Preparation method of lithium-ion battery material LiF-V2O3 / C
The LiF-V2O3/C nanofiber material is generated by electrospinning combined with high-temperature solid-state sintering method, which solves the problem of insufficient performance of lithium-ion battery anode materials under high energy density requirements, achieves high capacity and excellent cycle stability, and is suitable for It is a negative electrode material for lithium-ion batteries and is low-cost and environmentally friendly.
Patent Information
- Application Number
- CN202211071471.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-09-02
AI Technical Summary
Existing lithium-ion battery anode materials have insufficient performance under high energy density requirements, especially graphite carbon due to the limited amount of embedded Li+, lithium titanate due to low conductivity resulting in capacity fading, and metal oxides formed during the first discharge The structure is not conducive to the formation of a stable solid electrolyte interface layer (SEI).
LiF-V2O3/C nanofiber materials are generated in situ using electrospinning combined with high-temperature solid-state sintering. LiF modification is used to promote the formation of a stable SEI film on the surface. The fiber structure design and carbon composite are used to enhance reaction kinetics and improve electrochemical performance.
It significantly improves the electrochemical performance of LiF-V2O3/C, achieves high capacity and excellent cycle stability, is suitable for lithium-ion battery anode materials, is low-cost and environmentally friendly.
Smart Images

Figure 220901174816 
Figure 220901174818 
Figure 220901174821
Abstract
Description
Technical Field
[0001] The invention relates to a novel negative electrode material for lithium ion batteries, in particular to a method for in-situ generation of LiF-V2O3 / C nanofiber material as negative electrode material for lithium ion batteries by combining electrostatic spinning with high-temperature solid-phase sintering, and belongs to the field of electrochemical power sources. Background Art
[0002] As the main portable power source in modern life, lithium-ion batteries are unmatched by other commercial batteries in terms of energy density, power output and cycle stability. Although lithium-ion batteries have made significant leaps in almost every aspect due to huge global market competition in the past 20 years, the performance of lithium-ion batteries still cannot keep up with the needs of the booming consumer market for electronic products and electric vehicles.
[0003] Advanced negative electrode materials are the key to high storage capacity and high stability of lithium-ion batteries. The lithium storage mechanisms of current lithium-ion battery negative electrode materials can be divided into three types: intercalation and deintercalation, alloy and conversion. The only negative electrode materials officially put into commercial application are intercalation and deintercalation materials represented by graphite carbon and lithium titanate. However, graphite carbon can only embed a limited number of Li per unit mass. + , which limits the application of graphite carbon negative electrode materials in high energy density lithium-ion batteries. However, lithium titanate materials are gradually unable to meet the high energy density requirements of lithium-ion batteries due to their low conductivity and serious capacity decay during high current charging and discharging. Therefore, there is an urgent need to find new negative electrode materials with high theoretical capacity, environmental friendliness and low cost.
[0004] Metal oxides (M x O y , M is a transition metal) negative electrode material with high theoretical capacity and safer charging and discharging platform, and has potential application value in lithium-ion batteries. However, metal oxides will form metal elements and Li2O during the first discharge process, and this process is accompanied by the formation of a solid electrolyte interface layer (SEI). Usually, the structure formed by discharge is that the metal element is dispersed in the Li2O matrix in the form of nanoparticles, which is not conducive to the formation of a stable SEI. Therefore, the electrochemical performance of the prepared metal oxide negative electrode materials is often not ideal. LiF is an effective component of SEI, and its presence is conducive to the formation of SEI on the surface of the electrode material. Design and synthesis of M x O y -LiF composite materials are expected to promote the formation of a stable SEI film on the surface of the material during the charge and discharge process. x O y -LiF material morphology and composition can be regulated and optimized to obtain high-performance new negative electrode materials. However, no reports on such new negative electrode materials have been reported so far.
[0005] This patent aims to develop M with special morphology x O y -LiF / C composite materials, through LiF to promote the formation of a stable SEI film on the surface, combined with special morphology and carbon composite to regulate the reaction kinetics of the material, thereby ultimately improving the electrochemical performance of the material. To this end, for the first time, a LiF-V2O3 / C nanofiber material was proposed, which was in situ generated by electrospinning combined with high-temperature solid-phase sintering using lithium nitrate, ammonium metavanadate, polyvinyl alcohol and polytetrafluoroethylene as raw materials. Through LiF modification, the formation of a stable SEI film on the surface of the material is promoted, and the reaction kinetics are enhanced by fiber structure design and carbon composite, thereby significantly improving the electrochemical performance of LiF-V2O3 / C. The preparation process of this material uses water as a solvent, which is simple and easy to obtain, low cost, energy-saving and environmentally friendly, and is conducive to large-scale preparation. The prepared LiF-V2O3 / C nanofiber material has excellent electrochemical properties when used as a negative electrode material for lithium-ion batteries, and has potential application value in lithium-ion batteries. Summary of the invention
[0006] A method for obtaining LiF-V2O3 / C nanofiber material as a negative electrode material for lithium ion batteries based on electrospinning technology using lithium nitrate, ammonium metavanadate, polyvinyl alcohol, polytetrafluoroethylene, and deionized water as raw materials, wherein the steps are as follows:
[0007] (1) Add a certain amount of lithium nitrate and ammonium metavanadate to an appropriate amount of deionized water and stir in a constant temperature water bath at 70 °C for 0.5-2 h to obtain a uniform light yellow transparent solution; then add an appropriate amount of polyvinyl alcohol to the above solution and stir at room temperature for 8-24 h until a yellow opaque solution is formed; then add a certain amount of polytetrafluoroethylene aqueous dispersion with a mass fraction of 60% to the above solution and stir for 0.5 h to obtain a uniform electrospinning precursor solution;
[0008] (2) transferring the uniform solution obtained in step (1) into an electrospinning syringe, spinning for 8-10 h at a voltage of 18-22 kV, a temperature of 40-50 °C, and a humidity of ﹤30%, to obtain a flexible precursor fiber membrane;
[0009] (3) The fiber membrane obtained in step (2) is quickly transferred to a 60-80 °C forced air drying oven for drying for 10-12 h. After drying, it is placed in a N2 environment, pre-calcined at 250-300 °C for 2-5 h at a heating rate of 5 °C / min, and then calcined at 600-800 °C for 2 h to obtain LiF-V2O3 / C nanofiber material for lithium-ion battery negative electrode material.
[0010] This patent uses a polymer solution to perform jet spinning in a high-voltage electric field, and for the first time uses electrospinning combined with high-temperature solid-phase sintering to in-situ generate LiF-V2O3 / C nanofiber electrode materials. A large number of LiF-V2O3 nanoparticles are dispersed on the matrix carbon fiber, and the composite material has excellent electrochemical properties. The prepared zLiF-V2O3 / C nanofiber can be used as a new type of negative electrode material for lithium-ion batteries. 1) ammonium metavanadate is slightly soluble in water at room temperature, and it will completely dissolve when heated to 70°C; 2) the chemical formula of ammonium metavanadate is NH4VO3, and when dissolved, VO3 − V 5+ The solution becomes yellow and transparent. When lithium nitrate is added, VO3 − With Li + Forming Li3VO4 precursor; 3) The addition of polyvinyl alcohol will increase the viscosity of the solution system, and at the same time, the -OH on the molecular chain will form hydrogen bonds with the F atoms on the polytetrafluoroethylene molecules, which is conducive to the uniform dispersion of polytetrafluoroethylene nanoparticles in the solution. During low-temperature pre-sintering at 250-300 ℃ in nitrogen, the polyvinyl alcohol molecular chain is dehydrogenated and converted into a heat-resistant fiber structure. During the high-temperature sintering process at 600-800 ℃, polyvinyl alcohol is completely converted into carbon nanofibers, while providing a reducing environment to convert V 5+ Restore to V 3+ ; 4) PTFE is a fluorinated polymer with low dielectric constant, so the addition of PTFE can increase the conductivity of the solution, thereby improving the stability and yield of the electrospinning process. At the same time, the highly polar F ions produced by the decomposition of PTFE during the sintering process will react with the Li in the Li3VO4 precursor. + Combined to generate LiF, thus forming a special morphology of LiF-V2O3 nanoparticles embedded in C nanofibers. The fiber structure is conducive to enhancing the flexibility and structural stability of the material, and the ultrafine nanoparticles can significantly improve the electrochemical activity of the composite material; 5) LiF, as a favorable component of the electrolyte, can directly and stably provide fluoride ions during the electrode cycle, so that the negative electrode has a fluorinated SEI layer, thereby improving the stability of the negative electrode electrochemical reaction. The prepared LiF-V2O3 / C nanofibers show excellent comprehensive electrochemical properties as negative electrode materials for lithium-ion batteries.
[0011] This patent uses a polymer solution to perform jet spinning in a high-voltage electric field, combined with high-temperature solid-phase sintering to in-situ generate zLiF-V2O3 / C nanofiber electrode materials. The prepared zLiF-V2O3 / C nanofiber can be used as a new type of lithium-ion battery positive electrode material. 1) ammonium metavanadate is slightly soluble in water at room temperature, and will completely dissolve when heated to 70°C; 2) the chemical formula of ammonium metavanadate is NH4VO3, and when dissolved, VO3 − V 5+ The solution becomes yellow and transparent. When lithium nitrate is added, a V-containing5+ and Li + The precursor solution; 3) The addition of polyvinyl alcohol increases the viscosity of the solution system, and the -OH on the molecular chain forms hydrogen bonds with the F atoms on the polytetrafluoroethylene molecules, which is conducive to the uniform dispersion of polytetrafluoroethylene in the solution. During low-temperature pre-sintering at 250-300 ℃ in nitrogen, the polyvinyl alcohol molecular chain is dehydrogenated and converted into a heat-resistant fiber structure. During the high-temperature sintering process at 600-800 ℃, polyvinyl alcohol is completely converted into carbon nanofibers, while providing a reducing environment to convert V 5+ Reduction to V in V2O3 3+ . The amorphous carbon generated by in-situ carbonization of polyvinyl alcohol can effectively improve the conductivity of the material and enhance the reaction kinetics of lithium-ion batteries; 4) Polytetrafluoroethylene is a fluorine-containing polymer with a low dielectric constant, so the addition of polytetrafluoroethylene can increase the conductivity of the solution, thereby improving the stability and yield of the electrospinning process. At the same time, polytetrafluoroethylene decomposes during the sintering process to produce highly polar F ions that will react with V-containing 5+ and Li + Li in the precursor + Combined to form LiF, thus forming a special morphology of nanoparticles embedded in the matrix fiber. The fiber structure is conducive to enhancing the structural stability of the material, and ultrafine nanoparticles can significantly improve the electrochemical activity of the composite material; 5) During the charging process, the process of zLiF-V2O3 / C nanofibers releasing lithium ions is accompanied by V 3+ Theoretically, the V in V2O3 3+ Can be completely oxidized to V 5+ , which can release 4 lithium ions. Li in LiF can be used as the Li source of the positive electrode material, while F is the anion source for charge compensation, maintaining the overall stability of zLiF-V2O3 / C after releasing lithium ions and electrons. The prepared zLiF-V2O3 / C nanofibers can be used as a new type of high-capacity lithium-ion battery positive electrode material with great application potential.
[0012] The present invention relates to a method for preparing a LiF-V2O3 / C nanofiber composite material as a lithium ion battery material, which has the following significant characteristics:
[0013] (1) Using safe and non-toxic water as solvent, the preparation cost is low and it is environmentally friendly.
[0014] (2) LiF-V2O3 / C negative electrode material was prepared by electrospinning and high-temperature sintering process. The synthesis process is simple and has strong repeatability.
[0015] (3) The prepared LiF-V2O3 / C nanofiber composite material has a fiber diameter of about 300-400 nm, which is conducive to the diffusion and transfer of lithium ions. A large number of ultra-small nanoparticles with a diameter of about 20-70 nm are evenly dispersed on the fiber surface, which is conducive to the contact and penetration of the electrolyte.
[0016] (4) The LiF-V2O3 / C nanofiber composite material prepared by the in situ synthesis method was used as the negative electrode material for lithium-ion batteries for the first time, with high capacity and excellent cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 Optical photographs of the samples prepared in Example 1: (a) electrospinning precursor solution, (b) nanofiber membrane obtained by electrospinning.
[0018] Figure 2 Optical photographs of the samples prepared in Example 1: (a) nanofiber membrane before carbonization, (b) nanofiber membrane after carbonization.
[0019] Figure 3 XRD pattern of the sample prepared in Example 1.
[0020] Figure 4 SEM images of the samples prepared in Example 1: (a) overall morphology of LiF-V2O3 / C nanofibers (b) local magnified image of LiF-V2O3 / C nanofibers.
[0021] Figure 5 (a) The first three cyclic voltammetry curves (b) The first three charge and discharge curves (c) Cyclic performance diagram of the sample prepared in Example 1.
[0022] Figure 6 Optical photographs of the samples prepared in Example 2: (a) electrospinning precursor solution, (b) nanofiber membrane obtained by electrospinning.
[0023] Figure 7 Optical photographs of the samples prepared in Example 3: (a) dried spinning precursor solution, (b) carbonized spinning solution.
[0024] Figure 8 (a) The first three cyclic voltammetry curves (b) The first three charge and discharge curves (c) Cyclic performance diagram of the sample prepared in Example 3.
[0025] Fig. 9 Optical photographs of the samples prepared in Example 4: (a) polytetrafluoroethylene powder before carbonization, (b) polytetrafluoroethylene after carbonization.
[0026] Fig.10Optical photographs of the samples prepared in Example 5: (a) electrospinning precursor solution, (b) nanofiber membrane obtained by electrospinning.
[0027] Fig.11 Optical photographs of the samples prepared in Example 5: (a) nanofiber membrane before carbonization, (b) nanofiber membrane after carbonization.
[0028] Fig.12 SEM images of the samples prepared in Example 5: (a) overall morphology of zLiF-V2O3 / C nanofibers (b) local magnified image of zLiF-V2O3 / C nanofibers.
[0029] Fig.13 (a) The first three cyclic voltammetry curves and (b) the charge and discharge curves of the sample prepared in Example 5.
[0030] Fig.14 Optical photographs of the samples prepared in Example 6: (a) electrospinning precursor solution, (b) nanofiber membrane obtained by electrospinning.
[0031] Fig.15 Optical photographs of the samples prepared in Example 7: (a) dried spinning precursor solution, (b) carbonized spinning solution.
[0032] Fig.16 (a) The first three cyclic voltammetry curves and (b) the charge and discharge curves of the sample prepared in Example 7.
[0033] Fig.17 (a) LiF / C powder after sintering and (b) charge and discharge curves of the sample prepared in Example 8.
[0034] Fig.18 Optical photographs of the samples prepared in Example 9: (a) polytetrafluoroethylene powder before carbonization, (b) polytetrafluoroethylene after carbonization. DETAILED DESCRIPTION
[0035] Example 1
[0036] 7.5 mmol lithium nitrate and 2.5 mmol ammonium metavanadate were added to 10 ml deionized water and stirred in a 70 °C constant temperature water bath for 1 h to obtain a uniform yellow transparent solution. Then 0.8 g polyvinyl alcohol was added to the above solution and stirred at room temperature for 12 h to form a yellow opaque solution. Then 0.8 g of 60% polytetrafluoroethylene aqueous dispersion was added to the above solution and stirred for 0.5 h to obtain a uniform electrospinning viscous solution ( Figure 1The obtained solution was transferred to a 10 ml electrospinning syringe and electrospun at 22 kV high voltage, with a spinning temperature of about 40 °C, a humidity of ﹤30%, and a spinning time of 10 h to obtain a flexible precursor fiber membrane ( Figure 1 b). The electrospun fiber membrane was quickly transferred to a 60 ℃ forced air drying oven and dried for 12 h ( Figure 2 a), dried and placed in a N2 environment, pre-sintered at 280 °C for 3 h at a heating rate of 5 °C / min, and then calcined at 750 °C for 2 h to obtain LiF-V2O3 / C nanofiber material for lithium-ion battery negative electrode material ( Figure 2 b). The prepared samples were analyzed by XRD, and the obtained diffraction peaks corresponded well with LiF (PDF# 04-0857) and V2O3 (PDF# 34-0187). Figure 3 ). Scanning electron microscopy analysis shows that the carbonized LiF-V2O3 / C nanofiber material presents a relatively uniform fiber network structure as a whole ( Figure 4 In a), a large number of LiF-V2O3 nanocrystal particles are evenly distributed on the fiber surface ( Figure 4 (b)
[0037] The material was made into a battery as follows: the sintered LiF-V2O3 / C nanofiber material was ground with a conductive agent (acetylene black) and a binder (polyvinylidene fluoride) in a ratio of 8:1:1, and a slurry was prepared using N-methylpyrrolidone as a solvent. The slurry was coated on a copper foil with a thickness of 10 μm, dried at 60 °C for 10 h, cut into electrode sheets with a diameter of 14 mm, and vacuum dried at 120 °C for 12 h. A metal lithium sheet was used as the counter electrode, a Celgard membrane was used as the separator, and a solution of EC+DMC+DEC (volume ratio of 1:1:1) containing LiPF6 (1 mmol / L) was used as the electrolyte. The CR2025 type battery was assembled in an argon-protected glove box. After the battery was assembled, it was left to stand for 8 h, and then a constant current charge and discharge test was performed using a CT2001 battery test system. The test voltage was 0.1-3 V and the current density was 200 mA g -1 . Figure 5 The first three cyclic voltammetry curves of the prepared LiF-V2O3 / C nanofiber composite material ( Figure 5 In a), the first three charge and discharge curves ( Figure 5 b) and cycle performance diagram ( Figure 5 (c) The first charge and discharge specific capacities are 402.1 and 782.5 mAh g -1 After 35 cycles, the charge and discharge capacities were 297.5 and 300.9 mAhg, respectively. -1 , showing good electrochemical performance.
[0038] Example 2
[0039] The steps of this example are exactly the same as those of Example 1, but polytetrafluoroethylene is not added. 7.5 mmol lithium nitrate and 2.5 mmol ammonium metavanadate are weighed and added to 10 ml deionized water and stirred in a 70 °C constant temperature water bath for 1 h to obtain a yellow transparent solution. Then 0.8 g polyvinyl alcohol is added to the above solution and stirred at room temperature for 12 h until a yellow spinning precursor solution ( Figure 6 a). The obtained solution was transferred to a 10 ml electrospinning syringe and electrospun at 22 kV high voltage, with a spinning temperature of about 40 °C, a humidity of ﹤30%, and a spinning time of 4 h. Since no polytetrafluoroethylene was added, the solution itself had poor conductivity, resulting in an unstable spinning process, dripping of the spinning solution, and low filament yield. The spinning process could not proceed normally, so the spun fiber membrane could not be collected ( Figure 6 (b)
[0040] Example 3
[0041] The steps of this embodiment are exactly the same as those of embodiment 1, but electrospinning is not performed. The spinning precursor solution is directly dried and sintered. 7.5 mmol lithium nitrate and 2.5 mmol ammonium metavanadate are weighed and added to 10 ml deionized water and stirred in a constant temperature water bath at 70°C for 1 h to obtain a yellow transparent solution. Then 0.8 g polyvinyl alcohol is added to the above solution and stirred at room temperature for 12 h to form a yellow spinning precursor solution. The spinning solution is dried at 80°C ( Figure 7 a), and then placed in a N2 environment, pre-calcined at 280 °C for 3 h at a heating rate of 5 °C / min, and then calcined at 750 °C for 2 h to obtain a carbonized spinning solution ( Figure 7 b). The material was used to prepare a CR2025 battery according to the method of Example 1 and tested at a test voltage of 3-0.01 V and a current density of 200 mA g -1 . Figure 8 The first three cyclic voltammetry curves of the prepared unspun material ( Figure 8 In a), the first three charge and discharge curves ( Figure 8 b) and cycle performance diagram ( Figure 8 (c) The first charge and discharge specific capacities are 300.9 and 595.8 mAh g -1 After 35 cycles, the charge and discharge capacities were 159.4 and 162.0 mAh g -1 The electrochemical performance is significantly lower than that of LiF-V2O3 / C nanofiber material obtained by electrospinning.
[0042] Example 4
[0043] In this example, pure polytetrafluoroethylene powder (a in FIG. 9 ) was sintered under N2. The sintering conditions were pre-sintering at 280°C for 3 h and then sintering at 750°C for 2 h. The results showed that polytetrafluoroethylene was completely carbonized and decomposed at high temperature, with almost no residue (b in FIG. 9 ). This shows that when polytetrafluoroethylene is used as a fluorine source, only when it combines with lithium ions at high temperature can fluorine atoms be retained in the material to form LiF, otherwise it will be completely decomposed into products such as tetrafluoroethylene, perfluoropropylene, and octafluorocyclobutane and taken away by N2.
[0044] Example 5
[0045] 5 mmol lithium nitrate and 2.5 mmol ammonium metavanadate were added to 10 ml deionized water and stirred in a 70 °C constant temperature water bath for 1 h to obtain a uniform yellow transparent solution. Then 0.8 g polyvinyl alcohol was added to the above solution and stirred at room temperature for 12 h, and then 0.8 g of 60% polytetrafluoroethylene aqueous dispersion was added to the above solution and stirred for 0.5 h to obtain a uniform electrospinning solution ( Fig.10 The obtained solution was transferred into a 10 ml syringe and electrospun at 22 kV high voltage, with a spinning temperature of about 40 °C, a humidity of ﹤30%, and a spinning time of 10 h to obtain a flexible precursor fiber membrane ( Fig.10 b). The electrospun fiber membrane was quickly transferred to a 60 ℃ forced air drying oven and dried for 12 h ( Fig.11 a), dried and placed in a N2 environment, pre-sintered at 280 °C for 3 h at a heating rate of 5 °C / min, and then calcined at 750 °C for 2 h to obtain zLiF-V2O3 / C nanofiber material for lithium-ion battery positive electrode material ( Fig.11 b). The prepared samples were analyzed by XRD, and the obtained diffraction peaks corresponded well with LiF (PDF# 04-0857) and V2O3 (PDF# 34-0187) (same Figure 3 ), no other impurity peaks, indicating that the raw materials are fully reacted to obtain a stoichiometric ratio of 4LiF-V2O3 / C material. Scanning electron microscopy analysis shows that the carbonized zLiF-V2O3 / C nanofiber material presents a relatively uniform fiber network structure as a whole ( Fig.12 In a), a large number of nanocrystalline particles are evenly distributed on the fiber surface ( Fig.12 (b)
[0046] The material was made into a battery as follows: the zLiF-V2O3 / C nanofiber material prepared by sintering was ground with a conductive agent (acetylene black) and a binder (polyvinylidene fluoride) in a ratio of 8:1:1, and a slurry was prepared using N-methylpyrrolidone as a solvent. The slurry was coated on an aluminum foil with a thickness of 10 μm, dried at 60 °C for 10 h, cut into electrode sheets with a diameter of 14 mm, and vacuum dried at 120 °C for 10 h. The metal lithium sheet was used as the counter electrode, the Celgard membrane was used as the separator, and the EC+DMC+DEC (volume ratio of 1:1:1) solution containing LiPF6 (1 mmol / L) was used as the electrolyte. The CR2025 type battery was assembled in an argon-protected glove box. After the battery was assembled, it was left to stand for 8 h, and then the constant current charge and discharge test was performed using the CT2001 battery test system. The test voltage was 3~4.5 V and the current density was 50 mA g -1 . Figure 5 The first three cyclic voltammetry curves of the prepared zLiF-V2O3 / C nanofiber composite material ( Fig.13 a), charge and discharge curve ( Fig.13 (b) The first charge and discharge specific capacities are 220.1 and 37.8 mAhg, respectively. -1 , showing good electrochemical performance.
[0047] Example 6
[0048] The steps of this example are exactly the same as those of Example 1, but polytetrafluoroethylene is not added. 5 mmol lithium nitrate and 2.5 mmol ammonium metavanadate are weighed and added to 10 ml deionized water and stirred in a constant temperature water bath at 70 °C for 1 h to obtain a yellow transparent solution. Then 0.8 g polyvinyl alcohol is added to the above solution and stirred at room temperature for 12 h until a yellow spinning precursor solution ( Fig.14 a). The obtained solution was transferred to a 10 ml electrospinning syringe and electrospun at 22 kV high voltage, with a spinning temperature of about 40 °C, a humidity of ﹤30%, and a spinning time of 4 h. Since no polytetrafluoroethylene was added, the solution itself had poor conductivity, resulting in an unstable spinning process, dripping of the spinning solution, and low filament yield. The spinning process could not proceed normally, so the spun fiber membrane could not be collected ( Fig.14 (b)
[0049] Example 7
[0050] The steps of this embodiment are exactly the same as those of embodiment 1, but electrospinning is not performed. The spinning precursor solution is directly dried and sintered. 5 mmol lithium nitrate and 2.5 mmol ammonium metavanadate are weighed and added to 10 ml deionized water and stirred in a constant temperature water bath at 70 °C for 1 h to obtain a yellow transparent solution. Then 0.8 g polyvinyl alcohol is added to the above solution and stirred at room temperature for 12 h to form a yellow spinning precursor solution. The spinning solution is dried at 80 °C ( Fig.15 a), and then placed in a N2 environment, pre-calcined at 280 °C for 3 h at a heating rate of 5 °C / min, and then calcined at 750 °C for 2 h to obtain a carbonized spinning solution ( Fig.15 b). The material was used to prepare a CR2025 battery according to the method of Example 1 for testing. The test voltage was 3-4.5 V and the current density was 50 mA g -1 . Figure 8 The first three cyclic voltammetry curves of the prepared unspun material ( Fig.16 a), charge and discharge curve ( Fig.16 (b) The first charge and discharge specific capacities are 78.6 and 30.8 mAh g -1 The electrochemical performance is significantly lower than that of zLiF-V2O3 / C nanofiber material obtained by electrospinning.
[0051] Example 8
[0052] In this embodiment, lithium nitrate and polytetrafluoroethylene were mixed and ground, and then sintered at high temperature to prepare LiF / C material, and its electrochemical performance was tested. 5 mmol lithium nitrate and 0.2 g polytetrafluoroethylene were weighed and ground evenly in a mortar, and then placed in a N2 atmosphere, pre-sintered at 280 °C for 3 h at a heating rate of 5 °C / min, and then calcined at 750 °C for 2 h to obtain LiF / C powder material ( Fig.17 a). The material was used to prepare a CR2025 battery according to the method of Example 1 for testing. The test voltage was 3-4.5 V and the current density was 50 mA g -1 The prepared material has no charge and discharge capacity ( Fig.17 (b)
[0053] Example 9
[0054] In this embodiment, polytetrafluoroethylene powder (a in FIG. 18 ) was sintered under N2. The sintering conditions were pre-sintering at 280°C for 3 h and then sintering at 750°C for 2 h. The results showed that polytetrafluoroethylene was completely carbonized and decomposed at high temperature, with almost no residue (b in FIG. 18 ). This shows that when polytetrafluoroethylene is used as a fluorine source, only when it combines with lithium ions at high temperature can fluorine atoms be retained in the material to form LiF, otherwise it will be completely decomposed into tetrafluoroethylene, perfluoropropylene, octafluorocyclobutane and other products that are taken away by N2.
Claims
1. A method for preparing lithium-ion battery material LiF-V2O3 / C, characterized in that: The steps include: (1) Add lithium nitrate and ammonium metavanadate to water and stir in a constant temperature water bath to obtain a transparent solution; add an appropriate amount of polyvinyl alcohol to the above solution and stir at room temperature until a yellow opaque solution is obtained; then add polytetrafluoroethylene aqueous dispersion and stir evenly to obtain an electrospinning precursor solution; (2) transferring the electrospinning precursor solution obtained in step (1) to obtain a flexible precursor fiber membrane through electrospinning; (3) The flexible precursor fiber membrane obtained in step (2) is dried and placed in a N2 environment, pre-fired at 250-300°C for 2-3h, and then calcined at 600-800°C for 1-3h to obtain a LiF-V2O3 / C nanofiber material for a negative electrode material of a lithium-ion battery.
2. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of lithium nitrate to ammonium metavanadate in the mixed solution is 1-3:1; the mass of deionized water accounts for 75-80% of the total mass; the mass of polyvinyl alcohol accounts for 6-7% of the total mass; and the mass fraction of the polytetrafluoroethylene aqueous dispersion is 50-65%.
3. The preparation method according to claim 1, characterized in that: The electrospinning conditions in step (2) are: voltage of 18-22 kV, ambient temperature of 40-50 °C, humidity <30%, spinning distance of 20 cm, and spinning time of 8-10 h.
4. The preparation method according to claim 1, characterized in that: After the electrospinning in step (3) is completed, the fabric is quickly transferred to a 60-80 °C oven for drying for 10-12 h; then placed in a tubular furnace with a sintering atmosphere of N2, a pre-sintering temperature of 280 °C, a heating rate of 5 °C / min, and a pre-sintering time of 3 h; then calcined at 750 °C for 2 h at a heating rate of 5 °C / min.
5. Use of the LiF-V2O3 / C prepared according to any one of claims 1 to 4 as a negative electrode material for lithium-ion batteries.
6. Use of the LiF-V2O3 / C prepared according to any one of claims 1 to 4 as a positive electrode material for lithium-ion batteries.
Citation Information
Patent Citations
Composite lithium ion battery positive electrode material and preparation method thereof
CN109638237A
Lithium fluoride / lithium lanthanum titanate nanofiber solid electrolyte interface material as well as preparation method and application thereof
CN112467200A