] Preferably, in step 2, before spreading the refractory dry vibration material on the bottom and the wall of the water-cooled copper crucible for the suspension furnace, a layer of non-magnetic alarm stainless steel mesh is first arranged on the water-cooled copper crucible for the suspension furnace and the wall of the crucible.
[0044] Preferably, in step 2, after the surface of the refractory dry vibration material layer is scraped, a layer of non-magnetic alarm stainless steel mesh is provided on the refractory dry vibration material layer.
[0045] Preferably, in step 3, the weight content of the main components of the refractory ramming material is 70% to 80% alumina, 15% to 20% silicon dioxide, 2% to 8% silicon carbide, and 3% to 5% magnesium oxide; the refractory ramming material is mainly composed of 65% to 70% aggregate and 30% to 35% powder; the aggregate of the refractory ramming material contains coarse aggregate, medium aggregate and fine aggregate, and the particle size range of the coarse aggregate is 2 to 8 mm; the particle size range of the medium aggregate is 0.8 to 2 mm; the particle size range of the fine aggregate is 0.1 to 0.8 mm; the weight ratio of the coarse aggregate, the medium aggregate and the fine aggregate of the refractory ramming material is 1-5:1-3:4-6 (preferably 3:2:5); the powder has the same composition as the aggregate, which is a fine aggregate powder obtained by finely grinding the aggregate of the refractory ramming material, and the particle size range of the powder is 0.03-0.1 mm; the weight ratio of the aggregate and the powder of the refractory ramming material is (1-5):1 (preferably 3:1); the amount of the binder used is 3%-5% of the weight of the refractory ramming material, and the binder is high alumina cement.
[0046] Preferably, 2% to 4% of the total weight of the refractory ramming material is added to the refractory ramming material in step three, and the particle size of the vanadium aluminum alloy powder is ≤100 μm.
[0047] Preferably, in step 4, the low-temperature drying process is to heat up from room temperature to 200-300°C at a rate of 50°C / h, and keep warm for 1-2h; the medium-temperature consolidation process is to heat up from the drying temperature to 800°C at a rate of 100-150°C / h, keep warm for 1-2h, and then heat up to 1000°C at a rate of 150-200°C / h, and keep warm for 2-3h; the high-temperature sintering is to heat up to 1500°C at a rate of 200-250°C / h, and keep warm for 2-3h.
[0048] The following embodiments 2-4 are specific application embodiments of embodiment 1.
[0049] Example 2
[0050] The vanadium aluminum alloy smelting furnace of this embodiment is composed of a suspension furnace dedicated induction coil, a suspension furnace dedicated water-cooled copper crucible and refractory materials; the refractory materials are divided into refractory dry vibration materials, refractory ramming materials, and refractory castable materials; the refractory dry vibration materials and refractory ramming materials are used for the furnace bottom and furnace wall, and the refractory castable materials are used for the furnace mouth. The manufacturing method of the vanadium aluminum alloy smelting furnace is as follows:
[0051] Step 1: prefabricate the refractory castable into a trumpet-shaped furnace mouth, wherein the weight content of the main components of the refractory castable is 75% alumina, 8% titanium oxide, 4% magnesium oxide, and 3% water; the refractory castable ingredients are mainly composed of 70% aggregate, 10% binder, and 20% admixture; the aggregate of the refractory castable contains coarse aggregate and fine aggregate, and the particle size range of the coarse aggregate is 8-25mm; the particle size range of the fine aggregate is 0.1-8mm; the binder is alumina cement; the admixture has the same composition as the aggregate, which is the aggregate powder obtained by finely grinding the refractory aggregate, and the particle size range D90 of the aggregate powder is less than 0.06mm, the upper diameter of the furnace mouth is larger than the diameter of the special induction coil for the suspension furnace, the lower outer diameter of the furnace mouth is equal to the inner diameter of the special water-cooled copper crucible for the suspension furnace, the prefabricated furnace mouth is assembled inside the special water-cooled crucible for the suspension furnace, and the lower part of the furnace mouth extends 4cm into the special induction coil for the suspension furnace;
[0052] Step 2: assemble the water-cooled copper crucible for suspension furnace into the induction coil for suspension furnace, apply insulating putty on the induction coil for suspension furnace, spread refractory dry vibration material on the bottom and wall of the water-cooled copper crucible for suspension furnace, the weight content of the main components of the refractory dry vibration material is 81% of aluminum oxide, 6% of magnesium oxide, 3% of silicon carbide, and 1% of silicon dioxide; the refractory dry vibration material is mainly composed of 60% aggregate, 30% powder, 4% sintering agent, and 4% thermosetting binder; the aggregate of the refractory dry vibration material contains coarse aggregate, medium aggregate and fine aggregate. The particle size range of the coarse aggregate is 1-4mm; the particle size range of the medium aggregate is 0.3-1mm; the particle size range of the fine aggregate is 0.1-0.3mm; the weight ratio of the coarse aggregate, medium aggregate and fine aggregate of the refractory dry vibration material is 4:2:4; the powder has the same composition as the aggregate, which is the aggregate powder after fine grinding of the aggregate of the refractory dry vibration material, and the particle size range of the powder is 0.01-0.074mm; the weight ratio of the aggregate and the powder of the refractory dry vibration material is 3:1; the sintering agent is boric anhydride; the thermosetting binder is phenolic resin. Mix 4% of the total weight of the refractory dry vibration material into the refractory dry vibration material, and the particle size of the vanadium aluminum alloy powder is ≤100μm. Use a vibration tool to compact the refractory dry vibration material layer, and then shave the surface of the refractory dry vibration material layer;
[0053] Step 3: Mix the refractory ramming material and the binder. The weight content of the main components of the refractory ramming material is 70% alumina, 20% silicon dioxide, 5% silicon carbide, and 5% magnesium oxide. The refractory ramming material is mainly composed of 65% aggregate and 35% powder. The aggregate of the refractory ramming material contains coarse aggregate, medium aggregate and fine aggregate. The particle size range of the coarse aggregate is 2-8 mm; the particle size range of the medium aggregate is 0.8-2 mm; the particle size range of the fine aggregate is It is 0.1-0.8mm; the weight ratio of coarse aggregate, medium aggregate and fine aggregate of the refractory ramming material is 3:2:5; the powder has the same composition as the aggregate, which is a fine aggregate powder after fine grinding of the aggregate of the refractory ramming material, and the particle size range of the powder is 0.03-0.1mm; the weight ratio of aggregate and powder of the refractory ramming material is 3:1; the amount of the binder used is 3% of the weight of the refractory ramming material, and the binder is high-alumina cement. Add 2% of the total weight of the refractory ramming material to the refractory ramming material, and the particle size of the vanadium-aluminum alloy powder is ≤100μm. Spread the refractory ramming material on the dry vibration material layer after scraping, and compact it with a compaction tool;
[0054] Step 4: Place the molybdenum crucible mold in the refractory crucible prepared above, start the power supply of the vanadium-aluminum alloy smelting furnace to start heating, and use the induction heat of the molybdenum crucible mold to bake the refractory crucible. The baking furnace is divided into three process stages: low-temperature drying, medium-temperature consolidation and high-temperature sintering. The low-temperature drying process is to heat up from room temperature to 200°C at a rate of 50°C / h, and keep warm for 1h; the medium-temperature consolidation process is to heat up from the drying temperature to 800°C at a rate of 100°C / h, keep warm for 1h, and then heat up to 1000°C at a rate of 150°C / h, and keep warm for 2h; the high-temperature sintering is to heat up to 1500°C at a rate of 200°C / h, and keep warm for 2h. Stop heating after the baking is completed, and take out the molybdenum crucible mold;
[0055] Step 5: Continue to operate the cooling water system of the vanadium-aluminum alloy smelting furnace, and cool the special coil of the suspension furnace and the special water-cooled copper crucible of the suspension furnace by water until the temperature of the refractory crucible drops below 60°C, and the entire vanadium-aluminum alloy smelting furnace is completed.
[0056] The vanadium-aluminum alloy smelting furnace manufactured by the method of this embodiment is used to smelt the vanadium-aluminum alloy AlV55, and the composition of the obtained vanadium-aluminum alloy is analyzed, and the mass percentage is:
[0057] V: 55.12%, Fe: 0.30%, Si: 0.28%, C: 0.12%, O: 0.12%, and the rest is Al. It meets the composition range of national standard grade AIV55.
[0058] The vanadium-aluminum alloy smelting furnace with a capacity of 200KG or less manufactured by the method of this embodiment has a service life of about 52 furnace cycles, and a non-magnetic stainless steel mesh alarm prompts that the refractory material needs to be repaired or replaced.
[0059] Example 3
[0060] The vanadium aluminum alloy smelting furnace of this embodiment is composed of a suspension furnace dedicated induction coil, a suspension furnace dedicated water-cooled copper crucible and refractory materials; the refractory materials are divided into refractory dry vibration materials, refractory ramming materials, and refractory castable materials; the refractory dry vibration materials and refractory ramming materials are used for the furnace bottom and furnace wall, and the refractory castable materials are used for the furnace mouth. The manufacturing method of the vanadium aluminum alloy smelting furnace is as follows:
[0061] Step 1: Prefabricate the refractory castable into a bell-shaped furnace mouth, and add 2% stainless steel fiber by weight of the refractory castable during the prefabrication process. Stainless steel fiber is added to improve the toughness of the furnace mouth refractory material, making it more resistant to the erosion of the vanadium aluminum alloy melt during the pouring process. The weight content of the main components of the refractory castable is 88% aluminum oxide, 4% titanium oxide, 3% magnesium oxide, and 3% water; the refractory castable ingredients are mainly composed of 80% aggregate, 10% binder, and 10% admixture; the aggregate of the refractory castable contains coarse aggregate and fine aggregate, the particle size range of the coarse aggregate is 8-25mm; the particle size range of the fine aggregate is 0.1-8mm; the binder is alumina cement; the admixture has the same composition as the aggregate, which is fine aggregate powder after fine grinding of the refractory aggregate, and the particle size range D90 of the fine aggregate powder is less than 0.06mm; the upper diameter of the furnace mouth is larger than the diameter of the special induction coil for the suspension furnace, the outer diameter of the lower part of the furnace mouth is equal to the inner diameter of the special water-cooled copper crucible for the suspension furnace, the prefabricated furnace mouth is assembled inside the special water-cooled crucible for the suspension furnace, and the lower part of the furnace mouth extends into the special induction coil for the suspension furnace by 8cm;
[0062] Step 2: assemble the water-cooled copper crucible for suspension furnace into the induction coil for suspension furnace, apply insulating putty on the induction coil for suspension furnace, and spread refractory dry vibration material on the bottom and wall of the water-cooled copper crucible for suspension furnace. The weight content of the main components of the refractory dry vibration material is 85% of aluminum oxide, 3% of magnesium oxide, 5% of silicon carbide, and 3% of silicon dioxide; the refractory dry vibration material is mainly composed of 70% aggregate, 20% powder, 6% sintering agent, and 1% thermosetting binder; the aggregate of the refractory dry vibration material contains coarse aggregate, medium aggregate and fine aggregate. The refractory dry vibrating material has a coarse aggregate size range of 1 to 4 mm; the medium aggregate size range is 0.3 to 1 mm; the fine aggregate size range is 0.1 to 0.3 mm; the weight ratio of the coarse aggregate, medium aggregate and fine aggregate of the refractory dry vibrating material is 4:2:4; the powder has the same composition as the aggregate, which is the aggregate powder after fine grinding of the refractory dry vibrating material, and the particle size range of the powder is 0.01 to 0.074 mm; the weight ratio of the aggregate and powder of the refractory dry vibrating material is 3:1; the sintering agent is boric anhydride; the thermosetting binder is phenolic resin. 5% of the total weight of the refractory dry vibrating material is mixed with vanadium aluminum alloy powder, and the particle size of the vanadium aluminum alloy powder is ≤100μm. Before laying the refractory dry vibration material on the bottom and wall of the water-cooled copper crucible for the suspension furnace, a layer of non-magnetic alarm stainless steel mesh is first set on the bottom and wall of the water-cooled copper crucible. Then use a vibration tool to compact the refractory dry vibration material layer, and then shave the surface of the refractory dry vibration material layer. After shaving, a layer of non-magnetic alarm stainless steel mesh is also set on the refractory dry vibration material layer.
[0063] Step 3: Mix the refractory ramming material and the binder. The weight content of the main components of the refractory ramming material is 72% alumina, 15% silicon dioxide, 8% silicon carbide, and 5% magnesium oxide. The refractory ramming material is mainly composed of 70% aggregate and 30% powder. The aggregate of the refractory ramming material contains coarse aggregate, medium aggregate and fine aggregate. The particle size range of the coarse aggregate is 2-8mm; the particle size range of the medium aggregate is 0.8-2mm; the particle size range of the fine aggregate is It is 0.1-0.8mm; the weight ratio of coarse aggregate, medium aggregate and fine aggregate of the refractory ramming material is 3:2:5; the powder has the same composition as the aggregate, which is the aggregate powder after fine grinding of the aggregate of the refractory ramming material, and the particle size range of the powder is 0.03-0.1mm; the weight ratio of aggregate and powder of the refractory ramming material is 3:1; the amount of the binder used is 5% of the weight of the refractory ramming material, and the binder is high-alumina cement. Add 3% of the total weight of the refractory ramming material to the refractory ramming material, and the particle size of the vanadium-aluminum alloy powder is ≤100μm. Then spread the aforementioned refractory ramming material on the dry vibration material layer after scraping, and vibrate it with a compaction tool;
[0064] Step 4: Place the molybdenum crucible mold in the refractory crucible prepared above, start the power supply of the vanadium-aluminum alloy smelting furnace to start heating, and use the induction heat of the molybdenum crucible mold to bake the refractory crucible. The baking furnace is divided into three process stages: low-temperature drying, medium-temperature consolidation and high-temperature sintering. The low-temperature drying process is to heat up from room temperature to 300°C at a rate of 50°C / h, and keep warm for 2h; the medium-temperature consolidation process is to heat up from the drying temperature to 800°C at a rate of 150°C / h, keep warm for 2h, and then heat up to 1000°C at a rate of 200°C / h, and keep warm for 3h; the high-temperature sintering is to heat up to 1500°C at a rate of 250°C / h, and keep warm for 3h. Stop heating after the baking is completed and take out the molybdenum crucible mold;
[0065] Step 5: Continue to operate the cooling water system of the vanadium-aluminum alloy smelting furnace, and cool the special coil of the suspension furnace and the special water-cooled copper crucible of the suspension furnace by water until the temperature of the refractory crucible drops below 60°C, and the entire vanadium-aluminum alloy smelting furnace is completed.
[0066] The vanadium-aluminum alloy smelting furnace manufactured by the method of this embodiment is used to smelt the vanadium-aluminum alloy AIV55, and the composition of the obtained vanadium-aluminum alloy is analyzed, and the mass percentage is:
[0067] V: 56.72%, Fe: 0.28%, Si: 0.22%, C: 0.10%, O: 0.10%, and the rest is Al. It meets the composition range of national standard grade AIV55.
[0068] The vanadium-aluminum alloy smelting furnace with a capacity of 200KG or less manufactured by the method of this embodiment has a service life of about 58 furnace cycles, and a non-magnetic stainless steel mesh alarm will be issued to prompt that the refractory material needs to be repaired or replaced.
[0069] Example 4
[0070] The vanadium aluminum alloy smelting furnace of this embodiment is composed of a suspension furnace dedicated induction coil, a suspension furnace dedicated water-cooled copper crucible and refractory materials; the refractory materials are divided into refractory dry vibration materials, refractory ramming materials, and refractory castable materials; the refractory dry vibration materials and refractory ramming materials are used for the furnace bottom and furnace wall, and the refractory castable materials are used for the furnace mouth. The manufacturing method of the vanadium aluminum alloy smelting furnace is as follows:
[0071] Step 1: Prefabricate the refractory castable into a bell-shaped furnace mouth, and add 3% stainless steel fiber by weight of the refractory castable during the prefabrication process. Adding stainless steel fiber can improve the toughness of the furnace mouth refractory material and make it more resistant to the erosion of the vanadium aluminum alloy melt during the pouring process. The weight content of the main components of the refractory castable is 76% aluminum oxide, 4% titanium oxide, 4% magnesium oxide, and 6% water; the refractory castable ingredients are mainly composed of 70% aggregate, 15% binder, and 15% admixture; the aggregate of the refractory castable contains coarse aggregate and fine aggregate, the particle size range of the coarse aggregate is 8-25mm; the particle size range of the fine aggregate is 0.1-8mm; the binder is alumina cement; the admixture has the same composition as the aggregate, which is fine aggregate powder after fine grinding of the refractory aggregate, and the particle size range D90 of the fine aggregate powder is less than 0.06mm; the upper diameter of the furnace mouth is larger than the diameter of the special induction coil for the suspension furnace, the outer diameter of the lower part of the furnace mouth is equal to the inner diameter of the special water-cooled copper crucible for the suspension furnace, the prefabricated furnace mouth is assembled inside the special water-cooled crucible for the suspension furnace, and the lower part of the furnace mouth extends into the special induction coil for the suspension furnace by 6cm;
[0072] Step 2: assemble the water-cooled copper crucible for suspension furnace into the induction coil for suspension furnace, apply insulating putty on the induction coil for suspension furnace, and spread refractory dry vibration material on the bottom and wall of the water-cooled copper crucible for suspension furnace. The weight content of the main components of the refractory dry vibration material is 84% aluminum oxide, 5% magnesium oxide, 4% silicon carbide, and 3% silicon dioxide; the refractory dry vibration material is mainly composed of 65% aggregate, 25% powder, 6% sintering agent, and 4% thermosetting binder; the aggregate of the refractory dry vibration material contains coarse aggregate, medium aggregate and fine aggregate. The refractory dry vibrating material has a coarse aggregate size range of 1 to 4 mm; the medium aggregate size range is 0.3 to 1 mm; the fine aggregate size range is 0.1 to 0.3 mm; the weight ratio of the coarse aggregate, medium aggregate and fine aggregate of the refractory dry vibrating material is 4:2:4; the powder has the same composition as the aggregate, which is the aggregate powder after fine grinding of the refractory dry vibrating material, and the particle size range of the powder is 0.01 to 0.074 mm; the weight ratio of the aggregate and powder of the refractory dry vibrating material is 3:1; the sintering agent is boric anhydride; the thermosetting binder is phenolic resin. 7% of the total weight of the refractory dry vibrating material is mixed with vanadium aluminum alloy powder, and the particle size of the vanadium aluminum alloy powder is ≤100μm. Before laying the refractory dry vibration material on the bottom and wall of the water-cooled copper crucible for the suspension furnace, a layer of non-magnetic alarm stainless steel mesh is first set on the bottom and wall of the water-cooled copper crucible. Then use a vibration tool to compact the refractory dry vibration material layer, and then shave the surface of the refractory dry vibration material layer. After shaving, a layer of non-magnetic alarm stainless steel mesh is also set on the refractory dry vibration material layer.
[0073] Step 3: Mix the refractory ramming material and the binder. The weight content of the main components of the refractory ramming material is 80% alumina, 15% silicon dioxide, 2% silicon carbide, and 3% magnesium oxide. The refractory ramming material is mainly composed of 70% aggregate and 30% powder. The aggregate of the refractory ramming material contains coarse aggregate, medium aggregate and fine aggregate. The particle size range of the coarse aggregate is 2-8 mm; the particle size range of the medium aggregate is 0.8-2 mm; the particle size range of the fine aggregate is It is 0.1-0.8mm; the weight ratio of coarse aggregate, medium aggregate and fine aggregate of the refractory ramming material is 3:2:5; the powder has the same composition as the aggregate, which is a fine aggregate powder after fine grinding of the aggregate of the refractory ramming material, and the particle size range of the powder is 0.03-0.1mm; the weight ratio of aggregate and powder of the refractory ramming material is 3:1; the amount of the binder used is 5% of the weight of the refractory ramming material, and the binder is high-alumina cement. Add 4% of the total weight of the refractory ramming material to the refractory ramming material, and the particle size of the vanadium-aluminum alloy powder is ≤100μm. Then spread the aforementioned refractory ramming material on the dry vibration material layer after scraping, and compact it with a compaction tool;
[0074] Step 4: Place the molybdenum crucible mold in the refractory crucible prepared above, start the power supply of the vanadium-aluminum alloy smelting furnace to start heating, and use the heat generated by the induction heating of the molybdenum crucible mold to bake the refractory crucible. The baking process is divided into three process stages: low-temperature drying, medium-temperature consolidation and high-temperature sintering. The low-temperature drying process is to heat up from room temperature to 250°C at a rate of 50°C / h, and keep warm for 2h; the medium-temperature consolidation process is to heat up from the drying temperature to 800°C at a rate of 100°C / h, keep warm for 2h, and then heat up to 1000°C at a rate of 160°C / h, and keep warm for 3h; the high-temperature sintering is to heat up to 1500°C at a rate of 220°C / h, and keep warm for 3h. Stop heating after the baking is completed, and take out the molybdenum crucible mold;
[0075] Step 5: Continue to operate the cooling water system of the vanadium-aluminum alloy smelting furnace, and cool the special coil of the suspension furnace and the special water-cooled copper crucible of the suspension furnace by water until the temperature of the refractory crucible drops below 60°C, and the entire vanadium-aluminum alloy smelting furnace is completed.
[0076] The vanadium-aluminum alloy smelting furnace manufactured by the method of this embodiment is used to smelt the vanadium-aluminum alloy AIV55, and the composition of the obtained vanadium-aluminum alloy is analyzed, and the mass percentage is:
[0077] V: 58.42%, Fe: 0.25%, Si: 0.20%, C: 0.13%, O: 0.08%, and the rest is Al. It meets the composition range of national standard grade AIV55.
[0078] The vanadium-aluminum alloy smelting furnace with a capacity of 200KG or less manufactured by the method of this embodiment has an average service life of 64 furnaces for the refractory crucible whose inner layer of the furnace jacket is in direct contact with the vanadium-aluminum alloy. There will be a non-magnetic alarm stainless steel mesh alarm to prompt that the refractory material needs to be repaired or replaced.
Claims
1. A method for manufacturing a vanadium-aluminum alloy smelting furnace, wherein the vanadium-aluminum alloy smelting furnace is composed of a suspension furnace-specific induction coil, a suspension furnace-specific water-cooled copper crucible, and refractory materials, wherein the refractory materials are divided into refractory dry vibration materials, refractory ramming materials, and refractory castable materials; the refractory dry vibration materials and refractory ramming materials are used for the furnace bottom and furnace wall, and the refractory castable material is used for the furnace mouth. Features: The manufacturing method of the vanadium-aluminum alloy smelting furnace is as follows: Step 1: prefabricate the refractory castable into a trumpet-shaped furnace mouth, wherein the upper diameter of the furnace mouth is larger than the diameter of the special induction coil for the suspension furnace, and the lower outer diameter of the furnace mouth is equal to the inner diameter of the special water-cooled copper crucible for the suspension furnace. The prefabricated furnace mouth is assembled inside the special water-cooled copper crucible for the suspension furnace, and the lower part of the furnace mouth extends into the special induction coil for the suspension furnace by 4-8 cm; Step 2: Assemble the special water-cooled copper crucible for suspension furnace into the special induction coil for suspension furnace, apply insulating putty on the special induction coil for suspension furnace, spread the refractory dry vibration material on the bottom and wall of the special water-cooled copper crucible for suspension furnace, vibrate the refractory dry vibration material layer with a vibration tool, and then scrape the surface of the refractory dry vibration material layer; Step 3: Mix the refractory ramming material and the binder, spread them on the dry vibration material layer after scraping, and compact them with a compaction tool to obtain a refractory crucible; Step 4: placing the molybdenum crucible mold in the refractory crucible prepared in step 3, starting the power supply of the vanadium-aluminum alloy smelting furnace to start heating, and using the heat of the induction heating of the molybdenum crucible mold to bake the refractory crucible. The baking process is divided into three process stages: low-temperature drying, medium-temperature consolidation, and high-temperature sintering. After the baking process is completed, stop heating and take out the molybdenum crucible mold; Step 5: Continue to operate the cooling water system of the vanadium-aluminum alloy smelting furnace, and cool the special coil of the suspension furnace and the special water-cooled copper crucible of the suspension furnace by water until the temperature of the refractory crucible drops below 60°C, and the entire vanadium-aluminum alloy smelting furnace is completed.
2. The method for manufacturing the vanadium-aluminum alloy smelting furnace according to claim 1, Features: In step one, the weight content of the refractory castable components is 75% to 88% aluminum oxide, 4% to 8% titanium oxide, 3% to 4% magnesium oxide, and 3% to 6% water; the refractory castable ingredients are composed of three parts: 70% to 80% aggregate, 10% to 15% binder, and 10% to 20% admixture; the aggregate of the refractory castable contains coarse aggregate and fine aggregate, and the particle size range of the coarse aggregate is 8 to 25 mm; the particle size range of the fine aggregate is 0.1 to 8 mm; the binder is alumina cement; the admixture has the same composition as the aggregate, which is aggregate powder after fine grinding of the refractory aggregate, and the particle size range D90 of the aggregate powder is less than 0.06 mm.
3. The method for manufacturing the vanadium-aluminum alloy smelting furnace according to claim 1, Features: In the process of prefabricating the furnace mouth with refractory castables in step 1, 2%-3% of stainless steel fiber is added according to the weight of the refractory castables.
4. The method for manufacturing the vanadium-aluminum alloy smelting furnace according to claim 1, Features: Step 2: The weight content of the refractory dry vibration material is 81% to 85% alumina, 3% to 6% magnesium oxide, 3% to 5% silicon carbide, and 1% to 3% silicon dioxide; the refractory dry vibration material is composed of 60% to 70% aggregate, 20% to 30% powder, 4% to 6% sintering agent, and 1% to 4% thermosetting binder; the aggregate of the refractory dry vibration material contains coarse aggregate, medium aggregate, and fine aggregate, and the particle size range of the coarse aggregate is 1 to 4 mm; the particle size range of the medium aggregate is The particle size of the fine aggregate is 0.3-1mm; the particle size range of the fine aggregate is 0.1-0.3mm; the weight ratio of the coarse aggregate, the medium aggregate and the fine aggregate of the refractory dry vibration material is 4:2:4; the powder has the same composition as the aggregate, which is the aggregate powder obtained by finely grinding the aggregate of the refractory dry vibration material, and the particle size range of the powder is 0.01-0.074mm; the weight ratio of the aggregate and the powder of the refractory dry vibration material is 3:1; the sintering agent is boric anhydride; the thermosetting binder is phenolic resin.
5. The method for manufacturing the vanadium-aluminum alloy smelting furnace according to claim 1, Features: In step 2, vanadium-aluminum alloy powder in an amount of 4% to 7% of the total weight of the refractory dry vibrating material is mixed into the refractory dry vibrating material, wherein the particle size of the vanadium-aluminum alloy powder is ≤100 μm.
6. The method for manufacturing the vanadium-aluminum alloy smelting furnace according to claim 1, Features: In step 2, before laying the refractory dry vibration material on the bottom and crucible wall of the water-cooled copper crucible dedicated for the suspension furnace, a non-magnetic alarm stainless steel mesh is first set on the bottom and crucible wall of the water-cooled copper crucible.
7. The method for manufacturing the vanadium-aluminum alloy smelting furnace according to claim 1, Features: In step 2, after the surface of the refractory dry vibration material layer is shaved, a non-magnetic alarm stainless steel mesh is set on the refractory dry vibration material layer.
8. The method for manufacturing the vanadium-aluminum alloy smelting furnace according to claim 1, Features: In step 3, the weight content of the refractory ramming material components is 70% to 80% alumina, 15% to 20% silicon dioxide, 2% to 8% silicon carbide, and 3% to 5% magnesium oxide; the refractory ramming material ingredients are composed of 65% to 70% aggregate and 30% to 35% powder; the aggregate of the refractory ramming material contains coarse aggregate, medium aggregate and fine aggregate, the particle size range of the coarse aggregate is 2 to 8 mm; the particle size range of the medium aggregate is 0.8 to 2 mm; the particle size range of the fine aggregate is The circumference is 0.1-0.8mm; the weight ratio of coarse aggregate, medium aggregate and fine aggregate of the refractory ramming material is 3:2:5; the powder has the same composition as the aggregate, which is fine aggregate powder after fine grinding of the aggregate of the refractory ramming material, and the particle size range of the powder is 0.03-0.1mm; the weight ratio of aggregate and powder of the refractory ramming material is 3:1; the amount of the binder used is 3%-5% of the weight of the refractory ramming material, and the binder is high alumina cement.
9. The method for manufacturing the vanadium-aluminum alloy smelting furnace according to claim 1, Features: In step 3, 2% to 4% of the total weight of the refractory ramming material is added to the refractory ramming material, and the particle size of the vanadium aluminum alloy powder is ≤100 μm.
10. The method for manufacturing the vanadium-aluminum alloy smelting furnace according to claim 1, Features: In step 4, the low-temperature drying process is to heat up from room temperature to 200-300°C at a rate of 50°C / h, and keep warm for 1-2h; the medium-temperature consolidation process is to heat up from the drying temperature to 800°C at a rate of 100-150°C / h, keep warm for 1-2h, and then heat up to 1000°C at a rate of 150-200°C / h, and keep warm for 2-3h; the high-temperature sintering is to heat up to 1500°C at a rate of 200-250°C / h, and keep warm for 2-3h.