Samarium cobalt magnet and its preparation method and use of nickel

By introducing an appropriate amount of nickel into the Sm2Co17 samarium-cobalt magnet, the Fe2NiO5 crystal phase is solved, and the corrosion resistance and magnetic properties of the samarium-cobalt magnet are improved balanced.

CN115458266BActive Publication Date: 2024-11-19BAOTOU TIANHE MAGNETICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211270603.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-18
Publication Date
2024-11-19
Estimated Expiration
2042-10-18

AI Technical Summary

Technical Problem

Sm2Co17 samarium-cobalt magnets are easy to combine with oxygen elements, resulting in corrosion and attenuation of magnetic properties. The existing magnet materials have poor magnetic properties when improving corrosion resistance.

Method used

By introducing an appropriate amount of nickel into the Sm2Co17 samarium-cobalt magnet, the Fe2NiO5 crystal phase is formed, the inter-crystal structure of the main phase is changed, the surface dense oxide layer is enhanced, and the corrosion resistance is improved. At the same time, the nickel content is controlled between 1.2-2.3 wt% to balance the magnetic properties. Ability and corrosion resistance.

Benefits of technology

The corrosion resistance of samarium-cobalt magnets is significantly improved, and the reduction in magnetic properties is small, achieving a perfect balance between magnetic properties and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003895003290000131
    Figure BDA0003895003290000131
  • Figure BDA0003895003290000141
    Figure BDA0003895003290000141
Patent Text Reader

Abstract

The invention discloses a samarium cobalt magnet and a preparation method thereof and the use of nickel. The samarium cobalt magnet of the invention is Sm2Co 17 A samarium cobalt magnet, comprising Sm, Co, Fe, Ni and M; wherein M is selected from one or more of Cu and Zr; the magnetic property-corrosion resistance equilibrium constant I of the samarium cobalt magnet satisfies the following formula: 0.01
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a samarium cobalt magnet and a preparation method thereof, and also relates to a use of nickel. Background Art

[0002] Sm2Co 17 The iron element in the Sm2Co magnet is easy to combine with the oxygen element, causing the magnet to rust and corrode, and causing pits on the surface of the magnet and other undesirable conditions. 17 If the samarium cobalt magnet is corroded or its structure is destroyed, the magnetic properties will be weakened or even disappear, which will affect the service life and magnetic properties of the matrix.

[0003] CN105427984A discloses a composition of Sm(Co bal Fe 0.3 Cu 0.043 Zr 0.03 ) z A magnet, wherein z is 7.60 to 8.06. The magnet does not contain Ni, resulting in poor corrosion resistance. CN1089385A discloses a magnet composed of (R 1-x R' x ) α (Fe 1-y M y ) β C γ The rare earth-iron-permanent magnetic carbide has poor magnetic properties due to its high carbon content. CN109243745A discloses a single crystal magnetic powder, the composition of which is expressed in atomic percentage: R a T 100-a-b-c-d-v M1 b Cu c Zn d N v ; wherein R is Sm or a combination of rare earth elements other than Sm, T is iron or iron and cobalt, and M1 is at least one of Si, Al, Ni, Ti, V, Cr, Zr, Hf, Nb, Ta, Mn, Mo and W. The magnetic powder has a high nitrogen content, resulting in poor magnetic properties. In addition, CN112225539A discloses a corrosion-resistant cobalt-based material containing Li, which results in poor magnetic properties and does not belong to a magnetic material. Summary of the invention

[0004] An object of the present invention is to provide a samarium cobalt magnet having a higher degree of improved corrosion resistance and a lesser degree of reduced magnetic properties, and having a perfect balance between corrosion resistance and magnetic properties.

[0005] Another object of the present invention is to provide a method for preparing a samarium cobalt magnet.

[0006] Another object of the present invention is to provide a use of nickel in improving the corrosion resistance of samarium cobalt magnets, which can greatly improve the corrosion resistance of samarium cobalt magnets and reduce the magnetic properties to a small extent, so that the corrosion resistance and magnetic properties of the samarium cobalt magnets achieve a perfect balance.

[0007] The present invention achieves the above technical objectives through the following technical means.

[0008] In one aspect, the present invention provides a samarium cobalt magnet, wherein the samarium cobalt magnet is Sm2Co 17 A samarium cobalt magnet comprising Sm, Co, Fe, Ni and M; wherein M is selected from one or more of Cu and Zr;

[0009] The magnetic property-corrosion resistance equilibrium constant I of the samarium cobalt magnet satisfies the following formula:

[0010] 0.01 <I≤0.079;

[0011] Among them, the magnetic properties-corrosion resistance equilibrium constant I = (α + γ) / β;

[0012] Where, α = (Br0-Br1) / Br0;

[0013] Br1 is the remanence of the samarium cobalt magnet, in kGs;

[0014] Br0 is the remanence of a nickel-free magnet formed by replacing Ni in the samarium cobalt magnet with Fe, in kGs;

[0015] Where, γ = (Hcj0-Hcj1) / Hcj0;

[0016] Hcj1 is the coercive force of the samarium cobalt magnet, in kOe;

[0017] Hcj0 is the coercive force of a nickel-free magnet formed by replacing Ni in the samarium cobalt magnet with Fe, in kOe;

[0018] Where, β = (X0-X1) / X0;

[0019] X1 is the number of rust spots on the samarium cobalt magnet after the HAST test;

[0020] X0 is the number of rust spots on a nickel-free magnet formed by replacing Ni in the samarium-cobalt magnet with Fe after a HAST test.

[0021] According to the samarium cobalt magnet of the present invention, preferably, the samarium cobalt magnet does not contain C, N and Li.

[0022] According to the samarium cobalt magnet of the present invention, preferably, the content of Ni is 1.2-2.3 wt %.

[0023] According to the samarium cobalt magnet of the present invention, preferably, the content of Ni is 1.8-2.1 wt %.

[0024] According to the samarium cobalt magnet of the present invention, preferably, the content of Fe is 15.0-16.5 wt %.

[0025] According to the samarium cobalt magnet of the present invention, preferably, the content of Fe is 15.5-16.0 wt %.

[0026] According to the samarium cobalt magnet of the present invention, preferably, the content of Sm is 20-30wt%, the content of Co is 45-55wt%, and the content of M is 5-15wt%.

[0027] According to the samarium cobalt magnet of the present invention, preferably, the samarium cobalt magnet contains Fe2NiO5 crystal phase.

[0028] On the other hand, the present invention provides a method for preparing the above-mentioned samarium cobalt magnet, comprising the following steps:

[0029] (1) providing a magnet raw material according to the magnet component, and melting the magnet raw material to form a master alloy from the melted magnet raw material;

[0030] (2) crushing the master alloy obtained by smelting into alloy powder;

[0031] (3) mixing alloy powders;

[0032] (4) Under the action of an oriented magnetic field, the mixed alloy powder is pressed into a green body, and then isostatically pressed to form a green body;

[0033] (5) Sintering the green body and performing solid solution treatment to form a sintered magnet;

[0034] (6) The sintered magnet is subjected to aging treatment to obtain a samarium cobalt magnet.

[0035] In another aspect, the present invention provides a use of nickel in improving the corrosion resistance of samarium cobalt magnets, wherein the samarium cobalt magnets are Sm2Co 17 A samarium cobalt magnet comprising Sm, Co, Fe, Ni and M; and a magnetic property-corrosion resistance equilibrium constant of 0.01 <I≤0.079;

[0036] Wherein, M is selected from one or more of Cu and Zr; the content of Ni is 0.1 to 5 wt%;

[0037] Among them, the magnetic properties-corrosion resistance equilibrium constant I = (α + γ) / β;

[0038] Where, α = (Br0-Br1) / Br0;

[0039] Br1 is the remanence of the samarium cobalt magnet, in kGs;

[0040] Br0 is the remanence of a nickel-free magnet formed by replacing Ni in the samarium cobalt magnet with Fe, in kGs;

[0041] Where, γ = (Hcj0-Hcj1) / Hcj0;

[0042] Hcj1 is the coercive force of the samarium cobalt magnet, in kOe;

[0043] Hcj0 is the coercive force of a nickel-free magnet formed by replacing Ni in the samarium cobalt magnet with Fe, in kOe;

[0044] Where, β = (X0-X1) / X0;

[0045] X1 is the number of rust spots on the samarium cobalt magnet after the HAST test;

[0046] X0 is the number of rust spots on a nickel-free magnet formed by replacing Ni in the samarium-cobalt magnet with Fe after a HAST test.

[0047] Nickel can change Sm2Co 17 The main phase intergranular structure of the samarium cobalt magnet is expanded and proliferated by the Fe2NiO5 phase, which causes the crystal phase to precipitate and harden, and produces a pinning effect on the cell wall, thereby improving the corrosion resistance of the samarium cobalt magnet. However, too much or too little nickel will seriously affect the magnetic properties of the samarium cobalt magnet. When the nickel content in the samarium cobalt magnet is within a certain range, a dense nickel oxide can be formed on the surface of the samarium cobalt magnet to improve the corrosion resistance, while having little effect on the magnetic properties, thereby achieving a perfect balance between the magnetic properties and corrosion resistance. DETAILED DESCRIPTION

[0048] The present invention is further described below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited thereto.

[0049] The "remanent magnetism" mentioned in the present invention refers to the value of the magnetic flux density corresponding to the point where the magnetic field intensity is zero on the saturation hysteresis loop, usually denoted as Br, and the unit is Tesla (T) or Gauss (Gs). 1Gs = 0.0001T.

[0050] The "coercive force" mentioned in the present invention, also called intrinsic coercive force, refers to the magnetic field intensity when the magnetic field is monotonically reduced to zero and then increased in the opposite direction from the saturated magnetization state of the magnet, so that the magnetization intensity decreases to zero along the saturation hysteresis loop, usually recorded as Hcj, and the unit is Oersted (Oe) or Ampere / meter (A / m). 1Oe = 79.6A / m.

[0051] The "inert atmosphere" of the present invention refers to an atmosphere that does not react with the magnet and does not affect its magnetism. In the present invention, the "inert atmosphere" includes an atmosphere formed by an inert gas (helium, neon, argon, krypton, xenon).

[0052] The "vacuum" mentioned in the present invention refers to absolute vacuum; the smaller the value, the higher the vacuum. The vacuum of the present invention is less than or equal to 0.1Pa, preferably less than or equal to 0.01Pa, and more preferably less than or equal to 0.001Pa.

[0053] The "average particle size" in the present invention refers to D 50 Particle size refers to the equivalent diameter of the largest particle when the cumulative distribution in the particle size distribution curve is 50%.

[0054] <Samarium Cobalt Magnet>

[0055] The samarium cobalt magnet of the present invention is Sm2Co 17 The samarium cobalt magnet of the present invention may include Sm, Co, Fe, Ni and M. M may be selected from Cu or Zr. In some embodiments, the samarium cobalt magnet is composed of Sm, Co, Fe, Ni and M. Of course, there may be inevitable impurities in the samarium cobalt magnet. In some embodiments, the samarium cobalt magnet of the present invention does not contain C, N and alkali metal elements (such as Li). In this way, the samarium cobalt magnet of the present invention can be clearly distinguished from the prior art.

[0056] In the samarium cobalt magnet of the present invention, the mass percentage of Sm can be represented by a, the mass percentage of Co can be represented by b, the mass percentage of Fe can be represented by c, the mass percentage of Ni can be represented by d, and the mass percentage of M can be represented by e. The above mass percentages are all based on the total weight of the samarium cobalt magnet.

[0057] The mass percentage a of Sm can be 20-30wt%; preferably, the mass percentage a of Sm is 22-27wt%; more preferably, the mass percentage a of Sm is 25-26.5wt%. In this way, both the magnetic properties and corrosion resistance of the samarium cobalt magnet can be taken into account.

[0058] The mass percentage b of Co may be 45-55wt%; preferably, the mass percentage b of Co may be 46-52wt%; more preferably, the mass percentage b of Co may be 47-50wt%. In this way, both the magnetic properties and corrosion resistance of the samarium cobalt magnet can be taken into consideration.

[0059] The Fe content also affects the performance of the samarium cobalt magnet. The Fe mass percentage c can be 15.0-16.5wt%; preferably, the Fe mass percentage c is 15.5-16.0wt%. More preferably, the Fe mass percentage c is 15.6-15.8wt%. This can make the samarium cobalt magnet have higher magnetic properties and higher corrosion resistance.

[0060] The present invention has found that the Ni content has a great influence on the performance of samarium cobalt magnets. Although an increase in Ni content will improve the corrosion resistance of samarium cobalt magnets, too much Ni will cause the magnetic properties to decrease a lot. The mass percentage d of Ni in the present invention can be 1.2-2.3wt%. Preferably, the mass percentage d of Ni is 1.8-2.1wt%; more preferably, the mass percentage d of Ni is 1.9-2.0wt%. When the Ni content is lower than 1.2wt%, the improvement in corrosion resistance is lower, and the magnetic properties are also reduced, resulting in poor overall performance of the samarium cobalt magnet; when the Ni content is higher than 2.3wt%, although the corrosion resistance is improved, the magnetic properties are reduced too much, resulting in poor overall performance of the samarium cobalt magnet. The addition of an appropriate amount of Ni can make Sm2Co 17 The Fe2NiO5 crystal phase is formed in the Sm2Co magnet to improve the corrosion resistance of the magnet. 17 The surface of the SmCo magnet forms a dense nickel oxide, which improves the corrosion resistance of the magnet. Such a nickel content can achieve a perfect balance between the magnetic properties and corrosion resistance of the SmCo magnet.

[0061] The mass percentage e of M is greater than 0. Preferably, the mass percentage e of M can be 5 to 15 wt%; preferably, the mass percentage e of M is 6 to 13 wt%; more preferably, the mass percentage e of M is 8.5 to 9.5 wt%. According to one embodiment of the present invention, M is a combination of Cu and Zr. This can make Sm2Co 17 The samarium cobalt magnet has good magnetic properties and corrosion resistance. The content of Cu can be 4-10wt%, preferably 5-8wt%, more preferably 5.5-6.5wt%. The content of Zr can be 2-7wt%, preferably 2.5-5wt%, more preferably 2.7-3.5wt%.

[0062] The present invention uses the magnetic property-corrosion resistance balance constant I to measure the comprehensive performance of the samarium cobalt magnet. Generally speaking, the smaller the balance constant I, the less the magnetic property decreases, the more the corrosion resistance increases, and thus the better the comprehensive performance. The present invention finds that the magnetic property-corrosion resistance balance constant I is very suitable for evaluating the comprehensive performance of the samarium cobalt magnet.

[0063] The magnetic property-corrosion resistance equilibrium constant I is calculated by the following formula:

[0064] I=(α+γ)β (1)

[0065] In formula (1), α=(Br0-Br1) / Br0. Br1 is the remanence of the samarium cobalt magnet of the present invention, in kGs. Br0 is the remanence of the nickel-free magnet formed by replacing Ni in the samarium cobalt magnet of the present invention with Fe, in kGs. The mass percentage of Sm in the nickel-free magnet is a, the mass percentage of Co is b, the mass percentage of Fe is (c+d), and the mass percentage of M is e. The remanence of the magnet is tested by the following method: the magnet is made into a standard sample column of D10×10mm, saturated magnetized, and the remanence is tested in the NIM-2000BHTracer detection system of the Chinese Academy of Scientific Metrology.

[0066] In formula (1), γ = (Hcj0-Hcj1) / Hcj0. Hcj1 is the coercive force of the samarium cobalt magnet of the present invention, and the unit is kOe. Hcj0 is the coercive force of the nickel-free magnet formed by replacing Ni in the samarium cobalt magnet of the present invention with Fe, and the unit is kOe. The mass percentage of Sm in the nickel-free magnet is a, the mass percentage of Co is b, the mass percentage of Fe is (c+d), and the mass percentage of M is e. The coercive force of the samarium cobalt magnet is tested by the following method: the magnet is made into a standard sample column of D10×10mm, saturated magnetized, and the coercive force is tested in the NIM-2000BHTracer detection system of the Chinese Academy of Scientific Metrology.

[0067] In formula (1), β=(X0-X1) / X0. X1 is the number of rust spots on the samarium cobalt magnet of the present invention after the HAST test. X0 is the number of rust spots on the nickel-free magnet formed by replacing Ni in the samarium cobalt magnet of the present invention with Fe after the HAST test. The mass percentage of Sm in the nickel-free samarium cobalt magnet is a, the mass percentage of Co is b, the mass percentage of Fe is (c+d), and the mass percentage of M is e. The test method of the HAST experiment is as follows: the magnet is made into a block sample of 40×40×4mm, and the sample is subjected to a HAST corrosion resistance test. The HAST test conditions are: temperature 130°C, humidity 95%, pressure 2.7atm, and time 72h.

[0068] The magnetic properties-corrosion resistance balance constant I represents the ratio of the reduction in the magnetic properties (remanence and coercive force) of the samarium cobalt magnet to the increase in the corrosion resistance of the magnet. The smaller the value of the magnetic properties-corrosion resistance balance constant I is, the smaller the reduction in the magnetic properties of the samarium cobalt magnet is, and the greater the increase in corrosion resistance is. At this time, the magnetic properties and corrosion resistance of the samarium cobalt magnet can achieve a perfect balance.

[0069] The magnetic property - corrosion resistance balance constant of the samarium - cobalt magnet of the present invention satisfies 0.01 < I ≤ 0.079; preferably, 0.02 < I ≤ 0.070; more preferably, 0.05 ≤ I ≤ 0.068. In this way, the magnetic property and corrosion resistance of the samarium - cobalt magnet can reach a perfect balance.

[0070] <Preparation method of samarium - cobalt magnet>

[0071] The preparation method of the samarium - cobalt magnet of the present invention comprises the following steps: (1) melting step; (2) powder - making step; (3) mixing step; (4) magnetic field forming and isostatic pressing step; (5) sintering and solution - forming step; (6) aging treatment step.

[0072] Melting steps

[0073] In the melting step, magnet raw materials are provided according to the magnet composition, and the magnet raw materials are melted to form a master alloy. To prevent the magnet raw materials and the master alloy obtained therefrom from being oxidized, the melting is preferably carried out in a vacuum or an inert atmosphere. The melting preferably adopts an ingot - casting process or a rapid - solidification sheet process. The ingot - casting process is to cool and solidify the melted magnet raw materials to form a master alloy. The rapid - solidification sheet process is to rapidly cool and solidify the melted magnet raw materials and spin them into a master alloy. The melting of the present invention can be carried out in a high - vacuum high - frequency induction furnace. The melting temperature can be 1100 - 1600 °C, preferably 1450 - 1500 °C. The thickness of the master alloy of the present invention can be 0.01 - 5 mm, preferably 0.1 - 1 mm, more preferably 0.25 - 0.35 mm; the oxygen content is below 2000 ppm, preferably below 1500 ppm, more preferably below 1200 ppm. According to a specific embodiment of the present invention, the magnet raw materials are mixed and melted, and after the melting is completed, it is kept warm at 1450 - 1460 °C for 3 - 5 min, and then poured into a mold and cooled to obtain a master alloy. The melting can be carried out in a vacuum high - frequency induction furnace.

[0074] Flour making steps

[0075] In the powder - making step, the master alloy obtained by melting is broken into alloy powders. To prevent the master alloy and the coarse powders and alloy powders obtained by breaking it from being oxidized, the powder - making is preferably carried out in a vacuum or an inert atmosphere. The powder - making process preferably includes the following coarse - crushing process and powder - grinding process. The coarse - crushing process is to break the master alloy into particles; the powder - grinding process is to grind the particles obtained by the coarse - crushing process into alloy powders.

[0076] The coarse crushing process can adopt a mechanical crushing process. The mechanical crushing process is to use a mechanical crushing device to crush the master alloy into particles; the mechanical crushing device can be selected from a jaw crusher or a hammer crusher. The coarse crushing process can be divided into two steps. The first step is to crush the master alloy into larger coarse particles, and then the coarse particles are further crushed into particles with smaller particle sizes. The average particle size of the coarse particles is less than 10 mm, preferably less than 8 mm, and more preferably less than 7 mm. The average particle size of the particles is less than 5 mm, preferably less than 2 mm, and more preferably less than 500 μm.

[0077] The grinding process adopts ball milling and / or air flow milling. The ball milling process is to use a mechanical ball milling device to crush the coarse powder into alloy powder. The mechanical ball milling device can be selected from a rolling ball mill, a vibrating ball mill or a high-energy ball mill. The air flow milling process is to use an air flow to accelerate the coarse powder and then collide with each other to break it. The air flow can be a nitrogen flow, preferably a high-purity nitrogen flow. The N2 content in the high-purity nitrogen flow can be above 99.0wt%, preferably above 99.9wt%. The pressure of the air flow can be 0.1-2.0MPa, preferably 0.5-1.0MPa, and more preferably 0.6-0.7MPa. The average particle size of the alloy powder obtained by the grinding process is 3-5μm, preferably 3.5-4.5μm, and more preferably 3.5-4μm. By adjusting the speed of the air flow mill sorting wheel, alloy powder of suitable particle size can be obtained.

[0078] Mixing steps

[0079] In the mixing step, the obtained alloy powder is further mixed to make the particle size of the powder more uniform. The mixing time can be 180 to 240 minutes, preferably 190 to 230 minutes, and more preferably 210 to 230 minutes.

[0080] Magnetic field forming and isostatic pressing steps

[0081] In the magnetic field forming and isostatic pressing steps, the mixed alloy powder is pressed into a green body under the action of an oriented magnetic field, and then isostatically pressed to form a green body. In order to prevent the mixture from being oxidized, the magnetic field forming and isostatic pressing steps are preferably performed in a vacuum or inert atmosphere.

[0082] The magnetic powder pressing process preferably adopts a mold pressing process. The orientation magnetic field direction and the magnetic powder pressing direction are parallel to each other or perpendicular to each other. There is no special restriction on the strength of the orientation magnetic field, which can be determined according to actual needs. According to a preferred embodiment of the present invention, the intensity of the orientation magnetic field is at least 1 Tesla (T), preferably at least 1.5T, and more preferably above 2T. The pressure can be above 3MPa, preferably above 3.5MPa, and more preferably above 5MPa. The density of the blank obtained by magnetic field molding can be 3.8-4.5g / cm 3, preferably 3.9 to 4.2 g / cm 3 .

[0083] The isostatic pressing process can be carried out in an isostatic press. The green body is wrapped in a plastic bag, evacuated, and then cold isostatically pressed in an isostatic press. The pressure can be 15-24 MPa, preferably 16-23 MPa, and more preferably 18-20 MPa. The pressing time can be 10-30 seconds, preferably 15-25 seconds. The density of the green body obtained in the isostatic pressing step can be 4.8-5.4 g / cm 3 , preferably 5 to 5.3 g / cm 3 .

[0084] Sintering and solutionizing steps

[0085] In the sintering and solutionizing step, the green body is sintered and shaped, and solutionized to form a sintered magnet. In order to prevent the green body from being oxidized, the sintering and solutionizing step is preferably carried out in a vacuum or inert atmosphere and in a vacuum sintering furnace. The vacuum degree of the sintering and solutionizing step can be less than 1.0 Pa, preferably less than 0.5 Pa, and more preferably less than 0.2 Pa. The sintering temperature can be 1100-1300°C, preferably 1150-1250°C, and more preferably 1210-1230°C; the sintering time can be 0.5-1h, preferably 0.6-1h, and more preferably 0.8-1h. The solutionizing temperature can be 1100-1300°C, preferably 1150-1250°C, and more preferably 1180-1200°C; the solutionizing time can be 2-6h, preferably 3-6h, and more preferably 3-5h. After the solutionizing treatment, the magnet is rapidly air-cooled to 20-30°C to form a sintered magnet.

[0086] Aging treatment steps

[0087] In order to prevent the sintered rare earth magnet from being oxidized, the aging treatment is preferably carried out in a vacuum or inert atmosphere. The temperature of the aging treatment can be 300-900°C, preferably 400-550°C; the time of the aging treatment can be 5-28h, preferably 8-26h, and more preferably 10-25h. According to one embodiment of the present invention, the sintered magnet is heated to 800-850°C, preferably 800-830°C; kept warm for 10-20h, preferably 10-15h; cooled to 350-450°C, preferably 350-400°C at 0.5-0.8°C / min, preferably 0.5-0.6°C / min; kept warm for 4-10h, preferably 5-8h; and air-cooled to 20-30°C to obtain a samarium cobalt magnet.

[0088] According to an embodiment of the present invention, a magnet raw material is formed into an alloy powder with uniform mixing; the alloy powder is oriented and formed in a magnetic field press to obtain a green body with a density of 3.8 - 4.5 g / cm 3 ; the green body is wrapped with a plastic bag, evacuated, and then subjected to cold isostatic pressing in an isostatic pressing device, pressed at 15 - 24 MPa for 10 - 30 s to obtain a green compact with a density of 4.8 - 5.4 g / cm 3 ; the green compact is placed in a vacuum sintering furnace, evacuated to a vacuum degree ≤ 0.2 Pa, gradually heated, sintered at 1210 - 1230 °C for 0.5 - 1 h, then cooled to 1200 - 1180 °C, solution-treated for 2 - 6 h, and rapidly air-cooled to 20 - 30 °C; heated to 800 - 850 °C, held for 10 - 20 h, cooled to 350 - 450 °C at 0.5 - 0.8 °C / min, held for 4 - 10 h, and air-cooled to 20 - 30 °C to obtain the samarium-cobalt magnet.

[0089] <Use of nickel>

[0090] The present invention provides a use of nickel in improving the corrosion resistance of samarium-cobalt magnets. The samarium-cobalt magnet is a Sm2Co 17 type magnet. Corrosion resistance refers to the ability of a metal material to resist the corrosive damage of the surrounding medium. In the present invention, corrosion resistance includes but is not limited to acid and alkali resistance, moisture resistance, and oxidation resistance. Preferably, the present invention provides a use of nickel in improving the moisture resistance of samarium-cobalt magnets.

[0091] The samarium-cobalt magnet of the present invention includes Sm, Co, Fe, Ni, and M, and its magnetic property-corrosion resistance balance constant satisfies the following formula: 0.01 < I ≤ 0.79. The samarium-cobalt magnet of the present invention includes Sm, Co, Fe, Ni, and M. Among them, M is selected from Cu or Zr. In some embodiments, the samarium-cobalt magnet is composed of Sm, Co, Fe, Ni, and M. Of course, unavoidable impurities may exist in the samarium-cobalt magnet. The samarium-cobalt magnet can be prepared by the following steps: (1) melting step; (2) powder making step; (3) mixing step; (4) magnetic field forming and isostatic pressing step; (5) sintering and solution treatment step; and (6) aging treatment step. The element composition and content of each element of the samarium-cobalt magnet, the value range of the magnetic property-corrosion resistance balance constant I, and the preparation process are as described above.

[0092] The following introduces the test methods for the samarium-cobalt magnets of the examples and comparative examples:

[0093] Magnetic properties: The samarium-cobalt magnet is made into a standard sample column of D10×10 mm, saturated magnetized, and the magnetic properties are tested in the NIM-2000BH Tracer detection system of the National Institute of Metrology, China.

[0094] HAST corrosion resistance test: The samarium cobalt magnet was made into a block sample of 40×40×4mm, and the sample was subjected to HAST corrosion resistance test. The test conditions were: temperature 130℃, humidity 95%, pressure 2.7atm, time 72h, and the number of rust spots on the sample surface was observed after the test.

[0095] Examples 1 to 2 and Comparative Examples 1 to 4

[0096] Melting: According to the formula in Table 1, the raw materials of samarium, cobalt, iron, copper, zirconium and nickel (if any) are melted in a high vacuum high frequency induction furnace. After the melting is completed, they are kept and refined at 1460°C for 5 minutes, then poured into a mold and cooled to obtain a samarium-cobalt alloy.

[0097] Powder making: The samarium-cobalt alloy is mechanically crushed into coarse particles of less than 10 mm (e.g. 7 mm) in a jaw crusher, and then crushed into particles of less than 5 mm (e.g. 500 μm), and then ground by high-pressure air flow grinding to obtain alloy powder with an average particle size of 3.5 μm.

[0098] Mixing: Mix the alloy powder for 210 minutes to make the particle size of the alloy powder more uniform.

[0099] Magnetic field forming and isostatic pressing: The mixed alloy powder is oriented and formed in a magnetic field press to obtain a density of 4g / cm 3 The green body was wrapped in a plastic bag, vacuumed, and then cold isostatically pressed in a high pressure isostatic pressing device, maintained at 20 MPa for 25 seconds, and a density of 5 g / cm 3 of the green body.

[0100] Sintering and solution treatment: Place the green body into a vacuum sintering furnace, evacuate to a vacuum degree of 0.1 Pa, gradually increase the temperature, keep it at 1220℃ for 1h, then cool it to 1180℃, solution treat it for 3h, and quickly air cool it to room temperature.

[0101] Aging treatment: heating to 800°C, keeping the temperature for 15 hours, cooling to 400°C at 0.6°C / min, keeping the temperature for 6 hours, and air cooling to room temperature to obtain samarium cobalt magnets. The properties of the obtained magnets are shown in Table 2.

[0102] Table 1

[0103]

[0104] Table 2

[0105]

[0106] Note: X indicates the number of rust spots on the magnet after HAST test;

[0107] α=(Br0-Br1) / Br0; Br1 represents the remanence of the magnet of this embodiment; Br0 represents the remanence of the magnet formed by replacing Ni in the magnet of this embodiment with Fe, i.e., the remanence of the magnet obtained in Comparative Example 1;

[0108] β=(X0-X1) / X0; X1 represents the number of rust spots on the magnet of this embodiment after the HAST test; X0 represents the number of rust spots on the magnet formed by replacing Ni in the magnet of this embodiment with Fe after the HAST test, that is, the number of rust spots on the magnet obtained in Comparative Example 1 after the HAST test;

[0109] γ=(Hcj0-Hcj1) / Hcj0; Hcj1 represents the coercive force of the magnet of this embodiment; Hcj0 represents the coercive force of a magnet formed by replacing Ni in the magnet of this embodiment with Fe, that is, the coercive force of the magnet obtained in Comparative Example 1;

[0110] I is the magnetic property-corrosion resistance equilibrium constant; I = (α + γ) / β. The smaller the I value, the less the magnetic properties are reduced and the higher the corrosion resistance is improved.

[0111] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A samarium cobalt magnet, It is characterized in that The samarium cobalt magnet is Sm 2 Co 17 A samarium cobalt magnet comprising Sm, Co, Fe, Ni and M; wherein M is selected from one or more of Cu and Zr; and the samarium cobalt magnet does not contain C, N and Li; The content of Ni is 1.2-2.3wt%, the content of Fe is 15.0-16.5wt%, the content of Sm is 20-30wt%, the content of Co is 45-55wt%, and the content of M is 5-15wt%; The magnetic property-corrosion resistance equilibrium constant I of the samarium cobalt magnet satisfies the following formula: 0.01<I≤0.079; Among them, the magnetic properties-corrosion resistance equilibrium constant I = (α + γ) / β; where α = (Br 0 - Br 1 ) / Br 0 ; Br 1 is the remanence of the samarium cobalt magnet, in kGs; Br 0 The remanence of a nickel-free magnet formed by replacing Ni in the samarium cobalt magnet with Fe, in kGs; Where, γ=(Hcj 0 -Hcj 1 ) / Hcj 0 ; HkDJ 1 is the coercive force of the samarium cobalt magnet, in kOe; HkDJ 0 The coercive force of a nickel-free magnet formed by replacing Ni in the samarium cobalt magnet with Fe, in kOe; Where β=(X 0 -X 1 ) / X 0 ; X 1 is the number of rust spots on the samarium cobalt magnet after the HAST test; X 0 The number of rust spots on the nickel-free magnet formed by replacing Ni in the samarium cobalt magnet with Fe after the HAST test.

2. The samarium cobalt magnet according to claim 1, It is characterized in that The content of Ni is 1.8-2.1 wt%.

3. The samarium cobalt magnet according to claim 1, It is characterized in that The content of Fe is 15.5-16.0 wt%.

4. The samarium cobalt magnet according to any one of claims 1 to 3, It is characterized in that The samarium cobalt magnet contains Fe 2 NiO 5 Crystal phase.

5. The method for preparing the samarium cobalt magnet according to any one of claims 1 to 4, It is characterized in that The steps include: (1) providing a magnet raw material according to the magnet component, and melting the magnet raw material to form a master alloy from the melted magnet raw material; (2) crushing the master alloy obtained by smelting into alloy powder; (3) mixing alloy powders; (4) Under the action of an oriented magnetic field, the mixed alloy powder is pressed into a green body, and then isostatically pressed to form a green body; (5) Sintering the green body and performing solid solution treatment to form a sintered magnet; (6) The sintered magnet is subjected to aging treatment to obtain a samarium cobalt magnet.

6. Use of nickel in improving the corrosion resistance of samarium cobalt magnets, It is characterized in that The samarium cobalt magnet is Sm 2 Co 17 A samarium cobalt magnet comprising Sm, Co, Fe, Ni and M; wherein M is selected from one or more of Cu and Zr; and the samarium cobalt magnet does not contain C, N and Li; The content of Ni is 1.2-2.3wt%, the content of Fe is 15.0-16.5wt%, the content of Sm is 20-30wt%, the content of Co is 45-55wt%, and the content of M is 5-15wt%; The magnetic property-corrosion resistance equilibrium constant I of the samarium cobalt magnet satisfies the following formula: 0.01<I≤0.079; Among them, the magnetic properties-corrosion resistance equilibrium constant I = (α + γ) / β; where α = (Br 0 - Br 1 ) / Br 0 ; Br 1 is the remanence of the samarium cobalt magnet, in kGs; Br 0 The remanence of a nickel-free magnet formed by replacing Ni in the samarium cobalt magnet with Fe, in kGs; Where, γ=(Hcj 0 -Hcj 1 ) / Hcj 0 ; HkDJ 1 is the coercive force of the samarium cobalt magnet, in kOe; HkDJ 0 The coercive force of a nickel-free magnet formed by replacing Ni in the samarium cobalt magnet with Fe, in kOe; Where β=(X 0 -X 1 ) / X 0 ; X 1 is the number of rust spots on the samarium cobalt magnet after the HAST test; X 0 The number of rust spots on the nickel-free magnet formed by replacing Ni in the samarium cobalt magnet with Fe after the HAST test.