A nondestructive testing method for thermal barrier coatings based on perovskite quantum dots

Through the anion exchange method and photoluminescence spectroscopy of perovskite quantum dots, the non-destructive detection problem of thermal barrier coating is solved, and quantitative monitoring of the corrosion degree, cracks and pores of the coating are achieved, providing an efficient and non-destructive Testing scheme.

CN115452837BActive Publication Date: 2024-12-06XIANGNAN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211125422.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-16
Publication Date
2024-12-06
Estimated Expiration
2042-09-16

AI Technical Summary

Technical Problem

The prior art cannot effectively carry out non-destructive testing of thermal barrier coatings, especially in marine environments. Traditional methods have problems such as expensive testing equipment, long time, need to destroy the coating and low accuracy, making it difficult to accurately detect the pores of the coating and crack.

Method used

Using anion exchange method based on perovskite quantum dots, the chloride ion concentration and distribution in the coating are detected by photoluminescence spectroscopy technology, and the non-destructive detection of the coating's thermal corrosion and salt spray corrosion degree can be quantitatively monitored. Pores and cracks.

Benefits of technology

The non-destructive detection of thermal barrier coating is achieved, with simple operation and no damage to the coating. It can simultaneously monitor the corrosion degree, crack position and pore of the coating. It has the advantage of multi-performance parameter monitoring and is used as a non-failure detection method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115452837B_ABST
    Figure CN115452837B_ABST
Patent Text Reader

Abstract

The present invention discloses a nondestructive testing method for thermal barrier coatings based on perovskite quantum dots, comprising the following steps: step 1, preparing a halogen inorganic perovskite quantum dot CsPbX3 solution and a chloride ion compound aqueous solution; step 2, obtaining a blue shift degree fitting curve of the crack / hole depth-PL spectrum; step 3, detecting the area size and depth of cracks on the surface of the thermal barrier coating. The present invention uses a perovskite quantum dot anion exchange method to detect the chloride ion concentration and distribution of the coating to achieve a nondestructive testing scheme for the degree of thermal corrosion and salt spray corrosion of the coating, and the scheme can quantitatively monitor the holes and cracks of the coating at the same time through photoluminescence spectroscopy technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of detection technology, and in particular to a nondestructive detection method for thermal barrier coatings based on perovskite quantum dots. Background Art

[0002] The service environment of high-temperature components of aircraft engines and gas turbines is harsh. In order to meet the stringent performance requirements of materials, the main measure currently taken is thermal barrier coating technology, which can increase the operating temperature of hot end components, extend the service life of components, and improve engine fuel efficiency. Thermal barrier coatings are key materials for high-temperature components of aircraft engines and gas turbines. The service life of aircraft engines and ship gas turbines operating in the harsher marine environment is in urgent need of improvement. In the future, thermal barrier coatings for my country's seaworthiness will be an important area of ​​national defense development for our country. The service environment of aircraft engines and gas turbines in the marine environment is very harsh. The characterization technology of thermal barrier coatings is imperfect, and non-destructive testing and evaluation of their quality and performance are key issues that need to be solved urgently.

[0003] For the detection of thermal barrier coatings, traditional technologies use industrial cameras, eddy current detection, scanning electron microscope photos, ultrasonic detection, electrochemical impedance spectroscopy, etc. to focus on the coating thickness, coating porosity and stress state of the coating (i.e. elastic modulus). The visual inspection method based on industrial cameras is simple to operate and widely used, but it cannot accurately and quantitatively detect. The eddy current detection method can measure the thickness of the ceramic coating, but due to the non-conductivity of the ceramic coating, this method cannot detect the internal cracks of the ceramic layer. The ultrasonic detection method can be used to evaluate the coating thickness, elastic modulus, porosity and interface bonding quality, but because the coating is very thin (hundreds of microns) and has porous characteristics, it makes it difficult to distinguish the interface crack signal and the interface signal aliasing, and the signal cannot be effectively extracted for processing. The electrochemical impedance spectroscopy method has a certain effect on the detection of thermally grown oxide layers, but the detection accuracy strongly depends on the contact area. The above methods have the disadvantages of expensive testing equipment, long testing time, the need to destroy the coating and low testing accuracy.

[0004] Explanation of the name:

[0005] ODE: octadecene.

[0006] OA: oleic acid.

[0007] OAm: oleylamine. Summary of the invention

[0008] The technical problem to be solved by the present invention is to provide a nondestructive testing method for thermal barrier coatings based on perovskite quantum dots in view of the shortcomings of the existing technology. The present invention utilizes the perovskite quantum dot anion exchange method to detect the chloride ion concentration and distribution of the coating to achieve a nondestructive testing scheme for the degree of thermal corrosion and salt spray corrosion of the coating. The scheme can also quantitatively monitor the pores and cracks of the coating through photoluminescence spectroscopy technology.

[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0010] A nondestructive testing method for thermal barrier coatings based on perovskite quantum dots comprises the following steps:

[0011] Step 1, preparing a halogen inorganic perovskite quantum dot CsPbX3 solution and an aqueous solution of a chloride ion compound with a preset concentration;

[0012] Step 2: Setting a test board, forming holes and cracks of known depth and width on the surface of the test board, then pouring a chloride ion compound aqueous solution of a preset concentration into the holes and cracks, scraping off excess chloride ion compound aqueous solution of the preset concentration on the surface of the test board, and drying;

[0013] Step 3: Spin-coat, drop-coat or scrape-coat the prepared halogen inorganic perovskite quantum dot CsPbX3 solution on the surface of the test plate, dry it, then drop-coat a preset volume of deionized water, wait for the anion exchange reaction to be fully completed, and then evaporate it to dryness, detect the degree of blue shift of the PL spectrum of the test plate, and draw and fit the blue shift degree fitting curve of the crack / hole depth-PL spectrum according to the corresponding depth of the crack;

[0014] Step 4: Use the halogen inorganic perovskite quantum dot CsPbX3 solution to detect the area, size and depth of the holes and cracks in the thermal barrier coating.

[0015] For further improvement, the steps of step 4 are as follows:

[0016] Use clean water to clean the surface of the thermal barrier coating, dry it, and then apply a chloride ion compound aqueous solution of a preset concentration, then scrape off the excess chloride ion compound aqueous solution of a preset concentration on the surface, dry it, then apply a halogen inorganic perovskite quantum dot CsPbX3 solution, dry it, and then drop a preset volume of deionized water, wait for the anion exchange to fully react and then evaporate it, and then detect the PL spectrum of the halogen inorganic perovskite quantum dot CsPbX3 solution; the blue area is the area of ​​the holes and cracks, and the depth of the blue at different positions of the holes and cracks and the degree of blue shift of the crack / hole depth-PL spectrum are fitted to obtain the depth of the holes and cracks at different positions to complete the detection of the thermal barrier coating.

[0017] For further improvement, the steps of step 4 are as follows:

[0018] Use clean water to clean the surface of the thermal barrier coating, apply the halogen inorganic perovskite quantum dot CsPbX3 solution after drying, dry it, then drop-coat a preset concentration of chloride ion compound aqueous solution, then scrape off the excess preset concentration of chloride ion compound aqueous solution on the surface, wait for the anion exchange to fully react and then evaporate to dryness, and then detect the PL spectrum of the halogen inorganic perovskite quantum dot CsPbX3 solution; the blue area is the area of ​​the holes and cracks, and the depth of the blue at different positions of the holes and cracks and the degree of blue shift of the crack / hole depth-PL spectrum are fitted to obtain the depth of the empty holes and cracks at different positions to complete the detection of the thermal barrier coating.

[0019] As a further improvement, in steps 1 to 3, aqueous solutions of chloride ion compounds with different preset concentrations are selected to obtain corresponding fitting curves of crack / hole depth-PL spectrum blue shift degree; the steps of step 4 are as follows:

[0020] A standard sample with a known crack depth was selected and arranged with the thermal barrier coating as follows: the surface was directly coated with a halogen inorganic perovskite quantum dot CsPbX3 solution without being washed with water, dried, and then water was dripped on the surface of the thermal barrier coating. The water penetrated into the thermal barrier coating along the holes and cracks of the coating, dissolved the chloride ions in the cracks and holes of the thermal barrier coating, and formed a chloride ion compound aqueous solution. The chloride ions were fully exchanged with the perovskite CsPbBr3 quantum dots in situ and then evaporated to dryness. The halogen inorganic perovskite quantum dot CsPbX3 solution was then tested. PL spectrum; wherein the blue area is the area size of the holes and cracks; then, according to the crack depth and blue shift degree of the standard sample, the crack / hole depth-PL spectrum blue shift degree fitting curve of the chloride ion compound aqueous solution with a preset concentration closest to the concentration of the chloride ion compound aqueous solution in the thermal barrier coating is selected as the reference crack / hole depth-PL spectrum blue shift degree fitting curve of the thermal barrier coating, and the depth of the holes and cracks at different positions is obtained according to the depth of blue at different positions of the holes and cracks, thereby completing the detection of the thermal barrier coating.

[0021] A further improvement is that the PL spectrum of the halogen inorganic perovskite quantum dot CsPbX3 solution is detected by a test system and a spectral data acquisition system; the test system includes an excitation light source and an integrating sphere, the integrating sphere is connected to a spectrometer, the spectrometer is connected to a computer, and the spectral data acquisition system in the computer excites the light source to perform background subtraction processing, so that the obtained spectral data is only the photoluminescence data of the sample.

[0022] A further improvement is that the spectral range of the excitation light source is 200nm to 405nm; when detecting the PL spectrum of the halogen inorganic perovskite quantum dot CsPbX3 solution, a surface spectrum scanning method or a point spectrum scanning method is adopted; when the surface spectrum scanning method is adopted, the diameter of the integrating sphere is 30cm to 50cm, and when the point spectrum scanning method is adopted, the diameter of the integrating sphere is 10cm to 15cm.

[0023] In a further improvement, the chloride ion compound aqueous solution includes sodium chloride solution, potassium chloride solution, calcium chloride solution and magnesium chloride solution.

[0024] As a further improvement, the preparation method of the halogen inorganic perovskite quantum dot CsPbX3 solution is as follows:

[0025] (1) Preparation of cesium oleate precursor solution

[0026] Cs2CO3, ODE and OA were mixed, vacuum dried at room temperature, and then vacuum stirred at 120°C for 40 minutes, and then the mixture was heated for 1 hour under N2 atmosphere until all Cs2CO3 was dissolved to obtain a cesium oleate precursor solution; wherein the mass volume ratio of Cs2CO3 to ODE was 0.0305:10 g / ml to 3.305:10 g / ml, and the mass volume ratio of Cs2CO3 to OA was 0.0305:1 g / ml to 0.305:1 g / ml;

[0027] (2) Synthesis of CsPbBr3 quantum dots

[0028] PbBr2, ODE, OA and OAm were mixed, vacuum dried at room temperature for 30 minutes, and then vacuum stirred at 120°C for 40 minutes. Then, in a N2 atmosphere, the mixture was stirred at 120°C for 45 minutes, and then the temperature was raised to 150°C-180°C and stirred for 10 minutes. Then, the cesium oleate precursor solution was immediately injected and reacted for 5 seconds, and then immediately cooled to room temperature with ice water to obtain a crude reaction solution of CsPbBr3 quantum dots. The mass volume ratio of PbBr2 to ODE, OA, OAm and cesium oleate precursor solution was 0.01:1:0.1:0.1:0.2 g / ml to 2:100:10:10:20 g / ml.

[0029] (3) Extraction and cleaning of CsPbBr3 quantum dots

[0030] The crude reaction solution and methyl acetate solution are mixed at a volume ratio of 1:1 to 1:3, and the mixture is centrifuged at 8000 rpm for 3 to 5 minutes. The precipitate is dispersed with a non-polar solvent, and the volume ratio of the non-polar solvent to methyl acetate is 1:3; the mixture is centrifuged at 8000 rpm for 3 to 5 minutes, and the precipitate is dispersed with a non-polar solvent; the washing is repeated until the oily ligands on the surface of the halogen inorganic perovskite quantum dots CsPbX3 are cleaned, and the cleaned halogen inorganic perovskite quantum dots are dispersed in a non-polar solvent for storage to obtain a storage solution with a concentration of 0.1 mg / ml to 50 mg / ml. When using the storage solution, the storage solution is centrifuged, and then the precipitate is dispersed with n-hexane to obtain a halogen inorganic perovskite quantum dot CsPbX3 solution with a concentration of 0.1 mg / ml to 50 mg / ml.

[0031] As a further improvement, the depth and width of the cracks and holes of the test plate in step 2 are obtained through scanning electron microscope photos, or are set during prefabrication.

[0032] Further improvement includes step 5, according to the area of ​​the thermal barrier coating surface spin-coated with the halogen inorganic perovskite quantum dot CsPbX3 solution and the total volume occupied by the cracks, the degree of erosion of the thermal barrier coating is obtained: c = a / b, where a is the total volume occupied by the cracks, in units of cm 3 , b is the area of ​​the thermal barrier coating surface spin-coated with halogen inorganic perovskite quantum dot CsPbX3 solution, unit is cm 2 , c is the degree of erosion of the thermal barrier coating, that is, the average eroded thickness of the thermal barrier coating, in cm; a is obtained by the following method: the actual area represented by each pixel is obtained, and then multiplied by the actual depth of the pixel to obtain the volume corresponding to each pixel, and the total volume occupied by the crack is obtained by accumulation. The degree of erosion of the thermal barrier coating here is a relative degree of erosion, because it is accurate data only when most of the thermal barrier coating is not eroded. However, the longer the erosion time, the greater the average height difference of each point of the thermal barrier coating. Therefore, after most of the surface layer is eroded, this data can also be used as a reference.

[0033] Compared with the prior art, the present invention has the following advantages:

[0034] The present invention is simple to operate, will not damage the coating, and can quantitatively monitor the degree of thermal corrosion and salt spray corrosion of the coating, crack location and pores. In addition, previous detection technologies cannot quantitatively detect the degree of thermal corrosion and salt spray corrosion of the coating. The current detection technology can generally only quantitatively monitor one performance parameter of the coating. The present invention can simultaneously monitor three performance parameters of the coating (corrosion degree, crack location, pores), and has the advantage of being able to monitor multiple performance parameters. The detection technology developed by the present invention can be used as a non-failure detection method. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 PL spectra of perovskite CsPbBr3 quantum dots and drop-coated quantum dots;

[0036] Figure 2 This is a schematic diagram of the steps of Example 1;

[0037] Figure 3 This is a schematic diagram of the steps of Example 2;

[0038] Figure 4 This is a schematic diagram of the steps of Example 3;

[0039] Figure 5 is a curve diagram showing the change of PL peak wavelength of the preset test plate of Example 1 with the concentration of salt water;

[0040] Figure 6 The graph is a variation curve of the crack corrosion depth of the preset test plate of Example 1 with the salt spray corrosion time;

[0041] Figure 7 is a curve diagram showing the change of the PL peak wavelength of the preset test plate of Example 1 with the salt spray corrosion time;

[0042] Figure 8 It is a schematic diagram of the structure of the PL test system for coating sample surface scanning;

[0043] Fig. 9 Schematic diagram of the structure of the coating sample point scanning PL test system. DETAILED DESCRIPTION

[0044] Embodiment 1:

[0045] The principle of the present invention is as follows: Halogen inorganic perovskite quantum dots CsPbX3 (where X is Cl, Br, I), the emission spectrum of the quantum dots can be adjusted by changing the X component, and the quantum dots of CsPbBr3 emit green photoluminescence spectrum (PL) under a 365nm excitation light source, and are drop-coated, spin-coated or drop-coated on the coating surface. After the coating is corroded in the marine environment, there are a large number of Cl- ions inside, and the Br in the perovskite quantum dots - Ions easily react with Cl - Ion exchange (chemical reaction formula see formula 1), after exchange, CsPb (Br 1-x Cl x )3 perovskite quantum dots, whose PL spectrum blue-shifts, Figure 1 The PL spectra of quantum dots and the coating after drop coating of quantum dots. Because the coating is corroded by seawater in the marine application environment, grooves and cracks of different depths are formed. The deeper the Cl per unit area, the higher the -The higher the concentration of ions, the greater the blue shift of PL will be. Therefore, the degree of blue shift of PL spectrum can be used to quantitatively evaluate the Cl per unit area. - The concentration of ions can be used to monitor the degree (depth) of thermal corrosion and salt spray corrosion of the coating. It is difficult to detect the location of pores and cracks by direct visual inspection. The present invention uses the planar PL spectrum distribution of the coating surface to monitor the location of cracks and pores. The specific operation process is as follows:

[0046] (a) A test plate is provided, cracks and holes of different preset depths are formed on the surface of the test plate, and then a chloride ion compound aqueous solution of preset concentration is poured into the cracks and holes, and excess chloride ion compound aqueous solution of preset concentration on the surface of the test plate is scraped off.

[0047] (b) The halogen inorganic perovskite quantum dot CsPbX3 solution prepared by spin coating, drop coating or scraping is applied to the surface of the test plate, dried, and then a preset volume of deionized water is drop coated. After the anion exchange reaction is fully completed, the degree of blue shift of the PL spectrum of the test plate is detected, and the crack / hole depth-PL spectrum blue shift degree fitting curve is plotted and fitted according to the corresponding depth of the crack.

[0048] (c) Figure 2 As shown, the surface of the thermal barrier coating is cleaned with clean water, and after drying, a salt solution of a preset concentration is dripped on the surface of the coating (the mass of the chloride ion compound aqueous solution per unit area is controlled at 0.001 mg / cm 2 ~10.0mg / cm 2 ), heat evaporated to dryness, and then drop coated with CsPbBr3 quantum dots dispersed in a non-polar solvent at a preset concentration (the mass of quantum dots per unit area was controlled at 0.04 mg / cm 2 ~2.5mg / cm 2), the quantum dots then diffuse evenly into the interior of the coating. After the quantum dot solution on the surface of the coating is dried, the surface of the coating shows green photoluminescence under ultraviolet light. Then, a preset volume of water is dripped on the surface of the coating. The water will penetrate into the interior of the coating along the holes and cracks of the coating, dissolving the chloride ions to form a chloride ion compound aqueous solution. The ionic chlorine element can be in-situ exchanged with the perovskite CsPbBr3 quantum dots there, and blue luminescence appears at the holes and cracks. After the surface aqueous solution is thermally evaporated, the PL spectrum of the halogen inorganic perovskite quantum dot CsPbX3 solution is detected; the blue area is the area of ​​the crack, and the depth of the crack at different positions is obtained by fitting the curve according to the depth of the blue at different positions of the crack and the degree of blue shift of the crack / hole depth-PL spectrum, and the detection of cracks in the thermal barrier coating is completed. The bluer the blue spectrum, the more chloride ions have penetrated into the position, that is, the deeper the holes and cracks; the larger the blue luminescence range, the larger the holes and cracks at the position. The PL spectrum experimental data of the thermal barrier coating treated in Example 1 is compared with the PL spectrum experimental data of the preset test plate, thereby quantitatively monitoring the holes and cracks in the coating.

[0049]

[0050] 1) Preparation of CsPbBr3 quantum dots

[0051] (1) Preparation of cesium oleate precursor solution

[0052] Cs2CO3 (0.305 g), ODE (10 mL) and OA (1 mL) were placed in a 50 mL three-necked flask, dried under vacuum at room temperature for 30 minutes, and then stirred under vacuum at 120°C for 40 minutes. The mixture was then heated under N2 for 1 hour until all Cs2CO3 was dissolved. If the yield needs to be increased, the ratio can be increased.

[0053] (2) Synthesis of CsPbBr3 quantum dots

[0054] PbBr2 (0.2 g), ODE (10 mL), OA (1 mL), and OAm (1 mL) were added to a 50 mL three-necked flask, vacuum dried at room temperature for 30 minutes, and then stirred at 120 ° C for 40 minutes. Then, the mixture was stirred at 120 ° C for 45 minutes under N2. After that, the temperature was raised to (150 ° C-180 ° C) and stirred for 10 minutes; then, 2 mL of the prepared cesium oleate precursor was immediately injected and reacted for 5 seconds, and then immediately cooled to room temperature with ice water. If you need to increase the yield, you can increase it according to the ratio.

[0055] (3) Extraction and cleaning of CsPbBr3 quantum dots

[0056] The crude reaction solution is mixed with the methyl acetate solution in a ratio of 1:1, centrifuged at 8000 rpm for 5 minutes, and the precipitate is dispersed with non-polar solvents such as n-hexane, toluene, and n-octane. The dispersion is mixed with methyl acetate in a ratio of 1:3, centrifuged at 8000 rpm for 5 minutes, and the precipitate is dispersed with inorganic solvents such as n-hexane, toluene, and n-octane. This process can be repeated several times to clean the oily ligands on the surface of the quantum dots. The final quantum dots are dispersed in non-polar solvents such as n-hexane, toluene, and n-octane for storage. The dispersion concentration range is (0.1 mg / ml to 50 mg / ml). When used, the quantum dots are centrifuged and the precipitate is dispersed with n-hexane.

[0057] 2) Thermal barrier coating test sample pretreatment

[0058] Pretreatment 1: Apply a certain concentration of CsPbBr3 quantum dots dispersed in a non-polar solvent to the coating surface, then apply or drip a certain concentration of salt water, wait for a few seconds, complete the anion exchange process, and heat evaporate the surface water. The coating test sample is prepared. The specific process is shown in Figure 2 shown.

[0059] 3) Test system construction

[0060] The test system includes an integrating sphere, a spectrometer, an excitation light source (the spectrum range of the excitation light source is 200nm to 405nm, and the excitation light source includes an LED light source, a laser light source, and an ultraviolet mercury lamp), a computer, and a fiber optic lamp component. The specific structure of the system is shown in Figure 3 The prepared test sample is illuminated by an excitation light source, and the photoluminescence signal generated by the test sample is collected by a spectrometer.

[0061] 4) Spectral data collection preprocessing

[0062] The spectrum software is used to perform background subtraction on the excitation light source, and the spectrum data obtained is only the sample photoluminescence data. The integration time for collecting the spectrum signal is selected to be (1ms~1000ms).

[0063] 5) Quantitative analysis of spectral data

[0064] The spectrum signal collected by the spectrometer is analyzed, and the degree of salt spray corrosion of the coating sample can be quantitatively monitored by the degree of blue shift of the spectrum peak. The preset test plate is treated with different salt concentrations according to Example 1 to simulate different degrees of salt spray corrosion, and the following is obtained: Figure 5 The data shown can further quantitatively establish the mathematical model relationship between the spectrum and the salt concentration (the degree of salt spray corrosion of the preset test board). By corroding the preset test board for different time periods (0 to 640 hours), combined with the scanning electron microscope photos, the data model of crack depth and corrosion time is obtained, such as Figure 6The halogen inorganic perovskite quantum dot CsPbX3 solution was prepared by spin coating, drop coating or scraping on the surface of the preset test plates with different crack depths, and then the PL spectrum of the test plate was detected after the anion exchange reaction was fully completed to obtain the different corrosion time-PL spectrum data model (see Figure 7 ) as shown.

[0065] 6) Surface spectrum scanning method

[0066] Face scanning test system Figure 8 As shown, the excitation light source irradiates the entire surface of the test sample, and the signal collected by the integrating sphere is all the photoluminescence signals of the entire sample surface. The diameter of the integrating sphere used in this method is 30cm to 50cm.

[0067] 7) Point spectrum scanning method

[0068] Point scanning method test system Fig. 9 As shown, the scanning system can be electro-optical scanning and mechanical scanning. The scanning time is adjusted according to the integration time. An ultraviolet laser light source is used as the excitation light source, and the light source spot diameter can be set to 500nm to 2cm according to the specific details to be scanned. The diameter of the integrating sphere used is (10cm to 15cm).

[0069] Embodiment 2:

[0070] The difference between this embodiment and embodiment 1 lies in the order of applying salt water to the thermal barrier coating test sample. CsPbBr3 quantum dots dispersed in a non-polar solvent with a preset concentration are applied to the coating surface, dried, and then salt water with a preset concentration is applied to the coating surface. After waiting for a few seconds, the anion exchange process is completed, and the salt water that is not dried on the surface is thermally evaporated to dryness. The coating test sample is prepared.

[0071] The specific operation process is as follows:

[0072] (1) A test plate is provided, cracks and holes of different preset depths are formed on the surface of the test plate, and then a chloride ion compound aqueous solution of preset concentration is introduced into the cracks, and excess chloride ion compound aqueous solution of preset concentration on the surface of the test plate is scraped off and dried.

[0073] (2) The halogen inorganic perovskite quantum dot CsPbX3 solution prepared by spin coating, drop coating or scraping is applied on the surface of the test plate, dried, and then a preset volume of deionized water is drop coated. After the anion exchange reaction is fully completed, the degree of blue shift of the PL spectrum of the test plate is detected, and the crack / hole depth-PL spectrum blue shift degree fitting curve is plotted and fitted according to the corresponding depth of the crack.

[0074] (3) Figure 3As shown, the surface of the thermal barrier coating is cleaned with clean water, and after drying, a preset concentration of perovskite CsPbBr3 quantum dots (the mass of quantum dots per unit area is controlled at 0.04 mg / cm 2 ~2.5mg / cm 2 ), the quantum dots then diffuse evenly into the coating. After the quantum dot solution on the coating surface is dried, the coating surface shows green photoluminescence under ultraviolet light. Then, a chloride ion compound aqueous solution of preset concentration (the mass of the chloride ion compound aqueous solution per unit area is controlled at 0.001 mg / cm 2 ~10.0mg / cm 2 ), the salt water will penetrate into the coating along the holes and cracks of the coating, and then the excess chloride ion compound aqueous solution of preset concentration will be scraped off the surface. After a few seconds, the chloride ions that reach the holes and cracks will exchange in situ with the perovskite CsPbBr3 quantum dots there, and blue light will appear at the holes and cracks. After the chloride ion compound aqueous solution is evaporated to dryness, the PL spectrum of the halogen inorganic perovskite quantum dot CsPbX3 solution is detected; the blue area is the area of ​​the crack, and the depth of the crack at different positions is obtained by fitting the curve according to the depth of the blue at different positions of the crack and the degree of blue shift of the crack / hole depth-PL spectrum, so as to complete the detection of cracks in the thermal barrier coating. The bluer the blue spectrum, the more chloride ions have penetrated into the position, that is, the deeper the holes and cracks; the larger the blue light emission range, the larger the holes and cracks at the position. The PL spectrum experimental data of the thermal barrier coating treated in Example 1 is compared with the PL spectrum experimental data of the preset test plate, thereby quantitatively monitoring the holes and cracks in the coating.

[0075] Embodiment 3:

[0076] The difference between this embodiment and embodiment 1 is that the thermal barrier coating test sample does not need to be cleaned and pre-treated. A standard sample with a known crack depth is set, and CsPbBr3 quantum dots dispersed in a non-polar solvent with a preset concentration are dripped on the surface of the standard sample and the thermal barrier coating test sample. Then, a preset volume of water is dripped on the coating surface. After waiting for a few seconds, the anion exchange process is completed, and the water on the surface that has not dried is thermally evaporated to dryness. The coating test sample is prepared. The specific process is shown in Figure 4 shown.

[0077] The specific operation process is as follows:

[0078] (1) A plurality of test plates are provided, cracks and holes of different preset depths are formed on the surfaces of the test plates, and then a chloride ion compound aqueous solution of preset concentration is introduced into the cracks, and excess chloride ion compound aqueous solution of preset concentration on the surfaces of the test plates is scraped off.

[0079] (2) The prepared halogen inorganic perovskite quantum dot CsPbX3 solution was spin-coated, drip-coated or scraped onto the surface of the test plate, dried, and then drip-coated with a preset volume of deionized water. After the anion exchange reaction was fully completed, the degree of blue shift of the PL spectrum of the test plate was detected, and several crack / hole depth-PL spectrum blue shift degree fitting curves were plotted and fitted according to the corresponding depth of the crack.

[0080] (3) Figure 4 As shown in the figure, a standard sample with a known crack depth is set, and the thermal barrier coating is arranged as follows: the surface is not cleaned with water, and CsPbBr3 quantum dots dispersed in a non-polar solvent with a preset concentration are directly dripped (the mass of quantum dots per unit area is controlled at 0.04 mg / cm 2 ~2.5mg / cm 2 ), the quantum dots then diffuse evenly into the coating. After the quantum dot solution on the coating surface is dried, the coating surface shows green photoluminescence under ultraviolet light. Then, a preset volume of water is dripped on the coating surface, and the water will penetrate into the coating along the holes and cracks of the coating, dissolving the chloride ions remaining in the thermal barrier coating due to its own salt spray corrosion and forming a chloride ion compound aqueous solution. The ionic chlorine element can be in situ exchanged with the perovskite CsPbBr3 quantum dots there, and blue light appears in the holes and cracks. After the surface is hydrothermally evaporated, the PL spectrum of the halogen inorganic perovskite quantum dot CsPbX3 solution is detected; the closest crack / hole depth-PL spectrum blue shift degree fitting curve is obtained according to the standard standard sample with known crack depth, and then the blue area on the thermal barrier coating is the area of ​​the crack, and the depth of the crack at different positions is obtained according to the depth of the blue at different positions of the crack and the blue shift degree fitting curve of the crack / hole depth-PL spectrum, and the crack detection of the thermal barrier coating is completed. The bluer the blue spectrum, the more chloride ions have penetrated into the location, that is, the deeper the holes and cracks are; the larger the blue luminescence range, the larger the holes and cracks are at that location. The PL spectrum experimental data of the thermal barrier coating treated in Example 3 is compared with the PL spectrum experimental data of the preset test plate, thereby quantitatively monitoring the holes and cracks in the coating.

Claims

1. A nondestructive testing method for thermal barrier coatings based on perovskite quantum dots, characterized in that: The following steps are involved: Step 1, preparing a halogen inorganic perovskite quantum dot CsPbBr3 solution and an aqueous solution of a chloride ion compound with a preset concentration; Step 2: Setting a test plate, forming holes and cracks of known depth and width on the surface of the test plate, then pouring the chloride ion compound aqueous solution of the preset concentration into the holes and cracks, scraping off the excess chloride ion compound aqueous solution of the preset concentration on the surface of the test plate, and drying; Step 3: Spin-coat, drop-coat or scrape-coat the prepared halogen inorganic perovskite quantum dot CsPbBr3 solution on the surface of the test plate, dry it, then drop-coat a preset volume of deionized water, wait for the anion exchange reaction to be fully completed, and then evaporate it to dryness, detect the degree of blue shift of the PL spectrum of the test plate, and draw and fit the blue shift degree fitting curve of the crack / hole depth-PL spectrum according to the corresponding depth of the crack; Step 4: Detect the area and depth of holes and cracks in the thermal barrier coating using a halogen inorganic perovskite quantum dot CsPbBr3 solution: The specific steps are as follows: Use clean water to clean the surface of the thermal barrier coating, dry it and apply the chloride ion compound aqueous solution of the preset concentration, then scrape off the excess chloride ion compound aqueous solution of the preset concentration on the surface, dry it, then apply the halogen inorganic perovskite quantum dot CsPbBr3 solution, dry it, then drip a preset volume of deionized water, wait for the anion exchange to fully react and evaporate it, and then detect the PL spectrum of the halogen inorganic perovskite quantum dot CsPbBr3 solution; the blue area is the area of ​​the holes and cracks, and the depth of the holes and cracks at different positions is obtained by fitting the curve according to the depth of the blue at different positions of the holes and cracks and the degree of blue shift of the crack / hole depth-PL spectrum, so as to complete the detection of the thermal barrier coating; Or the specific steps are as follows: Use clean water to clean the surface of the thermal barrier coating, apply the halogen inorganic perovskite quantum dot CsPbBr3 solution after drying, dry it, then drip the chloride ion compound aqueous solution of the preset concentration, then scrape off the excess chloride ion compound aqueous solution of the preset concentration on the surface, wait for the anion exchange to fully react and evaporate to dryness, and then detect the PL spectrum of the halogen inorganic perovskite quantum dot CsPbBr3 solution; the blue area is the area of ​​the holes and cracks, and the depth of the empty holes and cracks at different positions is obtained by fitting the curve according to the depth of the blue at different positions of the holes and cracks and the degree of blue shift of the crack / hole depth-PL spectrum, so as to complete the detection of the thermal barrier coating; Or the specific steps are as follows: Steps 1 to 3 select aqueous solutions of chloride ion compounds with different preset concentrations to obtain fitting curves of the blue shift degree of the crack / hole depth-PL spectrum of the corresponding test plate; the steps of step 4 are as follows: The thermal barrier coating is arranged as follows: the surface is not cleaned with water, and the halogen inorganic perovskite quantum dot CsPbBr3 solution is directly applied, dried, and then water is dripped on the surface of the thermal barrier coating. The water penetrates into the thermal barrier coating along the holes and cracks of the coating, dissolves the chloride ions in the cracks and holes of the thermal barrier coating, and forms a chloride ion compound aqueous solution. The chloride ions are fully exchanged with the perovskite CsPbBr3 quantum dots in situ and then evaporated to dryness, and then the PL spectrum of the halogen inorganic perovskite quantum dot CsPbBr3 solution is detected; the blue area is the area of ​​the holes and cracks; Then, according to the crack depth and blue shift degree of the test plate, the crack / hole depth-PL spectrum blue shift degree fitting curve of the chloride ion compound aqueous solution with the preset concentration closest to the concentration of the chloride ion compound aqueous solution in the thermal barrier coating is selected as the reference crack / hole depth-PL spectrum blue shift degree fitting curve of the thermal barrier coating, and the depth of the holes and cracks at different positions is obtained according to the depth of blue at different positions of the holes and cracks to complete the detection of the thermal barrier coating.

2. The nondestructive testing method for thermal barrier coatings based on perovskite quantum dots according to claim 1, characterized in that: The PL spectrum of the halogen inorganic perovskite quantum dot CsPbBr3 solution is detected by a test system and a spectrum data acquisition system; the test system includes an excitation light source and an integrating sphere, the integrating sphere is connected to a spectrometer, the spectrometer is connected to a computer, and the spectrum data acquisition system in the computer excites the light source to perform background subtraction processing, so that the obtained spectrum data is only the photoluminescence data of the sample.

3. The nondestructive testing method for thermal barrier coatings based on perovskite quantum dots according to claim 2, characterized in that: The spectral range of the excitation light source is 200nm to 405nm; when detecting the PL spectrum of the halogen inorganic perovskite quantum dot CsPbBr3 solution, a surface spectrum scanning method or a point spectrum scanning method is adopted; when the surface spectrum scanning method is adopted, the diameter of the integrating sphere is 30cm to 50cm, and when the point spectrum scanning method is adopted, the diameter of the integrating sphere is 10cm to 15cm.

4. The nondestructive testing method for thermal barrier coatings based on perovskite quantum dots according to claim 1, characterized in that: The chloride ion compound aqueous solution includes sodium chloride solution, potassium chloride solution, calcium chloride solution and magnesium chloride solution.

5. The nondestructive testing method for thermal barrier coatings based on perovskite quantum dots according to claim 1, characterized in that: The preparation method of the halogen inorganic perovskite quantum dot CsPbBr3 solution is as follows: (1) Preparation of cesium oleate precursor solution Cs2CO3, ODE and OA were mixed, vacuum dried at room temperature, and then vacuum stirred at 120°C for 40 minutes, and then the mixture was heated for 1 hour under N2 atmosphere until all Cs2CO3 was dissolved to obtain a cesium oleate precursor solution; wherein the mass volume ratio of Cs2CO3 to ODE was 0.0305:10 g / ml to 3.305:10 g / ml, and the mass volume ratio of Cs2CO3 to OA was 0.0305:1 g / ml to 0.305:1 g / ml; (2) Synthesis of CsPbBr3 quantum dots PbBr2, ODE, OA and OAm were mixed, vacuum dried at room temperature for 30 minutes, and then vacuum stirred at 120°C for 40 minutes. Then, in a N2 atmosphere, the mixture was stirred at 120°C for 45 minutes, and then the temperature was raised to 150°C-180°C and stirred for 10 minutes. Then, the cesium oleate precursor solution was immediately injected and reacted for 5 seconds, and then immediately cooled to room temperature with ice water to obtain a crude reaction solution of CsPbBr3 quantum dots. The mass volume ratio of PbBr2 to ODE, OA, OAm and cesium oleate precursor solution was 0.01:1:0.1:0.1:0.2 g / ml to 2:100:10:10:20 g / ml. (3) Extraction and cleaning of CsPbBr3 quantum dots The crude reaction solution and the methyl acetate solution are mixed at a volume ratio of 1:1 to 1:3, and the mixture is centrifuged at 8000 rpm for 3 to 5 minutes. The precipitate is dispersed with a non-polar solvent, and the volume ratio of the non-polar solvent to methyl acetate is 1:3; the mixture is centrifuged at 8000 rpm for 3 to 5 minutes, and the precipitate is dispersed with a non-polar solvent; the washing is repeated until the oily ligands on the surface of the halogen inorganic perovskite quantum dots CsPbBr3 are cleaned, and the cleaned halogen inorganic perovskite quantum dots are dispersed in a non-polar solvent for storage to obtain a storage solution with a concentration of 0.1 mg / ml to 50 mg / ml. When using the storage solution, the storage solution is centrifuged, and then the precipitate is dispersed with n-hexane to obtain a halogen inorganic perovskite quantum dot CsPbBr3 solution with a concentration of 0.1 mg / ml to 50 mg / ml.

6. The nondestructive testing method for thermal barrier coatings based on perovskite quantum dots according to claim 1, characterized in that: The depth and width of the cracks and holes of the test board in step 2 are obtained through scanning electron microscope photos, or are set during prefabrication.

7. The nondestructive testing method for thermal barrier coatings based on perovskite quantum dots according to claim 1, characterized in that: The method further comprises the step of obtaining the degree of erosion of the thermal barrier coating according to the area of ​​the halogen inorganic perovskite quantum dot CsPbBr3 solution spin-coated on the surface of the thermal barrier coating and the total volume occupied by the cracks: c=a / b, wherein a is the total volume occupied by the cracks, in units of cm 3 , b is the area of ​​the thermal barrier coating surface spin-coated with the halogen inorganic perovskite quantum dot CsPbBr3 solution, unit is cm 2 , c is the degree of erosion of the thermal barrier coating, that is, the average eroded thickness of the thermal barrier coating, in cm; a is obtained by the following method: the actual area represented by each pixel is obtained, and then multiplied by the actual depth of the pixel to obtain the volume corresponding to each pixel, and the total volume occupied by the crack is obtained by accumulating them.