A method for preparing boron-modified wood liquefied carbon fiber spinning solution

By adding hexadecimal methyltetramine and boronide to the wood liquefied, the preparation process of boron-modified wood liquefied spinning liquid is simplified, the problem of poor performance of the spinning liquid is solved, and high strength and heat resistance are achieved and reduce production costs.

CN115467050BActive Publication Date: 2024-11-29GUANGXI UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211026912.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-25
Publication Date
2024-11-29
Estimated Expiration
2042-08-25

AI Technical Summary

Technical Problem

The existing wood liquefied spinning liquid has too many short-chain molecules, which affects the spinning effect, and has poor fiber force and thermal performance. In the current technology, additional catalyst is required to be added when synthesizing high ortho-boro modified spinning liquid. Complex and costly.

Method used

By mixing wood powder with phenol and adding phosphoric acid to react, wood liquefied product is obtained, hexadecimal methyltetramine and boron are added, and the temperature is raised and stirred to 120-130°C to prepare high ortho-boron modified wood liquefied spinning liquid , simplifies the process and improves the performance of the spinning liquid.

Benefits of technology

The spinning and heat resistance of the spinning liquid is improved, production costs are reduced, and the formation of high ortho-position spinning liquid is verified through infrared spectroscopy and XPS photoelectron spectroscopy, which significantly improves the strength and heat resistance of the fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115467050B_ABST
    Figure CN115467050B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a boron-modified wood liquefied carbon fiber spinning solution, comprising the following steps: (1) mixing wood powder and phenol, adding phosphoric acid, and reacting at 150°C-180°C to obtain a wood liquefied product; (2) adding 4%-5% hexamethylenetetramine by weight of the wood liquefied product and 3%-4% boride by weight of the wood liquefied product, mixing evenly, heating and continuously stirring, and keeping warm until the liquid becomes a spinnable viscous flow state after reaching 120-130°C, thereby obtaining a boron-modified wood liquefied carbon fiber spinning solution. The present invention adds boric acid or nano-boron carbide to the wood liquefied product to improve the performance of the spinning solution, which is macroscopically manifested as an increase in softening point, better spinnability, and an increase in residual carbon rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to wood liquefaction technology, in particular to a method for preparing boron-modified wood liquefaction carbon fiber spinning solution. Background Art

[0002] Wood liquefact is a liquid polymer material with active groups converted from wood. The commonly used liquefaction method at present is to use phenols or polyols as liquefiers under normal pressure, and acids or bases as catalysts to turn wood into liquefied products. In recent years, supercritical extraction technology has developed rapidly in the field of separation, and this technology has also been applied to the efficient liquefaction of wood. When polyols, such as ethylene carbonate, are used as liquefiers, rapid liquefaction of wood can also be achieved. The composition, structural characteristics and liquefaction mechanism of liquefied products made by different liquefaction processes are different. In the phenol liquefaction process under acidic conditions, phenol acts as a nucleophilic agent to cause the breakage of chemical bonds in wood; reacts with degraded small molecules to form compounds with phenolic structures; and slows down the condensation reaction of active small molecules. The structural characteristics of the three polymers, cellulose, hemicellulose, and lignin, determine the properties of wood liquefact. Lignin and hemicellulose are first liquefied to form phenolic products such as guaiacol compounds; cellulose is degraded into oligosaccharides, and oligosaccharides are further degraded into glucose, which forms compounds containing furan ring structures with phenol. Among acidic catalysts, sulfuric acid has the lowest residue rate and the highest liquefaction efficiency in the wood liquefaction reaction. However, as a strong acid, sulfuric acid is highly corrosive and the liquefaction process is prone to cause local carbonization and smoke. The liquefaction efficiency of wood phenol liquefaction using phosphoric acid and oxalic acid as catalysts is slightly lower, but it is safer. Compared with the wood phenol liquefaction catalyzed by sulfuric acid, its liquefaction product has a lower bound phenol content and retains more characteristics similar to the chemical structure of natural wood.

[0003] The wood liquefact contains a large amount of phenolic compounds. According to this characteristic, the wood liquefact can be applied to various fields, and has better biodegradability and environmental protection performance than conventional phenolic resins and derivative materials. At present, wood liquefact has been developed for a variety of uses, such as the manufacture of wood liquefact thermosetting resins used as wood processing adhesives, thermoplastic resins used as molding materials, foaming materials for building insulation, carbon fibers, etc. Among them, the preparation method of wood liquefact-based carbon fibers is: adding reactants such as hexamethylenetetramine, formaldehyde, and furfural to the wood liquefact, generating a viscous flow state and a spinnable linear structure resin (spinning solution) under appropriate temperature conditions, adjusting to the spinning temperature, and using a melt spinning machine to spin uniform filaments; after curing or thermal curing, it can be made into wood liquefact fibers; and after carbonization treatment, it can be made into wood liquefact carbon fibers.

[0004] Studies have shown that the abundant natural high molecular polymers such as cellulose, hemicellulose and lignin in wood make the chemical composition of wood liquefaction more complex, resulting in the presence of more short-chain molecules in the spinning solution made of wood liquefaction, which affects the fiber-forming effect of the spinning solution and also leads to poor mechanical and thermal properties of the fibers made of the spinning solution; and the skin-core structure of the wood liquefaction fiber has been produced during the solidification process of the initial fiber spun from the spinning solution, affecting the performance of the precursor and even the carbon fiber. Therefore, if you want to improve the performance of wood liquefaction fiber, the modification effect after the precursor is not good, and it is necessary to modify it in the spinning solution stage. When the reactant is formaldehyde or furfural, the polycondensation reaction with the liquefaction is mainly through the para-reaction of the phenolic hydroxyl group. Therefore, in the generated spinning solution molecules, the phenolic ring is mainly connected in the para-position, and the unblocked phenolic hydroxyl group will cause the thermal and mechanical properties of the spinning solution to be poor. In the prior art, when the reactant is formaldehyde or furfural, if you want to synthesize a spinning solution modified with high ortho-boron, you need to add an additional catalyst to activate the ortho position of the benzene ring, and then add boric acid to complete the preparation. The reaction time is long, the operation is complicated and filtration and purification are required before it can be used for spinning. Summary of the invention

[0005] In view of the above technical problems, the present invention invents a method for preparing a boron-modified wood liquefied material carbon fiber spinning solution. By selecting a wood liquefied material spinning solution reactant and performing boron doping treatment, a boron-containing high-ortho wood liquefied material spinning solution is prepared in a simple manner, thereby improving the performance of the spinning solution. The method can subsequently be used to prepare boron-modified wood liquefied material fibers and carbon fibers with better strength and heat resistance.

[0006] To achieve the above purpose, the technical solution provided by the present invention is as follows:

[0007] A method for preparing a boron-modified wood liquefact carbon fiber spinning solution comprises the following steps:

[0008] (1) mixing wood powder and phenol, adding phosphoric acid, and reacting at 150° C. to 180° C. to obtain a wood liquefied product;

[0009] (2) adding 4%-5% hexamethylenetetramine by weight of the wood liquefied material and 3%-4% boride by weight of the wood liquefied material to the wood liquefied material obtained in step (1), mixing them evenly, heating them to 120-130° C. and stirring them continuously. After reaching 120-130° C., the temperature is maintained until the liquid becomes a viscous flow state that can be spinned, thereby obtaining a boron-modified wood liquefied material carbon fiber spinning solution.

[0010] Preferably, the wood powder and phenol in step (1) are mixed in a mass ratio of 1:5.

[0011] Preferably, the amount of phosphoric acid added in step (1) is 8% of the mass of the phenol added.

[0012] Preferably, the reaction time in step (1) is 2 h.

[0013] Preferably, in step (2), the temperature is raised to 120° C. and stirring is continued.

[0014] Preferably, in step (2), 5% by mass of hexamethylenetetramine is added; and 4% by mass of boride is added.

[0015] Preferably, the boride in step (2) is boric acid or nano-boron carbide.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] The invention adds boric acid or nano boron carbide to wood liquefact, and reacts with hexamethylenetetramine to prepare a high-ortho-boron modified wood liquefact spinning solution. Boric acid or nano boron carbide is added to improve the performance of the spinning solution during the preparation process, and the macroscopic performance is an increase in softening point, better spinnability, and an increase in residual carbon rate. Furthermore, the invention is simple to operate, has simple steps, and reduces production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is the infrared image of the spinning solution prepared in Example 1-2 and Comparative Example 1-3.

[0019] Figure 2 It is the boron element spectrum of the boron-modified wood liquefied carbon fiber spinning solution prepared in Examples 1 and 2; the left figure represents the boron element spectrum of the spinning solution when boric acid is added, and the right figure represents the boron element spectrum of the spinning solution when nano-boron carbide is added.

[0020] Figure 3 It is a thermogravimetric comparison diagram of various embodiments and comparative examples. DETAILED DESCRIPTION

[0021] The following is described in detail in conjunction with the specific embodiments, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. The raw materials and reagents used in the examples are all commercially available unless otherwise specified. Hexamethylenetetramine is commercially available analytical pure hexamethylenetetramine, and boric acid and nano boron carbide are both high-purity boric acid and nano boron carbide.

[0022] Example 1

[0023] A method for preparing a boron-modified wood liquefied carbon fiber spinning solution, the operating steps are as follows:

[0024] (1) mixing wood powder and phenol in a mass ratio of 1:5, adding phosphoric acid with a mass ratio of 8% of the phenol, and reacting at 160° C. for 2 h to obtain a wood liquefied product;

[0025] (2) Add 5% hexamethylenetetramine by weight of the wood liquefied material and 4% boric acid by weight of the wood liquefied material to the wood liquefied material obtained in step (1), mix well, and then raise the temperature from 30°C to 120°C at a heating rate of 2.25°C / min while stirring continuously. After reaching 120°C, keep the temperature until the liquid becomes a viscous flow state that can be spun, thereby obtaining a boron-modified wood liquefied material carbon fiber spinning solution. The obtained boron-modified wood liquefied material carbon fiber spinning solution has an ortho-para ratio of benzene rings of 2.82, a softening temperature of 75°C, and a residual carbon rate of 42.281%.

[0026] Example 2

[0027] A method for preparing a boron-modified wood liquefied carbon fiber spinning solution, the operating steps are as follows:

[0028] (1) mixing wood powder and phenol in a mass ratio of 1:5, adding phosphoric acid with a mass ratio of 8% of the phenol, and reacting at 160° C. for 2 h to obtain a wood liquefied product;

[0029] (2) Add 5% hexamethylenetetramine by weight of the wood liquefied material and 4% nano boron carbide by weight of the wood liquefied material to the wood liquefied material obtained in step (1), mix well, and then raise the temperature from 30°C to 120°C at a heating rate of 2.25°C / min while stirring continuously. After reaching 120°C, keep the temperature until the liquid becomes a viscous flow state that can be spun, thereby obtaining a boron-modified wood liquefied material carbon fiber spinning solution. The obtained boron-modified wood liquefied material carbon fiber spinning solution has an ortho-para ratio of benzene rings of 1.72, a softening temperature of 65°C, and a residual carbon rate of 41.493%.

[0030] Example 3

[0031] A method for preparing a boron-modified wood liquefied carbon fiber spinning solution, the operating steps are as follows:

[0032] (1) mixing wood powder and phenol in a mass ratio of 1:5, adding phosphoric acid with a mass ratio of 8% of the phenol, and reacting at 150° C.-180° C. for 2 h to obtain a wood liquefied product;

[0033] (2) Add 5% hexamethylenetetramine by weight of the wood liquefied material and 3% nano boron carbide by weight of the wood liquefied material to the wood liquefied material obtained in step (1), mix well, and then raise the temperature from 30°C to 130°C at a heating rate of 2.5°C / min while stirring continuously. After reaching 130°C, keep the temperature until the liquid becomes a viscous flow state that can be spun, thereby obtaining a boron-modified wood liquefied material carbon fiber spinning solution. The obtained boron-modified wood liquefied material carbon fiber spinning solution has an ortho-para ratio of benzene rings of 1.72, a softening temperature of 75°C, and a residual carbon rate of 41.632%.

[0034] Comparative Example 1

[0035] (2) Add 5% formaldehyde by weight of the liquefied wood to the liquefied wood obtained in step (1) and mix well. The remaining operations are the same as those in Example 1 to obtain a spinning solution. The ortho-para ratio of the benzene ring in the obtained spinning solution is 0.852, the softening point is 50° C., and the residual carbon rate is 36.771%.

[0036] Comparative Example 2

[0037] A method for preparing a spinning solution, the operating steps are as follows:

[0038] (1) mixing wood powder and phenol in a mass ratio of 1:5, adding phosphoric acid with a mass ratio of 8% of the phenol, and reacting at 160° C. for 2 h to obtain a wood liquefied product;

[0039] (2) Add 20% formaldehyde and 5% zinc acetate by weight of the wood liquefied material to the wood liquefied material obtained in step (1), heat to boiling and keep for 30 minutes, add sulfuric acid (0.3 ml: 100 g) and boric acid (5% by weight of the wood liquefied material), continue boiling reaction for 2 hours, then add anhydrous ethanol to dilute and filter, and remove anhydrous ethanol and small molecular substances by rotary evaporation to prepare a spinning solution. The spinning solution has an ortho-para ratio of benzene ring of 1.23, a softening point of 55° C., and a residual carbon rate of 37.165%.

[0040] Comparative Example 3

[0041] In step (2), no boric acid is added, and the remaining operations are the same as those in Example 1, thereby obtaining a spinning solution having an ortho-para ratio of benzene rings of 1.72, a softening point of 65° C., and a residual carbon rate of 36.764%.

[0042] Comparative Example 4

[0043] In step (2), hexamethylenetetramine is not added, and the remaining operations are the same as those in Example 1, thereby obtaining an ester substance which cannot be used for spinning.

[0044] By infrared spectroscopy ( Figure 1 ) can be seen 825, 754cm -1 The peaks at the positions are respectively attributed to the stretching vibration peaks of the para- and ortho-substituents on the benzene ring. The area ratio of the two peaks can be calculated by peak fitting to see whether a high ortho-spinning solution has been synthesized. The infrared spectrum and XPS photoelectron spectrum can show the existence form of the boron element in the spinning solution.

[0045] Compared with the spinning solution of wood liquefaction, the spinning solution modified by boric acid or nano boron carbide with hexamethylenetetramine as the reactant has higher ortho-para positions, and the softening point and residual carbon rate are improved, which means that the molecular chain of the modified spinning solution is longer and the heat resistance is improved; and the synthesis steps are few and the synthesis method is simple.

[0046] The thermogravimetric diagram records the weight loss of the sample during the heating process, and can show the decomposition stage of the sample and the final weight loss rate (residual carbon rate). Figure 3 It can be seen that the carbon residue rate of the spinning solution prepared by the method of the present invention is significantly improved compared with the comparative example, indicating that the heat resistance of the spinning solution after modification is improved. Figure 3 Examples 1, 2, and 3 represent Example 1, Example 2, and Example 3, respectively; Comparative Examples 1, 2, and 3 represent Comparative Example 1, Comparative Example 2, and Comparative Example 3, respectively.

[0047] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A method for preparing a boron-modified wood liquefied carbon fiber spinning solution, characterized in that: The following steps are included: (1) Mix wood powder and phenol, add phosphoric acid, and react at 150°C-180°C to obtain wood liquefaction; (2) Add 5% by weight of hexamethylenetetramine and 4% by weight of boron compound to the wood liquefied product obtained in step (1), mix well, heat to 120-130° C. and continue stirring. After reaching 120-130° C., keep warm until the liquid becomes a viscous flow state that can be spun, thereby obtaining a boron-modified wood liquefied product carbon fiber spinning solution; the boron compound is boric acid or nano-boron carbide.

2. The method for preparing the boron-modified wood liquefied carbon fiber spinning solution according to claim 1, characterized in that: The wood powder and phenol described in step (1) are mixed in a mass ratio of 1:

5.

3. The method for preparing the boron-modified wood liquefied carbon fiber spinning solution according to claim 1, characterized in that: The amount of phosphoric acid added in step (1) is 8% of the mass of phenol added.

4. The method for preparing the boron-modified wood liquefied carbon fiber spinning solution according to claim 1, characterized in that: The reaction time in step (1) is 2 h.

5. The method for preparing the boron-modified wood liquefied carbon fiber spinning solution according to claim 1, characterized in that: In step (2), the temperature is raised to 120°C and stirring is continued.

Citation Information

Patent Citations

  • Preparation method of active wood-based carbon fibers

    CN102719935A